Transparent molded body and its manufacturing method
A method for producing transparent molded bodies using Group 4 element oxides through pre-oxidation and controlled heat treatment in specific oxygen partial pressures achieves monoclinic or rutile structures, addressing segregation issues and enhancing transmittance and durability.
Patent Information
- Application Number
- JP2020086904
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-05-18
AI Technical Summary
Existing methods for producing transparent molded bodies made of Group 4 element oxides, such as zirconium oxide and hafnium oxide, require the addition of third elements which can lead to segregation and concentration variations, and lack the ability to achieve monoclinic or rutile structures without additional steps.
A method involving pre-oxidation and controlled heat treatment in specific oxygen partial pressure atmospheres to produce transparent molded bodies with monoclinic or rutile structures, utilizing Group 4 element oxides without significant third element content, by controlling oxygen vacancy levels and crystal grain structure.
The method enables the production of transparent molded bodies with high transmittance and resistance to cracking, suitable for decorative and electronic applications, without the need for additional stabilizing elements and with simplified manufacturing processes.
Smart Images

Figure 0007595243000002 
Figure 0007595243000003 
Figure 0007595243000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a transparent molded article and a method for producing the same. [Background technology]
[0002] Group 4 element oxides such as titanium oxide, zirconium oxide, and hafnium oxide have high heat resistance and corrosion resistance and are used for high-temperature components, refractories for glass melting furnaces and ladles in steel refining, abrasives, etc. On the other hand, Group 4 element oxides with high transparency are also known, and these Group 4 element oxides are used for decorative components, window materials in the visible to infrared light range, etc. Patent documents relating to transparent sintered bodies mainly composed of Group 4 element oxides are also known.
[0003] For example, a transparent ceramic that is a zirconium oxide-based or hafnium oxide-based ceramic and has an average crystal grain size in the range of 5 to 300 μm has been proposed (Patent Document 1). Patent Document 1 describes that a transparent ceramic that is a zirconium oxide-based or hafnium oxide-based ceramic can provide advanced optical functions such as suppressing scattering loss and improving uniformity of optical quality. Patent Document 1 describes a method in which a raw material powder with an average grain size of 20 to 500 nm is molded, and then calcined at 500 to 900° C. to form a calcined body, which is then heated at a high temperature of 1400° C. or higher to form a transparent ceramic.
[0004] Also, a zirconium oxide sintered body with a sample thickness of 1 mm or more has been proposed (Patent Document 2). Patent Document 2 states that a zirconium oxide sintered body having a large crystal grain size of 50 μm or more has low mechanical strength. In the examples of Patent Document 2, zirconium oxide powder TZ-Y (yttrium oxide 8 mol%, specific surface area 13.5 m) is used. 2 It is described that a zirconium oxide sintered body is formed by press-molding a mixture of 0.1% by weight of zirconium oxide and 0.1% by weight of 1.0% by weight of 0.1 ...
[0005] As a method for producing zirconium oxide using zirconium other than the powder raw material, a method of oxidizing a pure zirconium plate in the air is known (Non-Patent Document 1). It is known that when pure zirconium is oxidized in the air, white zirconium oxide (ZrO2) is usually formed. However, Non-Patent Document 1 describes that a black zirconium oxide plate is formed by a method of controlling the oxidation in the air to a low temperature or a method of controlling the oxidation for a short period of time. The black zirconium oxide (ZrO 2-a ) has oxygen deficiencies. Figure 24 shows a pure zirconium plate before oxidation and black zirconium oxide after oxidation.
[0006] Zirconium oxide is white at room temperature, exhibits ionic conductivity, and has the property that its crystal structure undergoes a phase transition from monoclinic to tetragonal (approximately 1150°C; the change from tetragonal to monoclinic generally occurs at approximately 950°C) and from tetragonal to cubic (approximately 2200°C) depending on the heat treatment temperature. White zirconium oxide, which has such phase transition properties, is prone to embrittlement, with numerous cracks appearing throughout the sample due to volume expansion and contraction that accompanies temperature changes.
[0007] Non-Patent Document 2 describes how white zirconium oxide (ZrO2) is reduced with hydrogen (conditions: heat treatment in a 5% H2 / Ar atmosphere. In addition, heat treatment under high pressure is required for sintering) to produce black zirconium oxide (ZrO 2-a ) is formed. In Non-Patent Document 2, it is described that black titanium oxide (TiO) is formed by hydrogen reduction of white titanium oxide (TiO) in the same way as zirconium oxide. 2-a ) is reported to be formed. 2-a ) and titanium oxide (TiO 2-a ) has a smaller band gap compared to white zirconium oxide (ZrO2) and titanium oxide (TiO2) due to oxygen deficiency. Figure 23 is a photograph showing the colors of white zirconium oxide (ZrO2) powder and black zirconium oxide powder contained in a container. In addition, Non-Patent Document 3 reported that hafnium was heated in the air under controlled conditions to produce black hafnium oxide (HfO 2-a ) is formed. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2010-047460 A [Patent Document 2] JP 2011-051881 A [Non-patent literature]
[0009] [Non-Patent Document 1] Mitsuhiro Matsuda, Yuuta Himeno, Kenji Shida, Motohide Matsuda: Materials Letters 230 (2018) 117-119. [Non-Patent Document 2] Apurba Sinhamahapatra et al., Scientific Reports 6, (2016) [Non-Patent Document 3] Mitsuhiro Matsuda, Yuta Himeno, Kenji Shida, Motohide Matsuda:Ceramics International 46(2020) Summary of the Invention [Problem to be solved by the invention]
[0010] However, a transparent molded body made of a Group 4 element oxide is not known. In order to manufacture a transparent molded body containing a Group 4 element oxide as a main component, it has been thought that a step of adding a third element is essential. For example, in the method described in Patent Document 1, in addition to zirconium oxide or hafnium oxide, a stabilizer selected from Y2O3, Sc2O3, MgO, CaO and lanthanide rare earth oxides, and a fluoride selected from CaF2, MgF2, ScF3, YF3, ZrF4 and lanthanide rare earth element fluorides are used as raw material powders. Also, in the method described in Patent Document 2, yttrium oxide is essential as a stabilizer. Transparent molded bodies manufactured by these methods contain a large amount of a third element such as yttrium. If a third element is contained in the molded body, the third element segregates in the molded body, and there is a concern about variation in the third element concentration and grain boundary segregation. Also, in the manufacturing process, it is desirable not to add a third step from the viewpoint of reducing the number of steps and simplifying the manufacturing process.
