Nitride semiconductor light emitting device
By optimizing the nitride semiconductor layer's composition and structure, the device achieves enhanced optical output and spectral purity in ultraviolet light emission across a targeted wavelength range, addressing the limitations of existing nitride semiconductor light emitting devices.
Patent Information
- Application Number
- JP2023131101
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-08-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-05-20
AI Technical Summary
Existing nitride semiconductor light emitting devices do not adequately consider the need for improved optical output across specific ranges of emission wavelengths, particularly in ultraviolet light emission.
The device incorporates a substrate with a c-plane growth surface and a nitride semiconductor layer with specific compositions and structures, including an n-type semiconductor layer with controlled Al composition and thickness, a single or multi-quantum well active layer, and a p-type semiconductor layer, optimized for ultraviolet light emission between 320 nm and 365 nm, with controlled Al composition differences and layer thicknesses to enhance optical output.
This configuration significantly improves optical output and narrows the full width at half maximum of the emission spectrum, enhancing the device's performance in the specified wavelength range.
Smart Images

Figure 0007595715000019 
Figure 0007595715000020 
Figure 0007595715000021
Abstract
Description
[Technical field]
[0001] The present invention relates to a nitride semiconductor light emitting device. [Background technology]
[0002] Patent Document 1 discloses a nitride semiconductor light emitting device in which a plurality of layers made of nitride semiconductors are laminated on a substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2016 / 072150 Summary of the Invention [Problem to be solved by the invention]
[0004] In order to improve the light output of a nitride semiconductor light-emitting element, the configuration to be adopted should be changed for each emission wavelength. However, this is not taken into consideration in the nitride semiconductor light-emitting element described in Patent Document 1, and there is room for improvement.
[0005] The present invention has been made in view of the above circumstances, and has an object to provide a nitride semiconductor light-emitting device capable of improving the optical output in a specific range of emission wavelength. [Means for solving the problem]
[0006] In order to achieve the above-mentioned object, the present invention provides a nitride semiconductor light-emitting device comprising: a substrate having a c-plane as a growth surface; and a nitride semiconductor layer laminated on the growth surface of the substrate, the nitride semiconductor layer emitting ultraviolet light having a central wavelength longer than 320 nm and not exceeding 365 nm, the nitride semiconductor layer comprising: an n-type semiconductor layer containing Al, Ga, and N; an active layer of a single quantum well structure formed on the side of the n-type semiconductor layer opposite to the substrate and having one well layer containing Al, Ga, and N; and a p-type semiconductor layer formed on the side of the active layer opposite to the substrate, the n-type semiconductor layer having an Al composition ratio of 50% or less and a film thickness exceeding 2 μm, and a composition difference obtained by subtracting the Al composition ratio of the well layer from the Al composition ratio of the n-type semiconductor layer is 22% or more.
[0007] Furthermore, to achieve the above-mentioned object, the present invention provides a nitride semiconductor light-emitting device comprising: a substrate having a growth surface which is a c-plane; and a nitride semiconductor layer laminated on the growth surface of the substrate, the nitride semiconductor layer emitting ultraviolet light having a central wavelength of 300 nm or more and 320 nm or less, the nitride semiconductor layer comprising: an n-type semiconductor layer containing Al, Ga, and N; an active layer of a single quantum well structure formed on the n-type semiconductor layer opposite the substrate and having one well layer containing Al, Ga, and N; and a p-type semiconductor layer formed on the active layer opposite the substrate, the active layer comprising, in this order from the n-type semiconductor layer side, a first barrier layer containing Al and N, a second barrier layer containing Al, Ga, and N and having a smaller Al composition ratio than the first barrier layer, and the well layer.
[0008] Furthermore, to achieve the above-mentioned object, the present invention provides a nitride semiconductor light-emitting device comprising: a substrate whose growth surface is a c-plane; and a nitride semiconductor layer laminated on the growth surface of the substrate, and emitting ultraviolet light having a central wavelength of 265 nm or more and less than 300 nm, wherein the nitride semiconductor layer comprises an n-type semiconductor layer containing Al, Ga, and N; an active layer with a multiple quantum well structure formed on the side of the n-type semiconductor layer opposite to the substrate and having a plurality of well layers containing Al, Ga, and N; and a p-type semiconductor layer formed on the active layer opposite to the substrate, and an Al composition ratio of the n-type semiconductor layer is more than 50% and not more than 70%. Effect of the Invention
[0009] According to the present invention, it is possible to provide a nitride semiconductor light emitting device capable of improving the light output in a specific range of emission wavelength. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic diagram illustrating a configuration of a nitride semiconductor light-emitting device in a first embodiment. [Diagram 2] FIG. 11 is a schematic diagram illustrating a configuration of a nitride semiconductor light-emitting device according to a second embodiment. [Diagram 3] FIG. 13 is a schematic diagram illustrating a configuration of a nitride semiconductor light-emitting device according to a third embodiment. [Figure 4] 11 is a graph showing the relationship between emission wavelength and optical output in an experimental example. [Diagram 5] 1 is a graph showing the relationship between emission wavelength and full width at half maximum in an experimental example. [Figure 6] 13 is a graph showing the relationship between composition difference qs and optical output when the active layer has a single quantum well structure in an experimental example. [Figure 7] 13 is a graph showing the relationship between the composition difference qs and the full width at half maximum when the active layer has a single quantum well structure in an experimental example. [Figure 8]1 is a graph showing the relationship between the Al composition ratio of a well layer and the optical output when the active layer has a single quantum well structure in an experimental example. [Figure 9] 13 is a graph showing the relationship between the Al composition ratio of a well layer and the full width at half maximum when the active layer has a single quantum well structure in an experimental example. [Figure 10] 11 is a graph showing the relationship between the number of barrier layers and the optical output when the active layer has a single quantum well structure in an experimental example. [Figure 11] 11 is a graph showing the relationship between the number of barrier layers and the full width at half maximum when the active layer has a single quantum well structure in an experimental example. [Figure 12] 13 is a graph showing the relationship between the composition difference qs and the optical output when the active layer has a multiple quantum well structure in an experimental example. [Figure 13] 13 is a graph showing the relationship between the composition difference qs and the full width at half maximum when the active layer has a multiple quantum well structure in an experimental example. [Figure 14] 1 is a graph showing the relationship between the Al composition ratio of the uppermost well layer and the optical output when the active layer has a multiple quantum well structure in an experimental example. [Figure 15] 13 is a graph showing the relationship between the Al composition ratio of the uppermost well layer and the full width at half maximum when the active layer has a multiple quantum well structure in an experimental example. [Figure 16] 1 is a graph showing the relationship between the Al composition ratio q of an n-type semiconductor layer and the film thickness d [nm] of the n-type semiconductor layer for obtaining high optical output when the active layer has a multiple quantum well structure in an experimental example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [First embodiment] A first embodiment of the present invention will be described with reference to Fig. 1. Note that the embodiment described below is shown as a preferred specific example for carrying out the present invention, and while there are some parts that specifically exemplify various technical matters that are technically preferable, the technical scope of the present invention is not limited to this specific embodiment.
