Mat material, exhaust gas purification device, and method for manufacturing the mat material

The mat material with surface-treated inorganic fibers addresses the retention issue in exhaust gas purification devices by enhancing friction coefficient, ensuring stable retention and reducing costs.

JP7594455B2Active Publication Date: 2024-12-04IBIDEN CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021020048
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-10
Publication Date
2024-12-04
Estimated Expiration
2041-02-10

AI Technical Summary

Technical Problem

Existing exhaust gas purification devices face issues with the retention of exhaust gas treatment bodies due to insufficient friction coefficient between the holding seal material and the metal casing, leading to potential dislodgment and increased manufacturing complexity and cost.

Method used

A mat material made of inorganic fibers with at least one surface-treated main surface to enhance friction coefficient, utilizing raised inorganic fibers to improve holding power without additional materials, achieved through processes like napping.

Benefits of technology

The surface-treated mat material effectively enhances the friction coefficient, ensuring stable retention of the exhaust gas treatment body, reducing manufacturing costs and complexity while maintaining high holding force.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594455000004
    Figure 0007594455000004
  • Figure 0007594455000005
    Figure 0007594455000005
  • Figure 0007594455000006
    Figure 0007594455000006
Patent Text Reader

Abstract

To provide a mat material capable of improving a friction coefficient of a surface.SOLUTION: A mat material made of inorganic fibers, has a first main surface and a second main surface located on the opposite side of the first main surface, where at least one of the first main surface and the second main surface is subjected to surface processing to change its surface state.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a mat material, an exhaust gas purification device, and a method for manufacturing the mat material. [Background technology]

[0002] Exhaust gas emitted from internal combustion engines such as diesel engines contains particulate matter (hereinafter referred to as PM), and in recent years, the harm that this PM poses to the environment and human body has become a problem. In addition, exhaust gas also contains harmful gas components such as CO, HC, and NOx, and there are concerns about the impact that these harmful gas components have on the environment and human body.

[0003] In response to this, various exhaust gas purification devices have been proposed that capture PM in exhaust gas and purify harmful gas components, and are composed of an exhaust gas treatment body made of porous ceramics such as silicon carbide and cordierite, a metal casing that houses the exhaust gas treatment body, and a retaining seal material (mat material) disposed between the exhaust gas treatment body and the metal casing. The main purpose of the retaining seal material (mat material) is to prevent the exhaust gas treatment body from coming into contact with the metal casing that covers its outer periphery and being damaged by vibrations and impacts caused by the running of the automobile, and to prevent exhaust gas from leaking from between the exhaust gas treatment body and the metal casing.

[0004] When high-pressure exhaust gas flows into such an exhaust gas purification device, the exhaust gas treatment body is pushed by the exhaust gas and falls off the metal casing, which is a problem.

[0005] Patent Document 1 describes that in order to improve the holding performance of the holding seal material, inorganic particles are attached to the surface of inorganic fibers constituting the holding seal material, thereby improving the friction coefficient of the holding seal material.

[0006] Furthermore, Patent Document 2 describes that in order to improve the holding performance of the holding seal material, the inorganic fibers that make up the holding seal material are compressed and fixed with an organic binder to form grooves on the surface, thereby improving the friction coefficient of the holding seal material. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2013-213463 A [Patent Document 2] JP 2017-31870 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present inventors measured the coefficient of friction between the holding sealer and the metal casing of the holding sealer described in Patent Document 1, and as a result, the coefficient of friction was smaller than expected. The present inventors speculate that the reason for this is as follows.

[0009] The holding seal material as described in Patent Document 1 is used so that its main surface is in contact with the metal casing. It is considered that frictional force is generated between the surface of the holding seal material that is in contact with the metal casing and the surface of the metal casing. However, when the surface of the holding sealer is viewed microscopically, the inorganic fibers constituting the holding sealer are entangled with one another, and therefore the surface of the holding sealer is not uniform. When the surface of the holding sealing material is viewed microscopically, the area occupied by the inorganic fibers on the surface of the holding sealing material is smaller than the area of ​​the mat material. Therefore, it is considered that the inorganic fibers are in contact with the surface of the metal casing in a point-like manner.

[0010] Furthermore, in Patent Document 1, inorganic particles are disposed on the surface of inorganic fibers. Since particles make point contact with a surface, it is considered that even if inorganic particles are disposed on the surface of inorganic fibers, the holding sealing material will make point contact with the surface of the metal casing.

[0011] When the holding sealer is in point contact with the surface of the metal casing, the actual contact area between the holding sealer and the surface of the metal casing is small, and in this case, the coefficient of friction between the holding sealer and the metal casing is smaller than the coefficient of friction when it is assumed that the holding sealer and the metal casing are in surface contact.

[0012] That is, for the reasons mentioned above, it is considered that when the holding sealing material described in Patent Document 1 is used, the coefficient of friction between the holding sealing material and the metal casing becomes smaller than expected.

[0013] Furthermore, attaching inorganic particles to inorganic fibers complicates the manufacturing process, increasing the manufacturing cost.