[0011] In addition, the methods of Non-Patent Document 1, Non-Patent Document 2, and Non-Patent Document 3 do not include a step of adding a third element, but they cannot obtain a transparent molded body made of an oxide of a Group 4 element. 2-a ) is heated continuously in air to form white zirconium oxide (ZrO2), and the black hafnium oxide (HfO 2-a ) is continuously heated in air to form white hafnium oxide (HfO2).
[0012] The crystal structure of the transparent molded bodies described in Patent Documents 1 and 2 is a cubic structure (fluorite structure) or a mixed structure of cubic and tetragonal crystals. Transparent molded bodies having a monoclinic structure or a rutile structure are not known.
[0013] The present invention has been made in consideration of the above circumstances, and has an object to provide a transparent molded article having a monoclinic structure or a rutile structure and made of a Group 4 element. [Means for solving the problem]
[0014] As a result of intensive research, the present inventors have discovered that a Group 4 element oxide (black zirconium oxide (ZrO 2-a ) sheet material has an inner part made of a Group 4 element (e.g., pure zirconium) and an outer part made of a Group 4 element oxide (e.g., zirconium oxide (ZrO2)), and it has been found that when the sheet material is heated for a specified period of time in an environment where the oxygen partial pressure is controlled, the correlation between the rate at which oxygen is absorbed from the outside of the sheet material and the rate at which the oxygen absorbed into the sheet material progresses into the interior can be controlled, and a transparent molded body made of a Group 4 element oxide can be obtained.
[0015] That is, the gist and configuration of the present invention are as follows.
[0016] (1) A transparent molded article according to one aspect of the present invention is a transparent molded article made of an oxide of a Group 4 element, and has the composition formula AO 2-x (A is any one element selected from Zr, Hf, and Ti, and x represents the amount of oxygen deficiency, and x is greater than or equal to 0.) When A is Zr or Hf, it has a monoclinic structure, and when A is Ti, it has a rutile structure. When the thickness is 20 μm, the transmittance at a wavelength of 600 nm is 45% or more.
[0017] (2) A transparent molded article according to one aspect of the present invention is a transparent molded article made of an oxide of a Group 4 element, and has the composition formula AO 2-x (A is any one element selected from Zr, Hf, and Ti, and x represents the amount of oxygen deficiency, x≧0.) When A is Zr or Hf, it has a monoclinic structure, and when A is Ti, it has a rutile structure, and is made of a Group 4 element oxide having a surface layer containing equiaxed crystal grains and an inner layer inside the surface layer containing columnar crystal grains having an average length in the major axis direction longer than that of the equiaxed crystal grains.
[0018] (3) The transparent molded body described in (1) or (2) above may have a surface layer containing equiaxed crystal grains, and an internal layer inside the surface layer containing columnar crystal grains having an average length in the major axis direction longer than that of the equiaxed crystal grains, and the columnar crystal grains may have an average crystal grain size in the major axis direction of 100 nm to 5 μm and an average crystal grain size in the minor axis direction of 10 to 1000 nm.
[0019] (4) In the transparent molded article according to any one of (1) to (3) above, the amount of oxygen deficiency x may be x>0.
[0020] (5) In the transparent molded article according to any one of (1) to (4) above, the amount of a third element may be 0.8 mass percent or less. (6) The transparent molded article according to any one of the above (1) to (5) may not have a Group 4 element layer made of a Group 4 element.
[0021] (7) A method for producing a transparent molded body according to one embodiment of the present invention is a method for producing a transparent molded body made of a Group 4 element oxide described in any one of (1) to (6) above, and includes a first step of pre-oxidizing, in the atmosphere, a sheet material of a Group 4 element selected from the group consisting of zirconium, hafnium, and titanium, and a second step of heat-treating the pre-oxidized sheet material in an oxygen partial pressure atmosphere.
[0022] (8) In the method for producing a transparent molded body according to the above (7), the Group 4 element is zirconium, and in the first step, the zirconium plate is preheated at 600 to 900° C. for 10 minutes to 5 hours, and in the second step, the preoxidized zirconium plate is heated at 900 to 1100° C. for 10 minutes to 50 hours, and the oxygen partial pressure is 1.0×10 -5 ~1.0×10 -7 It may also be an ATM.
[0023] (9) In the method for producing a transparent molded body according to the above (7), the Group 4 element is hafnium, and in the first step, a hafnium plate material is preheated at 700 to 1000° C. for 10 minutes to 5 hours, and in the second step, the preoxidized hafnium plate material is heated at 900 to 1100° C. for 10 minutes to 50 hours, and the oxygen partial pressure is 1.0×10 -5 ~1.0×10 -7 It may also be an ATM.
