Optical thin film manufacturing method
The method of forming a mixed silicon oxide and titanium oxide thin film with controlled vacuum evaporation and sputtering addresses the hydrophilicity loss issue, ensuring sustained hydrophilicity and photocatalytic function, while maintaining a low refractive index.
Patent Information
- Application Number
- JP2023063847
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-04-18
- Filing Date
- 2023-04-11
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-04-11
AI Technical Summary
Existing optical thin films made of silicon oxide lose hydrophilicity when exposed to high temperature and high humidity due to the attachment of CH groups, and they lack a photocatalytic function.
A method involving vacuum evaporation using silicon oxide and sputtering with titanium or titanium oxide to form a mixed film with a contact angle of 10° or less, a refractive index of 1.44 or less, and a photocatalytic function, using a film forming apparatus that maintains different vacuum regions for simultaneous or alternating film formation.
The method produces an optical thin film with sustained hydrophilicity and photocatalytic function, capable of decomposing CH groups under UV irradiation, maintaining low refractive index and preventing fogging.
Smart Images

Figure 0007594760000002 
Figure 0007594760000003 
Figure 0007594760000004
Abstract
Description
[Technical field]
[0001] The present invention is an optical thin Membrane The present invention relates to a method for producing an optical thin film that is excellent in hydrophilicity and can suppress the decrease in hydrophilicity or restore the hydrophilicity. Membrane It relates to a manufacturing method. [Background technology]
[0002] When exposed to ultraviolet light, titanium oxide is excited and the surface of the thin film is covered with hydrophilic groups (-OH), which causes hydrophilicity. As a result, water droplets on the surface of the hydrophilic thin film made of titanium oxide become a thin layer of water, which prevents the diffuse reflection of light caused by water droplets and prevents fogging. In addition, hydrophilic thin films have a self-cleaning effect in which the hydrophilized water lifts and removes dirt that has adhered to the surface. Furthermore, since the evaporation surface area of hydrophilized water is large, hydrophilic thin films have a cooling effect in that they efficiently remove the latent heat of evaporation from materials that come into contact with them as they evaporate, thereby lowering the temperature of the materials. Such hydrophilic thin films are used in a wide range of fields, such as automobile side mirrors, road convex mirrors, exterior building materials for buildings and houses, tiles, and blinds.
[0003] However, when the thin film made of titanium oxide is no longer irradiated with ultraviolet light, the titanium oxide that was excited returns to its original ground state, the hydrophilic groups (-OH) on the surface decrease, the contact angle of water gradually increases, and the film returns from the hydrophilic state to the original hydrophobic state. In this hydrophobic state, the above-mentioned anti-fogging properties and self-cleaning effects cannot be expected. Titanium oxide is also a high refractive index material.
[0004] On the other hand, it is known that a thin film made of silicon oxide with a low refractive index can be formed by repeating deposition and sputtering (Patent Document 1). According to Patent Document 1, when the degree of vacuum of the deposition atmosphere decreases, the density of the film decreases, and the thin film becomes porous, which decreases the refractive index. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-123365 A Summary of the Invention [Problem to be solved by the invention]
[0006] A thin film made of silicon oxide formed by the method described in Patent Document 1 is presumed to exhibit high hydrophilicity because the film structure is porous. However, there is a problem in that when exposed to high temperature and high humidity, CH groups adhere to the surface, causing the hydrophilicity to be lost.