[0014] Furthermore, the present inventors measured the coefficient of friction between the holding sealer described in Patent Document 2 and the metal casing, but were unable to confirm any effect of improving the coefficient of friction.

[0015] The present invention has been made in view of the above problems, and has an object to provide a mat material capable of improving the surface friction coefficient. [Means for solving the problem]

[0016] That is, the mat material of the present invention is a mat material made of inorganic fibers, and is characterized in that the mat material has a first main surface and a second main surface located opposite the first main surface, and at least one of the first main surface and the second main surface has been subjected to a surface treatment to change the surface condition.

[0017] The mat material of the present invention has at least one of the first and second main surfaces subjected to surface treatment to change the surface condition, and therefore can improve the friction coefficient of the surface, particularly the surface to be processed of the first and second main surfaces that have been surface-treated. In addition, since no additional materials such as inorganic particles are required and the manufacturing process is simple, it is possible to reduce manufacturing costs.

[0018] In the mat member of the present invention, it is preferable that the first main surface and the second main surface are subjected to the surface treatment to change the surface state. Since each of the main surfaces is a processed surface that has been subjected to a surface treatment, the mat material can have a high coefficient of friction on each of the main surfaces.

[0019] In the mat member of the present invention, it is preferable that the surface to be processed, out of the first main surface and the second main surface, has raised inorganic fibers. This makes it possible to more suitably exhibit the effect of improving the friction coefficient. More specifically, when the processed surface has raised inorganic fibers, the fiber orientation is forced to change to a random orientation at the interface where friction occurs. This makes it difficult for the inorganic fibers to move in response to external forces, suppressing stepwise displacement and improving the holding force. As a result, the friction coefficient is effectively improved. As a result of measurements conducted by the present inventors, it has been confirmed that a mat material having brushed inorganic fibers on its main surface has a frictional force equal to or greater than that of a mat material having inorganic particles attached thereto, such as that described in Patent Document 1.

[0020] Here, "gradual displacement" means that the frictional resistance of the entire mat material decreases as a result of each inorganic fiber gradually displacing (moving) at the friction generating interface.

[0021] In the mat material of the present invention, it is preferable that the raised inorganic fibers form fiber agglomerates, and the fiber agglomerates are partially separated from the processed surface.

[0022] In the mat material of the present invention, it is preferable that the processed surface has a plurality of the fiber agglomerates, and that ends of the plurality of fiber agglomerates in the same direction are spaced apart from the processed surface. Such a mat material can be produced using a processing device such as a raising device, and therefore can be made into a mat material that is excellent in mass productivity.

[0023] In the mat material of the present invention, the friction coefficient of the processed surface of the first main surface or the second main surface that has been subjected to the surface treatment is 3 At 25° C., it is preferable that the ratio is 0.21 to 0.45.

[0024] In the mat material of the present invention, the bulk density of the first main surface and the second main surface near the processed surface that has been subjected to the surface processing is preferably smaller than the bulk density near the center in the thickness direction of the mat material.

[0025] In the mat material of the present invention, the bulk density of the first main surface and the second main surface in the vicinity of the processed surface on which the surface processing has been performed is 0.05 to 0.18 g / cm 3 The bulk density of the mat material near the center in the thickness direction is 0.11 to 0.20 g / cm 3 It is preferable that:

[0026] In the mat material of the present invention, the bulk density near the processed surface of the first main surface and the second main surface that has been subjected to the surface processing is preferably 45 to 95% of the bulk density near the center in the thickness direction of the mat material.

[0027] The exhaust gas purification device of the present invention is an exhaust gas purification device comprising an exhaust gas treatment body, a metal casing that houses the exhaust gas treatment body, and a mat material that is arranged between the exhaust gas treatment body and the metal casing and holds the exhaust gas treatment body, wherein the mat material is the mat material of the present invention.

[0028] As described above, the mat material of the present invention has the effect of improving the friction coefficient of the surface, and therefore, the exhaust gas purification device can be provided with an exhaust gas treatment body held with high holding force.

[0029] The manufacturing method of the mat material of the present invention is characterized by including a mat preparation step of preparing a mat made of inorganic fibers, and a surface processing step of applying a surface treatment to at least one of a first main surface of the mat and a second main surface of the mat located opposite the first main surface to change the surface condition.

[0030] In the method for producing a mat material of the present invention, it is preferable that in the surface processing step, at least one of the first main surface and the second main surface is subjected to a nap raising treatment.