[0024] (10) In the method for producing a transparent molded body according to the above (7), the Group 4 element is titanium, and in the first step, a titanium plate is preheated at 500 to 800° C. for 10 minutes to 50 hours, and in the second step, the preoxidized titanium plate is heated at 700 to 1000° C. for 10 minutes to 50 hours, and the oxygen partial pressure is 1.0 to 1.0×10 -5 It may also be an ATM. Effect of the Invention
[0025] According to the present invention, it is possible to provide a transparent molded article having a monoclinic structure or a rutile structure and made of a Group 4 element. [Brief description of the drawings]
[0026] [Figure 1] 1 is a photograph showing the appearance of a transparent molded body made of a Group 4 element oxide according to the present embodiment. [Diagram 2] 1 is a cross-sectional SEM image of a transparent molded article made of a Group 4 element oxide according to an embodiment of the present invention. [Diagram 3] 1 is a TEM image of a transparent molded body made of a Group 4 element oxide according to the present embodiment. [Figure 4] 2 is a photograph showing the appearance of a plate material used in the method for producing a transparent molded body according to the present embodiment. [Diagram 5] 2 is a photograph showing the appearance of a plate material after a first step in the method for producing a transparent molded body according to the present embodiment. [Figure 6] 3 is a cross-sectional SEM image of a plate material after a first step in the method for producing a transparent molded body according to the present embodiment. [Figure 7] 1 is a photograph showing the appearance of a plate material of a Group 4 element that can be used in the manufacturing method of a transparent molded body according to the present embodiment, showing the zirconium plate material used in Example 1. [Figure 8] 1 is a photograph showing the appearance of a plate material after a first step in a method for producing a transparent molded body according to the present embodiment, showing BZ in Example 1. [Figure 9] 1 shows a transparent molded body A produced in Example 1, which is a transparent molded body obtained by the method for producing a transparent molded body according to the present embodiment. [Figure 10] 1 is a TEM image of a BZ in Example 1. [Figure 11] 1 shows the results of XRD measurement of BrZ, transparent molded body A, and BZ in the examples. [Figure 12] 1 shows the results of XPS measurement of BZ in an example. [Figure 13] 1 shows the results of XPS measurement of the transparent molded body A produced in Example 1. [Figure 14] 1 is a photograph showing the appearance of transparent molded body B produced in Example 2. [Figure 15] 1 is a graph showing the transmittance of a transparent molded body B produced in Example 2. [Figure 16] 1 is a graph showing the transmittance of a transparent molded body B produced in Example 2, and is an enlarged view of a region having a wavelength of 1000 nm or less. [Figure 17] 1 is a photograph showing the appearance of BrZ produced in Comparative Example 1. [Figure 18] 1 is a cross-sectional SEM image of BrZ produced in Comparative Example 1. [Figure 19] 1 is a photograph showing the appearance of the WZ produced in Comparative Example 2. [Figure 20] 1 is a cross-sectional SEM image of a WZ produced in Comparative Example 2. [Figure 21] 1 is a TEM image of the WZ produced in Comparative Example 2. [Figure 22] 1 is a photograph showing the appearance of a sample prepared in a reference example. [Diagram 23] 1 is a photograph showing the colors of white zirconium oxide powder and black zirconium oxide powder contained in a container. [Figure 24]Zirconium plate material before and after oxidation in air. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics of the present invention easier to understand. For this reason, the dimensional ratios of each component may differ from the actual ones.
[0028] [Transparent molding] The transparent molded article according to this embodiment is a transparent molded article made of a Group 4 element oxide.
[0029] Here, the Group 4 elements include titanium (Ti), zirconium (Zr), and hafnium (Hf). The Group 4 element oxides are 2-x (A is any one element selected from Zr, Hf, and Ti, and x indicates the amount of oxygen deficiency, and 0≦x).
[0030] 1 is a photograph of the appearance of a transparent molded body 100. The transparent molded body 100 is an example of a transparent molded body according to the present embodiment. The shape of the transparent molded body 100 is, for example, a plate-like, foil-like, thin film-like, or the like at room temperature. These shapes are preferable because they are easy to manufacture, but the shape is not limited to these shapes and can be controlled to any shape.
[0031] The transparent molded body 100 has a transmittance for visible light having a measurement wavelength of 600 nm at a sample thickness of 20 μm of 45% or more, preferably 47% or more, more preferably 50% or more, even more preferably 55% or more, and particularly preferably 60% or more.
[0032] FIG. 2 is a cross-sectional scanning electron microscope (SEM) image showing a cross-section of the transparent molded body 100. The transparent molded body 100 exhibits a monoclinic structure when the Group 4 element is zirconium or hafnium, and has a rutile-type structure when the Group 4 element is titanium. As shown in FIG. 2, the transparent molded body 100 is transparent to visible light because no cracks or voids are formed.
[0033] The oxygen deficiency amount x of the transparent molded body 100 is a number satisfying 0 ≦ x < 0.2. x is a number including 0. The oxygen deficiency amount x preferably satisfies 0 < x < 0.1, and more preferably satisfies 0 < x < 0.05.