[0012] (Nitride semiconductor light-emitting device 1) FIG. 1 is a schematic diagram schematically showing the configuration of the nitride semiconductor light-emitting device 1 in this embodiment. In FIG. 1, the dimensional ratio in the stacking direction of each layer of the nitride semiconductor light-emitting device 1 (hereinafter, also simply referred to as "light-emitting device 1") does not necessarily match the actual one.
[0013] The light-emitting device 1 constitutes, for example, a light-emitting diode (LED: Light Emitting Diode) or a semiconductor laser (LD: Laser Diode). The light-emitting device 1 in this embodiment constitutes a light-emitting diode that emits ultraviolet light having a central wavelength exceeding 320 nm and not exceeding 365 nm. The light-emitting device 1 includes a substrate 2, a nitride semiconductor layer 3 stacked on the growth surface 21 of the substrate 2, and an n-side electrode 4 and a p-side electrode 5 connected to the nitride semiconductor layer 3. Hereinafter, the stacking direction of the substrate 2 and the nitride semiconductor layer 3 is referred to as the vertical direction, the side on which the nitride semiconductor layer 3 is stacked with respect to the substrate 2 (that is, the upper side in FIG. 1) is referred to as the upper side, and the opposite side (that is, the lower side in FIG. 1) is referred to as the lower side. The vertical expression is for convenience and does not limit the posture of the light-emitting device 1 with respect to the vertical direction, for example, when the light-emitting device 1 is in use.
[0014] The substrate 2 is made of a material that transmits the ultraviolet light emitted by the active layer 33 described later. In this embodiment, the substrate 2 is a sapphire (Al2O3) substrate. The growth surface 21, which is the surface of the substrate 2 on which the nitride semiconductor layer 3 is stacked, is the c-plane. This c-plane may have an off-angle. Note that, as the substrate 2, for example, an aluminum nitride (AlN) substrate or an aluminum gallium nitride substrate may be used.
[0015] Each layer of the nitride semiconductor layer 3 is, for example, Al a Ga b In 1-a-b N (0 ≦ a ≦ 1, 0 ≦ b ≦ 1, 0 < a + b ≦ 1) and is composed of a ternary or quaternary group III nitride semiconductor. In this embodiment, each layer of the nitride semiconductor layer 3 is Al c Ga 1-cThe nitride semiconductor layer 3 is made of a binary or ternary Group III nitride semiconductor represented by N (0≦c≦1). A part of the Group III element may be replaced with boron (B), thallium (Tl), etc. Furthermore, a part of the nitrogen may be replaced with phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), etc. Each layer of the nitride semiconductor layer 3 has a thickness in the vertical direction. The nitride semiconductor layer 3 includes, in order from the substrate 2 side, a buffer layer 31, an n-type semiconductor layer 32, an active layer 33, an electron blocking layer 34, and a p-type semiconductor layer 35.
[0016] The buffer layer 31 has a layer made of aluminum nitride. For example, the buffer layer 31 may be formed of a single layer of aluminum nitride, or may include a layer made of aluminum gallium nitride in addition to a layer made of aluminum nitride. The thickness of the buffer layer 31 is, for example, 1 μm or more and 4 μm or less. By making the thickness of the buffer layer 31 1 μm or more, dislocations caused by the difference in lattice constant between the buffer layer 31 and the substrate 2 are prevented from being formed up to the upper end of the buffer layer 31, and the lattice constant of the upper end of the buffer layer 31 can be made the original lattice constant of aluminum nitride. In addition, by making the thickness of the buffer layer 31 4 μm or less, the occurrence of cracks caused by the difference in thermal expansion coefficient between the buffer layer 31 and a layer adjacent to the buffer layer 31 can be prevented. Note that, when the substrate 2 is an aluminum nitride substrate or an aluminum gallium nitride substrate, the buffer layer 31 is not necessarily provided.