[0031] In the method for producing a mat material of the present invention, the mat is preferably produced by a needling method in the mat preparation step. [Brief description of the drawings]

[0032] [Figure 1] FIG. 1 is a perspective view that illustrates an example of the mat material of the present invention. [Diagram 2] FIG. 2 is a perspective view that typically shows the state of the mat material shown in FIG. 1 before surface treatment is applied thereto. [Diagram 3] FIG. 3 is a schematic diagram showing the contact mechanism when a rough surface is pressed against a flat surface with a load W and a lateral force F is applied. [Figure 4] FIG. 4 is an enlarged perspective view typically showing a part of the processed surface of the mat material shown in FIG. [Diagram 5] FIG. 5 is a cross-sectional view that shows a schematic example of a needle mat that has not been surface-treated. [Figure 6] FIG. 6 is a cross-sectional view that illustrates an example of the mat material of the present invention. [Figure 7] FIG. 7 is a cross-sectional view that illustrates an example of an exhaust gas purification device of the present invention. [Figure 8]FIG. 8 is a plan view that illustrates the processed surface of the mat member of the second embodiment. [Figure 9] FIG. 9 is a schematic diagram showing an apparatus for measuring the friction coefficient of a mat material. [Figure 10] FIG. 10 is a schematic diagram showing an apparatus for measuring the friction coefficient of a mat material. [Figure 11] FIG. 11 is a graph showing the measurement results of the friction coefficients of the mat members in the examples and the comparative examples. [Figure 12] FIG. 12 is a photograph of the processed surface of the mat material of Example 2 observed with a microscope.

[0033] Detailed Description of the Invention The mat material of the present invention will be described in detail below. The mat material of the present invention is a mat material made of inorganic fibers, characterized in that the mat material has a first main surface and a second main surface located opposite the first main surface, and at least one of the first main surface and the second main surface has been subjected to a surface treatment to change the surface condition.

[0034] FIG. 1 is a perspective view that illustrates an example of the mat material of the present invention. FIG. 1 shows a mat material 1 of the present invention that is rectangular in plan view. The shape of the mat material 1 in plan view is not limited to a rectangle, and may be other shapes depending on the place where it is used. In addition, a convex portion 2a is provided at one longitudinal end 2 of the mat material 1, and a concave portion 3a is provided at the other longitudinal end 3 of the mat material 1 so that the ends fit together when the mat material 1 is wrapped around an object. If such convex portions 2a and concave portions 3a are provided, the mat material 1 has improved sealing properties when placed in an exhaust gas purification device, which will be described later. The mat material of the present invention does not necessarily have to have any protrusions or recesses at the ends of the mat material. The ends of the mat material may be L-shaped so that the ends fit together when the mat material is wrapped around the object.

[0035] The mat material 1 is made of inorganic fibers. The inorganic fiber is not particularly limited, and examples thereof include alumina fiber, alumina-silica fiber, silica fiber, biosoluble fiber, glass wool, rock wool, etc. Among these, alumina-silica fiber is preferable. These inorganic fibers have high heat resistance, and a mat material formed from such inorganic fibers is unlikely to change shape due to temperature changes.

[0036] Furthermore, when the inorganic fibers are alumina-silica fibers, the composition ratio of alumina and silica, by weight, is preferably alumina (Al2O3):silica (SiO2)=60:40 to 80:20, and more preferably alumina (Al2O3):silica (SiO2)=70:30 to 74:26.

[0037] The average fiber length of the inorganic fibers is preferably from 1 to 150 mm, and more preferably from 10 to 80 mm. If the average fiber length of the inorganic fibers is less than 1 mm, the fiber length is too short, resulting in insufficient entanglement of the inorganic fibers with each other, making it difficult to obtain sufficient strength for the mat material, and the shape retention of the mat material is likely to decrease. Furthermore, when the average fiber length of the inorganic fibers exceeds 150 mm, the fiber length of the inorganic fibers is too long, so the number of fibers constituting the mat material decreases, and the density of the mat material decreases, resulting in a decrease in the shear strength of the mat material.

[0038] The average fiber diameter of the inorganic fibers is preferably from 1 to 20 μm, more preferably from 2 to 15 μm, and further preferably from 3 to 10 μm. If the average fiber diameter of the inorganic fibers is less than 1 μm, the breaking load is low and the inorganic fibers are easily broken by impact or the like. If the average fiber diameter of the inorganic fibers exceeds 20 μm, defects are likely to occur inside the fibers, reducing the strength of the inorganic fibers and lowering the surface pressure value as a mat material for holding the exhaust gas treatment body.

[0039] The average fiber length and average fiber diameter of the inorganic fibers are determined by observing 100 inorganic fibers selected at random within the field of view of the mat material under a scanning electron microscope (SEM).

[0040] As shown in FIG. 1, the mat material 1 has a first main surface 4 and a second main surface 5 located opposite the first main surface 4, and the first main surface 4 and the second main surface 5 have been subjected to surface treatment to change the surface condition. This makes it possible to improve the coefficient of friction of the processed surface 6, which is the surface of the mat material 1 that has been subjected to the surface treatment. Moreover, the mat member 1 can be produced at low cost through a simple manufacturing process without using additional materials such as inorganic particles.

[0041] FIG. 2 is a perspective view that typically shows the state of the mat material shown in FIG. 1 before surface treatment is applied thereto. As shown in Figs. 1 and 2, the first main surface 4 and the second main surface 5 of the mat material 1 have their surface conditions changed by being subjected to a surface treatment.

[0042] The mat material 1 may have only one of the first main surface 4 and the second main surface 5 as a processed surface 6 that has been subjected to surface treatment, but as shown in Figures 1 and 2, it is preferable that the surface condition of the first main surface 4 and the second main surface 5 of the mat material 1 has been changed by being subjected to surface treatment. In other words, it is preferable that each of the main surfaces 4 and 5 is the surface 6 to be processed. This allows the mat material to have a high coefficient of friction on each of the main surfaces 4 and 5.

