Method for producing modified carbide particles and composition

By modifying carbide particles with an oxidizing agent and surface modifier, the method addresses poor filling properties, enhancing their affinity with resin binders and improving material performance through reduced microvoids.

JP7595489B2Active Publication Date: 2024-12-06FUJIFILM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021037952
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-10
Publication Date
2024-12-06
Estimated Expiration
2041-03-10

AI Technical Summary

Technical Problem

Carbide particles used in materials with resin binders often exhibit poor filling properties, leading to insufficient affinity with other components and the formation of microvoids, which hinders the realization of their expected performance.

Method used

A method involving the modification of carbide particles by contacting them with an oxidizing agent in an aqueous solution, followed by a surface modification step using a surface modifier, to enhance their affinity with resin binders and reduce microvoids.

Benefits of technology

The modified carbide particles demonstrate improved filling properties, resulting in materials with higher specific gravity and enhanced performance due to reduced microvoids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595489000001
    Figure 0007595489000001
Patent Text Reader

Abstract

To provide a production method for a modified carbide particle excellent in a filling property and a composition relating to the production method for the modified carbide particle.SOLUTION: A production method for a modified carbide particle comprises a modification step of bringing a carbide particle and an oxidizing agent into contact with each other in an aqueous solution to obtain the modified carbide particle.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to methods for making modified carbide particles and compositions. [Background technology]

[0002] Carbide particles have a wide variety of industrial uses, including, for example, materials in which carbide particles are dispersed using a resin as a binder. For example, Patent Document 1 discloses a paste-like resin composition containing an epoxy resin, a liquid hardener, a thermally conductive filler including silicon carbide or the like, and a dispersant (claims 1 and 6). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 181737 Summary of the Invention [Problem to be solved by the invention]

[0004] In Patent Document 1, silicon carbide is used to improve the thermal conductivity of a cured product formed from the composition, but carbide particles have a variety of other uses. The present inventors have examined materials containing carbide particles (e.g., materials containing carbide particles and a resin binder), such as materials produced using the composition described in Patent Document 1, and have found that there is room for improvement in the filling properties of the carbide particles when they are dispersed in a material, and that in many cases the carbide particles are unable to fully perform the functions expected of them.

[0005] Therefore, an object of the present invention is to provide a method for producing modified carbide particles having excellent packing properties, and a further object of the present invention is to provide a composition related to the method for producing the modified carbide particles. [Means for solving the problem]

[0006] As a result of intensive research by the present inventors to solve the above problems, they have found that the above problems can be solved by the following configuration.

[0007] [1] A method for producing modified carbide particles, comprising a modification step of contacting carbide particles with an oxidizing agent in an aqueous solution to obtain modified carbide particles. [2] The method for producing modified carbide particles according to [1], wherein the standard oxidation-reduction potential of the oxidizing agent is 1.50 V or more. [3] The method for producing modified carbide particles according to [1] or [2], wherein the oxidizing agent is a persulfate. [4] The method for producing modified carbide particles according to any one of [1] to [3], wherein the aqueous solution has a pH of 12 or more. [5] contacting the modified carbide particles obtained in the modification step with a surface modifier in the presence of at least one of water and an organic solvent, A method for producing modified carbide particles according to any one of [1] to [4], comprising an adsorption step of obtaining modified carbide particles modified with the surface modifier. [6] The method for producing modified carbide particles according to any one of [1] to [5], wherein the carbide particles are one or more particles selected from the group consisting of silicon carbide particles, boron carbide particles, titanium carbide particles, and tungsten carbide particles. [7] A composition comprising modified carbide particles produced by the method for producing modified carbide particles according to any one of [1] to [5], and a resin binder or a precursor thereof. Effect of the Invention

[0008] According to the present invention, a method for producing modified carbide particles having excellent packing properties can be provided. Furthermore, a composition related to the method for producing the modified carbide particles can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for producing modified carbide particles of the present invention will now be described in detail. The following description of the configuration may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment.

[0010] In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0011] In this specification, when referring to values ​​of matters that may change depending on temperature (e.g., standard oxidation-reduction potential, pH, etc.), unless otherwise specified, the value is intended to be the value at 25° C. For example, when referring to the volume of water, the volume is intended to be the volume at 25° C., unless otherwise specified. In this specification, "pH" refers to a pH measured using a known pH meter according to a method in accordance with JIS Z8802-1984. The pH measurement temperature is 25°C. In this specification, "room temperature" is 25°C unless otherwise specified.

[0012] In this specification, the term "(meth)acryloyl group" means "either one or both of an acryloyl group and a methacryloyl group", and the term "(meth)acrylamide group" means "either one or both of an acrylamide group and a methacrylamide group".

[0013] In this specification, the acid anhydride group may be a monovalent group or a divalent group. When the acid anhydride group represents a monovalent group, examples of the substituents include those obtained by removing any hydrogen atom from acid anhydrides such as maleic anhydride, phthalic anhydride, pyromellitic anhydride, and trimellitic anhydride. When the acid anhydride group represents a divalent group, the group represented by *-CO-O-CO-* is intended (* represents a bond position).

[0014] In this specification, for substituents and the like that are not specified as substituted or unsubstituted, if possible, the group may further have a substituent (for example, a group of substituents Y described below) to the extent that the intended effect is not impaired. For example, the expression "alkyl group" means a substituted or unsubstituted alkyl group (an alkyl group that may have a substituent) to the extent that the intended effect is not impaired. In addition, in the present specification, when it is stated that "the group may have a substituent", the type of the substituent, the position of the substituent, and the number of the substituent are not particularly limited. The number of the substituents can be, for example, 1 or 2 or more. The substituents can be, for example, a monovalent nonmetallic atomic group other than a hydrogen atom, and are preferably a group selected from the following group of substituents Y. In this specification, examples of halogen atoms include a chlorine atom, a fluorine atom, a bromine atom, and an iodine atom.

[0015] Substituent group Y: Halogen atoms (-F, -Br, -Cl, -I, etc.), hydroxyl groups, amino groups, carboxylic acid groups and their conjugate base groups, carboxylic anhydride groups, cyanate ester groups, unsaturated polymerizable groups, epoxy groups, oxetanyl groups, aziridinyl groups, thiol groups, isocyanate groups, thioisocyanate groups, aldehyde groups, alkoxy groups, aryloxy groups, alkylthio groups, arylthio groups, alkyldithio groups, aryldithio groups, N-alkylamino groups, N,N-dialkylamino groups, N-arylamino groups, N,N-diarylamino groups, N-alkyl-N-arylamino groups, acyloxy group, carbamoyloxy group, N-alkylcarbamoyloxy group, N-arylcarbamoyloxy group, N,N-dialkylcarbamoyloxy group, N,N-diarylcarbamoyloxy group, N-alkyl-N-arylcarbamoyloxy group, alkylsulfoxy group, arylsulfoxy group, acylthio group, acylamino group, N-alkylacylamino group, N-arylacylamino group, ureido group, N'-alkylureido group, N',N'-dialkylureido group, N'-arylureido group, N',N'-diarylureido group, N'-alkyl-N'-arylureido group, N-alkylureido group, N-arylureido group, N'-alkyl-N-alkylureido group, N'-alkyl-N-arylureido group, N',N'-dialkyl-N-alkylureido group, N',N'-dialkyl-N-arylureido group, N'-aryl-N-alkylureido group, N'-aryl-N-arylureido group, N',N'-diaryl-N-alkylureido group, N',N'-diaryl-N-arylureido group, N'-alkyl-N'-aryl-N-alkylureido group , N'-alkyl-N'-aryl-N-arylureido group, alkoxycarbonylamino group, aryloxycarbonylamino group, N-alkyl-N-alkoxycarbonylamino group, N-alkyl-N-aryloxycarbonylamino group, N-aryl-N-alkoxycarbonylamino group, N-aryl-N-aryloxycarbonylamino group, formyl group, acyl group, alkoxycarbonyl group, aryloxycarbonyl group, carbamoyl group, N-alkylcarbamoyl group, N,N-dialkylcarbamoyl group, N-arylcarbamoyl group, N,N-diarylcarbamoyl group, N-alkyl-N-arylcarbamoyl group, alkylsulfinyl group, arylsulfinyl group, alkylsulfonyl group, arylsulfonyl group, sulfo group (-SO3H) and its conjugate base group, alkoxysulfonyl group, aryloxysulfonyl group, sulfinamoyl group, N-alkylsulfinamoyl group, N,N-dialkylsulfinamoyl group, N-arylsulfinamoyl group, N,N-diarylsulfinamoyl group, N-alkyl-N-arylsulfinamoyl group, sulfamoyl group, N-alkylsulfamoyl group, N,N-dialkylsulfamoyl group, N-arylsulfamoyl group, N,N-diarylsulfamoyl group, N-alkyl-N-arylsulfamoyl group, N-acylsulfamoyl group and its conjugate base group, N-alkylsulfonylsulfamoyl group (-SO2NHSO2(alkyl)) and its conjugate base group, N-arylsulfonylsulfamoyl group (-SO2NHSO2(aryl)) and its conjugate base group, N-alkylsulfonylcarbamoyl group (-CONHSO2(alkyl)) and its conjugate base group, N-arylsulfonylcarbamoyl group (-CONHSO2(aryl)) and its conjugate base group, alkoxysilyl group (-Si(Oalkyl)3), aryloxysilyl group (-Si(Oaryl)3), hydroxysilyl group (-Si(OH)3) and its conjugate base group, phosphono group (-PO3H2) and its conjugate base group, dialkylphosphono group (-PO3(alkyl) 2), diarylphosphono group (-PO3(aryl)2), alkylarylphosphono group (-PO3(alkyl)(aryl)), monoalkylphosphono group (-PO3H(alkyl)) and its conjugate base group, monoarylphosphono group (-PO3H(aryl)) and its conjugate base group, phosphonooxy group (-OPO3H2) and its conjugate base group, dialkylphosphonooxy group (-OPO3(alkyl)2), diarylphosphonooxy group (-OPO3(aryl)2), alkylarylphosphonooxy group (-OPO3(alkyl)(aryl)), monoalkylphosphonooxy group (-OPO3H(alkyl)) and its conjugate base group, monoarylphosphonooxy group (-OPO3H(aryl)) and its conjugate base group, cyano group, nitro group, aryl group, alkenyl group, alkynyl group, and alkyl group. Each of the above groups may further have a substituent (e.g., one or more of the above groups) if possible. For example, an aryl group which may have a substituent is also included as a group which can be selected from the substituent group Y. When the group selected from the substituent group Y has a carbon atom, the group has 1 to 20 carbon atoms, for example. The number of atoms other than hydrogen atoms contained in the group selected from the substituent group Y is, for example, 1 to 30. Furthermore, these substituents may or may not form a ring by bonding with each other or with a group that substitutes them, if possible. For example, an alkyl group (or an alkyl group portion in a group that contains an alkyl group as a partial structure, such as an alkoxy group) may be a cyclic alkyl group (cycloalkyl group) or an alkyl group having one or more cyclic structures as a partial structure.