[0034] The presence or absence of oxygen deficiency in the transparent molded body 100 can be evaluated using X-ray photoelectron spectroscopy (XPS). When the transparent molded body 100 has no oxygen deficiency, only a single peak (hereinafter sometimes referred to as the first peak) is confirmed in the XPS analysis result. On the other hand, when the transparent molded body 100 has oxygen deficiency, another peak is also confirmed in a higher energy region than the first peak. For example, the XPS analysis result shown in FIG. 13 is the XPS analysis result of the transparent molded body according to Example 1 described later, and a peak with a binding energy of about 531 eV is confirmed in addition to the peak at a position with a binding energy of about 530 eV. That is, it is confirmed that the transparent molded body according to Example 1 has oxygen deficiency. Note that the greater the amount of oxygen deficiency, the greater the peak intensity in the high energy region. Specifically, as a method for quantifying the oxygen deficiency amount, according to the method described in "X-ray Photoelectron Spectroscopy, Maruzen Publishing, edited by the Japan Society for Surface Science, P120", various peak areas can be separated and calculated using sensitivity coefficients.
[0035] Fig. 3 is a cross-sectional transmission electron microscope (TEM) image showing a cross section of the transparent molded body 100. The transparent molded body 100 has a surface layer L1 and an internal layer L2 located inside the surface layer L1. An interface B between the surface layer L1 and the internal layer L2 is located, for example, at a position of 1 to 3 µm from the surface of the transparent molded body 100. In Fig. 3, the interface B is located at a position of about 2 µm from the surface of the transparent molded body. The position of the interface B varies depending on the thickness of the transparent molded body 100 and the like, and is not limited to this example.
[0036] The surface layer L1 is a layer located on the surface side of the transparent molded body 100. The surface layer L1 includes equiaxed crystal grains 10. The average grain size of the equiaxed crystal grains 10 is, for example, 10 nm to 1000 nm, and may be 100 nm to 500 nm, or 100 nm to 200 nm.
[0037] The inner layer L2 is a layer located inside the surface layer L1. The inner layer L2 includes highly oriented columnar crystal grains 20. The average crystal grain size in the major axis direction of the columnar crystal grains 20 is 100 nm to 5 μm, may be 200 nm to 3 μm, or may be 500 nm to 2 μm. The average crystal grain size in the minor axis direction of the columnar crystal grains 20 is 10 nm to 1000 nm, may be 20 nm to 500 nm, or may be 50 nm to 300 nm.
[0038] The size of the equiaxed crystal grains L1 and the size of the columnar crystal grains are measured by known methods. For example, the size of the equiaxed crystal grains can be measured by a line segment method using an electron microscope. The size of the columnar crystal grains can be measured by a line segment method using an electron microscope and by calculating the aspect ratio. The line segment method can be performed, for example, according to the method described in "Metal Handbook, Japan Institute of Metals, 6th Revised Edition," edited by the Japan Institute of Metals, Maruzen Co., Ltd., June 1, 2000, pages 264 to 265.
[0039] The transparent molded body 100 contains a small amount of a third element other than the Group 4 element and oxygen. The amount of the third element is, for example, 0.8 mass percent or less, and preferably 0.4 mass percent or less.
[0040] Among the raw materials used in the manufacturing process of the transparent molded body 100, which will be described in detail later, raw materials other than oxygen gas do not react with the plate material made of a Group 4 element. Therefore, the amount of the third element contained in the transparent molded body 100 can be calculated based on the amount of the third element in the plate material that is the raw material. For example, when the amount of the third element contained in the plate material made of a Group 4 element is a mass percent, the mass of the plate material made of a Group 4 element is b, and the mass of the transparent molded body 100 is c, the amount of the third element contained in the transparent molded body 100 can be considered to be a x b / c mass percent.
[0041] In conventional Group 4 element oxides, cracks tend to occur from grain boundaries, but in the transparent molded body according to this embodiment, cracks do not occur from any part, including grain boundaries. Specifically, cubic or tetragonal Zr or Hf undergoes phase transformation to monoclinic crystals due to temperature changes or stress loads caused by the environment. When phase transformation occurs, cracks occur. However, when A is Zr or Hf, the transparent molded body according to this embodiment has a monoclinic structure and does not undergo phase transformation, so cracks and the like caused by phase transformation can be suppressed. Similarly, titanium with an anatase structure undergoes phase transformation to a rutile structure due to temperature changes or stress loads caused by the environment. However, when A is Ti, the transparent molded body according to this embodiment has a rutile structure and does not undergo phase transformation, so cracks and the like caused by phase transformation can be suppressed.
[0042] The transparent molded article according to this embodiment exhibits high transmittance in the visible and infrared regions, and can therefore be used in a wide range of fields, such as decorative materials, exterior parts for electronic devices, and cosmetic dental materials.
[0043] [Method of manufacturing transparent molded body] The method for producing a transparent molded body according to this embodiment is a method for producing the transparent molded body according to the above embodiment. The method for producing a transparent molded body according to this embodiment includes a first step of pre-oxidizing a plate material of a Group 4 element in the atmosphere, and a second step of heat-treating the pre-oxidized plate material in an oxygen atmosphere.
[0044] (1st step) In the first step, a plate material of a Group 4 element selected from the group consisting of zirconium, hafnium, and titanium is pre-oxidized in the atmosphere. Fig. 4 is an external photograph showing an example of a plate material of a Group 4 element. That is, Fig. 4 shows an example of the plate material before the first step is performed. Fig. 5 is an external photograph showing an example of the plate material after the first step is performed.
[0045] The plate material may be a commercially available product. The thickness of the plate material is arbitrary, but is, for example, 5 μm to 2 mm. The plate material is preferably made of only Group 4 elements. On the other hand, the plate material may be a plate material containing a third element other than the Group 4 element.