[0043] When each of the main surfaces 4, 5 is a surface to be processed 6, the first main surface 4 and the second main surface 5 may be subjected to different types of surface treatments, but are usually subjected to the same type of surface treatment (preferably brushing).

[0044] As shown in FIG. 1, of the first main surface 4 and the second main surface 5, the surface-treated surface 6 preferably has raised inorganic fibers 10. This makes it possible to more suitably exhibit the effect of improving the friction coefficient. Such a processed surface 6 can be effectively formed by carrying out a nap raising treatment as the above-mentioned surface treatment.

[0045] Here, the function and effect of the raised inorganic fibers 10 will be described in more detail with reference to FIG. First, in a general elastic body such as a mat material, the mechanism by which a holding force is generated is as follows. FIG. 3 is a schematic diagram showing the contact mechanism when a rough surface is pressed against a flat surface with a load W and a lateral force F is applied. F (holding force) is generally expressed as W (surface pressure) × μ (friction coefficient). In the case of an elastic body such as a mat material, as shown in Figure 3, when each protrusion of the elastic body E is pressed against a plane P with a load W, the contact pressure p n The tip of the protrusion is deformed, and the contact area A n In order to form a contact surface of , the shear force τ of the real contact point (each protrusion) where friction occurs is expressed as follows (1): n ×A n The sum of these is F (retentive force). F=τ1×A1+τ2×A2+τ3×A3+···=Στ n ×A n (1) Here, τ n indicates the average shear force of each protrusion, and n indicates the number of each protrusion. Therefore, if a step misalignment occurs between the protrusions, the stress of the protrusion is relaxed and the shear force decreases or disappears, resulting in a decrease in F (holding force).

[0046] The coefficient of friction of the elastic body is μ M is expressed by the following equation (2). μ M =μ K +C(μ S -μ K )W -1 / 3 (2) Here, μ K indicates the coefficient of kinetic friction, and μ S denotes the static friction coefficient, W denotes the load, and C denotes the stiffness.

[0047] On the other hand, when the processed surface of the mat material of the present invention has raised inorganic fibers, the fiber orientation is forced to change to a random orientation at the interface where friction occurs. Therefore, the inorganic fibers are less likely to move in response to external forces, and stepwise displacement is suppressed, making it possible to improve the holding force F. As a result, the friction coefficient is effectively improved.

[0048] FIG. 4 is an enlarged perspective view typically showing a part of the processed surface of the mat material shown in FIG. As shown in FIG. 4, the raised inorganic fibers 10 form fiber agglomerates 11, and the fiber agglomerates 11 are preferably partially spaced apart from the surface 6 to be processed.

[0049] The term "fiber aggregate" used herein means a fiber aggregate in which a plurality of inorganic fibers are integrated together. The fiber mass 11 is formed when inorganic fibers on the work surface 6 are caught by a needle and partially peeled off from the work surface 6. Therefore, the fiber agglomerations 11 and other inorganic fibers (for example, inorganic fibers at the center in the thickness direction of the mat material) basically differ only in the fiber orientation direction. However, since fiber agglomeration 11 is formed by being hooked on a needle, there is usually a low-density part 12 of inorganic fibers in its center, as shown in Fig. 4. In other words, the center part of fiber agglomeration 11 may have a lower density of inorganic fibers than the surrounding area. By having the low-accumulation portion 12 at the center of the fiber agglomerate 11, it is possible to more effectively improve the coefficient of friction. On the other hand, if the fiber agglomerate 11 does not have the low-accumulation portion 12 at the center and has a uniform overall accumulation degree (density), the fiber agglomerate 11 will become a hard mass, and there is a risk that the effect of improving the coefficient of friction will not be effectively obtained. In addition, the presence of the low-accumulation portion 12 allows the fiber mass 11 to absorb the shock of pressure when assembling the exhaust gas treatment body and the mat material in the manufacturing process of the exhaust gas purification device, thereby preventing the mat material body from being damaged. On the other hand, if the fiber agglomeration 11 is a hard mass without the low-pile portion 12 in the center, the fiber agglomeration 11 may press against the main body of the mat material during assembly, destroying the inorganic fibers of the main body of the mat material.

[0050] As shown in FIG. 4, the work surface 6 of the mat material has a plurality of fiber agglomerates 11, and it is preferable that the ends 13 of the plurality of fiber agglomerates 11 in the same direction D are spaced apart from the work surface 6. In other words, it is preferable that one end 13 of fiber agglomerate 11 in a certain direction D is separated from the work surface 6, and the other end 14 of fiber agglomerate 11 in the same direction D is integrated with work surface 6 without being separated from same. Such a mat material can be produced using a processing device such as a raising device, and therefore can be made into a mat material that is excellent in mass productivity.

[0051] In addition, in FIG. 4, the direction D in which the end portion 13 away from the work surface 6 is oriented is shown as the longitudinal direction of the mat material, but the direction D is not particularly limited and can be set as appropriate.