[0016] [Method of manufacturing modified carbide particles] The method for producing modified carbide particles in the present invention (hereinafter also referred to as "the method of the present invention") includes a modification step of contacting carbide particles with an oxidizing agent in an aqueous solution to obtain modified carbide particles. The mechanism by which the problem of the present invention is solved by adopting such a configuration is not necessarily clear, but the present inventors speculate as follows. Although carbide particles have excellent properties in various respects, ordinary carbide particles often have insufficient packing properties. That is, for example, the measured specific gravity of a material containing ordinary carbide particles is significantly lower than the ideal specific gravity calculated from the content ratio of each component contained in the composition used to form the material, and the difference is also large. This is believed to be due to the fact that ordinary carbide particles have insufficient affinity with other components constituting the material containing carbide particles or their precursors (such as resin binders or their precursors). In other words, due to such insufficient affinity, it is believed that in materials containing ordinary carbide particles, many tiny gaps (microvoids) are generated between the carbide particles and other materials in the material. The presence of such microvoids may hinder the realization of various performances expected of carbide particles and materials containing carbide particles. Therefore, in the method of the present invention, the carbide particles are surface-modified by contacting them with an oxidizing agent in an aqueous solution. It is believed that the modified carbide particles obtained by the method of the present invention have improved affinity with other components or their precursors constituting the material containing the modified carbide particles, have good packing properties, and are able to reduce the presence of microvoids in the material formed. As a result, the material produced using the composition containing the modified carbide particles obtained by the method of the present invention has a high specific gravity, and it is believed that the performance expected of carbide particles and materials containing carbide particles can be realized to a higher degree. Hereinafter, when the packing property of the modified carbide particles produced by the method of the present invention is superior, this is also referred to as when the effect of the present invention is superior.

[0017] [Manufacturing method] The production method of the present invention includes at least a modification step. It is also preferred that the method of the present invention further comprises an adsorption step.

[0018] <Denaturation process> The modification step is a step in which the carbide particles are contacted with an oxidizing agent in an aqueous solution to obtain modified carbide particles. The pH of the aqueous solution is, for example, greater than 7, preferably greater than 10, more preferably greater than 12, particularly preferably greater than 13, and most preferably greater than 13. There is no upper limit to the pH of the aqueous solution, and it is, for example, 14 or less. The pH of the aqueous solution means the pH of the aqueous solution in a state in which the carbide particles and the oxidizing agent are contained, that is, the aqueous solution contains at least water, the carbide particles, and the oxidizing agent.

[0019] The time for which the carbide particles are contacted with the oxidizing agent in the aqueous solution is preferably from 0.1 to 24 hours, more preferably from 0.5 to 10 hours, and even more preferably from 1.5 to 6 hours. The temperature of the aqueous solution when the carbide particles are brought into contact with the oxidizing agent is preferably from 1 to 95°C, more preferably from 25 to 80°C, and even more preferably from 45 to 65°C.

[0020] There are no limitations on the method of contacting the carbide particles with the oxidizing agent in the aqueous solution, and examples of the method include a method of contacting the carbide particles with the oxidizing agent by mixing using a grinding machine or disintegrator such as a rocking mill, a piece mill, a ball mill, a Henschel mixer, a jet mill, a Starburst, or a paint conditioner, a method of contacting the carbide particles with the oxidizing agent while stirring using a mechanical stirrer such as a Three-One Motor or a magnetic stirrer, and a method of contacting the carbide particles with an aqueous oxidizing agent solution containing the oxidizing agent, while circulating the aqueous oxidizing agent solution using a pump in a cartridge filled with the carbide particles. In addition, as a method for contacting the carbide particles with the oxidizing agent in the aqueous solution, a method that does not destroy the carbide particles or modified carbide particles in the aqueous solution as much as possible may be selected. The destruction referred to here includes, for example, destruction of the aggregated form of the carbide particles to be treated, when the carbide particles are aggregated carbide particles.

[0021] It is preferable that after the carbide particles are contacted with the oxidizing agent in the aqueous solution, the resulting modified carbide particles are taken out from the aqueous solution. There is no limitation on the method for extracting the modified carbide particles from the aqueous solution. For example, the aqueous solution may be filtered to separate (filter) the modified carbide particles as a residue. It is also preferable to wash the extracted modified carbide particles with water and / or an organic solvent.

[0022] (Carbide particles) The aqueous solution contains carbide particles. The carbide particles may be particles substantially composed of carbide. For example, the content of carbide in the carbide particles is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more, based on the total mass of the carbide particles. The upper limit of the content is not particularly limited, but is, for example, 100% by mass or less. The carbide is a compound of carbon and an element that is more electropositive than carbon, and is preferably a compound of carbon and a metal (including metalloid elements such as silicon and boron), more preferably a compound of carbon and a transition metal or metalloid, and is more preferably one or more selected from the group consisting of silicon carbide, boron carbide, titanium carbide, tungsten carbide, iron carbide, vanadium carbide, tantalum carbide, zirconium carbide, nickel carbide, molybdenum carbide, niobium carbide, chromium carbide, and hafnium carbide, and is particularly preferably one or more selected from the group consisting of silicon carbide, boron carbide, titanium carbide, and tungsten carbide. The carbide may be an interstitial carbide, a covalent carbide, or an ionic carbide, with the covalent carbide being preferred among the interstitial carbides. The carbide particles may contain one type of the above carbides alone or two or more types. The carbide particles are preferably one or more selected from the group consisting of silicon carbide particles, boron carbide particles, titanium carbide particles, tungsten carbide particles, iron carbide particles, vanadium carbide particles, tantalum carbide particles, zirconium carbide particles, nickel carbide particles, molybdenum carbide particles, niobium carbide particles, chromium carbide particles, and hafnium carbide particles, and more preferably one or more selected from the group consisting of silicon carbide particles, boron carbide particles, titanium carbide particles, and tungsten carbide particles. These carbide particles are preferably particles in which a predetermined carbide (for example, silicon carbide in silicon carbide particles) is the main component (the component with the largest amount) of the particles. For example, the content of the predetermined carbide is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more, based on the total mass of the particles. The upper limit of the content is not particularly limited, but is, for example, 100% by mass or less. The carbide particles may be used alone or in combination of two or more kinds.

[0023] The shape of the carbide particles is not particularly limited, and may be any of a scale shape, a plate shape, a rice grain shape, a spherical shape, a cubic shape, a spindle shape, and an irregular shape. The carbide particles may be aggregated particles (secondary particles) formed by aggregation of fine particles of these shapes. The aggregated particles may be, for example, spherical or irregular in shape as a whole.

[0024] The size of the carbide particles (if the carbide particles are secondary particles, the size as secondary particles) is not particularly limited. In particular, in terms of better dispersibility of the carbide particles, the particle diameter of the carbide particles (usually the average primary particle diameter, if the carbide particles are secondary particles, the average particle diameter as secondary particles) is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 60 μm or less. The lower limit of the particle diameter is not particularly limited, but in terms of handleability, it is preferably 100 nm or more, more preferably 500 nm or more, and even more preferably 1 μm or more. In this specification, when a commercially available product is used, the value in the catalog is used as the particle size. If there is no catalog value, the particle size is measured by randomly selecting 100 inorganic particles using an electron microscope, measuring the particle size (major axis) of each inorganic particle, and calculating the arithmetic average.

[0025] The content of the carbide particles in the aqueous solution is not limited, and is, for example, 0.1 to 10,000 parts by mass, preferably 0.1 to 100 parts by mass, more preferably 1 to 30 parts by mass, and even more preferably 3 to 20 parts by mass, relative to 100 parts by mass of water in the aqueous solution. The carbide particles may be used alone or in combination of two or more kinds.

[0026] (water) The aqueous solution contains water. The content of water in the aqueous solution is preferably 20 to 99% by mass, more preferably 50 to 95% by mass, and even more preferably 65 to 90% by mass, based on the total mass of the aqueous solution.

[0027] (Oxidizing agent) The aqueous solution contains an oxidizing agent. The oxidizing agent is not limited, and examples thereof include persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate; nitrates such as cerium ammonium nitrate, sodium nitrate, and ammonium nitrate; peroxides such as hydrogen peroxide and tert-butyl hydroperoxide; permanganates such as potassium permanganate; divalent copper compounds and transition metal compounds; hypervalent iodine compounds such as potassium periodate and sodium periodate; quinone compounds such as benzoquinone, naphthoquinone, anthraquinone, and chloranil; and salts of halogen oxoacids such as sodium hypochlorite and sodium chlorite. Among these, the oxidizing agent preferably contains a persulfate, and more preferably is a persulfate. In addition, a catalyst may be used in addition to the oxidizing agent to assist the action of the oxidizing agent. Examples of the catalyst include divalent iron compounds (FeSO4, etc.) and trivalent iron compounds. The oxidizing agent and / or the catalyst may be a hydrate.

[0028] The standard redox potential of the oxidizing agent is preferably 0.30 V or more, more preferably 1.50 V or more, further preferably 1.70 V or more, and particularly preferably 1.80 V or more. There is no upper limit to the standard redox potential of the oxidizing agent, and it is preferably, for example, 4.00 V or less, and more preferably 2.50 V or less. The above standard oxidation-reduction potentials are based on the standard hydrogen electrode.

[0029] The content of the oxidizing agent in the aqueous solution is preferably 0.05 to 20 parts by mass, more preferably 0.1 to 20 parts by mass, and even more preferably 1 to 20 parts by mass, relative to 100 parts by mass of water in the aqueous solution. The oxidizing agent may be used alone or in combination of two or more kinds. When the aqueous solution contains a catalyst, the content thereof is preferably 0.005 to 2 parts by mass, more preferably 0.01 to 2 parts by mass, and even more preferably 0.1 to 2 parts by mass, relative to 100 parts by mass of water in the aqueous solution. The content of the catalyst in the aqueous solution is preferably 0.1 to 80 parts by mass, more preferably 1 to 50 parts by mass, and even more preferably 5 to 20 parts by mass, relative to 100 parts by mass of the oxidizing agent in the aqueous solution. The catalyst may be used alone or in combination of two or more. The amount of the oxidizing agent to be brought into contact with the carbide particles is preferably 0.1 to 1000 parts by mass, more preferably 1 to 250 parts by mass, and even more preferably 15 to 120 parts by mass, per 100 parts by mass of the carbide particles.

[0030] (Alkaline source) The aqueous solution preferably contains an alkali source in addition to the above-mentioned components in order to adjust the pH of the aqueous solution. The alkali source includes, for example, inorganic bases such as alkali metal hydroxides (eg, sodium hydroxide) and alkaline earth metal hydroxides; and organic bases. The content of the alkali source in the aqueous solution may be appropriately adjusted so that the pH of the aqueous solution can be adjusted to a desired temperature, and is, for example, 0.1 to 10 parts by mass per 100 parts by mass of water in the aqueous solution.

[0031] <Adsorption process> The adsorption step is a step of contacting the modified carbide particles obtained in the modification step with a surface modifier in the presence of at least one of water and an organic solvent to obtain modified carbide particles modified with the surface modifier. Here, the modified carbide particles modified with a surface modifier are particularly referred to as surface-modified carbide particles. The surface-modified carbide particles refer to modified carbide particles in a surface-modified state by adsorbing a surface modifier, and the surface-modified carbide particles are also included in the modified carbide particles. In addition, modified carbide particles that have not been surface-modified, and the portions of surface-modified carbide particles other than the surface modifier, are also referred to as oxidized carbide particles. That is, the surface-modified carbide particles are materials that include oxidized carbide particles and a surface modifier adsorbed onto the surfaces of the oxidized carbide particles.