[0017] The n-type semiconductor layer 32 is, for example, Al doped with n-type impurities. q Ga 1-qN (0≦q≦1). The n-type semiconductor layer 32 has an Al composition ratio q (also called AlN mole fraction) of 50% or less and a thickness of more than 2 μm. This causes lattice relaxation in the n-type semiconductor layer 32. In the present embodiment, when the center wavelength of the ultraviolet light emitted by the light-emitting element 1 is longer than 320 nm and shorter than 365 nm and the active layer 33 has a single quantum well (SQW) structure as described below, the light output of the light-emitting element 1 is improved by the lattice relaxation in the n-type semiconductor layer 32. The reason for this is presumably that, when the center wavelength of the ultraviolet light emitted by the light-emitting element 1 is longer than 320 nm and shorter than 365 nm and the active layer 33 has a single quantum well structure, the lattice relaxation in the n-type semiconductor layer 32 causes the distortion of the active layer 33 formed on the n-type semiconductor layer 32 to become a distortion suitable for light emission. In addition, since lattice relaxation occurs in the n-type semiconductor layer 32, the strain generated in the n-type semiconductor layer 32 is smaller than when the n-type semiconductor layer 32 is grown coherently, and the strain generated in the active layer 33 formed thereon is also smaller.
[0018] The thickness of the n-type semiconductor layer 32 is preferably 2.5 μm or more. This brings the n-type semiconductor layer 32 closer to a completely lattice-relaxed state, improving the crystallinity of the active layer 33 formed on the n-type semiconductor layer 32 and improving the light output. In addition, the thickness of the n-type semiconductor layer 32 is preferably 4 μm or less. This prevents the time required for forming the n-type semiconductor layer 32 from being unnecessarily long, improving the productivity of the light-emitting element 1.
[0019] In this embodiment, the n-type semiconductor layer 32 is composed of a single n-type cladding layer. The n-type semiconductor layer 32 may be composed of multiple layers. In this case, unless otherwise specified, the Al composition ratio of the n-type semiconductor layer 32 means the Al composition ratio of each layer of the n-type semiconductor layer 32, and the thickness of the n-type semiconductor layer 32 means the overall thickness of the n-type semiconductor layer 32, that is, the total thickness of each layer of the n-type semiconductor layer 32.
[0020] In this embodiment, silicon (Si) is used as the n-type impurity for doping the n-type semiconductor layer 32. The same applies to the semiconductor layer containing the n-type impurity other than the n-type semiconductor layer 32. Note that, as the n-type impurity, germanium (Ge), selenium (Se), tellurium (Te), or the like may be used. An active layer 33 is formed on the n-type semiconductor layer 32.
[0021] The active layer 33 is formed to have a single quantum well structure having one well layer 332. The bandgap of the active layer 33 is adjusted so that it can emit ultraviolet light with a central wavelength exceeding 320 nm and equal to or less than 365 nm. The active layer 33 has a barrier layer 331 and a well layer 332 in this order from the n-type semiconductor layer 32 side.
[0022] The barrier layer 331 is formed of Al r Ga 1-r N (0 < r ≦ 1). The Al composition ratio r of the barrier layer 331 is larger than the Al composition ratio q of the n-type semiconductor layer 32 (that is, r > q). The Al composition ratio r of the barrier layer 331 is, for example, 50% or more. The film thickness of the barrier layer 331 is, for example, 5 nm or more and 50 nm or less.
[0023] The well layer 332 is formed of Al s Ga 1-s N (0 < s < 1). The Al composition ratio s of the well layer 332 is smaller than the Al composition ratio q of the n-type semiconductor layer 32 (that is, s < q). From the viewpoint of improving the light output and narrowing the full width at half maximum (FWHM) of the emission spectrum of the light-emitting element 1, the Al composition ratio s of the well layer 332 is preferably 10% or less, and more preferably less than 6%. Hereinafter, the full width at half maximum of the emission spectrum of the light-emitting element 1 may be simply referred to as the "half width at half maximum".
[0024] The composition difference q - s obtained by subtracting the Al composition ratio s of the well layer 332 from the Al composition ratio q of the n-type semiconductor layer 32 is 22% or more. Thereby, the light output of the light-emitting element 1 is improved. From this viewpoint, the composition difference q - s is more preferably 28% or more. Further, when the Al composition ratio of the n-type semiconductor layer 32 becomes excessively high, the electrical resistance value of the n-type semiconductor layer 32 becomes excessively high. From the viewpoint of suppressing the performance degradation of the light-emitting element 1 while suppressing the electrical resistance value of the n-type semiconductor layer 32, the composition difference q - s is preferably 34% or less. The film thickness of the well layer 332 is, for example, 1 nm or more and 5 nm or less. An electron blocking layer 34 is formed on the well layer 332.
[0025] The electron blocking layer 34 has a role of improving the electron injection efficiency into the active layer 33 by suppressing the occurrence of an overflow phenomenon in which electrons leak from the active layer 33 to the p-type semiconductor layer 35 side (hereinafter, also referred to as an electron blocking effect). The electron blocking layer 34 has a stacked structure in which a first layer 341 and a second layer 342 are stacked in order from the lower side.
[0026] The first layer 341 is provided on the active layer 33. The first layer 341 is composed of, for example, Al t Ga 1-t N (0 < t ≦ 1). The Al composition ratio t of the first layer 341 is, for example, 90% or more. The film thickness of the first layer 341 is, for example, 0.5 nm or more and 5.0 nm or less.
[0027] The second layer 342 is composed of, for example, Al u Ga 1-u N (0 < u < 1). The Al composition ratio u of the second layer 342 is smaller than the Al composition ratio t of the first layer 341 and is, for example, 70% or more and 90% or less. The film thickness of the second layer 342 is larger than the film thickness of the first layer 341 and is, for example, 15 nm or more and 100 nm or less.
[0028] Since the electrical resistance of a semiconductor layer increases as the Al composition ratio increases, if the thickness of the first layer 341, which has a relatively high Al composition ratio, is made too large, the electrical resistance of the entire light-emitting element 1 increases excessively. For this reason, it is preferable to make the thickness of the first layer 341 small to a certain extent. On the other hand, if the thickness of the first layer 341 is made small, the probability that electrons will pass through the first layer 341 from the lower side to the upper side due to the tunnel effect may increase. Therefore, in the light-emitting element 1 of this embodiment, the second layer 342 is formed on the first layer 341 to prevent electrons from passing through the entire electron blocking layer 34.