[0007] The problem to be solved by the present invention is to provide an optical thin film having excellent hydrophilicity and photocatalytic function. [Means for solving the problem]
[0009] The present invention provides a method for forming a film by repeating a step of forming a film by a vacuum deposition method using silicon oxide as a deposition material and a step of forming a film by a sputtering method using titanium or titanium oxide as a target constituent material, Contains silicon, titanium and oxygen, The above problems are solved by a method for producing an optical thin film that forms an optical thin film having a contact angle with water of 10° or less, a photocatalytic function, and a refractive index with respect to light with a wavelength of 550 nm of 1.44 or less. Effect of the Invention
[0014] According to the present invention, an optical thin film having excellent hydrophilicity and photocatalytic function can be provided. [Brief description of the drawings]
[0015] [Figure 1] 1 is a vertical cross-sectional view showing an example of a film forming apparatus used in a method for producing an optical thin film according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] 1A to 1C are process diagrams showing an embodiment of a film forming method according to the present invention. [Figure 4] 1 is a graph showing the spectral characteristics of an example of the present invention and a comparative example. [Diagram 5] 1 is a graph showing X-ray diffraction in Examples 1 to 3 of the present invention. [Figure 6] 1 is a graph showing the photocatalytic functions of examples of the present invention and comparative examples. [Figure 7] 1 is a photographic image showing the anti-fogging properties of an embodiment of the present invention and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] An embodiment of the present invention will be described below with reference to the drawings. Fig. 1 is a schematic vertical cross-sectional view showing an example of a film forming apparatus 1 used in the method for producing an optical thin film according to the present invention, and Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1. The method for producing an optical thin film according to the present invention is not limited to the use of the film forming apparatus 1 shown in Figs. 1 and 2, and may be any film forming apparatus capable of realizing the constituent features of the present invention.
[0017] The film formation apparatus 1 of this example includes a film formation chamber 2 configured to be able to reduce the pressure from an atmospheric pressure atmosphere, an exhaust device 3 for reducing the pressure inside the film formation chamber 2, a disk-shaped substrate holder 5 rotatable about a rotation axis 4b rotated by a drive unit 4a and capable of holding a substrate S on a substrate holding surface 5a, a differential pressure vessel 6 provided opposite a sputtering portion 5b that is a part of the substrate holding surface 5a of the substrate holder 5, a sputtering mechanism 7 provided inside the differential pressure vessel 6, a gas introduction system 8 for introducing a sputtering gas into the differential pressure vessel 6, and an evaporation mechanism 9 for vacuum evaporation provided inside the film formation chamber 2 opposite the substrate holding surface 5a.
[0018] 1 and 2, the substrate holder 5 of this embodiment is formed in a disk shape, and a rotation shaft 4b that rotates in one direction by a drive unit 4a is fixed to the center of the disk. The lower surface of the substrate holder 5 is a substrate holding surface 5a that fixes and holds the substrate S. An example of mounting the substrate S by the substrate holder 5 is shown in FIG. 2, but the method for manufacturing an optical thin film of the present invention is not limited to this mounting form, and various forms can be adopted.
[0019] In this example, in order to provide a gap G between the substrate holding surface 5a of the substrate holder 5 and the upper end surface 6a of the differential pressure vessel 6, which allows slight gas communication between the differential pressure region B inside the differential pressure vessel 6 and the high vacuum region A outside the differential pressure vessel 6, the substrate holder 5 is formed in a disk shape that makes it easy to adjust the appropriate size of the gap G. However, as long as the gap G can be appropriately adjusted, the shape is not limited to a disk shape, and the holder may be formed in a dome shape or a cylindrical shape used in a carousel-type rotary film forming apparatus.
[0020] The substrate S on which the film is formed is not particularly limited, and in addition to a glass substrate, an acrylic or other plastic substrate, a metal plate, etc. can be used. In particular, the effect of the present invention is more pronounced when a substrate for optical applications is used, which requires high hydrophilicity that can exhibit anti-fogging performance, self-cleaning performance, cooling performance, etc., and further requires suppression of reflectance due to a large refractive index.
[0021] The differential pressure vessel 6 in this example is formed in a cylindrical shape and is a bottomed cylindrical vessel body with one axial end face 6b (lower face in FIG. 1) closed and the other axial end face 6a (upper face in FIG. 1) open. The differential pressure vessel 6 separates the inside of the film formation chamber 2 into a high vacuum region A outside the differential pressure vessel 6 and a differential pressure region B inside the differential pressure vessel 6.