[0032] The adsorption step is carried out in a mixed liquid containing at least one of the water and the organic solvent, the modified carbide particles obtained in the modification step, and the surface modifier. The time for which the modified carbide particles (such as oxidized carbide particles) obtained in the modification step are contacted with the surface modifier in the mixed liquid is preferably 0.1 to 24 hours, more preferably 0.5 to 10 hours, and even more preferably 1.5 to 6 hours. The temperature of the mixture when the modified carbide particles (such as oxidized carbide particles) obtained in the modification step are brought into contact with the surface modifier varies depending on the type of surface modifier, but is preferably, for example, 1 to 200°C, more preferably 10 to 160°C, and even more preferably 15 to 140°C.

[0033] There is no limitation on the method of contacting the modified carbide particles (oxide carbide particles, etc.) obtained in the modification step with the surface modifier in the mixed liquid, and examples of the method include a method of contacting them while stirring using a mechanical stirrer such as a three-one motor or a magnetic stirrer, and a method of contacting them while circulating a solution of the surface modifier in a cartridge filled with the modified carbide particles using a pump, etc. Note that even if, during the method of contacting them while circulating, a part of the solution of the surface modifier is in contact with the modified carbide particles filled in the cartridge and another part of the solution of the surface modifier is present in the pump or the like and is not in contact with the modified carbide particles, all of the modified carbide particles and the solution of the surface modifier provided to the adsorption step are considered to be the mixed liquid as a whole. In addition, as a method for contacting the modified carbide particles (such as oxidized carbide particles) obtained in the modification step with a surface modifier, a method may be selected that destroys the modified carbide particles as little as possible in the mixed liquid.

[0034] The modified carbide particles (such as oxidized carbide particles) obtained in the modification step may be contacted with a surface modifier in the mixed liquid, and then the obtained surface-modified carbide particles may be taken out of the mixed liquid. There is no limitation on the method for extracting the surface-modified carbide particles from the mixed liquid. For example, the mixed liquid may be filtered to separate (collect) the surface-modified carbide particles as a residue. It is also preferable to wash the extracted surface-modified carbonized particles with water and / or an organic solvent. The washed surface-modified carbide particles are also preferably subjected to a drying treatment using an oven or the like. In addition, the above-mentioned mixed liquid may contain solid components other than the modified carbide particles that constitute the composition described below (such as all or part of a resin binder such as an epoxy compound described below or its precursor), and for example, surface-modified carbide particles may be produced in the composition at the same time as the composition is produced.

[0035] (Organic solvent) Examples of the organic solvent used in the adsorption step include methanol, ethanol, 2-propanol, acetonitrile, cyclopentanone, cyclohexanone, ethyl acetate, methyl ethyl ketone, dichloromethane, and tetrahydrofuran. When an organic solvent is used in the adsorption step, the content of the organic solvent is preferably 5 to 99 mass%, more preferably 20 to 90 mass%, and even more preferably 30 to 80 mass%, relative to the total mass of the mixture when the modified carbide particles (such as oxidized carbide particles) obtained in the modification step are contacted with the surface modifier. The organic solvent may be used alone or in combination of two or more kinds.

[0036] (water) When water is used in the adsorption step, the content of water relative to the total mass of the mixed liquid when the modified carbide particles (such as oxidized carbide particles) obtained in the modification step are contacted with the surface modifier is preferably 5 to 99 mass%, more preferably 20 to 90 mass%, and even more preferably 30 to 80 mass%.

[0037] The total content of water and organic solvent relative to the total mass of the mixed liquid when the modified carbide particles (such as oxidized carbide particles) obtained in the modification step are contacted with the surface modifier is preferably 5 to 99 mass%, more preferably 20 to 90 mass%, and even more preferably 30 to 80 mass%.

[0038] (Modified carbide particles obtained in the modification process) In the adsorption step, the modified carbide particles obtained in the above modification step are used. The modified carbide particles obtained in the above modification step are usually oxidized carbide particles. The amount of the modified carbonized particles obtained in the modification step is, for example, preferably 1 to 100 parts by mass, more preferably 10 to 80 parts by mass, and even more preferably 30 to 70 parts by mass, per 100 parts by mass of the total content of water and the organic solvent.

[0039] (Surface Modifier) In the adsorption step, a surface modifier is used. The surface modifier is a compound capable of modifying the surface of inorganic components (particularly carbide oxide particles). In this specification, the term "surface modification" refers to a state in which an organic substance is adsorbed on at least a part of the surface of an inorganic component (such as oxidized carbide particles). The form of adsorption is not particularly limited as long as it is in a bonded state. In other words, the surface modification also includes a state in which an organic group obtained by part of the organic substance being detached is bonded to the surface of the inorganic component (such as oxidized carbide particles). The bond may be any bond such as a covalent bond, a coordinate bond, an ionic bond, a hydrogen bond, a van der Waals bond, and a metallic bond. The surface modification may be such that a monolayer is formed on at least a part of the surface. The monolayer is a monolayer film formed by chemical adsorption of organic molecules, and is known as a Self-Assembled MonoLayer (SAM). In this specification, the surface modification may be only a part of the surface of the inorganic substance (such as oxidized carbide particles) or the entire surface.

[0040] As the surface modifier, for example, a metal coupling agent, a resin, a carboxylic acid such as a long-chain alkyl fatty acid, an organic phosphonic acid, an organic phosphate ester, or other conventionally known surface modifiers can be used. In addition, for example, the surface modifiers described in JP 2009-502529 A, JP 2001-192500 A, Japanese Patent No. 4694929, paragraphs

[0021] to

[0093] of WO 2018 / 004660, paragraphs

[0020] to

[0065] of WO 2019 / 013325, paragraphs

[0020] to

[0067] of WO 2019 / 013261, and paragraphs

[0020] to

[0087] of WO 2019 / 013323 may be used.

[0041] Metal coupling agents The surface modifier is preferably a metal coupling agent. Metal coupling agents are compounds that have a hydrolyzable group directly bonded to a metal atom. Examples of the metal atom include Si, Ti, Zr, and Al. Examples of the hydrolyzable group include an alkoxy group (preferably having 1 to 10 carbon atoms) and a halogen atom such as a chlorine atom. The number of hydrolyzable groups directly bonded to a metal atom in the metal coupling agent is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more. There is no upper limit to the number, and it is, for example, 10,000.

[0042] The metal coupling agent also preferably has a reactive group. The reactive group is preferably a group capable of crosslinking with a resin binder or a precursor thereof, as described below. Specific examples of the reactive group include an epoxy group, an oxetanyl group, a vinyl group, a (meth)acrylic group, a styryl group, an amino group, an isocyanate group, a mercapto group, and an acid anhydride group (such as a carboxylic acid anhydride or a phosphoric acid anhydride). The number of reactive groups possessed by the metal coupling agent is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more. There is no upper limit to the number, and it is, for example, 10,000.

[0043] Examples of metal coupling agents include silane coupling agents, titanium coupling agents, zirconia coupling agents, aluminum coupling agents, and zirconium aluminate coupling agents. Among these, the metal coupling agent is preferably a silane coupling agent or a titanium coupling agent.

[0044] Examples of the silane coupling agent include aminosilane-based silane coupling agents such as γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and trimethoxy[3-(phenylamino)propyl]silane; epoxysilane-based silane coupling agents such as 3-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; vinylsilane-based silane coupling agents such as triethoxyvinylsilane and vinyl-tri(β-methoxyethoxy)silane; cationic silane-based silane coupling agents such as N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride; phenylsilane-based silane coupling agents such as phenyltrimethoxysilane and phenyltriethoxysilane. silane-based silane coupling agents; methacrylsilane-based silane coupling agents such as 3-methacryloxypropyltrimethoxysilane; acrylsilane-based silane coupling agents such as 3-acryloxypropyltrimethoxysilane; isocyanate silane-based silane coupling agents such as 3-isocyanatepropyltriethoxysilane; isocyanurate silane-based silane coupling agents such as tris-(trimethoxysilylpropyl)isocyanurate; mercaptosilane-based silane coupling agents such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; ureidosilane-based silane coupling agents such as 3-ureidopropyltrialkoxysilane; and styrylsilane-based silane coupling agents such as p-styryltrimethoxysilane.

[0045] Examples of titanium-based coupling agents include PLENACT 38S, PLENACT TTS, PLENACT 46B, PLENACT 55, PLENACT 41B, PLENACT 138S, PLENACT 238S, PLENACT 338X, PLENACT 44, PLENACT 9SA, and PLENACT ET (all manufactured by Ajinomoto Fine-Techno Co., Ltd.). An example of an aluminum coupling agent is PLENACT AL-M (manufactured by Ajinomoto Fine-Techno Co., Ltd.). An example of the zirconia coupling agent is Kenreact NZ01 (manufactured by Kenrich Co., Ltd.).

[0046] The metal coupling agent may also be a polymeric type metal coupling agent. The molecular weight is preferably 1000 or more, more preferably 2000 or more. The upper limit is preferably 100000 or less, more preferably 10000 or less. The reactive functional group equivalent capable of crosslinking with the resin binder or its precursor is preferably 1000 g / mol or less, more preferably 500 g / mol or less.

[0047] When the metal coupling agent is brought into contact with the modified carbide particles (such as oxidized carbide particles) obtained in the above modification step, the hydrolyzable groups in the metal coupling agent may be hydrolyzed in advance before the contact. In this case, it is also preferable to crosslink the metal coupling agent with the modified carbide particles (such as oxidized carbide particles) obtained in the above modification step using hydroxy metal groups (groups in which a hydroxy group is directly bonded to a metal atom) generated by prior hydrolysis of the hydrolyzable groups in the metal coupling agent.

[0048] ·Curable compound As the surface modifier, a curable compound can also be used. The curable compound herein refers to a component different from the above-mentioned metal coupling agent.

[0049] The curable compound is preferably a compound that is soluble in the above organic solvent. The curable compound may be a polymeric compound (resin) or a low molecular weight compound. The molecular weight of the curable compound is, for example, 300 to 1,000,000.

[0050] The curable compound, which is a resin, may or may not have thermoplasticity.

[0051] The curable compound has a crosslinkable group. The crosslinkable group is also preferably a group capable of undergoing a crosslinking reaction with a resin binder or a precursor thereof (preferably a precursor of a resin binder) described below. It is also preferable that the crosslinkable group is a group capable of undergoing a crosslinking reaction with a hydroxyl group. Examples of the crosslinkable group include an epoxy group, an oxetanyl group, a cyanate group, an isocyanate group, an ethylenic double bond-containing group (such as a (meth)acryloyl group), and a carboxy group. The number of the crosslinkable groups in the curable compound is preferably 1 or more, more preferably 2 or more. There is no upper limit to the number, and it is, for example, 10,000.