[0052] In the mat material of the present invention, the friction coefficient of the surface to be processed, which is one of the first main surface and the second main surface, is 0.3 g / cm 3 At 25° C., the viscosity is preferably 0.21 to 0.45, and more preferably 0.23 to 0.45.

[0053] When each main surface is a surface to be processed, the friction coefficients of the first main surface and the second main surface may be different from each other. However, from the viewpoint of simple production using the same processing device, it is preferable that they are substantially the same.

[0054] In the mat material of the present invention, the bulk density in the vicinity of the surface to be processed is preferably smaller than the bulk density in the vicinity of the center in the thickness direction of the mat material.

[0055] More specifically, the bulk density of the mat material of the present invention near the processed surface is 0.05 to 0.18 g / cm 3 The bulk density of the mat material near the center in the thickness direction is 0.11 to 0.20 g / cm3 It is preferable that the bulk density in the vicinity of the processed surface is 0.05 to 0.14 g / cm 3 The bulk density of the mat material near the center in the thickness direction is 0.11 to 0.20 g / cm 3 It is more preferable that: More specifically, in the mat material of the present invention, the bulk density in the vicinity of the processed surface is preferably 45 to 95%, and more preferably 60 to 90%, of the bulk density in the vicinity of the center in the thickness direction of the mat material. Here, the bulk density near the processed surface refers to the bulk density of the processed portion (the portion including the processed surface) when the mat material is divided into thirds in the thickness direction, and the bulk density near the center of the thickness direction of the mat material refers to the bulk density in the center portion (the portion not including the processed surface) when the mat material is divided into thirds in the thickness direction.

[0056] When each main surface is a surface to be processed, the bulk densities in the vicinity of the first main surface and the second main surface may be different from each other, but from the viewpoint of simple production using the same processing equipment, it is preferable that they are substantially the same.

[0057] The mat material of the present invention may be a mat produced by a papermaking method (hereinafter referred to as a papermaking mat) that has been surface-treated, but it is preferable that the mat material is a mat produced by a needling method (hereinafter referred to as a needle mat) that has been surface-treated. When a needle mat is used, it is possible to obtain a more effective improvement effect on the coefficient of friction than when a paper-formed mat is used. The reasons for this will be explained in detail below with reference to FIGS. FIG. 5 is a cross-sectional view that shows a schematic example of a needle mat that has not been surface-treated. FIG. 6 is a cross-sectional view that illustrates an example of the mat material of the present invention. 5 and 6 show cross sections of a portion that has not been needle punched. In addition, the upper right corner of FIG. 6 shows a partially enlarged view of the processed surface of the mat material.

[0058] The needle mat is basically produced by laminating fibers in a cross layer, so that the inorganic fibers 10 oriented in the in-plane direction of the mat are oriented so as to overlap in the thickness direction of the mat, as shown in FIG. For this reason, it is believed that each inorganic fiber 10 is likely to move, and step misalignment is likely to occur at the interface where friction occurs, and the holding force is likely to decrease.

[0059] However, as shown in Fig. 6, in the mat material 1 manufactured by the needling method and having a brushed surface 6, the orientation of the inorganic fibers 10 is forced to change to a random orientation at the interface where friction occurs, as shown in the enlarged view of Fig. 6. Therefore, the inorganic fibers are less likely to move in response to an external force, and stepwise displacement can be effectively suppressed, making it possible to significantly improve the holding force F.

[0060] On the other hand, the fiber orientation of the papermaking mat is less biased than that of the needle mat, so the inorganic fibers are less likely to move and stepwise displacement is less likely to occur. Therefore, the effect of improving the friction coefficient by the nap raising treatment is smaller than that of the needle mat.

[0061] Next, a method for producing the mat material of the present invention will be described. The manufacturing method of the mat material of the present invention is characterized by including a mat preparation step of preparing a mat made of inorganic fibers, and a surface processing step of applying a surface treatment to at least one of a first main surface of the mat and a second main surface of the mat located opposite the first main surface to change the surface condition.

[0062] The inorganic fiber mat can be obtained by various methods, for example, a papermaking method or a needling method, but it is preferable to produce it by the needling method, which can more effectively improve the friction coefficient as described above, compared to the case where the mat is produced by the papermaking method. In the case of the papermaking method, the paper can be produced, for example, by the following method. The inorganic fibers are opened and dispersed in a solvent to obtain a mixture. The mixture is poured into a molding machine having a filtering mesh formed on the bottom surface, and the solvent in the mixture is removed to obtain an inorganic fiber aggregate. The inorganic fiber aggregate is then dried to obtain a mat. In the case of the needling method, the production can be carried out, for example, by the following method. A spinning mixture made of a basic aluminum chloride aqueous solution and silica sol or the like is spun by a blowing method to produce an inorganic fiber precursor. The inorganic fiber precursor is then compressed to produce a continuous sheet-like product of a predetermined size, and a mat is obtained by subjecting the product to a firing treatment. A needle punching treatment is performed either before or after the firing treatment to entangle the inorganic fibers.