[0022] The open end surface 6a of the differential pressure vessel 6 is, for example, circular, and is disposed with a predetermined gap G from the substrate holding surface 5a of the substrate holder 5. This gap G is set so that when sputtering gas is introduced from the gas introduction system 8 into the differential pressure region B, the sputtering gas leaks through the gap G into the high vacuum region A, thereby enabling the differential pressure region B to be adjusted to a predetermined pressure higher than that of the high vacuum region A (in other words, a lower degree of vacuum than that of the high vacuum region A). The suitable size of the gap G can be determined mainly by the volume of the differential pressure vessel 6, the flow rate of the sputtering gas, and the pressures in the high vacuum region A and the differential pressure region B to be adjusted.
[0023] The differential pressure vessel 6 is not limited to the cylindrical shape shown in the figure, and may have any shape as long as it faces a part of the substrate holder 5, has a communication part such as a hole or gap through which gas can slightly communicate with another high vacuum region A inside the film formation chamber 2, and can be physically isolated. For example, the differential pressure region B may be formed by providing a shielding wall or the like on the inner wall of the film formation chamber 2. Also, instead of providing the gap G between the end face 6a and the substrate holding surface 5a, the end face 6a and the substrate holding surface 5a may be disposed close to each other, and a gas communication hole may be provided in the differential pressure vessel 6.
[0024] A sputtering mechanism 7 is provided in the differential pressure vessel 6. The sputtering mechanism 7 in this example includes a target 7a disposed inside the differential pressure vessel 6, a sputtering electrode 7b on which the target 7a is set, a sputtering power supply 7c that supplies power to the sputtering electrode 7b, and a shutter 7d that is disposed between the target 7a and the substrate holder 5 and covers or opens the target 7a. The sputtering mechanism 7 in this example employs a DC (direct current) or RF (radio frequency) sputtering method.
[0025] The target 7a is a film source material formed into a flat plate shape, and is disposed inside the differential pressure vessel 6 so as to face the substrate holding surface 5a of the substrate holder 5. As the target 7a in this example, a titanium (Ti) metal target can be used, and in addition, a metal oxide target such as titanium oxide (TiO2) may also be used.
[0026] A gas introduction system 8 is provided inside the differential pressure container 6 to introduce sputtering gas into the differential pressure region B. The gas introduction system 8 includes gas cylinders 8a and 8d for storing the sputtering gas, valves 8b and 8e provided corresponding to the gas cylinders 8a and 8d, mass flow controllers 8c and 8f for adjusting the flow rate of the sputtering gas, and a pipe 8g serving as a sputtering gas supply path.
[0027] A gas cylinder 8a, a valve 8b, and a mass flow controller 8c are used to supply oxygen gas, and a gas cylinder 8d, a valve 8e, and a mass flow controller 8f are used to supply argon gas. In this example, an inert gas such as argon or helium, and a reactive gas such as oxygen are introduced as the sputtering gas.
[0028] In order to increase the film formation rate in sputtering film formation, DC (direct current) sputtering using a metal target is effective. When obtaining a dielectric film or an oxide film, it is necessary to react with oxygen or nitrogen, but the reaction may not necessarily proceed, resulting in an incomplete state. In this example, a metal target is used, and the amount of reactive gas such as oxygen is set to a small amount, for example, reactive gas:inert gas=1:80, relative to the amount of inert gas such as argon gas, to form a film. As a result, by supplying a complete oxide in the high vacuum region A where the vacuum deposition film formation described later is performed, a film close to a complete oxide as a whole can be obtained. As a result, a film can be obtained that has a high film formation rate, high adhesion, low stress, and no optical absorption. The ratio of the reactive gas to the inert gas introduced into the differential pressure region B is 0.5% to 15%, preferably 0.5% to 8%.
[0029] The deposition mechanism 9 is an electron beam deposition source, and includes a crucible 9a filled with a deposition material, and an electron gun 9b that irradiates the deposition material filled in the crucible 9a with an electron beam. A shutter 9c that opens and closes the upper opening of the crucible 9a is movably provided above the crucible 9a. Silicon oxide (SiO2) can be used as the deposition material in this example.