[0052] Examples of the curable compound that is a resin include epoxy resins, cyanate resins, phenolic resins, imide resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins. Among these, the resin is preferably an epoxy resin or a cyanate resin, and more preferably an epoxy resin.

[0053] The epoxy resin is preferably an epoxy resin having one or more (preferably two or more) epoxy groups in one molecule. In this specification, phenoxy resins are also included in the epoxy resins. Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, bixylenol type epoxy resins, phenol novolac type epoxy resins, tert-butylcatechol type epoxy resins, naphthol type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, naphthylene ether type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, anthracene type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane dimethanol type epoxy resins, trimethylol type epoxy resins, and halogenated epoxy resins.

[0054] Examples of the cyanate resin include bisphenol type cyanate resins such as novolac type cyanate resins, bisphenol A type cyanate resins, bisphenol E type cyanate resins, and tetramethylbisphenol F type cyanate resins, and prepolymers of these partially converted to triazine.

[0055] As the surface modifier (for example, a surface modifier that is a curable compound), the below-mentioned resin binder or a precursor thereof (preferably a precursor of a resin binder) may be used, or others may be used.

[0056] The amount of the surface modifier used is, for example, preferably 0.0001 to 20 parts by mass, more preferably 0.01 to 15 parts by mass, and even more preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the total content of the organic solvent and the water. The surface modifier may be used alone or in combination of two or more kinds.

[0057] <Changes in particle size> In the method of the present invention, it is preferable that the rate of change in particle size between the carbide particles used in the manufacturing method and the modified carbide particles obtained before and after the series of manufacturing methods is small. In addition, when the carbide particles used in the present invention are aggregated particles, the aggregated state of the particles may be maintained without being destroyed during the series of manufacturing methods. Specifically, the rate of change in particle diameter calculated by the following formula is preferably less than 10%, more preferably less than 5%. There is no particular lower limit to the rate of change in particle diameter, and for example, the rate of change in particle diameter may be -5% or more, and is preferably 0% or more. Formula: Rate of change in particle size (%) = [1 - (particle size of modified carbide particles produced) / (particle size of carbide particles used to produce modified carbide particles)] x 100 An example of a method for adjusting the rate of change in particle diameter is a method for adjusting the shear force applied when mixing and / or stirring the aqueous solution and / or mixed liquid in the method of the present invention.

[0058] The particle size of the modified carbide particles produced by the method of the present invention (usually the average primary particle size, when the modified carbide particles are secondary particles, the average particle size as secondary particles) is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 60 μm or less. There is no particular lower limit to the particle size, but from the viewpoint of handleability, it is preferably 100 nm or more, more preferably 500 nm or more, and even more preferably 1 μm or more.

[0059] [Composition] The present invention also relates to a composition. The composition of the present invention comprises the modified carbide particles produced by the process of the present invention and a resin binder or a precursor thereof. The modified carbide particles contained in the composition of the present invention are particles with excellent packing properties as described above, although it is impossible or impractical to grasp their characteristics from the physical properties and / or structure. Therefore, by using the composition of the present invention, a material that can fully realize the performance expected of carbide particles (modified carbide particles) can be obtained. The composition is also preferably a composition for forming a specific material. The composition is also preferably a curable composition that hardens upon heating, drying, exposure to light, cooling, and / or aging.

[0060] [Modified carbide particles] The modified carbide particles that the composition comprises are modified carbide particles produced by the process of the present invention. Hereinafter, the modified carbide particles produced by the method of the present invention will also be referred to simply as "modified carbide particles". The contents of the modified carbide particles and other components in the composition may be appropriately adjusted depending on the application of the composition. For example, the content of the modified carbide particles is preferably 10% by volume or more, more preferably 20% by volume or more, and even more preferably 35% by volume or more, based on the total solid content of the composition. The upper limit is less than 100% by volume, and preferably 85% by volume or less. The modified carbide particles may be used alone or in combination of two or more kinds. The total solid content refers to all components other than the solvent contained in the composition, and any component other than the solvent is considered to be a solid content even if it is in a liquid state. For example, when the composition is a composition for forming a specific material, the solid content may be a component whose chemical structure changes as a result of reaction (polymerization) when the material is formed.

[0061] [Resin binder or its precursor (binder component)] The composition includes a resinous binder or a precursor thereof. Hereinafter, the resin binder or a precursor thereof will also be collectively referred to as a binder component. The binder component may be a resin binder itself or a precursor of a resin binder.

[0062] An example of a composition using a resin binder itself is a composition containing a solvent and a resin binder that is a polymer (resin) dissolved in the solvent. When the solvent of this composition evaporates, the resin binder precipitates, and a material is obtained in which the resin binder functions as a binder (binding agent). In addition, when the composition contains a thermoplastic resin as a resin binder, the composition may be, for example, a composition containing a resin binder that is a thermoplastic resin and not containing a solvent. This composition may be heated and melted, and then cooled and solidified in a desired form to obtain a material in which the resin binder that is a thermoplastic resin functions as a binder (binding agent).

[0063] The resin binder precursor is, for example, a component that becomes a resin binder (polymer and / or crosslinked body) by polymerization and / or crosslinking under a predetermined condition during the process of forming a material from the composition. The resin binder thus formed functions as a binder (binding agent) in the material. The precursor of the resin binder may be, for example, a curable compound. The curable compound may be a compound that undergoes polymerization and / or crosslinking and hardens due to heat or light (such as ultraviolet light). That is, it may be a thermosetting compound or a photocurable compound. These compounds may be polymers or monomers. The curable compound may be a mixture of two or more compounds (for example, a base agent and a hardener). The precursor of the resin binder may chemically react with a surface modifier.

[0064] Examples of resin binders (including resin binders formed from resin binder precursors) include epoxy resins, silicone resins, phenolic resins, polyimide resins, polyester resins, bismaleimide resins, melamine resins, isocyanate-based resins (polyurethane resins, polyurea resins, polyurethane urea resins, etc.), and resins formed by chain polymerization of two or more monomers having polymerizable double bonds, such as radical polymers ((meth)acrylic resins, etc.).

[0065] Furthermore, the resin binder (including a resin binder formed from a resin binder precursor) may be, for example, a resin formed by a reaction between different monomers and one or more combinations of the following (functional group 1 / functional group 2): (Functional group 1 / Functional group 2) = (polymerizable double bond / polymerizable double bond), (polymerizable double bond / thiol group), (carboxylic acid halide group (carboxylic acid chloride group, etc.) / primary or secondary amino group), (carboxyl group / primary or secondary amino group), (carboxylic acid anhydride group / primary or secondary amino group), (carboxyl group / aziridine group), (carboxyl group / isocyanate group), (carboxyl group / epoxy group), (carboxyl group / halogenated benzyl group), (primary or secondary amino group / isocyanate group), (primary, secondary, or tertiary amine group), amino group / halogenated benzyl group), (primary amino group / aldehydes), (isocyanate group / isocyanate group), (isocyanate group / hydroxyl group), (isocyanate group / epoxy group), (hydroxyl group / halogenated benzyl group), (hydroxyl group / carboxylic anhydride group), (hydroxyl group / alkoxysilyl group), (epoxy group / primary or secondary amino group), (epoxy group / carboxylic anhydride group), (epoxy group / hydroxyl group), (epoxy group / epoxy group), (oxetanyl group / epoxy group), (alkoxysilyl group / alkoxysilyl group), etc. The polymerizable double bond refers to a carbon-carbon double bond that can undergo polymerization such as radical polymerization, and examples of such double bonds include carbon-carbon double bonds in a (meth)acryloyl group and a vinyl group.

[0066] In particular, the composition preferably contains, as the binder component, a precursor of a resin binder, and more preferably contains a precursor of a resin binder capable of forming an epoxy resin. The resin binder may be used alone or in combination of two or more kinds.

[0067] <Epoxy resin> The resin binder (particularly, the resin binder formed from a resin binder precursor) is preferably an epoxy resin. That is, the composition also preferably contains a binder component capable of forming an epoxy resin (that is, an epoxy compound, etc.). The epoxy resin can be formed by polymerizing an epoxy compound alone or an epoxy compound with another compound (an active hydrogen group-containing compound such as a phenol compound or an amine compound, and / or an acid anhydride, etc.). Among them, the epoxy resin is preferably formed by reacting an epoxy compound with another compound (preferably a phenol compound).

[0068] (Epoxy compounds) An epoxy compound is a compound having at least one epoxy group (oxiranyl group) in one molecule. The epoxy group is a group obtained by removing one or more hydrogen atoms (preferably one hydrogen atom) from an oxirane ring. If possible, the epoxy group may further have a substituent (such as a linear or branched alkyl group having 1 to 5 carbon atoms).

[0069] The number of epoxy groups in the epoxy compound is preferably 2 or more, more preferably 2 to 40, further preferably 2 to 10, and particularly preferably 2, in one molecule. The molecular weight of the epoxy compound is preferably 150-10,000, more preferably 150-1,000, and further preferably 200-290.

[0070] The epoxy group content of the epoxy compound is preferably from 2.0 to 20.0 mmol / g, more preferably from 5.0 to 15.0 mmol / g, and further preferably from 5.5 to 14.0 mmol / g. The epoxy group content refers to the number of epoxy groups per 1 g of the epoxy compound. The epoxy compound also preferably has an aromatic ring group (preferably an aromatic hydrocarbon ring group).

[0071] The epoxy compound may or may not exhibit liquid crystallinity. That is, the epoxy compound may be a liquid crystal compound, in other words, a liquid crystal compound having an epoxy group.

[0072] Examples of epoxy compounds include compounds that at least partially contain a rod-like structure (rod-like compounds) and compounds that at least partially contain a disc-like structure (disk-like compounds). The rod-shaped compounds and discotic compounds will be described in detail below.

[0073] ·Rod-shaped compound Examples of epoxy compounds that are rod-shaped compounds include azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexane carboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles. Not only the low molecular weight compounds as described above, but also polymer compounds can be used. The polymer compounds are polymer compounds obtained by polymerizing rod-shaped compounds having low molecular weight reactive groups.

[0074] The rod-shaped compound may have a biphenyl skeleton. In other words, the epoxy compound preferably has a biphenyl skeleton, and in this case, the epoxy compound is preferably a rod-shaped compound.

[0075] Discoid Compounds The epoxy compound which is a discotic compound has at least a partial discotic structure. The discotic structure has at least an alicyclic ring or an aromatic ring. In particular, when the discotic structure has an aromatic ring, the discotic compound can form a columnar structure by forming a stacking structure due to intermolecular π-π interactions. Specific examples of the discotic structure include the triphenylene structure described in Angew. Chem. Int. Ed. 2012, 51, 7990-7993 or JP-A-7-306317, and the tri-substituted benzene structures described in JP-A-2007-2220 and JP-A-2010-244038.

[0076] The discotic compound preferably has three or more epoxy groups. A cured product of a composition containing a discotic compound having three or more epoxy groups tends to have a high glass transition temperature and high heat resistance. The number of epoxy groups contained in the discotic compound is preferably 8 or less, more preferably 6 or less.