[0029] Each of the first layer 341 and the second layer 342 may be an undoped layer, a layer containing n-type impurities, a layer containing p-type impurities, or a layer containing both n-type impurities and p-type impurities. Magnesium (Mg) may be used as the p-type impurity, but zinc (Zn), beryllium (Be), calcium (Ca), strontium (Sr), barium (Ba), carbon (C), or the like may also be used. The same applies to other semiconductor layers containing p-type impurities. When each electron block layer 34 contains an impurity, the impurity contained in each electron block layer 34 may be contained in the entirety of each electron block layer 34 or may be contained in a part of each electron block layer 34. A p-type semiconductor layer 35 is formed on the electron block layer 34.
[0030] In this embodiment, the p-type semiconductor layer 35 is made of a p-type contact layer. The p-type contact layer is a layer to which a p-side electrode 5 (described later) is connected, and is made of Al doped with a high concentration of p-type impurities. v Ga 1-v N (0≦v≦1). The p-type semiconductor layer 35 serving as a p-type contact layer is configured to have a low Al composition ratio in order to realize ohmic contact with the p-side electrode 5, and from this viewpoint, it is preferable to form the p-type semiconductor layer 35 from p-type gallium nitride (GaN).
[0031] The n-side electrode 4 is formed on the upper surface of the n-type semiconductor layer 32. The n-side electrode 4 may be, for example, a multilayer film in which titanium (Ti), aluminum, titanium, and gold (Au) are laminated in this order on the n-type semiconductor layer 32. In addition, when the light-emitting element 1 is flip-chip mounted as described later, the n-side electrode 4 may be made of a material capable of reflecting ultraviolet light emitted by the active layer 33.
[0032] The p-side electrode 5 is formed on the upper surface of the p-type semiconductor layer 35. The p-side electrode 5 may be, for example, a multilayer film in which nickel (Ni) and gold are laminated in this order on the p-type semiconductor layer 35. In addition, when the light-emitting element 1 is flip-chip mounted as described later, the p-side electrode 5 may be made of a material capable of reflecting ultraviolet light emitted by the active layer 33.
[0033] The light emitting element 1 may be flip-chip mounted on a package substrate (not shown) for use. That is, the side of the light emitting element 1 on which the n-side electrode 4 and the p-side electrode 5 are provided in the up-down direction faces the package substrate, and each of the n-side electrode 4 and the p-side electrode 5 is mounted on the package substrate via a gold bump or the like. The flip-chip mounted light emitting element 1 extracts light from the substrate 2 side (i.e., the lower side). However, the light emitting element may be mounted on the package substrate by wire bonding or the like. In this embodiment, the light emitting element 1 is a so-called horizontal type light emitting element in which both the n-side electrode 4 and the p-side electrode 5 are provided on the upper side of the nitride semiconductor layer 3, but the light emitting element may be a vertical type light emitting element. The vertical type light emitting element is a light emitting element in which the nitride semiconductor layer is sandwiched between the n-side electrode and the p-side electrode. When the light emitting element is a vertical type, it is preferable to remove the substrate and the buffer layer by laser lift-off or the like.
[0034] (Method of manufacturing the nitride semiconductor light emitting element 1) Next, an example of a method for manufacturing the light-emitting element 1 will be described. In this embodiment, each layer of the nitride semiconductor layer 3 is epitaxially grown in order on a disk-shaped substrate 2 by metal organic chemical vapor deposition (MOCVD). That is, in this embodiment, the disk-shaped substrate 2 is placed in a chamber, and the source gases of each layer to be formed on the substrate 2 are introduced into the chamber to form the nitride semiconductor layer 3 on the substrate 2. As source gases for epitaxially growing each layer, trimethylaluminum (TMA) as an aluminum source, trimethylgallium (TMG) as a gallium source, ammonia (NH3) as a nitrogen source, tetramethylsilane (TMSi) as a silicon source, and biscyclopentadienylmagnesium (Cp2Mg) as a magnesium source can be used. The manufacturing conditions such as the growth temperature, growth pressure, and growth time for epitaxially growing each layer can be general conditions according to the configuration of each layer.
[0035] The MOCVD method is sometimes called Metal Organic Vapor Phase Epitaxy (MOVPE). When epitaxially growing each layer of the nitride semiconductor layer 3 on the substrate 2, other epitaxial growth methods such as Molecular Beam Epitaxy (MBE) and Hydride Vapor Phase Epitaxy (HVPE) can also be used.
[0036] After the nitride semiconductor layer 3 is formed on the disk-shaped substrate 2, a mask is formed on a portion of the p-type semiconductor layer 35, i.e., on a portion other than the portion that will become the exposed surface 321 of the n-type semiconductor layer 32. Then, the region where the mask is not formed is removed by etching from the upper surface of the p-type semiconductor layer 35 to the middle of the n-type semiconductor layer 32 in the vertical direction. As a result, the exposed surface 321 that is exposed toward the upper side is formed in the n-type semiconductor layer 32. After the exposed surface 321 is formed, the mask is removed.
[0037] Next, an n-side electrode 4 is formed on the exposed surface 321 of the n-type semiconductor layer 32, and a p-side electrode 5 is formed on the p-type semiconductor layer 35. The n-side electrode 4 and the p-side electrode 5 may be formed by a well-known method such as an electron beam evaporation method or a sputtering method. By cutting the thus completed one into desired dimensions, a plurality of light-emitting elements 1 as shown in FIG. 1 are manufactured from one wafer.
[0038] [Second Embodiment] FIG. 2 is a schematic diagram schematically showing the configuration of the light-emitting element 1 in this embodiment.