[0030] In this manner, the film formation apparatus 1 used in this example is provided with the sputtering mechanism 7 and the deposition mechanism 9 inside the single film formation chamber 2. In this film formation apparatus 1, the structure for enabling compatibility between the two film formation methods, sputtering and vacuum deposition, which require significantly different degrees of vacuum, is provided by the differential pressure container 6 in which the target 7a of the sputtering mechanism 7 is stored.
[0031] By introducing a sputtering gas into the differential pressure vessel 6, the pressure in the differential pressure region B of the differential pressure vessel 6 is made higher than the high vacuum region A inside the film formation chamber 2, thereby achieving a vacuum degree of 1 to 10 at which sputtering is possible. -1 Pa. At this time, the pressure in the differential pressure region B is controlled by adjusting the flow rate of the sputtering gas and the size of the gap G. That is, if the gap G is set to a small width, a large amount of gas does not flow from the differential pressure vessel 6 into the high vacuum region A inside the film formation chamber 2, so that the degree of vacuum near the evaporation source of the deposition mechanism 9 can be set to a vacuum degree of 10 at which vacuum deposition is possible. -1 ~10 -6 Pa. This configuration makes it possible to perform sputtering film formation and vacuum evaporation film formation inside the same film formation chamber 2. Moreover, since a process of adjusting the internal pressure of the film formation chamber 2 to a pressure suitable for each film formation method while switching between sputtering film formation and vacuum evaporation film formation is not required, sputtering film formation and vacuum evaporation film formation can be repeated continuously.
[0032] The film forming apparatus 1 used in this example is equipped with a rotary substrate holder 5 that holds and rotates the substrate S. Therefore, the substrate S rotates inside the film forming chamber 2 around the rotation axis 4b during film formation. As a result, the substrate S moves between the differential pressure region B for sputtering film formation and the high vacuum region A for vacuum evaporation film formation, and the time the substrate S stays in each region A, B can be adjusted to any time by controlling the rotation speed of the substrate holder 5 by the drive unit 4a. This shows that a film formed by sputtering and a film formed by vacuum evaporation can be formed in the same film forming chamber 2.
[0033] Furthermore, according to this embodiment, the substrate S is rotated to pass through the high vacuum region A, which has a higher vacuum than the pressure suitable for the sputtering method, while sputtering deposition is performed. This makes it possible to suppress adhesion of particles other than deposition particles to the substrate S, leading to the production of a high-quality film.
[0034] When sputtering film formation and vacuum evaporation film formation are performed simultaneously, i.e., alternately and repeatedly, the residence time of the substrate S in the pressure difference region B for sputtering film formation and the high vacuum region A for vacuum evaporation film formation, the film formation conditions of the sputtering mechanism 7 or the evaporation mechanism 9, etc. can be adjusted to set the ratio of the film weight by sputtering to the film weight by vacuum evaporation and the total film formation amount (film thickness) to the desired value.
[0035] Although it is possible to realize regions with different degrees of vacuum using a differential pumping device, this requires two pumping systems and the piping system becomes complicated. In contrast, in this example, the regions A and B with different degrees of vacuum can be realized with a simple structure called a differential pressure container 6, and the entire device is simplified and made compact.
[0036] Next, an embodiment of the method for producing an optical thin film according to the present invention will be described. FIG. 3 is a process diagram showing one embodiment of the method for producing an optical thin film according to the present invention. This embodiment is an example of a film formation method in which a step of forming a titanium-based thin film on one side of a glass substrate S by a sputtering method using titanium as a target 7a, and a step of forming a silicon oxide-based thin film by a vacuum deposition method using silicon oxide as a deposition material are continuously and alternately repeated. Note that in the method for producing an optical thin film according to the present invention, it is not necessarily necessary to alternately repeat sputtering film formation and deposition film formation once each, and one of the steps may be repeated multiple times before the other is performed.
[0037] As a preliminary step, the substrate S is set on the substrate holder 5, which is then attached to the film formation chamber 2. Titanium is set as the target 7a, and the crucible 9a is filled with silicon oxide as a deposition material, after which the process of FIG.