[0077] Specific examples of the discotic compound include compounds described in C. Destrade et al., Mol. Crysr. Liq. Cryst., vol. 71, page 111 (1981); Quarterly Review of Chemistry, No. 22, Chemistry of Liquid Crystals, Chapter 5, Chapter 10, Section 2 (1994), edited by the Chemical Society of Japan; B. Kohne et al., Angew. Chem. Soc. Chem. Comm., page 1794 (1985); J. Zhang et al., J. Am. Chem. Soc., vol. 116, page 2655 (1994), and Japanese Patent No. 4592225, in which at least one (preferably three or more) of the terminals are epoxy groups. Examples of the discotic compound include the triphenylene structure described in Angew. Chem. Int. Ed. 2012, 51, 7990-7993 and JP-A-7-306317, and the trisubstituted benzene structure described in JP-A-2007-2220 and JP-A-2010-244038 in which at least one (preferably three or more) of the terminals is an epoxy group.

[0078] Other examples of the epoxy compound include glycidyl ethers of bisphenol A, F, S, AD, etc., such as bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, and bisphenol AD ​​type epoxy compounds; hydrogenated bisphenol A type epoxy compounds, hydrogenated bisphenol AD ​​type epoxy compounds, etc.; phenol novolac type glycidyl ethers (phenol novolac type epoxy compounds), cresol novolac type glycidyl ethers (cresol novolac type epoxy compounds), bisphenol A novolac type glycidyl ethers, etc.; dicyclopentadiene type glycidyl ethers (dicyclopentadiene type epoxy compounds); dihydroxypentadiene type glycidyl ethers (dihydroxypentadiene type epoxy compounds); trisphenolmethane type epoxy compounds; phenoxy resins, etc.; and acrylic resins having epoxy groups on their side chains. A compound in which one or more of the glycidyl ether groups and / or glycidyl ester groups in each of the above-mentioned compounds are replaced with a diglycidylamino group or a diglycidylaminoalkylene group (such as a diglycidylaminomethylene group) may be used as the epoxy compound. Each of the above compounds may have a substituent. For example, the aromatic ring group, the cycloalkane ring group, and / or the alkylene group contained in each of the above compounds may have a substituent other than a glycidyl ether group, a glycidyl ester group, a diglycidylamino group, and / or a diglycidylaminoalkylene group.

[0079] Examples of the epoxy compound include polyhydroxy aromatic ring-type glycidyl ethers (polyhydroxy aromatic ring-type epoxy compounds) such as glycidyl ethers of dihydroxybenzenes such as resorcinol, and polycarboxy aromatic ring-type glycidyl esters (polycarboxy aromatic ring-type epoxy compounds). The polyhydroxy aromatic ring-type glycidyl ether is a compound having a structure in which an aromatic ring having two or more (preferably 2 to 6, more preferably 2 to 3, and even more preferably 2) hydroxyl groups as substituents has the two or more hydroxyl groups converted into glycidyl ether. The polycarboxy aromatic ring-type glycidyl ester is a compound having a structure in which the two or more hydroxyl groups in an aromatic ring having two or more (preferably 2 to 6, more preferably 2 to 3, and even more preferably 2) carboxy groups as substituents are glycidyl esterified. The aromatic ring may be an aromatic hydrocarbon ring or an aromatic heterocycle, and is preferably an aromatic hydrocarbon ring. The aromatic ring may be a polycycle or a monocycle. The number of ring members in the aromatic ring is preferably 5 to 15, more preferably 6 to 12, and more preferably 6. The aromatic ring may or may not have a substituent other than a hydroxyl group. An example of the polyhydroxy aromatic ring type glycidyl ether is 1,3-phenylene bis(glycidyl ether). Compounds in which one or more of the glycidyl ether groups or glycidyl ester groups in the above-mentioned polyhydroxy aromatic ring-type glycidyl ethers and the above-mentioned polycarboxy aromatic ring-type glycidyl esters are replaced with a diglycidylamino group or a diglycidylaminoalkylene group (such as a diglycidylaminomethylene group) may be used as the epoxy compound.

[0080] The epoxy compound may also be a compound in which the epoxy group is condensed into a ring, such as 3,4:8,9-diepoxybicyclo[4.3.0]nonane.

[0081] In addition, the epoxy compounds described in paragraphs

[0051] to

[0134] of WO 2020 / 067364 can also be used as the epoxy compound.

[0082] When the composition contains an epoxy compound, the content thereof is preferably from 1 to 40% by volume, more preferably from 3 to 30% by volume, and even more preferably from 6 to 20% by volume, based on the total solid content of the composition. The epoxy compounds may be used alone or in combination of two or more.

[0083] (active hydrogen group-containing compound) The epoxy resin is preferably formed by reacting an epoxy compound with an active hydrogen group-containing compound. The active hydrogen group-containing compound is a compound that has one or more (preferably two or more, more preferably 2 to 10) groups having active hydrogen (active hydrogen groups). Examples of the active hydrogen group include a hydroxyl group, a primary or secondary amino group, and a mercapto group, and among these, a hydroxyl group is preferred. The active hydrogen group-containing compound is preferably a polyol having two or more (preferably three or more, more preferably 3 to 6) hydroxyl groups.

[0084] Among these, the active hydrogen group-containing compound used in combination with the epoxy compound is preferably a phenol compound. That is, the composition of the present invention preferably contains an epoxy compound and a phenol compound as the resin binder or a precursor thereof. The phenol compound is a compound having one or more (preferably two or more, more preferably three or more, and further preferably three to six) phenolic hydroxyl groups.

[0085] Preferred examples of the active hydrogen group-containing compound include benzene polyols such as benzene triol, biphenyl aralkyl type phenol resins, phenol novolac resins, cresol novolac resins, aromatic hydrocarbon formaldehyde resin-modified phenol resins, dicyclopentadiene phenol addition type resins, phenol aralkyl resins, polyhydric phenol novolac resins synthesized from polyhydric hydroxy compounds and formaldehyde, naphthol aralkyl resins, trimethylol methane resins, tetraphenylol ethane resins, naphthol novolac resins, naphthol phenol co-condensed novolac resins, naphthol cresol co-condensed novolac resins, biphenyl-modified phenol resins, biphenyl-modified naphthol resins, aminotriazine-modified phenol resins, and alkoxy group-containing aromatic ring-modified novolac resins.

[0086] As the active hydrogen group-containing compound, the phenol compounds described in paragraphs

[0037] to

[0059] of WO 2020 / 158259 can also be used.

[0087] The lower limit of the hydroxyl group content of the active hydrogen group-containing compound is preferably 3.0 mmol / g or more, more preferably 4.0 mmol / g or more, and the upper limit is preferably 25.0 mmol / g or less, more preferably 20.0 mmol / g or less. The hydroxyl group content refers to the number of hydroxyl groups (preferably phenolic hydroxyl groups) contained in 1 g of the active hydrogen group-containing compound. In addition, the active hydrogen group-containing compound may have an active hydrogen-containing group (such as a carboxylic acid group) capable of polymerizing with an epoxy compound in addition to a hydroxyl group. The lower limit of the active hydrogen content (the total content of hydrogen atoms in the hydroxyl group and the carboxylic acid group) of the active hydrogen group-containing compound is preferably 3.0 mmol / g or more, more preferably 4.0 mmol / g or more. The upper limit is preferably 25.0 mmol / g or less, more preferably 20.0 mmol / g or less. The above-mentioned active hydrogen content refers to the number of active hydrogen atoms contained in 1 g of the active hydrogen group-containing compound.

[0088] The upper limit of the molecular weight of the active hydrogen group-containing compound is preferably 2000 or less, more preferably 1500 or less, and even more preferably 1000 or less. The lower limit is preferably 110 or more, and more preferably 300 or more.

[0089] When the composition contains an active hydrogen group-containing compound, the content thereof is preferably 1 to 40% by volume, more preferably 3 to 30% by volume, and even more preferably 5 to 20% by volume, based on the total solid content of the composition. The active hydrogen group-containing compound may be used alone or in combination of two or more kinds.

[0090] When the composition contains an epoxy compound and an active hydrogen group-containing compound, the ratio of the content of the epoxy compound to the content of the active hydrogen group-containing compound is such that the equivalent ratio ("number of epoxy groups" / "number of active hydrogen groups") of the epoxy compound to the active hydrogen groups (preferably hydroxyl groups, more preferably phenolic hydroxyl groups) of the active hydrogen group-containing compound is preferably 30 / 70 to 70 / 30, more preferably 40 / 60 to 60 / 40, and even more preferably 45 / 55 to 55 / 45. When the composition contains an epoxy compound and / or an active hydrogen group-containing compound, the total content of the epoxy compound and the active hydrogen group-containing compound is preferably 20 to 100% by volume, more preferably 60 to 100% by volume, and even more preferably 90 to 100% by volume, based on the total binder components.

[0091] <Silicone resin> It is also preferred that the resin binder (particularly the resin binder formed from a resin binder precursor) is a silicone resin. A silicone resin as the resin binder is preferable since it easily imparts flexibility to the thermally conductive material. Examples of silicone resins include addition reaction curing type silicone resins and condensation curing type silicone resins. In this specification, a precursor capable of forming a silicone resin is also referred to as a silicone compound. That is, the composition of the present invention preferably contains a silicone compound as a binder component. In addition, when the silicone resin is formed by chemically bonding two or more resin binder precursors, each of the two or more resin binder precursors is also called a silicone compound.

[0092] The silicone resin is preferably one which has been cured by crosslinking with silicone compound A and silicone compound B, which will be described below, as binder components.

[0093] An organopolysiloxane having two or more alkenyl groups is used as the silicone compound A. The organopolysiloxane having two or more alkenyl groups is preferably an organopolysiloxane having two or more vinyl groups, and more preferably an organopolysiloxane having vinyl groups at both ends. Examples of organopolysiloxanes having vinyl groups at both ends include polydimethylsiloxane having vinyl groups at both ends, polyphenylmethylsiloxane having vinyl groups at both ends, a dimethylsiloxane-diphenylsiloxane copolymer having vinyl groups at both ends, a dimethylsiloxane-phenylmethylsiloxane copolymer having vinyl groups at both ends, and a dimethylsiloxane-diethylsiloxane copolymer having vinyl groups at both ends. The weight average molecular weight of the organopolysiloxane having two or more alkenyl groups is preferably 4,000 to 50,000, and more preferably 7,500 to 25,000. The silicone compound A may be used alone or in combination of two or more kinds.

[0094] The silicone compound B may be any compound capable of crosslinking the silicone compound A, and may be a compound having two or more hydrosilyl groups (SiH). Polyorganosiloxanes having two or more hydrosilyl groups (hereinafter also referred to as "hydrosilyl group-containing polyorganosiloxanes") are preferred. Polyorganosiloxanes having three or more hydrosilyl groups (for example, 3 to 1000) are more preferred. Examples of hydrosilyl-containing polyorganosiloxanes include methylhydrosiloxane-dimethylsiloxane copolymers, polymethylhydrosiloxanes, polyethylhydrosiloxanes, and methylhydrosiloxane-phenylmethylsiloxane copolymers. These may or may not have hydrosilyl groups at their ends, and may be capped at both ends with, for example, trimethylsilyl groups or triethylsilyl groups. The weight average molecular weight of the hydrosilyl group-containing polyorganosiloxane is preferably 800 to 5,000, and more preferably 1,500 to 4,000. In the composition of the present invention, the content of silicone compound B relative to 100 parts by mass of silicone compound A is, for example, 0.1 to 250 parts by mass, preferably 0.1 to 10 parts by mass, more preferably 0.2 to 7 parts by mass, and even more preferably 0.3 to 3 parts by mass. The silicone compound B may be used alone or in combination of two or more kinds. In the composition of the present invention, silicone compound A and silicone compound B may be partially reacted.

