Method for detecting tribochemical reactions at the interface between abrasive grains and diamond wafer substrate

By coating a nanoindentation diamond indenter with active metal or metal oxide abrasive grains and using Raman spectroscopy, the method addresses the limitations of existing tribochemical reaction detection, enabling efficient and precise ultra-precision processing of semiconductor wafers.

JP7593690B2Active Publication Date: 2024-12-03HUAQIAO UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023547419
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-25
Filing Date
2021-12-31
Publication Date
2024-12-03
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

Existing methods for detecting interfacial tribochemical reactions between abrasive grains and diamond wafer substrates are limited to macroscopic conditions, failing to analyze atomic-level interactions and are not versatile enough to detect weak reactions, leading to inefficient and unsatisfactory processing of new semiconductor materials like silicon carbide, gallium nitride, and diamond.

Method used

A method involving coating the tip of a nanoindentation diamond indenter with an active metal or metal oxide abrasive grain layer using magnetron sputtering, scratching the diamond wafer substrate, and analyzing the scratched area with a scanning probe micro-Raman spectrometer to detect chemical components, optimizing parameters such as temperature and sputtering conditions for effective bonding and reaction detection.

Benefits of technology

Enables precise detection of tribochemical reactions at the atomic level, enhancing the efficiency and quality of ultra-precision processing of semiconductor wafers by controlling interfacial friction and chemical interactions, thus improving processing efficiency and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593690000001
    Figure 0007593690000001
  • Figure 0007593690000002
    Figure 0007593690000002
  • Figure 0007593690000003
    Figure 0007593690000003
Patent Text Reader

Abstract

The present invention discloses a method for detecting the interfacial tribochemical reaction between active metal or metal oxide abrasive grains and a diamond wafer substrate, by coating the surface of a nanoindentation diamond indenter with a shell of active metal abrasive grains or metal oxide with a uniform thickness by magnetron sputtering, controlling the interfacial action relationship between the abrasive grains and the wafer by scratching the diamond wafer substrate, and further detecting the chemical components in the interaction region on the surface of the diamond wafer substrate by a scanning probe micro-Raman spectrometer, thereby clarifying the mechanism of the interfacial tribochemical reaction between the active abrasive grains and the wafer substrate, which is simple in operation and has good prospects for application in the field of efficient ultra-precision machining of semiconductor wafer substrates.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the field of ultra-precision machining of semiconductor wafers, and in particular to a method for detecting tribochemical reactions between active metal abrasive grains and a diamond wafer substrate interface. [Background technology]

[0002] The advent of the electronic information age has greatly promoted the development of the semiconductor industry, and the generation of semiconductor materials is the key to the continued development of the electronic information industry. Conventional semiconductor power elements, represented by single crystal silicon, are approaching the limits of their material development, and it is becoming difficult to meet the new requirements for semiconductor devices, such as high frequency, high temperature, high power, high energy efficiency, environmental resistance, and small and lightweight. New semiconductor materials, represented by silicon carbide, gallium nitride, diamond, etc., have become the main force in the development of future semiconductor devices due to their excellent properties.

[0003] However, these new semiconductor materials have the characteristics of high hardness, high brittleness, and chemical stability, and are known as typical difficult-to-machine materials. Ultra-precision polishing technology follows the conventional method of polishing silicon wafers, namely, chemical mechanical polishing technology. Wafers made of these new semiconductor materials have a much higher hardness than silicon wafers, which leads to low processing efficiency, high processing costs, and unsatisfactory wafer surface quality. Therefore, a deep analysis of the interface action process between abrasive grains and wafers is helpful to understand the abrasive polishing removal mechanism of new semiconductor wafers, and further realize efficient ultra-precision damage-free processing of wafers made of new semiconductor materials.