[0063] The thickness of the mat is not particularly limited, but is preferably from 2 to 40 mm, and more preferably from 5 to 20 mm. If the thickness of the mat is less than 2 mm, the retaining force of the mat material will be insufficient, and the exhaust gas treatment body will easily fall off. If the thickness of the mat exceeds 40 mm, the mat loses its flexibility, making it difficult to handle when wrapping the mat material around the exhaust gas treatment body. In addition, the mat material is prone to wrinkles and cracks.

[0064] Next, a surface treatment step is performed in which at least one of a first main surface of the mat and a second main surface of the mat located on the opposite side to the first main surface is subjected to a surface treatment to change the surface state.

[0065] In the method for producing a mat material of the present invention, it is preferable that in the surface processing step, at least one of the first main surface and the second main surface is subjected to a nap raising treatment. This makes it possible to generate raised inorganic fibers on the first main surface and / or the second main surface, so that the effect of improving the coefficient of friction as described above is more suitably exhibited. The specific means for performing the nap raising treatment is not particularly limited, and examples thereof include a treatment device such as a nap raising device, sandpaper, etc. The nap raising treatment may also be performed manually with a needle. From the viewpoint of mass productivity, it is preferable to carry out the raising treatment using a treatment device such as a raising device. The raising device, for example, has one or more rollers wrapped with cardboard clothing having a large number of needles, and the mat is run over the roller while rotating, thereby scraping out the inorganic fibers from the main surface of the mat.

[0066] The exhaust gas purification device of the present invention will be described below. The exhaust gas purification device of the present invention is an exhaust gas purification device comprising an exhaust gas treatment body, a metal casing that houses the exhaust gas treatment body, and a mat material that is arranged between the exhaust gas treatment body and the metal casing and holds the exhaust gas treatment body, wherein the mat material is the mat material of the present invention.

[0067] As described above, the mat material of the present invention has an effect of improving the friction coefficient of the surface. Therefore, the exhaust gas treatment device of the present invention can be an exhaust gas purification device in which the exhaust gas treatment body is held with high holding force.

[0068] FIG. 7 is a cross-sectional view that illustrates an example of an exhaust gas purification device of the present invention. As shown in FIG. 7, the exhaust gas purification device 100 of the present invention comprises a metal casing 50, an exhaust gas treatment body 40 housed in the metal casing 50, and a mat material 1 disposed between the exhaust gas treatment body 40 and the metal casing 50 and holding the exhaust gas treatment body 40.

[0069] The exhaust gas treatment body 40 has a columnar shape in which a large number of cells 41 are arranged in parallel in the longitudinal direction with cell walls 42 separating them. In addition, if necessary, an inlet pipe for introducing exhaust gas discharged from the internal combustion engine and an exhaust pipe for discharging exhaust gas that has passed through the exhaust gas purification device to the outside will be connected to the end of the metal casing 50.

[0070] A case where exhaust gas passes through the exhaust gas purification device 100 having the above-mentioned configuration will be described below with reference to FIG. As shown in Fig. 7, exhaust gas discharged from an internal combustion engine and flowing into the exhaust gas purification device 100 (in Fig. 7, the exhaust gas is indicated by G and the flow of the exhaust gas is indicated by arrows) flows into one cell 41 opening into the exhaust gas inlet end face of the exhaust gas treatment body (honeycomb filter) 40, and passes through a cell wall 42 separating the cells 41. At this time, PM in the exhaust gas is captured by the cell wall 42, and the exhaust gas is purified. The purified exhaust gas flows out from the other cell 41 opening into the exhaust gas outlet end face, and is discharged to the outside.

[0071] In the exhaust gas purification device 100 shown in FIG. 7, the mat material 1 is the mat material of the present invention, and it is preferable that the first and second main surfaces of the mat material 1 are both processed surfaces whose surface conditions have been changed by surface treatment (preferably brushing treatment).

[0072] The material of the metal casing constituting the exhaust gas purification device of the present invention is not particularly limited as long as it is a heat-resistant metal, and specific examples thereof include metals such as stainless steel, aluminum, and iron.

[0073] The shape of the casing may be a substantially cylindrical shape, a clamshell shape, or a substantially elliptical or polygonal shape in cross section.

[0074] 7 is a filter in which one end of the cell 41 is sealed with a sealing material 43, but the exhaust gas treatment body constituting the exhaust gas purifying device of the present invention may not have sealed ends of the cells. Such an exhaust gas treatment body can be suitably used as a catalyst carrier.

[0075] The exhaust gas treatment body 40 may be made of a non-oxide porous ceramic such as silicon carbide or silicon nitride, or may be made of an oxide porous ceramic such as alumina, cordierite, mullite, etc. Among these, silicon carbide is preferable.

[0076] The cell density in the cross section of the exhaust gas treatment body 40 is not particularly limited, but the preferred lower limit is 31.0 cells / cm 2 (200 pieces / inch 2 ), the preferred upper limit is 93.0 particles / cm 2 (600 pieces / inch 2 ) A more preferable lower limit is 38.8 particles / cm 2 (250 pieces / inch 2 ), and a more preferable upper limit is 77.5 particles / cm 2 (500 pieces / inch 2 ).