[0095] The content of the binder component in the composition is preferably from 5 to 90% by volume, more preferably from 10 to 50% by volume, and even more preferably from 15 to 40% by volume, based on the total solid content of the composition.

[0096] [Curing Accelerator] The composition may further comprise a cure accelerator. In particular, when the composition contains a precursor of a resin binder, it is preferable that the composition contains a curing accelerator for forming the resin binder from the precursor of the resin binder. The type of the curing accelerator to be used may be appropriately determined in consideration of the type of the precursor of the resin binder, etc. In particular, when the resin binder or the precursor thereof contains an epoxy compound, it is preferable that the composition further contains a curing accelerator. Examples of the curing accelerator include tris-orthotolylphosphine, triphenylphosphine, boron trifluoride amine complex, and the compounds described in paragraph 0052 of JP-A-2012-67225. Further examples include onium salt-based curing accelerators such as quaternary phosphonium compounds (phosphonium salts) such as tetraphenylphosphonium tetraphenylborate (TPP-K), tetraphenylphosphonium tetra-p-tolylborate (TPP-MK), tetra-n-butylphosphonium laurate (TBP-LA), bis(tetra-n-butylphosphonium)pyromellitate, and tetraphenylphosphonium bis(naphthalene-2,3-dioxy)phenylsilicate adducts. Other examples include 2-methylimidazole (trade name: 2MZ), 2-undecylimidazole (trade name: C11-Z), 2-heptadecylimidazole (trade name: C17Z), 1,2-dimethylimidazole (trade name: 1.2DMZ), 2-ethyl-4-methylimidazole (trade name: 2E4MZ), 2-phenylimidazole (trade name: 2PZ), 2-phenyl-4-methylimidazole (trade name: 2P4MZ), 1-benzyl-2-methylimidazole (trade name: 1B2 ... 1-cyanoethyl-2-phenylimidazole (trade name; 1B2PZ), 1-cyanoethyl-2-methylimidazole (trade name; 2MZ-CN), 1-cyanoethyl-2-undecylimidazole (trade name; C11Z-CN), 1-cyanoethyl-2-phenylimidazolium trimellitate (trade name; 2PZCNS-PW), 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine (trade name; 2MZ-A), 2,4-diamino-6-[2'-undecylimidazolyl- (1')]-ethyl-s-triazine (trade name; C11Z-A), 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine (trade name; 2E4MZ-A), 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct (trade name; 2MA-OK), 2-phenyl-4,5-dihydroxymethylimidazole (trade name; 2PHZ-PW), 2-phenyl-4-methyl-5-hydroxymethyl Examples of the imidazole-based curing accelerator include imidazole (trade name: 2P4MHZ-PW), 1-cyanoethyl-2-phenylimidazole (trade name: 2PZ-CN), 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine (trade name: 2MZA-PW), and 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct (trade name: 2MAOK-PW) (all manufactured by Shikoku Chemical Industry Co., Ltd.). In addition, examples of the triarylphosphine-based curing accelerator include the compounds described in paragraph 0052 of JP-A-2004-43405.Examples of phosphorus-based curing accelerators in which triphenylborane is added to triarylphosphine include the compounds described in paragraph 0024 of JP-A 2014-5382. Among these, the curing accelerator preferably contains a compound containing a phosphorus atom, and more preferably contains a phosphonium salt, in terms of obtaining a stronger cured product. Although the reason for this is unclear, it is speculated that because compounds containing phosphorus atoms (particularly phosphonium salts) can cause curing to proceed slowly, there is time for the resin binder or its precursor to flow between the start of curing of the composition and when it is completely cured, which improves the adhesion between the resin binder and the modified carbide particles and thereby improves strength. The curing accelerator may be a compound containing a phosphorus atom or a phosphonium salt itself. The content of the compound containing a phosphorus atom or the phosphonium salt is preferably 10 to 100% by volume, more preferably 50 to 100% by volume, and further preferably 80 to 100% by volume, based on the total volume of the curing accelerator. The curing accelerator may be used alone or in combination of two or more kinds. The content of the curing accelerator is preferably 0.002% by volume or more, more preferably 0.02% by volume or more, and even more preferably 0.07% by volume or more, based on the total solid content of the composition. The content of the curing accelerator is preferably 5% by volume or less, more preferably 2% by volume or less, and even more preferably 1% by volume or less, based on the total solid content of the composition. For example, when the composition contains an epoxy compound, the content of the curing accelerator is preferably 0.01 to 10% by volume, and more preferably 0.1 to 5% by volume, based on the total amount of the epoxy compound.

[0097] 〔solvent〕 The composition may further comprise a solvent. The type of the solvent is not particularly limited, and is preferably an organic solvent, such as cyclopentanone, cyclohexanone, ethyl acetate, methyl ethyl ketone, dichloromethane, and tetrahydrofuran. When the composition contains a solvent, the content of the solvent is preferably an amount that makes the solids concentration of the composition 20 to 95 volume %, more preferably an amount that makes the solids concentration of the composition 30 to 85 volume %, still more preferably an amount that makes the solids concentration of the composition 30 to 80 volume %, and particularly preferably an amount that makes the solids concentration of the composition 30 to 60 volume %. That is, the content of the solvent is preferably from 5 to 80% by volume, more preferably from 15 to 70% by volume, further preferably from 20 to 70% by volume, and particularly preferably from 40 to 70% by volume, based on the total volume of the composition.

[0098] [Other ingredients] The composition may contain other ingredients than those mentioned above. Examples of other components include particles other than modified carbide particles (inorganic particles or organic particles, etc.), dispersants, surface modifiers, and polymerization initiators (photopolymerization initiators or thermal polymerization initiators, etc.).

[0099] [Method of producing the composition] The method for producing the composition is not particularly limited, and the method for producing the composition is preferably the above-mentioned method including the method of the present invention. For example, there is mentioned a method for producing a composition, which includes a particle production step of obtaining modified carbide particles by the method of the present invention, and a mixing step of mixing at least the modified carbide particles obtained by the method of the present invention and a resin binder or a precursor thereof. In addition to the resin binder or a precursor thereof, the components that are mixed with the modified carbide particles in the mixing step include other components that may be included in the composition of the present invention. When the components are mixed in the mixing step, the components may be mixed all at once or sequentially. The method for mixing the components is not particularly limited, and known methods can be used. The mixing device used for mixing is preferably a submerged dispersing device, and examples thereof include agitators such as a planetary centrifugal mixer, a high-speed rotary shear type agitator, a colloid mill, a roll mill, a high-pressure jet type dispersing device, an ultrasonic dispersing device, a bead mill, and a homogenizer. The mixing device may be used alone or in combination with two or more types. Degassing treatment may be performed before, after, and / or at the same time as mixing.

[0100] [Method of curing the composition] The compositions of the present invention are preferably curable compositions. When the composition of the present invention is a curable composition, it is subjected to a curing treatment to obtain a cured product. The method for curing the curable composition is not particularly limited, and examples thereof include a thermal curing reaction and a photocuring reaction.

[0101] The heating temperature during the thermosetting reaction is not particularly limited and may be appropriately selected within the range of, for example, 50 to 250° C. Furthermore, when carrying out the thermosetting reaction, heat treatments at different temperatures may be carried out multiple times. The curing treatment may be carried out on the composition in the form of a film or sheet. Specifically, for example, the composition may be applied to form a film, and then a curing reaction may be carried out. When performing the curing treatment, it is preferable to apply the composition onto a substrate to form a coating film and then cure the composition. In this case, the coating film formed on the substrate may be brought into contact with a different substrate before the curing treatment. The cured product (material) obtained after curing may or may not be separated from one or both of the substrates. In addition, when performing the curing treatment, the composition may be applied to separate substrates to form coating films on each substrate, and the curing treatment may be performed in a state where the obtained coating films are in contact with each other. The cured product (material) obtained after curing may or may not be separated from one or both substrates.

[0102] The curing treatment may be terminated when the composition is in a semi-cured state, or after the composition is in a semi-cured state, a further curing treatment may be carried out to complete the curing. The curing treatment for bringing the composition into a semi-cured state (also referred to as "semi-curing treatment") and the curing treatment for complete curing (also referred to as "main curing treatment") may be carried out in separate steps.

[0103] For example, in the semi-curing treatment, after applying a composition onto a substrate to form a coating film, the coating film on the substrate may be heated without pressure to form a semi-cured material (also referred to as a "semi-cured film"). Alternatively, the coating film on the substrate may be heated while simultaneously using press processing to form a semi-cured film. When press processing is performed, the press processing may be performed before, after, or during the heating process. When press processing is performed in the semi-curing treatment, it may be easier to adjust the thickness of the resulting semi-cured film and / or reduce the amount of voids in the semi-cured film. In the semi-curing treatment, the coating films formed on different substrates may be laminated together, or the coating films may not be laminated together. The semi-curing treatment may be performed in a state where the coating film formed from the composition is in contact with a material other than the coating film.

[0104] The resulting semi-cured film may be used as it is as a material for a desired application if possible, or may be further subjected to a main curing treatment and then used as a completely cured material. In the main curing treatment, the semi-cured film may be heated as it is without pressure, or may be heated after or while being pressed. In this case, the main curing treatment may be performed in a state where separate semi-cured films are laminated on each other, or may be performed without laminating the semi-cured films on each other. The main curing treatment may be carried out in a state where the semi-cured film is placed so as to be in contact with a device or the like in which it is to be used. It is also preferable that the main curing treatment results in adhesion between the device and a material formed from the composition of the present invention.

[0105] There is no limitation on the press used for the press working that may be carried out during the hardening treatment in the semi-hardening treatment and / or the full hardening treatment, and for example, a flat plate press or a roll press may be used. When using a roll press, for example, it is preferable to clamp the substrate with a coating film obtained by forming a coating film on a substrate between a pair of opposing rolls, and apply pressure in the thickness direction of the substrate with a coating film while rotating the pair of rolls to pass the substrate with a coating film. The substrate with a coating film may have a substrate on only one side of the coating film, or may have substrates on both sides of the coating film. The substrate with a coating film may be passed through the roll press once or multiple times. During the hardening treatment in the semi-hardening treatment and / or the full hardening treatment, only one of the treatment by plate press and the treatment by roll press may be carried out, or both may be carried out.