[0004] Current countermeasure designs and detections of interfacial tribochemical reactions are mainly aimed at the interaction of different materials in a macro-contact system. For example, CN112147040A discloses an apparatus and method for detecting interfacial friction between hydrate monomers and sediments, CN104677783A discloses an electrochemical method for detecting the Al4C3 product after the reaction of aluminum with carbon to quantify the degree of aluminum-carbon interfacial reaction, and "Chemical modification of the interfacial frictional properties of vanadium carbide through ethanol adsorption" discloses the use of an atomic force microscope to detect the change in the frictional properties of vanadium carbide interfaces under ethanol adsorption conditions. The above prior art test methods have the following problems: (1) all of the examined interfacial tribochemical reactions occur under macro-conditions, making it difficult to analyze the interfacial frictional action occurring at the atomic level, (2) only interfacial tribochemical reactions occurring between specific materials can be detected, making them non-versatile, and (3) the above methods may fail when the interfacial tribochemical reactions are very weak. Summary of the Invention [Problem to be solved by the invention]

[0005] It is an object of the present invention to overcome the shortcomings of the prior art and to provide a method for detecting tribochemical reactions at the interface between active metal abrasive grains and a diamond wafer substrate. [Means for solving the problem]

[0006] A method for detecting an interface tribochemical reaction between an abrasive grain and a diamond wafer substrate, comprising: (1) Coating the tip surface of the diamond indenter of the nanoindentation with an active metal abrasive layer or a metal oxide abrasive layer by magnetron sputtering; (2) mounting a diamond indenter having an active metal abrasive layer on a nanoindenter, causing the diamond indenter to scratch the surface of a diamond wafer substrate, and obtaining a wafer substrate after scratching; (3) placing the indented substrate in a scanning probe Raman spectrometer to detect chemical components in the scratched area of ​​the scratched wafer substrate.

[0007] In a preferred embodiment of the present invention, the magnetron sputtering target comprises iron, cobalt, chromium and titanium to form the metallic abrasive layer.

[0008] In a preferred embodiment of the present invention, the target for magnetron sputtering includes copper, iron, zinc, cobalt, nickel and manganese, the reactive gas introduced is oxygen gas, and a metal oxide abrasive layer is formed.

[0009] More preferably, in the magnetron sputtering method, the diamond indenter fixed in the chamber is heated to 300 to 600° C., and the sputtering time is 4 to 6 minutes.

[0010] In a preferred embodiment of the present invention, the lubricating medium in scratching is deionized water at a temperature of 40-90°C.

[0011] More preferably, the temperature at said scratching is 50°C.

[0012] More preferably, in the scratching, the indentation load of the diamond indenter is 1 to 30 mN, and the scratching speed is 1 to 10 μm / s.

[0013] In a preferred embodiment of the present invention, the radius of curvature of the diamond indenter is 1 to 50 μm. More preferably, the radius of curvature of the diamond indenter is 25 μm. Effect of the Invention

[0014] The present invention uses magnetron sputtering to coat the surface of the diamond indenter of nanoindentation with a shell of active metal abrasive grains or metal oxides with a uniform thickness, controls the interfacial action relationship between the abrasive grains and the wafer through indentation experiments with the diamond wafer substrate, and uses a scanning probe Raman microscope to detect the chemical components in the interaction region on the surface of the diamond wafer substrate, thereby clarifying the mechanism of the interfacial tribochemical reaction between the active abrasive grains and the wafer substrate. The operation is simple, and has good application prospects in the field of efficient ultra-precision processing of semiconductor wafer substrates, and has industrial practicality. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic diagram of a diamond indenter having an active metal abrasive layer in Example 1 of the present invention and a scanning electron microscope photograph. [Diagram 2] FIG. 2 is a schematic diagram of scratches on the surface of a diamond wafer substrate caused by active metal abrasive grains in Example 1 of the present invention and Comparative Examples 1 to 3. [Diagram 3] 1 shows the detection results of scratch locations on a diamond wafer substrate surface caused by active metal abrasive grains in Example 1 of the present invention. [Figure 4] 1 shows scratching results of active metal abrasive grains having different adhesion forms in Comparative Example 1 of the present invention. [Diagram 5] 1 is a schematic diagram of a diamond indenter having an active metal oxide abrasive layer in Example 1 of the present invention and a scanning electron microscope photograph. [Figure 6] FIG. 2 is a schematic diagram of scratches on the surface of a diamond wafer substrate caused by active metal oxide abrasive grains in Example 1 of the present invention and Comparative Examples 1 to 3. [Figure 7] FIG. 2 shows the results of Raman detection of copper oxide abrasive grains in scratches on the surface of a diamond wafer substrate in Example 1 of the present invention. [Figure 8] FIG. 2 shows the results of Raman measurement of copper oxide abrasive grains in non-scratched areas on the surface of a diamond wafer substrate in Example 1 of the present invention. [Figure 9]1 shows the results of XRD measurement of a scratched portion of a diamond wafer substrate in Example 1 of the present invention. [Figure 10] 1 shows the results of scratching of active metal oxide abrasive grains with different deposition forms in Comparative Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0017] <Example 1> (1) The tip surface of the diamond indenter is coated with active abrasive grains of metallic titanium using the magnetron sputtering method. Specifically, a single metallic titanium with a purity of 99.99% is selected as the target, a diamond indenter with a curvature radius of 25 μm is fixed in the chamber, and the base pressure of the magnetron sputter wheel is set to 6.0 × 10 -5 The sputtering time was set to 5 minutes, and the diamond indenter was heated to 450°C, the radio frequency power was set to 100W, and the sputtering time was set to 5 minutes. As a result, the surface of the diamond indenter was coated with titanium metal active abrasive grains in a uniform thickness, and the shape of the diamond indenter coated with the titanium metal abrasive grain shell was as shown in Figure 1.