[0039] This embodiment is a form in which, compared with the first embodiment, the center wavelength of the emission wavelength is set to 300 nm or more and 320 nm or less, and the configurations of the n-type semiconductor layer 32 and the active layer 33 are changed.
[0040] The n-type semiconductor layer 32 of this embodiment may have lattice relaxation or may be coherently grown. The Al composition ratio q of the n-type semiconductor layer 32 is not particularly limited, but as an example, the Al composition ratio q can be 30% or more and 70% or less. The film thickness of the n-type semiconductor layer 32 is preferably 1 μm or more and 4 μm or less. By setting the film thickness of the n-type semiconductor layer 32 to 1 μm or more, it is possible to suppress an increase in the overall electrical resistance value of the light-emitting element 1 due to a decrease in the cross-sectional area of the n-type semiconductor layer 32. By setting the film thickness of the n-type semiconductor layer 32 to 4 μm or less, it is possible to suppress an unnecessarily long film formation time of the n-type semiconductor layer 32 and improve the productivity of the light-emitting element 1.
[0041] The active layer 33 has a single quantum well structure as in the first embodiment. The band gap of the active layer 33 is adjusted so that it can emit ultraviolet light having a center wavelength of 300 nm or more and 320 nm or less. The active layer 33 includes a first barrier layer 331a, a second barrier layer 331b, and a well layer 332 in this order from the n-type semiconductor layer 32 side.
[0042] The first barrier layer 331a is formed of Al r1 Ga 1-r1 N(0 < r1 ≦ 1), and the second barrier layer 331b is formed of Alr2 Ga 1-r2 It is formed by N(0 < r2 < 1). The Al composition ratio r1 of the first barrier layer 331a is larger than the Al composition ratio r2 of the second barrier layer 331b (i.e., r1 > r2). The Al composition ratio r1 of the first barrier layer 331a is, for example, 80% or more, and the Al composition ratio r2 of the second barrier layer 331b is larger than the Al composition ratio s of the well layer 332 and is, for example, 65% or more and 95% or less. The film thickness of the first barrier layer 331a is smaller than the film thickness of the second barrier layer 331b. The first barrier layer 331a is a layer with a high Al composition ratio r1. If its film thickness is made too large, the overall electrical resistance value of the light-emitting element 1 will increase. Therefore, it is preferable that the film thickness of the first barrier layer 331a is smaller than the film thickness of the second barrier layer 331b. The film thickness of the first barrier layer 331a is, for example, 1 nm or more and 5 nm or less, and the film thickness of the second barrier layer 331b is, for example, 5 nm or more and 20 nm or less.
[0043] From the viewpoint of improving the light output, the Al composition ratio s of the well layer 332 is preferably 15% or more and 26% or less, and more preferably further satisfies 22% or less. Also, from the viewpoint of narrowing the full width at half maximum of the emission spectrum of the light-emitting element 1, the Al composition ratio s of the well layer 332 is preferably 18% or more.
[0044] The composition difference q - s obtained by subtracting the Al composition ratio s of the well layer 332 from the Al composition ratio q of the n-type semiconductor layer 32 is preferably 28% or more and 41% or less from the viewpoint of improving the light output. Also, from the viewpoint of narrowing the full width at half maximum of the emission spectrum of the light-emitting element 1, the n-type semiconductor layer 32 satisfies at least one of an Al composition ratio of more than 50% and a film thickness of 2 μm or less (i.e., the n-type semiconductor layer 32 is formed by coherent growth), and it is preferable that the composition difference q - s satisfies 30% or more and 40% or less.
[0045] Other aspects are the same as those in the first embodiment. Among the reference numerals used in the second embodiment and subsequent embodiments, those that are the same as the reference numerals used in the previous embodiments represent the same components and the like as those in the previous embodiments unless otherwise specified.
[0046] [Third Embodiment] FIG. 3 is a schematic diagram illustrating the configuration of the light-emitting element 1 in this embodiment.
[0047] In this embodiment, unlike the first embodiment, the center wavelength of the emission wavelength is set to be equal to or greater than 265 nm and less than 300 nm, the n-type semiconductor layer 32 is formed by coherent growth, and the active layer 33 has a multi-quantum well (MQW) structure.
[0048] In the present embodiment, when the center wavelength of the ultraviolet light emitted by the light emitting element 1 is 265 nm or more and less than 300 nm and the active layer 33 has a multiple quantum well structure having a plurality of well layers 332a to 332c, the light output of the light emitting element 1 is improved by forming the n-type semiconductor layer 32 by coherent growth. This is presumably because, when the center wavelength of the ultraviolet light emitted by the light emitting element 1 is 265 nm or more and less than 300 nm and the active layer 33 has a multiple quantum well structure, the strain of the n-type semiconductor layer 32 is relaxed in the active layer 33 of the multiple quantum well structure by forming the n-type semiconductor layer 32 by coherent growth, and the strain generated in the well layer 332c located at the top becomes a strain suitable for light emission. Note that, when the active layer 33 has a multiple quantum well structure, the well layer 332c located closest to the p-type semiconductor layer 35 (i.e., the uppermost well layer 332c described later) of the multiple well layers 332a to 332c constituting the active layer 33 tends to emit light most strongly. Furthermore, when the central wavelength of the ultraviolet light emitted by the light-emitting element 1 is short, such as 265 nm or more and less than 300 nm, the light in directions other than the c-axis direction of the substrate 2 (e.g., the a-axis direction, the m-axis direction, etc.) tends to be strong, making it difficult to extract the ultraviolet light from the bottom side of the substrate 2; however, in this embodiment, the light output from the bottom side of the substrate 2 can be improved.