[0106] [Application] The applications of the modified carbide particles obtained by the method of the present invention and the composition of the present invention are not particularly limited. Applications of modified carbide particles include, for example, thermally conductive fillers that utilize their high thermal conductivity; abrasive fillers, fillers for imparting abrasion resistance, and fillers for reinforcing materials that utilize the high hardness of carbide particles; acoustic matching fillers that utilize the speed of sound; colored fillers (black fillers, etc.) that utilize the color (e.g., blackness) of the particles; insulating fillers that utilize their electrical insulating properties; neutron absorption fillers that utilize their neutron absorption properties; density adjustment fillers; and light diffusion fillers to compensate for the poor light distribution characteristics of LEDs and the like. Uses of the composition of the present invention include a composition for forming a thermally conductive material, an abrasive-containing resin composition for producing a polishing wheel or the like, a composition for forming a protective layer for imparting abrasion resistance or the like, a composition for forming an acoustic matching material, a composition for forming an insulating material, a composition for forming a neutron shielding material, a coloring composition for producing a light-shielding member (e.g., a black matrix in a color filter) or the like, and a composition for forming a light diffusion material for producing a light diffusion material such as a lighting cover or a light diffusion plate for a transmission type display. The composition of the present invention may be used in combination with modified carbide particles and conductive metal powder to form a conductive material or conductive coating material. Such compositions can be used, for example, for electromagnetic wave shielding, antistatic properties, and / or electrical conductivity. EXAMPLES

[0107] The present invention will be described in more detail below based on examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples.

[0108] [Production of modified carbide particles] Modified carbide particles of the examples and comparative examples were produced by the methods described below.

[0109] [Example 1 (Example 1A, Example 1B)] Silicon carbide particles (50 g) were added to NaOH water (NaOH: 40 g / water: 400 ml) and stirred. Sodium persulfate water (sodium persulfate: 9.6 g / water: 100 ml) was further added to the NaOH water, and the NaOH water was heated to 50°C and stirred for another 3 hours (modification step). A Three-One motor manufactured by Shinto Scientific Co., Ltd. was used for stirring at 150 rpm. After cooling the NaOH water to room temperature, the silicon carbide particles in the NaOH water were filtered out, and the filtered silicon carbide particles were washed with water (500 ml) and acetonitrile (250 ml) to obtain modified silicon carbide particles A1 (SiC-A1). The above process is referred to as Example 1A. The obtained silicon carbide particles A1 were stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (KBM-573, manufactured by Shin-Etsu Chemical Co., Ltd.) was added. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment (adsorption step). The modified silicon carbide particles in the acetonitrile were filtered, and then the filtered modified silicon carbide particles were washed with acetonitrile (100 ml) and dried in an oven at 40°C to obtain modified silicon carbide particles B1 (SiC-B1). The above steps are referred to as Example 1B. The hydrolysis adjustment liquid of the silane coupling agent was prepared by mixing the silane coupling agent (1 g), ethanol (500 μl), 2-propanol (500 μl), water (720 μl), and acetic acid (100 μl) and stirring for 1 hour. In the following examples and comparative examples, the composition of the hydrolysis adjustment liquid of the silane coupling agent is the same unless otherwise specified. In Example 1A, the production of modified carbide particles was terminated when modified silicon carbide particles A1 (SiC-A1) were obtained. In Example 1B, separate from Example 1A, modified silicon carbide particles A1 (SiC-A1) were produced in the same manner as in Example 1A, and the resulting modified silicon carbide particles A1 (SiC-A1) were subjected to an adsorption process to obtain modified silicon carbide particles B1 (SiC-B1), thereby completing the production of modified carbide particles. In the subsequent Examples NA and NB (N is an integer), modified carbide particles that were not subjected to the adsorption process and modified carbide particles that were subjected to the adsorption process were obtained by the same method, respectively.

[0110] [Example 2 (Example 2A, Example 2B)] Silicon carbide particles (50 g) were added to NaOH water (NaOH: 40 g / water: 400 ml) and stirred. Sodium persulfate water (sodium persulfate: 9.6 g / water: 100 ml) and iron sulfate heptahydrate (1.1 g) were further added to the NaOH water, and the NaOH water was then heated to 50°C and stirred for another 3 hours (modification step). A three-one motor manufactured by Shinto Scientific Co., Ltd. was used for stirring at 150 rpm. After cooling the NaOH water to room temperature, the silicon carbide particles in the NaOH water were filtered out, and the filtered silicon carbide particles were washed with 1N hydrochloric acid water (500 ml), water (500 ml), and acetonitrile (250 ml) to obtain modified silicon carbide particles A2 (SiC-A2). The above process is referred to as Example 2A. The obtained modified silicon carbide particles A2 were stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (KBM-573) was further added to the acetonitrile. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment (adsorption step). The modified silicon carbide particles in the acetonitrile were filtered out, and then the filtered modified silicon carbide particles were washed with acetonitrile (100 ml) and dried in an oven at 40° C. to obtain modified silicon carbide particles B2 (SiC-B2). The above is referred to as Example 2B.

[0111] [Example 3 (Example 3A, Example 3B)] Silicon carbide particles (50 g) were added to water (400 ml) and stirred to obtain a mixed solution. Sodium hypochlorite water (sodium hypochlorite pentahydrate: 48 g / water: 100 ml) was further added to the mixed solution, and the mixed solution was heated to 50° C. and stirred for another 3 hours (modification step). A Three-One motor manufactured by Shinto Scientific Co., Ltd. was used for stirring at 150 rpm. After cooling the mixture to room temperature, the silicon carbide particles in the mixture were filtered out, and the filtered silicon carbide particles were washed with water (500 ml) and acetonitrile (250 ml) to obtain modified silicon carbide particles A3 (SiC-A3). The above process is referred to as Example 3A. The obtained modified silicon carbide particles A3 were stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (KBM-573) was further added to the acetonitrile. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment (adsorption step). The modified silicon carbide particles in the acetonitrile were filtered out, and then the filtered modified silicon carbide particles were washed with acetonitrile (100 ml) and dried in an oven at 40° C. to obtain modified silicon carbide particles B3 (SiC-B3). The above is referred to as Example 3B.

[0112] [Example 4 (Example 4A, Example 4B)] Silicon carbide particles (50 g) were added to NaOH water (NaOH: 40 g / water: 400 ml) and stirred. Cerium ammonium nitrate water (cerium ammonium nitrate: 9.6 g / water: 100 ml) was further added to the NaOH water, and the NaOH water was then heated to 50° C. and stirred for another 3 hours (modification step). A Three-One motor manufactured by Shinto Scientific Co., Ltd. was used for stirring at 150 rpm. After cooling the NaOH water to room temperature, the silicon carbide particles in the NaOH water were filtered out, and the filtered silicon carbide particles were washed with 1N hydrochloric acid water (500 ml), water (500 ml), and acetonitrile (250 ml) to obtain modified silicon carbide particles A4 (SiC-A4). The above process is referred to as Example 4A. The obtained modified silicon carbide particles A4 were stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (KBM-573) was further added to the acetonitrile. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment (adsorption step). The modified silicon carbide particles in the acetonitrile were filtered out, and then the filtered modified silicon carbide particles were washed with acetonitrile (100 ml) and dried in an oven at 40° C. to obtain modified silicon carbide particles B4 (SiC-B4). The above is referred to as Example 4B.

[0113] [Example 5 (Example 5A, Example 5B)] Modified silicon carbide particles A5 (SiC-A5) and modified silicon carbide particles (SiC-B5) were obtained in the same manner as in Example 1, except that the sodium persulfate water having a composition of "sodium persulfate: 9.6 g / water: 100 ml" in Example 1 was changed to the sodium persulfate water having a composition of "sodium persulfate: 48 g / water: 400 ml".

[0114] [Example 6 (Example 6A, Example 6B)] Modified silicon carbide particles A6 (SiC-A6) and modified silicon carbide particles B6 (SiC-B6) were obtained in the same manner as in Example 1, except that the NaOH water having a composition of "NaOH: 40 g / water: 400 ml" in Example 1 was changed to the NaOH water having a composition of "NaOH: 2 g / water: 400 ml".

[0115] [Example 7 (Example 7A, Example 7B)] Modified silicon carbide particles A7 (SiC-A7) and modified silicon carbide particles B7 (SiC-B7) were obtained in the same manner as in Example 1, except that the sodium persulfate water having a composition of "sodium persulfate: 9.6 g / water: 100 ml" in Example 1 was changed to potassium iodate water having a composition of "potassium iodate: 9.6 g / water: 100 ml".

[0116] [Example 8 (Example 8A, Example 8B)] Modified silicon carbide particles A8 (SiC-A8) and modified silicon carbide particles B8 (SiC-B8) were obtained in the same manner as in Example 1, except that the NaOH water in Example 1 with a composition of "NaOH: 40 g / water: 400 ml" was changed to the NaOH water with a composition of "NaOH: 0.02 g / water: 400 ml".

[0117] [Example 9 (Example 9A, Example 9B)] Modified silicon carbide particles A9 (SiC-A9) and modified silicon carbide particles B9 (SiC-B9) were obtained in the same manner as in Example 1, except that the sodium persulfate water having a composition of "sodium persulfate: 9.6 g / water: 100 ml" in Example 1 was changed to potassium persulfate water having a composition of "potassium persulfate: 9.6 g / water: 400 ml."

[0118] Example 10 (Example 10A, Example 10B) Modified silicon carbide particles A10 (SiC-A10) and modified silicon carbide particles B10 (SiC-B10) were obtained in the same manner as in Example 1, except that the sodium persulfate water having a composition of "sodium persulfate: 9.6 g / water: 100 ml" in Example 1 was changed to the ammonium persulfate water having a composition of "ammonium persulfate: 9.6 g / water: 400 ml."

[0119] [Example 11 (Example 11A, Example 11B)] Modified silicon carbide particles A11 (SiC-A11) and modified silicon carbide particles B10 (SiC-B11) were obtained in the same manner as in Example 1, except that the silane coupling agent in Example 1 was changed to a titanium coupling agent (Plenact-38S, manufactured by Ajinomoto Fine-Techno Co., Ltd.). It should be noted that the modified silicon carbide particles A11 (SiC-A11) are the same as the modified silicon carbide particles A1 (SiC-A1).

[0120] [Example 12 (Example 12A, Example 12B)] Modified boron carbide particles A1 (B4C-A1) and modified boron carbide particles B1 (B4C-B1) were obtained under the same conditions as in Example 1, except that the silicon carbide particles in Example 1 were changed to boron carbide particles.

[0121] Example 13 (Example 13A, Example 13B) Modified titanium carbide particles A1 (TiC-A1) and modified titanium carbide particles B1 (TiC-B1) were obtained under the same conditions as in Example 1, except that the silicon carbide particles in Example 1 were changed to titanium carbide particles.

[0122] [Example 14 (Example 14A, Example 14B)] Modified tungsten carbide particles A1 (WC-A1) and modified tungsten carbide particles B1 (WC-B1) were obtained under the same conditions as in Example 1, except that the silicon carbide particles in Example 1 were changed to tungsten carbide particles.

[0123] Comparative Example 1 Untreated silicon carbide particles (SiC) were used as the carbide particles of Comparative Example 1. The untreated silicon carbide particles are the same as the modified silicon carbide particles prepared in the above-mentioned Examples, or the silicon carbide particles used as a raw material for the modified silicon carbide particles prepared in Comparative Example 2 described below.