[0018] (2) The diamond indenter coated with the shell of the metal abrasive grain obtained in (1) above is attached to a nanoindentation device (KLA, model: Nano Indenter G200), and the indentation load is 10 mN, the scratching speed is 5 μm / s, and the lubricating medium for scratching is neutral deionized water with a pH of 7 and a temperature of 80° C. With the above parameters, a scratching test is performed on a diamond wafer substrate with reference to FIG.

[0019] (3) After the scratch test, the diamond wafer substrate is removed, and the chemical composition of the scratched area on the surface of the diamond wafer substrate is measured using a scanning probe Raman spectrometer (WITEC, a device that combines an atomic force microscope and a Raman spectrometer). As shown in Figure 3, the Raman spectrum shows that -1 In addition to the diamond peaks at the top, there are also 248, 345, 430 and 609 cm -1 It was found that a clear characteristic peak appeared at the location, confirming the presence of TiC, proving that a frictional chemical reaction induced by mechanical force occurred between the active metal abrasive titanium and the diamond wafer substrate, and that TiC was produced by a chemical reaction between the metallic titanium and diamond.

[0020] Those skilled in the art will appreciate that other metal abrasives (iron, cobalt, chromium) will react similarly to titanium and diamond to achieve the same and similar technical effects.

[0021] <Comparative Example 1> (1) Using the optical microscope of nanoindentation (same as in Example 1), attach active metal abrasive grains to a diamond indenter with a radius of curvature of 25 μm with 502 colloidal water, drip a small amount of 502 colloidal water evenly onto a slide glass, fix the slide glass on a table, move the table so that a small amount of colloidal water is attached to the surface of the diamond indenter, then move it further to the abrasive grain position, adjust the height of the indenter to attach the abrasive grains, and after 5 seconds of contact, raise the indenter to obtain a diamond indenter with active metal abrasive grains attached. The active metal abrasive grains are active metal titanium abrasive grains with a diameter of 50 μm.

[0022] (2) The diamond wafer substrate is scratched with the diamond indenter with the active metal abrasive grains obtained in step (1), the indentation load is 10 mN, the scratching speed is 5 μm / s, and the lubrication conditions for scratching are neutral deionized water with pH 7 and temperature 80 ° C. as the lubricating medium. With the above parameters, referring to FIG. 2, a scratch test of the diamond wafer substrate is performed. However, in the test, it was found that the attached abrasive grains are easily removed by the force, and an effective scratch test on the diamond wafer substrate cannot be performed. The main reason is that the bonding means of bonding the active metal abrasive grains with glue, as shown in FIG. 4, has too low a bonding strength between the active metal abrasive grains and the diamond indenter, so it is necessary to find a bonding means with a more reliable bonding strength. The method of coating the surface of the diamond indenter with a shell of active metal abrasive grains using the magnetron sputtering method of Example 1 is highly reliable and practical.