[0049] In this embodiment, the n-type semiconductor layer 32 is formed by coherent growth by satisfying an Al composition ratio of more than 50%. The Al composition ratio of the n-type semiconductor layer 32 further satisfies 70% or less. The thickness of the n-type semiconductor layer 32 is preferably 1 μm or more and 4 μm or less. By making the thickness of the n-type semiconductor layer 32 1 μm or more, it is possible to suppress an increase in the overall electrical resistance value of the light-emitting element 1 caused by a reduction in the cross-sectional area of the n-type semiconductor layer 32. By making the thickness of the n-type semiconductor layer 32 4 μm or less, it is possible to suppress an unnecessary increase in the deposition time of the n-type semiconductor layer 32, thereby improving the productivity of the light-emitting element 1.
[0050] It is preferable that the Al composition ratio q of the n-type semiconductor layer 32 and the film thickness d [μm] of the n-type semiconductor layer 32 satisfy the relationship 4.1q-0.6≦d≦4.1q. Since the n-type semiconductor layer 32 has a lower carrier concentration and a higher electrical resistance as the Al composition ratio increases, by increasing the film thickness d in accordance with the increase in the Al composition ratio of the n-type semiconductor layer 32, the increase in the electrical resistance of the n-type semiconductor layer 32 can be suppressed.
[0051] The active layer 33 is formed to have a multiple quantum well structure having a plurality of well layers 332a-332c. The band gap of the active layer 33 is adjusted so that the active layer 33 can emit ultraviolet light having a central wavelength of 265 nm or more and less than 300 nm. In this embodiment, an example will be described in which the active layer 33 includes three barrier layers 331 and three well layers 332a-332c. From the viewpoint of improving the optical output, the number of well layers 332a-332c in the active layer 33 is preferably three or less.
[0052] The barrier layer 331 and the well layers 332a to 332c are alternately stacked. The barrier layer 331 is formed at the lower end of the active layer 33, and the well layer 332c is formed at the upper end of the active layer 33. The configuration of each barrier layer 331 can be the same as that of the first embodiment.
[0053] Among the three well layers 332a to 332c, the well layer arranged at the bottom is the bottom well layer 332a, the well layer arranged at the top is the top well layer 332c, and the well layer arranged between the bottom well layer 332a and the top well layer 332c is the middle well layer 332b. In this embodiment, the three well layers 332a to 332c have different configurations between the bottom well layer 332a and the well layers other than the bottom well layer 332a (i.e., the middle well layer 332b and the top well layer 332c). The film thickness of the bottom well layer 332a is larger than the film thickness of each of the middle well layer 332b and the top well layer 332c. This flattens the bottom well layer 332a, and improves the flatness of each layer of the active layer 33 formed on the bottom well layer 332a, thereby improving the monochromaticity of the output light. For example, the thickness of the bottom well layer 332a may be 4 nm or more and 6 nm or less, and the thickness of each of the intermediate well layer 332b and the top well layer 332c may be 2 nm or more and 4 nm or less. The Al composition ratio of each of the three well layers 332a to 332c may be, for example, 25% or more and 45% or less. From the viewpoint of improving the optical output and narrowing the full width at half maximum, the Al composition ratio of each of the three well layers 332a to 332c is preferably 28% or more and 36% or less. The Al composition ratio of the bottom well layer 332a may be higher than the Al composition ratio of each of the intermediate well layer 332b and the top well layer 332c. This makes the difference in Al composition ratio between the n-type semiconductor layer 32 and the bottom well layer 332a relatively small, and improves the crystallinity of each layer of the active layer 33.
[0054] The composition difference qs obtained by subtracting the Al composition ratio s of the uppermost well layer 332c from the Al composition ratio q of the n-type semiconductor layer 32 is preferably 15% or more and 31% or less, and more preferably 20% or more and less than 30%, from the viewpoint of improving the optical output. Moreover, from the viewpoint of narrowing the full width at half maximum of the light-emitting element 1, the composition difference qs is preferably 22% or less. The rest is similar to the first embodiment.
[0055] [Experimental Example] In this experimental example, a large number of light emitting devices with different emission wavelengths, active layer configurations, growth modes of the n-type semiconductor layer, etc. were prepared, and the optical output and full width at half maximum were measured for each of the light emitting devices.
[0056] In this experimental example, light-emitting elements according to Samples 1 to 131 were prepared. First, Table 1 shows the general configurations of Samples 1 to 131.
[0057] [Table 1]
[0058] In Table 1, the notation "SQW" means a single quantum well structure, and the notation "MQW" means a multiple quantum well structure. The column for the growth mode of the n-type semiconductor layer indicates whether lattice relaxation occurs in the n-type semiconductor layer or whether the n-type semiconductor layer grows coherently. If the conditions that the Al composition ratio of the n-type semiconductor layer is 50% or more and the film thickness of the n-type semiconductor layer is more than 2 μm are met, the growth mode of the n-type semiconductor layer is determined to be lattice relaxation, and if these conditions are not met, the growth mode of the n-type semiconductor layer is determined to be coherent growth. It has been confirmed that lattice relaxation occurs in the n-type semiconductor layer when this condition is met, and that the n-type semiconductor layer grows coherently when the above-mentioned condition is not met.
[0059] Tables 2 to 9 show the detailed configurations of Samples 1 to 17, Samples 18 to 39, Samples 40 to 53, Sample 54, Samples 55 to 72, Samples 73 to 129, Sample 130, and Sample 131, respectively.
[0060] [Table 2]
[0061] [Table 3]
[0062] [Table 4]
[0063] [Table 5]
[0064] [Table 6]
[0065] [Table 7]
[0066] [Table 8]
[0067] [Table 9]
[0068] The thickness of each layer shown in Tables 2 to 9 was measured by a transmission electron microscope, and the Al composition ratio of each layer shown in Tables 2 to 9 was estimated from the secondary ion intensity of Al measured by secondary ion mass spectrometry (SIMS).