[0077] The exhaust gas treatment body 40 may support a catalyst for purifying the exhaust gas. The catalyst to be supported is preferably a precious metal such as platinum, palladium, or rhodium, and among these, platinum is more preferable. In addition, other catalysts such as alkali metals such as potassium or sodium, or alkaline earth metals such as barium may also be used. These catalysts may be used alone or in combination of two or more kinds. When these catalysts are supported, PM can be easily burned and removed, and toxic exhaust gas can also be purified.

[0078] (Example) EXAMPLES Hereinafter, examples that more specifically disclose the present invention will be described, however, the present invention is not limited to these examples.

[0079] Example 1 A mat made of inorganic fibers (mullite fibers) was prepared by a needling method. This mat was punched out into a square with sides of 50 mm. The mat had a thickness of 8.5 mm, and the inorganic fibers constituting the mat had fiber lengths of 1 to 150 mm, an average fiber length of 10 mm, and an average fiber diameter of 5.5 μm.

[0080] Next, one main surface of the mat punched into a square was uniformly processed with sandpaper (grit 150) and the nap-raising treatment was repeated three times to produce the mat material of Example 1.

[0081] Example 2 FIG. 8 is a plan view that illustrates the processed surface of the mat member of the second embodiment. The mat used in Example 1 was punched out into a square with each side measuring 50 mm. Next, one main surface of the mat punched into a square was subjected to a nap raising treatment using a needle having a diameter of 1 mm, thereby producing a mat material of Example 2. In detail, a needle was manually inserted obliquely into the main surface to a depth of about 2 mm and then pulled up to scratch out the inorganic fibers on the main surface, and this process was carried out at intervals of about 3 mm across the entire main surface, as shown in Figure 8.

[0082] Comparative Example 1 The mat used in Example 1 was punched out into a square with each side measuring 50 mm, and the resulting material was used as is.

[0083] (Measurement of coefficient of friction) The friction coefficients of the mat materials of the examples and comparative examples were measured by the following method. 9 and 10 are schematic diagrams showing a friction coefficient measuring device for a mat material. In the friction coefficient measuring device 200, stainless steel flat plates (a left plate 210 and a right plate 220) are arranged on the left and right sides of the device so as to face each other.

[0084] First, the two mat materials 1a and 1b and the middle plate 230 were arranged in the following order: left plate 210, mat material 1a, stainless steel flat plate (middle plate 230), mat material 1b, and right plate 220. Protruding members 240 are provided on the surfaces of the left plate 210 and the right plate 220 to prevent slippage between the left plate 210 and the mat material 1a, and between the right plate 220 and the mat material 1b (between the plates and the mat materials). In the mat material of the embodiment, the surface that was subjected to the nap-raising process was placed on the side of the middle plate 230. The mat material 1 a is sandwiched between the left plate 210 and the middle plate 230 , and the mat material 1 b is sandwiched between the middle plate 230 and the right plate 220 . Furthermore, the middle plate 230 is a load cell, and the load applied to the middle plate can be measured.

[0085] First, pressure is applied to the left plate 210 and the right plate 220 in the direction of the middle plate 230, and the bulk density (GBD) of the mat material is 0.3 g / cm 3 It was compressed until The compressed state was maintained (relaxed) for 10 minutes.

[0086] Next, with the temperature between the mat material and the middle plate being 25°C, 100°C, 200°C or 300°C, the middle plate 230 was moved in the direction indicated by the arrow in Figure 10 (upward) at a speed of 25 mm / min, and a shear stress was applied to the main surface of the mat material. FIG. 10 shows the state in which the middle plate has been moved. The direction in which the mid-plate is moved is the same as the direction in which the shear stress is applied to the main surface of the mat material on the side in contact with the mid-plate. The load value of the load cell during movement and the static friction force acting on the middle plate were measured, and the coefficient of friction when the static friction force was at its maximum (static friction coefficient) was measured.

[0087] (Measurement of bulk density) First, a mat material was punched out into a square with sides of 50 mm and cut into three equal parts in the thickness direction. Next, the weight and thickness of each of the three cut mat pieces were measured. The thickness was measured using a dial gauge (measurement probe φ20 mm, load 4.9 kPa). Then, the bulk density near the processed surface (processed portion) and the bulk density near the center of the thickness of the mat material (central portion) were calculated from the surface specific gravity (weight / area) calculated from the weight, as shown in the formula below. (weight / area) / thickness = bulk density [g / cm 3 ]

[0088] FIG. 11 and Table 1 show the measurement results of the friction coefficients of the mat materials in the examples and comparative examples. Table 2 also shows the ratio of the friction coefficient of the mat material of the embodiment to the friction coefficient of the mat material of the comparative example.

[0089] [Table 1]

[0090] [Table 2]

[0091] As shown in FIG. 11 and Tables 1 and 2, the mat material of the embodiment having a brushed surface has a higher friction coefficient than the mat material of the comparison example having no surface treatment, and it was confirmed that the friction coefficient was improved by 5% or more. Furthermore, the mat member of the embodiment does not require any additional materials and the manufacturing process is simple, so that it can be manufactured at low cost.