[0023] <Comparative Example 2> (1) Prepare five diamond indenters with a radius of curvature of 25 μm, and coat the surface of the diamond indenters with metallic titanium active abrasive grains at different sputtering temperatures. Select single metallic titanium with a purity of 99.99% as the target, fix the diamond indenters in the chamber, and set the base pressure of the magnetron sputtering wheel to 6.0 × 10 -5 Pa, the distance between the target and the diamond indenter is 5 cm. Five diamond indenters are heated to 280, 300, 450, 600, and 620 °C, respectively, with a radio frequency power of 100 W and a sputtering time of 5 minutes. That is, five sets of diamond indenters coated with titanium metal abrasive grains are obtained by changing the sputtering temperature.

[0024] (2) Scratch the diamond wafer substrate with the five sets of active metal abrasive grains sputtered from step (1), with a pressing load of 10 mN, a scratching speed of 5 μm / s, and a lubricating medium of neutral deionized water with a pH of 7 and a temperature of 80°C. With the above parameters, a scratch test of the diamond wafer substrate is performed with reference to FIG. 2. After the scratch test is completed, a phenomenon in which a part of the shell of the metallic titanium abrasive grain peels off is observed on the surface of the diamond indenter at 280°C, which indicates that the bonding strength of the interface between the shell of the abrasive grain and the diamond indenter is insufficient at this temperature, and the shell of the abrasive grain is easily peeled off under the force during scratching. When the sputtering temperature is 300°C, no shell peeling phenomenon is observed on the surface of the diamond indenter, which indicates that this is the lower limit of the sputtering temperature. When the sputtering temperature is 450°C and 600°C, no shell peeling phenomenon is observed on the surface of the diamond indenter, which indicates that the interfacial bonding between the shell and the diamond substrate is good. When the sputtering temperature is 620℃, the coating layer peels off over a large area on the diamond indenter surface, because the diamond is thermally damaged in a high-temperature (over 600℃) environment, and the interfacial bonding strength between the diamond surface and the abrasive coating layer is reduced. Through several sets of experiments, it has been determined that the suitable temperature range for sputtering the shell of metal titanium abrasive grains on the diamond indenter is 300-600℃.

[0025] <Comparative Example 3> (1) Prepare five diamond indenters with a radius of curvature of 25 μm, and coat the surfaces of the diamond indenters with metallic titanium active abrasive grains at the same sputtering temperature. Select single metallic titanium with a purity of 99.99% as the target, fix the diamond indenters in the chamber, and set the base pressure of the magnetron sputtering wheel to 6.0 × 10 -5 The sputtering temperature was set to 100 W, and the distance between the target and the diamond indenter was set to 5 cm. The diamond indenter was then heated to 450°C, and the radio frequency power was set to 100 W and the sputtering time to 5 minutes. That is, five sets of diamond indenters coated with titanium metal abrasive grains at the same sputtering temperature were obtained.

[0026] A diamond wafer substrate is scratched with five sets of diamond indenters sputtered with the same active metal abrasive grains obtained in step (1), with an indentation load of 10 mN, a scratching speed of 5 μm / s, and lubrication conditions for scratching, with neutral deionized water having a pH of 7 and temperatures of 35° C., 40° C., 50° C., 90° C., and 95° C., respectively, as the lubricating medium. With the above parameters and referring to FIG. 2, a scratch test of the diamond wafer substrate is performed. However, when the lubricating medium temperature is 35° C., the diamond peak (1331 cm ) is not observed in the Raman spectrum of the scratched area. -1 ) was observed, suggesting that this lubricant temperature is difficult to promote the chemical reaction between the active metal abrasive grains and diamond. When the lubricant temperature was 40 °C, only weak TiC signals (248, 345, 430, 609 cm) were observed in the Raman spectrum of the scratched area. -1 ) was detected, indicating that at this temperature, active metal titanium can chemically react with diamond, but the reactivity is low. When the lubricant temperature is 50℃ and 90℃, obvious TiC characteristic peaks appear in the Raman spectrum of the scratch area, but when the lubricant temperature is 95℃, the lubricant is easily volatilized, which raises certain safety concerns. Through multiple sets of experiments, it has been determined that the lubricant temperature range of 40 to 90℃ is the appropriate indentation temperature range.