[0069] In this experimental example, the optical output and full width at half maximum of each of Samples 1 to 131 were measured. The optical output of each sample was measured when a current of 20 mA was applied to each sample in an on-wafer state. The optical output of each sample was measured by a photodetector installed on the lower side (i.e., on the substrate side) of each of Samples 1 to 131.
[0070] Tables 10 to 18 show the relationship between the specific configuration of the main parts of each sample and the emission wavelength, optical output, and full width at half maximum. FIG. 4 shows the relationship between the emission wavelength and optical output of each sample, and FIG. 5 shows the emission wavelength and full width at half maximum (FWHM) of each sample. In FIG. 4 and FIG. 5, the measurement results of the sample in which the active layer has a single quantum well structure and the growth mode of the n-type semiconductor layer is lattice relaxation are plotted with filled squares, the measurement results of the sample in which the active layer has a single quantum well structure and the growth mode of the n-type semiconductor layer is coherent growth are plotted with filled squares, the measurement results of the sample in which the active layer has a multiple quantum well structure and the growth mode of the n-type semiconductor layer is lattice relaxation are plotted with filled diamonds, and the measurement results of the sample in which the active layer has a multiple quantum well structure and the growth mode of the n-type semiconductor layer is coherent growth are plotted with filled diamonds.
[0071] [Table 10]
[0072] [Table 11]
[0073] [Table 12]
[0074] [Table 13]
[0075] [Table 14]
[0076] [Table 15]
[0077] [Table 16]
[0078] [Table 17]
[0079] [Table 18]
[0080] (Effects of the First Embodiment) The effects of the first embodiment will be examined from the results of the experiment. The first embodiment is a light-emitting device that emits ultraviolet light having a central wavelength longer than 320 nm and not exceeding 365 nm, the growth mode of the n-type semiconductor layer is lattice relaxation, the active layer has a single quantum well structure, and the composition difference qs obtained by subtracting the Al composition ratio of the well layer from the Al composition ratio of the n-type semiconductor layer is 22% or more.
[0081] 4 and 5, among the samples plotted with black squares, those having an emission wavelength of more than 320 nm and not more than 365 nm and having a composition difference qs obtained by subtracting the Al composition ratio s of the well layer from the Al composition ratio q of the n-type semiconductor layer of 22% or more are light-emitting devices that satisfy the configuration of the first embodiment. As can be seen from Figures 4 and 5, those samples plotted with black squares and having an emission wavelength of more than 320 nm and not more than 365 nm (i.e., those satisfying a part of the configuration of the first embodiment) have high optical output and narrow full width at half maximum.
[0082] Next, reference is made to Figs. 6 to 9, which show the results of Figs. 4 and 5 from different viewpoints. Fig. 6 is a diagram showing the relationship between the composition difference qs between the n-type semiconductor layer and the well layer and the optical output for a sample whose active layer has a single quantum well structure. Fig. 7 is a diagram showing the relationship between the composition difference qs between the n-type semiconductor layer and the well layer and the full width at half maximum for a sample whose active layer has a single quantum well structure. Fig. 8 is a diagram showing the relationship between the Al composition ratio of the well layer and the optical output for a sample whose active layer has a single quantum well structure. Fig. 9 is a diagram showing the relationship between the Al composition ratio of the well layer and the full width at half maximum for a sample whose active layer has a single quantum well structure. 6 to 9, the results of the samples in which the growth mode of the n-type semiconductor layer is lattice relaxation and the emission wavelength is less than 300 nm are plotted with a cross symbol, the results of the samples in which the growth mode of the n-type semiconductor layer is lattice relaxation and the emission wavelength is 300 nm to 320 nm are plotted with a white circle symbol, and the results of the samples in which the growth mode of the n-type semiconductor layer is lattice relaxation and the emission wavelength is more than 320 nm and less than 365 nm are plotted with a black circle symbol. Also, in FIG. 6 to FIG. 9, the results of the samples in which the growth mode of the n-type semiconductor layer is coherent and the emission wavelength is less than 300 nm are plotted with a cross symbol, the results of the samples in which the growth mode of the n-type semiconductor layer is coherent and the emission wavelength is 300 nm to 320 nm are plotted with a white triangle, and the results of the samples in which the growth mode of the n-type semiconductor layer is coherent and the emission wavelength is more than 320 nm and less than 365 nm are plotted with a black triangle.
[0083] In FIGS. 6 and 7, among the samples plotted with black circles, samples that satisfy the composition difference qs of 22% or more are light-emitting devices that satisfy the configuration of the first embodiment.
[0084] From Fig. 6, it can be seen that the samples plotted with black circles have a particularly high optical output when the composition difference qs is 22% or more. Therefore, it can be seen that high optical output can be obtained by satisfying the configuration of the first embodiment. It can also be seen that, among them, a particularly high optical output can be obtained when the composition difference qs is 28% or more.
[0085] 8 and 9, it can be seen that in the samples plotted with black circles, the optical output is improved and the full width at half maximum is narrowed by setting the composition ratio of the well layer to 10% or less. From this viewpoint, it can be seen that in the samples plotted with black circles, the composition ratio of the well layer is preferably set to less than 6%.
[0086] (Effects of the second embodiment) Next, the effects of the second embodiment will be considered. The second embodiment is a light emitting device that emits ultraviolet light having a central wavelength of 300 nm or more and 320 nm or less, has an active layer with a single quantum well structure, and includes a first barrier layer and a second barrier layer.