[0046] The heat treatment temperature in the first step is 500 to 1000° C. The first step can be performed using a known electric furnace or the like. The heat treatment temperature is 600 to 900° C., preferably 800 to 900° C., when pre-oxidizing a zirconium plate material, 700 to 1000° C., preferably 800 to 900° C., when pre-oxidizing a hafnium plate material, and 500 to 800° C., preferably 600 to 700° C., when pre-oxidizing a titanium plate material.
[0047] A transparent molded body can be obtained by controlling the heat treatment temperature in the first step within these ranges and performing the second step described below. If the heat treatment temperature in the first step is 1000°C or higher, cracks will occur from the grain boundaries, and a transparent molded body cannot be obtained. If the heat treatment temperature in the first step is less than 500°C, the Group 4 elements cannot be sufficiently oxidized, and cracks will occur during the second step described below, and a transparent molded body cannot be obtained.
[0048] The heat treatment time for the first step is 10 minutes to 5 hours, preferably 10 minutes to 2 hours, and more preferably 30 minutes to 1 hour, when the Group 4 element is zirconium, 10 minutes to 5 hours, preferably 10 minutes to 2 hours, and more preferably 30 minutes to 1 hour, when the Group 4 element is hafnium, and 10 minutes to 50 hours, preferably 30 minutes to 30 hours, and more preferably 2 hours to 20 hours, when the Group 4 element is titanium.
[0049] The heat treatment time here refers to the time during which the above-mentioned heat treatment temperature is maintained after it has been reached. The heat treatment time may be shortened when the heat treatment temperature is high, and may be lengthened when the heat treatment temperature is low. By controlling the heat treatment time within the above range, it is possible to prevent cracks and fractures from occurring.
[0050] 6 is a TEM image showing a cross section of the plate material preliminarily oxidized in the first step. The plate material after the first step has a group 4 element layer La and oxide layers Lb sandwiching the group 4 element layer La. The group 4 element layer La is a layer containing an unoxidized group 4 element, and the plate material before the first step is composed only of the group 4 element layer La. The oxide layer Lb is a layer containing a group 4 element oxide. Since oxidation progresses from the surface of the plate material in the first step, the oxide layer Lb is located on the surface side of the group 4 element layer La.
[0051] (2nd process) The second step is a step of heat treating the plate material preliminarily oxidized in the first step in an oxygen partial pressure atmosphere. The second step can be performed using a known electric furnace.
[0052] The oxygen partial pressure atmosphere is an atmosphere in which the oxygen partial pressure is controlled. For example, the oxygen partial pressure atmosphere is an atmosphere in which oxygen gas, nitrogen gas, high-purity argon gas, and air gas are combined and controlled. The oxygen partial pressure atmosphere may contain only oxygen, or may contain an inert gas such as N2 or Ar as a process gas in addition to oxygen. It is preferable that the oxygen partial pressure atmosphere is composed of only oxygen, or of only oxygen and an inert gas.
[0053] The oxygen partial pressure for the second step is 1.0×10 -5 ~1.0×10 -7 atm, preferably 1.0 × 10 -5 ~1.0×10 -6 atm, more preferably 5.0 × 10 -6 ~1.0×10 -6 atm, and when a pre-oxidized hafnium plate is heat treated, the-5 ~1.0×10 -7 atm, preferably 1.0 × 10 -5 ~1.0×10 -6 atm, more preferably 5.0 × 10 -6 ~1.0×10 -6 atm, and when pre-oxidized titanium plate is heat treated, the -5 atm, preferably 1.0 × 10 -1 ~1.0×10 -4 atm, and more preferably 1.0×10 -2 ~1.0×10 -3 It's an ATM.
[0054] By controlling the lower limit of the oxygen partial pressure to the above value, it is possible to suppress the occurrence of cracks on the surface due to the rate at which oxygen is taken in from the outside of the sheet material being excessive compared to the rate at which the oxygen taken in progresses into the sheet material. Also, by controlling the upper limit of the oxygen partial pressure to the above value, it is possible to suppress the occurrence of an insufficient amount of oxygen being taken in to the sheet material, resulting in the center of the sheet material in the thickness direction remaining as the Group 4 element layer La.
[0055] The oxygen partial pressure can be controlled by a known method, for example, by using an oxygen partial pressure controller.
[0056] The heat treatment temperature in the second step is 900 to 1100 ° C, preferably 900 to 1000 ° C, more preferably 950 to 1000 ° C, when a pre-oxidized zirconium plate is heat treated, 900 to 1100 ° C, preferably 900 to 1000 ° C, more preferably 950 to 1000 ° C, when a pre-oxidized hafnium plate is heat treated, and 700 to 1000 ° C, preferably 800 to 900 ° C, more preferably 850 to 900 ° C, when a pre-oxidized titanium plate is heat treated.
[0057] The heat treatment time for the second step is not limited to the type of Group 4 element, and is 10 minutes to 50 hours, preferably 30 minutes to 30 hours, and more preferably 2 hours to 20 hours.
[0058] The heat treatment time here refers to the time during which the heat treatment temperature is maintained after the heat treatment temperature is reached in the oxygen partial pressure atmosphere. The heat treatment time may be shortened when the heat treatment temperature is high, and may be lengthened when the heat treatment temperature is low.
[0059] By carrying out the second step, the correlation between the rate at which oxygen is taken in from the outside of the sheet material and the rate at which the oxygen taken in progresses into the sheet material is able to be controlled, thereby obtaining a transparent molded body made of a Group 4 element oxide.