[0092] Table 3 shows the measurement results of the bulk density of the mat material in the examples and comparative examples. Table 3 also shows the results of calculating the ratio of the bulk density of the processed part (the upper part in Comparative Example 1) to the bulk density of the center part in each example and comparative example.

[0093] [Table 3]

[0094] As shown in Table 3, in the mat material of the comparative example that had no surface treatment, the bulk density was similar at the top and center, and the entire mat material had a uniform bulk density, whereas in the mat material of the example that had a brushed surface, the bulk density of the processed part was lower than that of the center, and it was confirmed that the bulk density decreased near the brushed processed surface.

[0095] (Surface observation) Fig. 12 is a photograph of the processed surface of the mat material of Example 2 observed with a microscope. In Fig. 12, the state before the surface processing by the nap raising treatment is shown on the left side, and the state after the surface processing by the nap raising treatment is shown on the right side. As shown in Figure 12, the mat material of the embodiment having a brushed surface has inorganic fibers 10 brushed on the work surface 6, and it was confirmed that these brushed inorganic fibers 10 form fiber agglomerates 11 partially separated from the work surface 6. Furthermore, many of the fiber agglomerates 11 had low-density portions 12 in their centers where the density of inorganic fibers was lower than that of the surrounding areas. [Explanation of symbols]

[0096] 1 Mat material 1a Mat material 1b Mat material 2 One end 2a Convex part 3 The other end 3a Recess 4 First main surface 5 Second main surface 6 Processed surface 10 Inorganic Fibers 11 Fiber mass 12 Low concentration area 13 One end of the fiber mass 14 The other end of the fiber mass 40 Exhaust gas treatment body 41 Cell 42 Cell Wall 43 Encapsulating materials 50 Metal Casing 100 Exhaust gas purification equipment 200 Friction coefficient measuring device 210 Left board 220 Right plate 230 Middle Plate 240 Protruding parts G. Exhaust gas

Claims

1. A mat material made of inorganic fibers, The mat material has a first main surface and a second main surface located opposite to the first main surface, At least one of the first main surface and the second main surface is surface-treated to have inorganic fibers raised on the surface to be treated; The raised inorganic fibers form a fiber mass, and a low-density portion of the inorganic fibers is present in the center of the fiber mass.

2. 2. The mat member according to claim 1, wherein the first main surface and the second main surface have a surface condition changed by the surface treatment.

3. The mat material according to claim 1 , wherein the fiber agglomerates are partially spaced apart from the surface to be processed.

4. The processed surface has a plurality of the fiber agglomerates, The mat material according to claim 3 , wherein ends of the plurality of fiber agglomerates in the same direction are spaced apart from the surface to be processed.

5. The friction coefficient of the surface to be processed of the first main surface and the second main surface is such that the bulk density of the mat material is 0.3 g / cm 3 5. The mat material according to claim 1, wherein the viscosity at 25° C. is 0.21 to 0.

45.

6. A mat material according to any one of claims 1 to 5, wherein the bulk density of the first main surface and the second main surface near the processed surface on which the surface processing has been performed is smaller than the bulk density near the center of the thickness direction of the mat material.

7. The bulk density of the first main surface and the second main surface in the vicinity of the processed surface on which the surface processing is performed is 0.05 to 0.18 g / cm 3 and The bulk density of the mat material near the center in the thickness direction is 0.11 to 0.20 g / cm 3 The mat material according to any one of claims 1 to 6, wherein

8. A mat material according to any one of claims 1 to 7, wherein the bulk density of the first main surface and the second main surface near the processed surface on which the surface processing has been performed is 45 to 95% of the bulk density near the center in the thickness direction of the mat material.

9. An exhaust gas treatment body; A metal casing that houses the exhaust gas treatment body; An exhaust gas purification apparatus comprising: a mat material disposed between the exhaust gas treatment body and the metal casing and holding the exhaust gas treatment body, 9. An exhaust gas purification device, comprising the mat material according to claim 1.

10. A mat preparation step of preparing a mat made of inorganic fibers; a surface treatment step of performing a surface treatment on at least one of a first main surface of the mat and a second main surface of the mat located opposite to the first main surface to change a surface state; A method for producing a mat material, comprising: In the surface processing step, a needle is inserted obliquely into at least one of the first and second main surfaces and then pulled up to scrape out the inorganic fibers, so that the raised inorganic fibers form a fiber mass and a low-density portion of the inorganic fibers is present in the center of the fiber mass. This is a method for manufacturing a mat material.

11. The method for producing a mat material according to claim 10, wherein in the mat preparation step, the mat is produced by a needling method.

Citation Information

Patent Citations

  • Structure for purifying exhaust gas

    JP1990061313A

  • Holding sealant and catalytic converter using the same

    JP2003214156A

  • Mat material, method for manufacturing mat material, muffler, and method for manufacturing muffler

    JP2010096171A

  • Holding sealing material, and exhaust emission control device

    JP2013213463A

  • Holding material for contamination control element, method of manufacturing the same, and contamination control device

    JP2015222064A