[0027] <Example 2> (1) Using the magnetron sputtering method, the tip surface of a diamond indenter is coated with active abrasive grains of copper oxide. Specifically, a single metal copper with a purity of 99.99% is selected as the target, a diamond indenter with a curvature radius of 25 μm is fixed in a chamber, and the base pressure of the magnetron sputtering wheel is set to 6.0 × 10 -5 The reaction gas introduced was oxygen gas with a purity of 99.99%, the working gas pressure was 0.5 Pa, and the distance between the target and the diamond indenter was 5 cm. Next, the diamond indenter was heated to 450°C, and the radio frequency power was set to 100 W and the sputtering time to 5 minutes. As a result, the surface of the diamond indenter was coated with copper oxide abrasive grains of a uniform thickness, and the shape of the diamond indenter coated with a shell of copper oxide abrasive grains was as shown in Figure 5.

[0028] (2) The diamond indenter coated with the copper oxide abrasive shell obtained in (1) above is attached to a nanoindentation device (KLA, model: Nano Indenter G200), and the indentation load is 10 mN, the scratching speed is 5 μm / s, and the lubricating medium for scratching is neutral deionized water with a pH of 7 and a temperature of 80° C. Using the above parameters, a scratching test of the diamond wafer substrate is performed with reference to FIG.

[0029] (3) After the scratch test, the diamond substrate was peeled off and the chemical composition of the scratched and non-scratched areas on the diamond substrate surface was measured using a scanning probe Raman spectrometer (WITEC, an instrument that combines an atomic force microscope and a Raman spectrometer). As shown in Figures 7 and 8, the Raman spectrum showed no obvious characteristic signal in the scratched area, and a clear diamond characteristic peak was observed in the non-scratched area (1331 cm -1 ) It can be seen that the main reason is that the copper oxide abrasive grains and the diamond wafer substrate undergo a frictional chemical reaction due to mechanical force, causing a substitution reaction between the copper oxide and diamond, resulting in the metallic copper generated by the reaction adhering to the scratched area, and the metallic copper does not have a Raman characteristic peak and hides other signal peaks. This is common knowledge among those skilled in the art. Furthermore, as shown in Figure 9, when the chemicals in the scratched area were analyzed by XRD, significant signal peaks of copper and diamond elements were detected, confirming the analytical accuracy of the Raman results.

[0030] Those skilled in the art will know that other oxide abrasives (iron oxide, zinc oxide, cobalt oxide, nickel oxide, manganese oxide) will also undergo substitution reactions similar to the reaction between copper oxide and diamond, and the Raman spectrum detection results will be similar, with the same or similar effects being obtained.

[0031] <Comparative Example 4> (1) Using nanoindentation (same as in Example 1), attach copper oxide abrasive grains to a diamond indenter with a curvature radius of 25 μm using 502 colloidal water, drip a small amount of 502 colloidal water evenly onto a slide glass, fix the slide glass to a table, move the table so that a small amount of colloidal water is attached to the surface of the diamond indenter, then move it further to the abrasive grain position, adjust the height of the indenter to attach the abrasive grains, and after 5 seconds of contact, raise the indenter to obtain a diamond indenter with active metal abrasive grains attached. The diameter of the copper oxide abrasive grains is 50 μm.