[0038] First, in step ST1, the film formation chamber 2 is sealed, and the inside of the film formation chamber 2 is evacuated (reduced pressure) using the exhaust device 3. In the following step ST2, the inside of the film formation chamber 2 is measured to see if it is at a predetermined pressure, 10 -1 ~10 -6 in the Pa range, e.g. 7 x 10-4 It is judged whether the inside of the film formation chamber 2 reaches a predetermined pressure, for example, 7×10 -4 If the pressure does not reach 7×10 Pa, return to step ST1. -4 Repeat evacuation until the pressure reaches 1 Pa.
[0039] When the inside of the film formation chamber 2 reaches a predetermined pressure, it is assumed that the pressure has been reduced to a degree of vacuum suitable for vacuum deposition by the deposition mechanism 9, and the process proceeds to step ST3, where the rotation of the substrate holder 5 is started. In this embodiment, the rotation of the substrate holder 5 in step ST3 is started before the introduction of gas in step ST4, but the rotation of the substrate S may be started during or after the introduction of gas. However, since the rotation of the substrate holder 5 affects the flow rate of gas leaking out of the differential pressure container 6 from the gap G between the substrate holder 5 and the differential pressure container 6, it is preferable to start the rotation of the substrate holder 5 before or during the introduction of gas.
[0040] In step ST4, the valves 8b and 8e are opened to introduce oxygen gas and argon gas from the gas cylinders 8a and 8d, respectively, into the differential pressure region B inside the differential pressure vessel 6. When the oxygen gas and argon gas are introduced into the differential pressure region B, the exhaust device 3 exhausts 7×10 -4 Oxygen gas and argon gas are locally introduced into differential pressure region B, which has been reduced in pressure to about Pa, and these gases leak in minute amounts at a constant flow rate through gap G to the outside of differential pressure container 6.
[0041] When the amount of gas introduced into the differential pressure region B and the amount of gas leaking from the differential pressure region B through the gap G reach a predetermined balance, the pressure in the differential pressure region B reaches a desired pressure, in this embodiment, a pressure of 1 to 10 suitable for sputtering film formation. -1 The pressure in the differential pressure region B may be detected by a pressure gauge provided inside the differential pressure container 6. -1 It has been confirmed by experiments by the present inventors that plasma is generated when the pressure reaches a predetermined pressure of 1 to 10 Pa. Therefore, in this embodiment, when plasma is generated inside the differential pressure container 6, -1It is determined that the pressure has reached 1 Pa. In step ST4, if plasma is not generated even after waiting for a while, it is expected that the pressure inside the differential pressure container 6 has not risen sufficiently because the introduction speed of the oxygen gas and argon gas is slow compared to the leakage speed of the gas from the gap G. Therefore, the flow rates of the oxygen gas and argon gas are increased by adjusting the mass flow controllers 8c and 8f.
[0042] In step ST5, the shutter 7d that had been covering the target 7a is opened to start sputtering deposition, and the shutter 9c that had been covering the crucible 9a is opened and an electron beam is irradiated from the electron gun 9b onto the crucible 9a to start vacuum deposition deposition.
[0043] In step ST6, it is determined whether the thickness of the thin film formed on the substrate S reaches a predetermined required thickness by the non-contact type film thickness sensor 11. If the thickness of the thin film formed on the substrate S does not reach the predetermined required thickness, step ST5 is repeated until the required thickness is reached.
[0044] When the thickness of the thin film formed on the substrate S reaches a predetermined required thickness, in step ST7, the target 7a is covered with the shutter 7d, the valves 8b and 8e are closed to end the sputtering deposition, the electron gun 9b is turned off, and the shutter 9c is closed to end the vacuum evaporation deposition. Thereafter, the internal pressure of the deposition chamber 2 is returned to atmospheric pressure, and the substrate holder 5 is removed from the deposition chamber 2.
[0045] As described above, in the method for producing an optical thin film of the present embodiment, a step of forming a film of silicon oxide as a deposition material on the surface of a substrate S by a vacuum deposition method and a step of forming a film of titanium (or titanium oxide) as a target constituent material by a sputtering method are successively repeated, thereby making it possible to obtain an optical thin film having excellent hydrophilicity and a photocatalytic function of decomposing a CH group.