[0060] According to the method for producing a transparent molded body of this embodiment, a transparent molded body can be obtained, as shown in the external photograph in Fig. 1, the cross-sectional SEM image in Fig. 2, and the TEM image in Fig. 3. Comparing Fig. 2 and Fig. 6, it is confirmed that by carrying out the second step, a plate material having a single layer of a Group 4 element oxide with a substantially homogeneous composition is formed from a plate material having multiple layers with different compositions. According to the method for producing a transparent molded body of this embodiment, a transparent molded body can be obtained by a simple process. EXAMPLES
[0061] EXAMPLES Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0062] [Example 1] A sample according to Example 1 was prepared under the following conditions, and its characteristics were evaluated.
[0063] (Sample Preparation for Example 1) First, a zirconium plate having a thickness of 20 μm was prepared. The zirconium plate used in Example 1 was 99.2 mass percent zirconium, and the remaining 0.8 mass percent was elements other than zirconium. FIG. 7 is a photograph of the appearance of the zirconium plate used in Example 1.
[0064] Next, the zirconium plate material was pre-oxidized in air to produce black zirconium oxide (BZ: Black-ZrO 2-a) was prepared. Pre-oxidation was performed by placing the sample in an electric furnace. The heat treatment temperature for pre-oxidation was 800°C, and the heat treatment time was 15 minutes. After the heat treatment, the sample was cooled in the furnace (at a rate of about 1°C / min). Figure 8 is a photograph of the appearance of the BZ.
[0065] Next, BZ was heat-treated in an oxygen partial pressure atmosphere and furnace-cooled (cooled at a rate of about 1°C / min) to produce a transparent molded body A made of zirconium oxide. The heat treatment was performed by placing the sample in an electric furnace. In addition to oxygen gas, argon gas was used as a process gas in the oxygen partial pressure atmosphere. The heat treatment was performed at a heat treatment temperature of 900°C, for a heat treatment time of 15 hours, and with an oxygen partial pressure of 1×10 -6 The transparent molded body A was produced under the conditions of 1000 MPa atm.
[0066] In order to better understand the characteristics of the transparent molded body A, which is an example of the transparent molded body according to this embodiment, the characteristics of BZ will be described.
[0067] Figure 6 is a cross-sectional SEM image of the BZ cut perpendicular to the in-plane direction and observed with a scanning electron microscope. The cross-sectional SEM image confirms that the BZ has layers with different compositions in the stacking direction. The BZ has an oxide layer on the surface side in the stacking direction, and a Group 4 element layer on the inside of the oxide layer in the stacking direction. The average thickness of the oxide layer in the BZ was 9 μm.
[0068] Figure 10 is a TEM image of a cross section of the BZ observed with a transmission electron microscope. This TEM image confirms that the BZ has equiaxed grains (average grain size: about 200 nm) in the region from the surface to about 5 μm inward, and that the portion inside from the surface to the inside of about 5 μm has a structure containing columnar crystal grains with grain sizes of several μm in the minor axis direction and several hundred μm in the major axis direction.
[0069] Figure 11(c) shows the results of X-ray diffraction (XRD) performed on the BZ. In the thin film XRD measurement, the incident angle on the sample surface was set to 1°.
[0070] From Fig. 11(c), it was confirmed that BZ has monoclinic ZrO2 and hexagonal close-packed Zr. The monoclinic ZrO2 is the composition that constitutes the layer on the surface side in the stacking direction in the cross-sectional SEM image, and the hexagonal close-packed Zr is the element that constitutes the Group 4 element layer.
[0071] 11(a) and (b) show the results of thin film XRD measurement of BrZ according to Comparative Example 1 and transparent molded body A according to Example 1, which will be described in detail later.
[0072] Fig. 12 shows the results of evaluating the composition of elements constituting the sample surface using X-ray photoelectron spectroscopy (XPS) for the BZ. For convenience of explanation, Fig. 12 also shows the analysis results (short dashed line) of white zirconium oxide (ZrO2) without oxygen deficiency according to Comparative Example 2 described later.
[0073] It is known that the results of XPS measurements of 1s orbitals are shifted to the higher energy side when oxygen vacancies are present in the sample. In the results shown in Figure 12, zirconium oxide A is also shifted to the higher energy side compared to white zirconium oxide (ZrO2). Specifically, it shows a peak in a higher energy region than the analysis results of white zirconium oxide (ZrO2), and the XPS analysis results of BZ can be interpreted as a superposition of the analysis results of the short dashed line and the analysis results of the long dashed line. In other words, it has been confirmed that oxygen vacancies exist in BZ.
[0074] (Sample Evaluation of Example 1) The transparent molded body A was subjected to the following measurements to evaluate its properties.
[0075] First, thin film XRD measurement was performed on the transparent molded body A. The thin film XRD measurement was performed at an incident angle of 1° to the sample surface. Figure 11(b) shows the results of the thin film XRD measurement on the transparent molded body A.
[0076] From Figure 11(b), it is confirmed that the transparent molded body A is composed only of ZrO2 with a monoclinic structure. In addition, the 211 peak, which is very low intensity in the JCPDS card of white zirconium oxide (ZrO2), is high intensity, and it is considered that the transparent molded body A is oriented in 11-1 and 211.