[0032] (2) The diamond wafer substrate is scratched with the diamond indenter with the copper oxide abrasive grains obtained in step (1), the indentation load is 10 mN, the scratching speed is 5 μm / s, and the lubrication conditions for scratching are neutral deionized water with a pH of 7 and a temperature of 80° C. as the lubricating medium. With the above parameters, a scratch test of the diamond wafer substrate is performed as shown in FIG. 6. However, it is found that the attached abrasive grains are easily removed by the force during the experiment, and an effective scratch test cannot be performed on the diamond wafer substrate. As shown in FIG. 10, the main reason is that the bonding means of attaching the copper oxide abrasive grains with glue has too low a bonding strength between the copper oxide abrasive grains and the diamond indenter, so it is necessary to find a bonding means with a more reliable bonding strength. The method of coating the surface of the diamond indenter with a shell of copper oxide abrasive grains using the magnetron sputtering method in Example 2 is highly reliable and practical. Comparative Example 5

[0033] (3) Five diamond indenters with a radius of curvature of 25 μm are prepared, and the surface of the diamond indenter is coated with copper oxide active abrasive grains at different sputtering temperatures. As the target material, single metal copper with a purity of 99.99% is selected, the diamond indenter is fixed in the chamber, and the base pressure of the magnetron sputter wheel is set to 6.0 × 10 -5The reaction gas introduced is oxygen gas with a purity of 99.99%, the working gas pressure is 0.5 Pa, and the distance between the target and the diamond indenter is 5 cm. Five diamond indenters are heated to 280, 300, 450, 600, and 620 °C, respectively, with a radio frequency power of 100 W and a sputtering time of 5 minutes. That is, five sets of diamond indenters coated with copper oxide abrasive grains are obtained at different sputtering temperatures.

[0034] (4) Scratch the diamond wafer substrate with the diamond indenter coated with the five sets of copper oxide abrasive grains obtained in step (1), with an indentation load of 10 mN, a scratching speed of 5 μm / s, and a lubricating medium of neutral deionized water with a pH of 7 and a temperature of 80°C. With the above parameters, a scratch test of the diamond wafer substrate is performed with reference to FIG. 6. After the scratch test is completed, a phenomenon in which a part of the shell of the copper oxide abrasive grain peels off is observed on the surface of the diamond indenter at 280°C, which indicates that the bonding strength of the interface between the shell of the abrasive grain and the diamond indenter is insufficient at this temperature, and the shell of the abrasive grain is easily peeled off under the force during indentation. When the sputtering temperature is 300°C, no shell peeling phenomenon is observed on the surface of the diamond indenter, which indicates that this is the lower limit of the sputtering temperature. When the sputtering temperature is 450°C and 600°C, no shell peeling phenomenon is observed on the surface of the diamond indenter, which indicates that the interfacial bonding between the shell and the diamond substrate is good. When the sputtering temperature is 620℃, the diamond is thermally damaged in an oxygen atmosphere (high temperature above 600℃), and the interfacial bonding strength between the diamond surface and the coating layer of the abrasive grain is reduced, so a large area of ​​shell peeling is found on the diamond indenter surface. Through several sets of experiments, it was confirmed that the suitable temperature range for sputtering the shell of copper oxide abrasive grains onto the diamond indenter is 300-600℃.

[0035] <Comparative Example 6> (2) Prepare five diamond indenters with a radius of curvature of 25 μm, and coat the diamond indenter surfaces with copper oxide active abrasive grains at the same sputtering temperature. Select single metal copper with a purity of 99.99% as the target material, fix the diamond indenters in the chamber, and set the base pressure of the magnetron sputtering wheel to 6.0 × 10 -5 The reaction gas introduced is oxygen gas with a purity of 99.99%, the working gas pressure is 0.5 Pa, and the distance between the target and the diamond indenter is 5 cm. Next, the diamond indenter is heated to 450°C, the radio frequency power is set to 100 W, and the sputtering time is set to 5 minutes. That is, five sets of diamond indenters coated with copper oxide abrasive grains are obtained at the same sputtering temperature.