[0046] Here, hydrophilicity means that the contact angle with water is 10° or less. When a film is formed using the above-mentioned film forming apparatus 1, the degree of vacuum in the high vacuum region A decreases due to gas leaking from the differential pressure container 6 (differential pressure region B), which reduces the density of the film and makes it porous, making it easier for moisture to penetrate. In addition, the film exhibits high hydrophilicity due to the chemical action of the OH groups of the silicon oxide component.
[0047] On the other hand, hydrophilic thin films made of silicon oxide have a problem that CH groups adhere to the surface when exposed to high temperature and high humidity, causing hydrophilicity to disappear, but in this example, titanium oxide is sputtered to give the resulting optical thin film a photocatalytic function that decomposes CH groups. That is, even if CH groups adhere to the surface and hydrophilicity is reduced or lost, when ultraviolet light is irradiated, the photocatalytic function of titanium oxide decomposes and removes the CH groups adhered to the surface of the optical thin film. This makes it possible to suppress the decrease in hydrophilicity and restore the lost hydrophilicity.
[0048] The optical thin film of this example contains silicon, titanium, and oxygen as main components. In order to exhibit the above-mentioned hydrophilicity and photocatalytic function, it is more preferable that the atomic percentage of silicon is 26% to 32%, the atomic percentage of titanium is 1% to 8%, and the remainder is oxygen, as measured by atomic percentage using X-ray photoelectron spectroscopy. If the atomic percentage of silicon exceeds 32%, the atomic percentage of titanium decreases, resulting in insufficient photocatalytic function. Conversely, if the atomic percentage of silicon is less than 26%, hydrophilicity decreases. Also, if the atomic percentage of titanium exceeds 8%, the atomic percentage of silicon decreases, resulting in insufficient hydrophilicity. Conversely, if the atomic percentage of titanium is less than 1%, photocatalytic function is insufficient.
[0049] The optical thin film of this example contains silicon, titanium and oxygen as main components, but is composed of a mixed film of silicon oxide and titanium oxide, and is not a laminated film in which a thin film of silicon oxide and a thin film of titanium oxide are laminated. It is more preferable that the atomic ratio of titanium oxide is 3% to 24%, with the remainder being silicon oxide, as measured by atomic ratio measurement using X-ray photoelectron spectroscopy. If the atomic ratio of titanium oxide exceeds 24%, the atomic ratio of silicon oxide decreases, and hydrophilicity decreases. Conversely, if the atomic ratio of titanium oxide is less than 3%, the photocatalytic function becomes insufficient.
[0050] In the optical thin film of this example, the degree of vacuum in the high vacuum region A is reduced by the gas leaking from the differential pressure container 6 (differential pressure region B), so the density of the film is reduced and it becomes porous. Therefore, the optical thin film has a low refractive index, and the refractive index for light with a wavelength of 550 nm is preferably 1.44 or less, and more preferably 1.31 to 1.44. With such a low refractive index, light reflection on the substrate surface can be suppressed, so that the occurrence of flare and ghosting, reflection of external light, etc. can be prevented. In addition, for a film-forming material with a higher refractive index than glass, a thin film with a low refractive index can be formed, so that a desired refractive index can be freely selected without being bound by the refractive index of existing materials, and the degree of freedom in designing the optical thin film can be increased.