[0077] Next, the transparent molded body A was cut perpendicular to the in-plane direction, and the cut surface was observed using a scanning electron microscope. Figure 2 is a cross-sectional SEM image of the transparent molded body A. Comparing with the cross-sectional SEM image of the BZ shown in Figure 6, it is confirmed that the BZ has layers of different compositions formed in the stacking direction, whereas the transparent molded body A consists of a single layer that is uniform in the stacking direction. In other words, the transparent molded body A does not have a Group 4 element layer consisting only of Group 4 elements. Furthermore, by observing the transparent molded body A, it is confirmed that dense crystal grains are formed that cannot be observed even in the cross-sectional SEM image.
[0078] Next, a cross section of the transparent molded body A was observed using a transmission electron microscope. FIG.
[0079] In the TEM image of transparent molded body A, the area from the surface to about 2 μm inward was made up of equiaxed crystal grains. In addition, the area inside from the surface to about 2 μm inward contained columnar crystal grains whose average length in the major axis direction was longer than that of the equiaxed crystal grains. The columnar crystal grains of transparent molded body A also showed high orientation.
[0080] Next, the transparent molded body A was evaluated for the composition of elements constituting the sample surface using XPS. FIG. 13 shows the results of evaluating the composition of elements constituting the sample surface using XPS for the transparent molded body A. For convenience of explanation, FIG. 13 also shows the analysis result (short dashed line) of white zirconium oxide (ZrO2) according to Comparative Example 2 described later. It is known that the result of XPS measurement of 1s orbital shows high strength even in the high energy region when oxygen vacancies exist in the sample, and the XPS analysis result of the transparent molded body A has high strength even in the high energy region compared to the analysis result of white zirconium oxide (ZrO2). The long dashed line in FIG. 13 is a line drawn for convenience to explain that the transparent molded body A has high strength even in the high energy region, and the XPS analysis result of the transparent molded body A can be roughly calculated as the sum of the long dashed line and the short dashed line. That is, it is confirmed that oxygen vacancies are also generated in the transparent molded body A. Incidentally, the peak intensity in the high energy region is higher in BZ than in transparent molded body A, and it is considered that transparent molded body A has a smaller amount of oxygen vacancy than BZ.
[0081] [Example 2] A sample (transparent molded body B) according to Example 2 was produced under the following conditions, and its characteristics were evaluated.
[0082] (Sample Preparation for Example 2) In Example 2, the oxygen partial pressure when the BZ is heat-treated in an oxygen partial pressure atmosphere is set to 1×10 -5 A transparent molded body B was produced under the same conditions as in Example 1, except that the pressure was changed to atm. FIG.
[0083] (Sample Evaluation of Example 2) The transmittance was measured for the transparent molded body B. The transmittance was measured using an ultraviolet, visible, and infrared spectrometer (manufacturer: Shimadzu Corporation, device name: UV-3600).
[0084] Fig. 15 is a graph showing the results of measuring the transmittance, and Fig. 16 is an enlarged view of Fig. 15 in the region up to a wavelength of 1000 nm. The summary of the results of measuring the transmittance is summarized in Table 1.
[0085] [Table 1]
[0086] The transparent molded body B had a transmittance of 47% at a wavelength of 600 nm. It has been confirmed that the transmittance can be further improved by controlling the amount of oxygen vacancies and by making the crystal grains finer and denser. For example, it has been confirmed that the transparent molded body A according to Example 1 has a higher transmittance than the transparent molded body B according to Example 2.
[0087] [Comparative Example 1] Brown zirconium oxide (BrZ) according to Comparative Example 1 was prepared under the following conditions. 2-b ) was fabricated and its properties were evaluated.
[0088] (Preparation of Sample for Comparative Example 1) In Comparative Example 1, in the step of heat treating the BZ, the heat treatment temperature was 1000° C., the heat treatment time was 10 hours, and the oxygen partial pressure was 1×10 -10 Except for changing the pressure to atm, BrZ was produced under the same conditions as in Example 1. Figure 17 is a photograph of the appearance of BrZ.
[0089] (Sample Evaluation of Comparative Example 1) First, thin-film XRD measurement was performed on BrZ. The thin-film XRD measurement was performed with the incident angle to the sample surface set at 1°. Figure 11(a) shows the results of the thin-film XRD measurement on BrZ.
[0090] From Fig. 11(a), it was confirmed that BrZ has ZrO2 with a monoclinic structure, Zr with a hexagonal close-packed structure, and ZrO with a cubic structure. In other words, BrZ has a portion made of Zr and a portion made of ZrO.
[0091] Next, the BrZ was cut perpendicular to the in-plane direction, and the cut surface was observed using a scanning electron microscope. Figure 18 is a cross-sectional SEM image of the BrZ. It was confirmed that the BrZ has layers with different compositions in the stacking direction. The BrZ has an oxide layer on the surface side in the stacking direction, and a Group 4 element layer on the inside of the oxide layer in the stacking direction. The average thickness of the oxide layer of the BrZ was 10 μm.
[0092] [Comparative Example 2] White zirconium oxide (WZ: White-ZrO2) according to Comparative Example 2 was produced under the following conditions, and its characteristics were evaluated.
[0093] (Preparation of Sample for Comparative Example 2) In Comparative Example 2, a WZ was produced by oxidizing only in air a zirconium plate having the same composition as in Example 1. The oxidation of the zirconium plate was carried out under the conditions of a heat treatment temperature of 1100° C. and a heat treatment time of 1 hour. FIG. 19 is a photograph of the appearance of the WZ.