[0036] The diamond wafer substrate is scratched with five sets of diamond indenters coated with copper oxide abrasive grain layers at the same sputtering temperature obtained in step (1), the indentation load is 10 mN, the scratching speed is 5 μm / s, and the indentation lubrication conditions are neutral deionized water with pH 7 and set at 35 ° C, 40 ° C, 50 ° C, 90 ° C, and 95 ° C, respectively, as the lubricating medium. With the above parameters, the scratch test of the diamond wafer substrate is performed as shown in Figure 6. However, when the lubricating medium temperature is 35 ° C, the Raman spectrum of the scratched area shows a very obvious diamond signal, suggesting that copper oxide and diamond do not react with each other by substitution. When the lubricating medium temperature is 40 ° C, 50 ° C, and 90 ° C, there is no significant characteristic peak in the Raman spectrum of the scratched area, but a significant diamond characteristic peak appears in the Raman spectrum of the non-scratched area, suggesting that copper oxide and diamond undergo a substitution reaction, and the metallic copper produced by the reaction adheres to the diamond surface in the scratched area, so there is no significant signal in the Raman spectrum. When the lubricant temperature is 95℃, the lubricant is easily volatilized, which raises certain safety concerns. Through multiple experiments, it has been confirmed that the lubricant temperature range is 40 to 90℃.

[0037] The above description is merely a preferred embodiment of the present invention, and therefore the scope of the present invention cannot be limited thereby; that is, any equivalent changes and modifications based on the claims and the contents of the specification of the present invention fall within the comprehensive scope of the present invention. [Industrial Applicability]

[0038] The present invention discloses a method for detecting the interfacial tribochemical reaction between active metal or metal oxide abrasive grains and a diamond wafer substrate, by coating the surface of a diamond indenter of nanoindentation with a shell of active metal abrasive grains or metal oxide with a uniform thickness by magnetron sputtering, controlling the interfacial action relationship between the abrasive grains and the wafer by scratching test with the diamond wafer substrate, and detecting the chemical components on the interaction region of the surface of the diamond wafer substrate by a scanning probe micro-Raman spectrometer, thereby clarifying the mechanism of the interfacial tribochemical reaction between the active abrasive grains and the wafer substrate. The operation is simple, has good application prospects in the field of efficient ultra-precision processing of semiconductor wafer substrates, and has industrial practicality.

Claims

1. A method for detecting an interface tribochemical reaction between an abrasive grain and a diamond wafer substrate, comprising: (1) Coating the tip surface of a diamond indenter for nanoindentation with an active metal abrasive layer or a metal oxide abrasive layer by using a magnetron sputtering method; (2) mounting a diamond indenter having an active metal abrasive layer on a nanoindenter, causing the diamond indenter to scratch the surface of a diamond wafer substrate, and obtaining the wafer substrate after scratching; (3) A method for detecting an interfacial tribochemical reaction between an abrasive grain and a diamond wafer substrate, comprising the steps of: placing the scratched wafer substrate in a scanning probe Raman spectrometer and detecting chemical components in the scratched areas of the scratched wafer substrate.

2. 2. The method of claim 1, wherein the target for the magnetron sputtering method includes iron, cobalt, chromium and titanium, and the surface of the diamond indenter is coated with a metal oxide abrasive layer.

3. 2. The detection method according to claim 1, wherein the target of the magnetron sputtering method contains copper, iron, zinc, cobalt, nickel, and manganese, the reactive gas introduced is oxygen gas, and the surface of the diamond indenter is coated with a metal oxide abrasive layer.

4. The detection method according to claim 2 or 3, characterized in that in the magnetron sputtering method, the diamond indenter fixed in a working chamber is heated to 300 to 600°C, and the sputtering time is 4 to 6 minutes.

5. The detection method according to claim 1, characterized in that the lubricating medium in the scratch is deionized water at a temperature of 40-90°C.

6. 5. The method according to claim 4, wherein the temperature at the scratch is 50.degree.

7. 5. The detection method according to claim 4, wherein in the scratching, an indentation load of the diamond indenter is 1 to 30 mN, and a scratching speed is 1 to 10 μm / s.

Citation Information

Patent Citations

  • Device for implementing friction chemical reaction between abrasive and wafer substrate and implementing method thereof

    CN113084694A

  • Friction testing method and device therefor

    JP1998132731A

  • Probe microscope and frictional sliding, cmp, and hard disk inspection device including the same

    JP2011232177A

  • Apparatus and Method for In-Line Testing and Surface Analysis of Test Material with Participation of Raman Spectroscopy

    US20180344166A1