[0124] Comparative Example 2 The silicon carbide particles were stirred in acetonitrile (100 ml), and a hydrolysis adjustment solution (1.25 g) of a silane coupling agent (KBM-573, Shin-Etsu Chemical Co., Ltd.) was added. The acetonitrile was stirred at room temperature for 3 hours to perform an adsorption treatment (adsorption step). The modified silicon carbide particles A1 in the acetonitrile were filtered out, and then the filtered modified silicon carbide particles were washed with acetonitrile (100 ml) and dried in an oven at 40° C. to obtain modified silicon carbide particles C1 (SiC-C1).

[0125] Comparative Example 3 Untreated boron carbide particles (B4C) were used as the carbide particles of Comparative Example 3. The untreated boron carbide particles are the same as the boron carbide particles used as the raw material for the modified boron carbide particles produced in the above-mentioned examples.

[0126] Comparative Example 4 Untreated titanium carbide particles (TiC) were used as the carbide particles of Comparative Example 4. The untreated titanium carbide particles are the same as the titanium carbide particles used as the raw material for the modified titanium carbide particles produced in the above-mentioned Examples.

[0127] Comparative Example 5 Untreated tungsten carbide particles (WC) were used as the carbide particles of Comparative Example 5. The untreated tungsten carbide particles are the same as the tungsten carbide particles used as the raw material for the modified tungsten carbide particles produced in the above-mentioned examples.

[0128] The characteristics of the series of examples or the carbide particles (untreated carbide particles) in the examples are as follows. Silicon carbide particles: particle size 25-33μm, manufactured by Shinano Electric Smelting Co., Ltd., SSC-A30 Boron carbide particles: particle size 50 μm, Fujifilm Wako Pure Chemical Industries, Ltd. Titanium carbide particles: particle size 1-2 μm, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Tungsten carbide particles: particle size 14-16μm, A.L.M.T., WC100S Although modified carbide particles were formed by the treatment in each Example, the particle size of the modified carbide particles was not substantially changed from that of the untreated carbide particles used as the raw material.

[0129] [test] The above-mentioned carbide particles (including modified carbide particles) were used to prepare compositions of the respective Examples and Comparative Examples, and the packing properties of each of the carbide particles (including modified carbide particles) were evaluated. The characteristics of the composition and the test methods carried out using the composition are shown below.

[0130] [Various components used in preparing the composition] Epoxy compound: Bisphenol F type epoxy compound (EPICLON 830-S) Phenolic compounds: Novolac-type phenolic compounds (MEH-7500) Curing accelerator: Triphenylphosphine Solvent: Cyclopentanone Carbide particles: any of the modified carbide particles mentioned above, modified silicon carbide particles C1 (SiC-C1), or untreated carbide particles that have not undergone a modification process (silicon carbide particles, boron carbide particles, titanium carbide particles, or tungsten carbide particles).

[0131] [Preparation of Composition] The solvent, phenol compound, epoxy compound, and curing accelerator were mixed in this order, and then the carbide particles were added. The mixture was treated for 5 minutes with a planetary centrifugal mixer (THINKY Corporation, Awatori Rentaro ARE-310) to obtain compositions (curable compositions) of the respective Examples and Comparative Examples.

[0132] The amount of the solvent added was set so that the solid content of the composition became 30 to 60% by volume. The solids concentration of each composition was adjusted within the above range for each composition so that the viscosity of each composition was approximately the same. The content of the carbide particles in the composition was adjusted to 63% by volume based on the total solid content of the composition. The content of the curing accelerator in the composition was adjusted to 0.6% by volume based on the total solid content of the composition. The remainder of the composition is an epoxy compound and a phenol compound. The amounts of the epoxy compound and the phenol compound in the composition were adjusted to be equivalent (the amount in which the number of epoxy groups in the epoxy compound is equal to the number of hydroxyl groups in the phenol compound).

[0133] 〔evaluation〕 The packing property of the carbide particles was evaluated by the method described below.

[0134] <Preparation of resin sheet> Using an applicator, any of the compositions of the Examples or Comparative Examples prepared as described above was uniformly applied onto the release surface of a release-treated polyester film (NP-100A, manufactured by PANAC Corporation, film thickness 100 μm), and left to stand at 120° C. for 5 minutes to obtain a semi-cured sheet (semi-cured film). The resulting semi-cured sheet was heat-pressed in air (heat plate temperature 180°C, pressure 5MPa for 5 minutes, and then further treated at normal pressure 180°C for 90 minutes) to cure the coating film and obtain a sheet. The polyester film was peeled off from the sheet to obtain a resin sheet with an average thickness of 120 μm.

[0135] <Evaluation of filling ability> Using a Mettler Toledo balance "XS204," the specific gravity of the resin sheet was measured by the Archimedes method (using a "solid specific gravity measurement kit"). The higher the specific gravity, the smaller the amount of voids in the resin sheet. The specific gravity of a resin sheet produced using untreated carbonized particles as the carbonized material was used as the standard, and the increase in specific gravity of a resin sheet produced using modified carbonized particles obtained using the same type of carbonized particles as the carbonized material was classified according to the following categories to evaluate the filling rate of the carbonized particles used in each resin sheet. For example, a resin sheet (referred to as resin sheet X) made using modified silicon carbide particles A1 (SiC-A1) as the carbide particles was compared in specific gravity with a resin sheet (referred to as resin sheet Y) made using silicon carbide particles (untreated silicon carbide particles, SiC) as the carbide particles, and the increase in specific gravity was calculated as "increase = specific gravity of resin sheet X - specific gravity of resin sheet Y", and classified according to the following classification to evaluate the filling rate. In addition, for example, the specific gravity of a resin sheet prepared using modified silicon carbide particles C1 (SiC-C1) as the carbide particles was compared with that of a resin sheet prepared using silicon carbide particles (untreated silicon carbide particles, SiC) as the carbide particles to determine the increase in specific gravity. Note that specific gravity 1 is 1g / cm 3 It is. AA: Increase is 0.05 or more A: The increase is 0.04 or more but less than 0.05 B: The increase is 0.02 or more but less than 0.04 C: The increase is 0.01 or more and less than 0.02 D: No change or less than 0.01 increase

[0136] [result] The types of carbide particles (including modified carbide particles) produced and used in each Example or Comparative Example, the characteristics of the production procedures used to produce the carbide particles, and the evaluation results are shown below. The "Amount of carbide (g)" column indicates the amount (g) of untreated carbide particles used in producing the modified carbide particles. The "Oxidizing agent" column indicates the type, standard redox potential, and amount (g) of the oxidizing agent used in producing the modified carbide particles. The "pH" column indicates the pH of the aqueous solution when the carbide particles are modified by contacting them with an oxidizing agent in the aqueous solution. For example, in the case of producing modified carbide particles A1 (SiC-A1) in Example 1A, the pH value of the liquid (aqueous solution) in which NaOH water (NaOH: 40 g / water: 400 ml), silicon nitride particles (50 g), and sodium persulfate water (sodium persulfate: 9.6 g / water: 100 ml) are mixed is shown in the "pH" column.

[0137] [Table 1]

[0138] As shown in the results in the table, when a composition containing the modified carbide particles of the present invention is used, the specific gravity of the formed resin sheet is increased, indicating that the filling property of the modified carbide particles of the present invention is good.

[0139] It was also confirmed that the effects of the present invention are better when the pH of the aqueous solution when the carbonized particles are brought into contact with the oxidizing agent is 12 or higher (see comparison of the results of Examples 6A and 8A, comparison of the results of Examples 6B and 8B, etc.).

[0140] It was also confirmed that the effects of the present invention are more excellent when the oxidizing agent used is a persulfate (see comparison of the results of Examples 1A and 4A, comparison of the results of Examples 1B and 4B, etc.).

[0141] It was confirmed that the effect of the present invention is more excellent when the oxidation-reduction potential of the oxidizing agent used is 1.50 V or more. (See the comparison of results between examples in which the pH of the aqueous solution when contacting the carbide particles with the oxidizing agent is 14.)

[0142] It was also confirmed that the effect of the present invention is more excellent if an adsorption step is carried out in the method of the present invention.

[0143] [Additional Test] As an additional test, a composition using a silicone resin as the resin binder was also tested. That is, first, the epoxy compound, phenol compound, and curing accelerator used in the above-mentioned test were changed to a 1:1 (volume ratio) mixture of agent A and agent B of "KE-1012 A / B (manufactured by Shin-Etsu Chemical Co., Ltd.)," a precursor of a silicone resin binder, the solvent was changed to toluene, and the solid content concentration of the composition was changed to 55 volume % to prepare compositions (silicone resin compositions) of each Example or Comparative Example. Using an applicator, the silicone resin composition of each Example or Comparative Example was evenly applied to the release surface of a release-treated polyester film to a thickness of 1 mm, and then left to stand at 80°C for 30 minutes to obtain a coating film. A new polyester film was then laminated onto the coating of the thus obtained coated film, with the release surfaces facing each other, to obtain a laminate having a "polyester film-coating-polyester film" structure. The laminate was heat-pressed (heat plate temperature 100° C.) under air under conditions such that the thickness of the resulting thermally conductive sheet (thermally conductive material) was 500 μm. The polyester films on both sides of the laminate were peeled off to obtain silicone resin sheets (cured coating films, average thickness 500 μm) of each Example or Comparative Example. Using the obtained silicone resin sheets of each Example or Comparative Example, the filling rate of the carbide particles (including modified carbide particles) was evaluated in the same manner as described above, and the results were similar to those shown in Table 1.

Claims

1. A method for producing modified carbide particles, comprising a modification step of contacting carbide particles with an oxidizing agent in an aqueous solution to obtain modified carbide particles, which are oxidized carbide particles, the method comprising the steps of: the aqueous solution comprises an alkaline source; The pH of the aqueous solution is 12 or more; The carbide particles are at least one selected from the group consisting of silicon carbide particles, boron carbide particles, titanium carbide particles, tungsten carbide particles, iron carbide particles, vanadium carbide particles, tantalum carbide particles, zirconium carbide particles, nickel carbide particles, molybdenum carbide particles, niobium carbide particles, chromium carbide particles, and hafnium carbide particles. Method for producing modified carbide particles.

2. The method for producing modified carbide particles according to claim 1 , wherein the standard oxidation-reduction potential of the oxidizing agent is 1.50 V or more.

3. The method for producing modified carbide particles according to claim 1 or 2, wherein the oxidizing agent is a persulfate.

4. contacting the modified carbide particles obtained in the modification step with a surface modifier in the presence of at least one of water and an organic solvent, The method for producing modified carbide particles according to any one of claims 1 to 3, further comprising an adsorption step of adsorbing the surface modifier to obtain surface-modified modified carbide particles.

5. The method for producing modified carbide particles according to any one of claims 1 to 4, wherein the carbide particles are one or more selected from the group consisting of silicon carbide particles, boron carbide particles, titanium carbide particles, and tungsten carbide particles.

Citation Information

Patent Citations

  • Modification method for silicon carbide particles

    CN104610780A

  • Resin material blended with silicon carbide and its preparation

    JP1985090261A

  • Method for modifying surface of sic whisker

    JP1987113800A

  • Polishing method for silicon carbide using a water-soluble oxidizing agent

    JP2010503232A

  • Manufacturing method of semiconductor chip, semiconductor chip and semiconductor device

    JP2015119170A