[0051] The optical thin film of this example may be formed as a single layer on the surface of a substrate made of metal, plastic, or inorganic material, or may be included as one or more thin films in a laminated multilayer film. EXAMPLES
[0052] Example and Comparative Example: Using the deposition apparatus shown in FIG. 1 and FIG. 2, a glass substrate S (N-BK7 manufactured by SCHOTT, plate thickness 1.0 mm, 40×40 mm, refractive index n dA mixed film of silicon oxide and titanium oxide was formed on one side of a glass substrate (Teflon-coated glass) with a target thickness of 500 nm, and the spectral transmittance was measured using a spectrophotometer (V-670 manufactured by JASCO Corporation). The refractive index (550 nm wavelength light) of the film after film formation was calculated from the transmittance. The contact angle θ of the same film was also determined based on the wettability test method for glass substrate surfaces (JIS R3257) to evaluate hydrophilicity. This contact angle was measured immediately after film formation, after a high temperature and high humidity test, and using an ultraviolet lamp (UVGL-58, 6W, peak wavelength 254 nm, 150 μW / cm manufactured by Funakoshi Corporation). 2 ) was irradiated onto the sample from a distance of 2 cm, and then the test was performed three times in total. The high temperature and high humidity test was performed at 85°C, 85%, and for 24 hours using an environmental tester (SH-641 manufactured by ESPEC Corporation). The film formation conditions of the film formation device 1 at this time were as follows:
[0053] The ratio of the volume of the vacuum vessel 2 to the volume of the differential pressure vessel 6 is 1:0.02, the vertical distance H between the crucible 9a of the vacuum evaporation mechanism 9 shown in FIG. 1 and the substrate S is 35 to 50 cm, and the target vacuum degree of the high vacuum region A is 7×10 -4 Pa, the target vacuum level in differential pressure area B is 1 to 10 -1 The sputtering deposition was performed by DC sputtering using a DC power source as the sputtering power source 7c, and the DC power of the sputtering power source 7c was set to 1500 W. A titanium target (manufactured by USTRON Corporation) was used as the target 7a, and oxygen gas at 100 sccm and argon gas at 500 sccm were introduced as sputtering gas from the bottom of the target 7a, to perform reactive sputtering.
[0054] For the vacuum deposition, silicon oxide (Merck) was used as the deposition material. No reactive gas such as oxygen gas was introduced into the high vacuum area A. The substrate S was heated to 200°C. In the following Table 1, Examples 1 to 3 were prepared by fixing the deposition conditions for sputtering deposition (DC power of the sputtering power supply 7c was 1500W) and setting the deposition rate of the deposition deposition, specifically the current of the electron gun 9b, to three levels, 150mA (Example 1), 180mA (Example 2), and 200mA (Example 3), to obtain optical thin films of Examples 1 to 3 with different mixture ratios of silicon oxide and titanium oxide. Comparative Example 1 shows an example in which the same deposition apparatus 1 was used, but the DC power was set to 0, the sputtering gas flow rate was set to 0, and deposition was performed only by vacuum deposition.
[0055] The atomic ratios of the composition elements Si, Ti, and O constituting each of the optical thin films produced in Examples 1 to 3, and the atomic ratios of silicon oxide and titanium oxide were analyzed by X-ray photoelectron spectroscopy (XPS). The atomic ratios and refractive indexes of Examples 1 to 3 and Comparative Example 1 are shown in Table 1.
[0056] [Table 1]
[0057] The spectral transmittance of Examples 1 to 3, Comparative Example 1, and the glass substrate was measured using a spectrophotometer (V-670 manufactured by JASCO Corporation), and the results are shown in Fig. 4. As shown in Fig. 4, no optical absorption was observed in any of Examples 1 to 3 and Comparative Example 1.
[0058] The crystal structure of each of the optical thin films of Examples 1 to 3 was analyzed by X-ray diffraction (XRD). The results are shown in Figure 5. From the analysis results by X-ray photoelectron spectroscopy (XPS) shown in Table 1, it can be seen that each of the optical thin films of Examples 1 to 3 was prepared as a mixed film of silicon oxide and titanium oxide. Furthermore, from the analysis results by X-ray diffraction (XRD) shown in Figure 5, no difference was observed in the crystal structure of each of the optical thin films of Examples 1 to 3.
[0059] Next, evaluation of hydrophilicity will be described. First, the contact angle with water of each of the optical thin films of Examples 1 to 3 was measured immediately after deposition, and all were 10° or less, and no difference was observed. Next, each of the optical thin films of Examples 1 to 3 was placed in an environmental tester (SH-641 manufactured by ESPEC) set at a temperature of 85°C and a humidity of 85% for 24 hours, and a high-temperature, high-humidity test was performed. When the contact angle with water was measured immediately after the high-temperature, high-humidity test, the optical thin film of Example 1 had a contact angle of θ=49°, the optical thin film of Example 2 had a contact angle of θ=53°, and the optical thin film of Example 3 had a contact angle of θ=58°. It was confirmed that the hydrophilicity of each of the optical thin films of Examples 1 to 3 was lost when the high-temperature, high-humidity test was performed.