[0094] (Sample Evaluation of Comparative Example 2) First, the WZ was cut perpendicular to the in-plane direction, and the cut surface was observed using a scanning electron microscope. Figure 20 shows a cross-sectional SEM image of the WZ. The cross-sectional SEM image confirms that numerous cracks have appeared throughout the sample, causing embrittlement, due to volume expansion and contraction accompanying temperature changes. The cracks and voids are thought to originate from grain boundaries.
[0095] Next, the cross section of the WZ was observed using a transmission electron microscope. The TEM image of the WZ is shown in Figure 21. The white areas observed in the TEM image of the WZ are cracks or voids.
[0096] In the TEM image of the WZ, the entire area, that is, from the surface to the inside, was equiaxed with a grain size of several hundred nm. No other grains, such as columnar grains, were observed in the WZ. Cracks and voids were generated within the grains, and cracks and voids were also generated from the grain boundaries.
[0097] [Reference example] 22(a) and 22(b) are photographs of the appearance of samples prepared under other conditions. The sample shown in Fig. 22(a) was prepared by subjecting the BZ to a heat treatment temperature of 1000°C, a heat treatment time of 1 hour, and an oxygen partial pressure of 1 × 10 -10 The sample shown in FIG. 22(b) was fabricated under the same conditions as in Example 1, except that the BZ was heat-treated at a temperature of 900° C. for 20 hours and at an oxygen partial pressure of 1×10 -10 This sample was heat-treated at 1000 MPa (atm). In the oxygen partial pressure atmosphere, argon gas was used as the process gas in addition to oxygen gas. After the heat treatment, the sample was furnace-cooled (cooled at a rate of about 1°C / min). Under these heat treatment conditions, a transparent molded body could not be obtained. [Industrial Applicability]
[0098] The transparent molded article of the present invention is a material with excellent transmittance in the visible light range, and can be produced in complex shapes by a simple process, so it can be used in a wide range of fields, such as decorative materials, window materials, exterior parts for electronic devices, cosmetic dentistry materials, etc. In particular, the transparent molded article in which the Group 4 element is hafnium can be expected to be used as a high dielectric constant material. [Explanation of symbols]
[0099] 100: Transparent molding 10:Equiaxed grain 20: Columnar grains L1: Surface layer L2:Inner layer La: Group 4 element layer Lb: Oxide layer
Claims
1. A transparent molded article made of a Group 4 element oxide, which is in the form of a plate, foil, or thin film and has a thickness of 5 μm or more and 2 mm or less, Composition formula AO 2-x (A is Zr or Hf, x is the amount of oxygen deficiency, and 0<x<0.2), No Group 4 element layer made of a Group 4 element is provided, It has a monoclinic crystal structure, A transparent molded article made of an oxide of a Group 4 element, comprising a surface layer containing equiaxed crystal grains, and an internal layer located inside the surface layer and containing columnar crystal grains having an average length in the major axis direction longer than that of the equiaxed crystal grains.
2. 2. The transparent molded article made of a Group 4 element oxide according to claim 1, wherein the columnar crystal grains have an average crystal grain size in the major axis direction of 100 nm to 5 μm and an average crystal grain size in the minor axis direction of 10 to 1000 nm.
3. 3. The transparent molded article made of a Group 4 element oxide according to claim 1, wherein the amount of a third element other than the element represented by A in the composition formula and oxygen is 0.8 mass percent or less.
4. A method for producing a transparent molded article made of a Group 4 element oxide and having a plate, foil, or thin film shape, comprising the steps of: Composition formula ZrO 2-x (x represents the amount of oxygen deficiency, and x≧0), No Group 4 element layer made of a Group 4 element is provided, A method for producing a transparent molded body having a monoclinic structure, comprising the steps of: A first step of preheating a substrate made of zirconium at 600 to 900° C. for 10 minutes to 5 hours; The pre-oxidized substrate was heated at 900 to 1100°C under an oxygen partial pressure of 1.0×10 -5 ~1.0 x 10 -7 a second step of heating at 1000 MPa for 10 minutes to 50 hours; The method for producing a transparent molded article made of an oxide of a Group 4 element, wherein the substrate is in the form of a plate, foil, or thin film.
5. A method for producing a transparent molded article made of a Group 4 element oxide and having a plate, foil, or thin film shape, comprising the steps of: Composition formula HfO 2-x (x represents the amount of oxygen deficiency, and x≧0), No Group 4 element layer made of a Group 4 element is provided, A method for producing a transparent molded body having a monoclinic structure, comprising the steps of: A first step of preheating a substrate made of hafnium at 700 to 1000° C. for 10 minutes to 5 hours; The pre-oxidized substrate was heated at 900 to 1100°C under an oxygen partial pressure of 1.0×10 -5 ~1.0 x 10 -7 a second step of heating at 1000 MPa for 10 minutes to 50 hours; The method for producing a transparent molded article made of an oxide of a Group 4 element, wherein the substrate is in the form of a plate, foil, or thin film.
6. The method for producing a transparent molded article according to claim 4 or 5, wherein the thickness of the substrate is from 5 μm to 2 mm.
Citation Information
Patent Citations
Transparent ceramic, its producing method, and optical element using the transparent ceramics
JP2010047460A
Transparent zirconia sintered body, method for producing the same, and use of the same
JP2011051881A
High-strength transparent zirconia sintered body
JP2011102227A
Conductive molding comprising group 4 element oxide, inclined material containing the same, and method for producing the same
JP2019153424A
PROCESS FOR PRODUCING RUTILE (TiO2) SINGLE CRYSTAL, RUTILE (TiO2) SINGLE CRYSTAL, AND OPTICAL ISOLATOR COMPRISING THE SAME
WO2007052632A1