[0060] For each of the samples of Examples 1 to 3 that were subjected to the high temperature and high humidity test, an ultraviolet lamp (UVGL-58, 6 W, peak wavelength 254 nm, 150 μW / cm, manufactured by Funakoshi Co., Ltd.) was placed 2 cm away. 2 ) was used to irradiate ultraviolet light. After the start of irradiation with ultraviolet light, the contact angle of each of the optical thin films of Examples 1 to 3 with water was measured every hour. The results are shown in FIG. 6. The optical thin film of Comparative Example 1, which does not contain titanium oxide, did not decrease in contact angle even when irradiated with ultraviolet light, and recovery of hydrophilicity was not observed. In contrast, it was confirmed that the contact angle of each of the optical thin films of Examples 1 to 3 decreased and hydrophilicity was restored by irradiating with ultraviolet light. At the same time, it was confirmed that, when the irradiation time (irradiation light amount) was the same, the decrease in contact angle was more significant in Example 1, which contains a higher proportion of titanium oxide. In addition, it was also confirmed that, although the irradiation time (irradiation light amount) was different, the optical thin films of Examples 1 to 3 all recovered to their original contact angle of 10° or less.
[0061] The optical thin films of Example 1 and Comparative Example 1 were each placed in a desiccator immediately after deposition and stored indoors for one year, after which a fogging test was performed in which each sample was exposed to water vapor. The results are shown in Figure 7. It was confirmed that the optical thin film of Example 1 maintained high hydrophilicity even one year after deposition, whereas the optical thin film of Comparative Example 1 had lost its hydrophilicity. [Explanation of symbols]
[0062] A…High vacuum area B…Differential pressure area G…Gap S...Substrate 1...Film deposition equipment 2. Film deposition chamber 3. Exhaust system 4a…Drive unit 4b…Rotation axis 5...Substrate holder 5a...Board holding surface 5b…Sputtering section 6...Differential pressure vessel 6a,6b…end face 7…Sputtering mechanism 7a…Target 7b…Sputter electrode 7c…Sputter power supply 7d…Shutter 8...Gas introduction system 8a, 8d…Gas cylinders 8b, 8e…Valve 8c, 8f...Mass flow controller 8g…Pipe 9...Deposition mechanism 9a...crucible 9b…Electron gun 9c…Shutter 10…Pressure gauge 11…Film thickness sensor
Claims
1. Repeating a step of forming a film by a vacuum deposition method using silicon oxide as a deposition material and a step of forming a film by a sputtering method using titanium or titanium oxide as a target constituent material; A method for producing an optical thin film, which comprises depositing an optical thin film that contains silicon, titanium and oxygen, has a contact angle with water of 10° or less, has a photocatalytic function, and has a refractive index with respect to light with a wavelength of 550 nm of 1.44 or less.
2. The method for producing an optical thin film according to claim 1 , wherein the photocatalytic function is a photocatalytic function that decomposes a CH group.
3. 3. The method for producing an optical thin film according to claim 1, wherein an atomic percentage of said silicon is 26% to 32%, an atomic percentage of said titanium is 1% to 8%, and the remainder is said oxygen, as determined by atomic percentage measurement using X-ray photoelectron spectroscopy.
4. the optical thin film is made of a mixed film of silicon oxide and titanium oxide, 3. The method for producing an optical thin film according to claim 1, wherein the atomic ratio of said titanium oxide is 3% to 24%, and the remainder is said silicon oxide, as determined by atomic ratio measurement using X-ray photoelectron spectroscopy.
Citation Information
Patent Citations
Color antifog mirror
JP2001141916A
Reflection mirror
JP2011107189A
Photocatalyst-coated object, and photocatalyst coating liquid therefor
JP2012250133A
Film deposition method
JP2018123365A