[0087] In Fig. 4 and Fig. 5, among the samples plotted with black squares and white squares, the samples having an emission wavelength of 300 nm or more and 320 nm or less and an active layer including a first barrier layer and a second barrier layer are light-emitting devices that satisfy the configuration of the second embodiment. As can be seen from Fig. 4 and Fig. 5, the samples plotted with black squares and white squares and having an emission wavelength of 300 nm or more and 320 nm or less (i.e., samples that satisfy a part of the configuration of the second embodiment) have high optical output and narrow full width at half maximum. In other words, when the active layer has a single quantum well structure, regardless of whether the growth mode of the n-type semiconductor layer is lattice relaxed or coherent growth, high optical output and narrow full width at half maximum are obtained when the emission wavelength is 300 nm or more and 320 nm or less.
[0088] 10 and 11 are diagrams comparing the optical output and full width at half maximum of three samples, two of samples 44-53 listed in Table 4 and sample 54 listed in FIG. 5. These three samples have the same configuration except for the number of barrier layers. These three samples have an emission wavelength of 300 nm or more and 320 nm or less, and the n-type semiconductor layer is formed by coherent growth. Of these three samples, the one with two barrier layers is the sample that satisfies the configuration of the second embodiment. As can be seen from FIG. 10 and FIG. 11, the sample with two barrier layers has improved optical output and narrower full width at half maximum than the sample with one barrier layer. Therefore, it can be seen that a higher optical output and a narrower full width at half maximum can be obtained by satisfying the configuration of the second embodiment.
[0089] Furthermore, in Figures 6 to 9, among the samples plotted with open circles and open triangles, the samples in which the active layer includes a first barrier layer and a second barrier layer are light-emitting devices that satisfy the configuration of the second embodiment.
[0090] It can be seen from Fig. 6 that the samples plotted with open circles and open triangles have particularly high optical output when the composition difference qs is 28% or more and 41% or less. Also, from Fig. 7 that, of the samples plotted with open circles and open triangles, the samples plotted with open triangles in particular have narrow full width at half maximum when the composition difference qs is 30% or more and 40% or less.
[0091] 8 shows that the samples plotted with open circles and open triangles have improved optical output by setting the Al composition ratio in the well layer to 15% or more and 26% or less, and Fig. 9 shows that the samples plotted with open circles and open triangles have narrowed full width at half maximum by setting the Al composition ratio in the well layer to 18% or more.
[0092] (Effects of the third embodiment) Next, the effects of the third embodiment will be considered. The third embodiment is a light emitting device that emits ultraviolet light having a central wavelength of 265 nm or more and less than 300 nm, the growth mode of the n-type semiconductor layer is coherent growth, and the active layer has a multiple quantum well structure.
[0093] In Figures 4 and 5, among the samples plotted with open diamonds, samples with an emission wavelength of 265 nm or more and less than 300 nm are light-emitting devices that satisfy the configuration of the third embodiment. As can be seen from Figures 4 and 5, samples plotted with open diamonds and having an emission wavelength of 265 nm or more and less than 300 nm (i.e., samples that satisfy the configuration of the third embodiment) tend to have high optical output and narrow full width at half maximum. Among them, samples with an emission wavelength of 285 nm or more tend to have particularly high optical output.
[0094] Next, reference is made to Figs. 12 to 15, which are views of the results of Figs. 4 and 5 from different viewpoints. Fig. 12 is a diagram showing the relationship between the composition difference qs between the n-type semiconductor layer and the top well layer and the optical output for a sample whose active layer has a multiple quantum well structure. Fig. 13 is a diagram showing the relationship between the composition difference qs between the n-type semiconductor layer and the top well layer and the full width at half maximum for a sample whose active layer has a multiple quantum well structure. Fig. 14 is a diagram showing the relationship between the Al composition ratio of the top well layer and the optical output for a sample whose active layer has a multiple quantum well structure. Fig. 15 is a diagram showing the relationship between the Al composition ratio of the top well layer and the full width at half maximum for a sample whose active layer has a multiple quantum well structure. 12 to 15, the results of samples having an active layer with three well layers (i.e., 3QW), a growth mode of the n-type semiconductor layer being lattice relaxed, and an emission wavelength of 265 nm or more and less than 300 nm are plotted with open circles, and the results of samples having an active layer with three well layers, a growth mode of the n-type semiconductor layer being lattice relaxed, and an emission wavelength of 300 nm or more and 365 nm or less are plotted with filled circles. 12 to 15, the results of samples having an active layer with three well layers, a coherent growth mode for the n-type semiconductor layer, and an emission wavelength of less than 265 nm are plotted with crosses, the results of samples having an active layer with three well layers, a coherent growth mode for the n-type semiconductor layer, and an emission wavelength of 265 nm or more and less than 300 nm are plotted with open triangles, and the results of samples having an active layer with three well layers, a coherent growth mode for the n-type semiconductor layer, and an emission wavelength of 300 nm or more and 365 nm or less are plotted with filled triangles. 12 to 15, the results of samples having an active layer with four well layers (i.e., 4QW), a growth mode of the n-type semiconductor layer being coherent, and an emission wavelength of 265 nm or more and less than 300 nm are plotted as open squares, and the results of samples having an active layer with two well layers (i.e., 2QW), a growth mode of the n-type semiconductor layer being coherent, and an emission wavelength of 265 nm or more and less than 300 nm are plotted as filled squares.
[0095] In FIGS. 12 to 15, the samples plotted with open triangles, open squares, and filled squares are light-emitting elements that satisfy the configuration of the third embodiment.
[0096] From Fig. 12, it can be seen that, from the viewpoint of improving the light output, it is preferable that the composition difference qs of the samples corresponding to the plots of the open triangles, open squares, and filled squares is 15% or more and 31% or less, and more preferably 20% or more and less than 30%. Also, from the viewpoint of narrowing the full width at half maximum, it can be seen that, from the viewpoint of narrowing the full width at half maximum, it is preferable that the composition difference qs of the samples corresponding to the plots of the open triangles, open squares, and filled squares is 22% or less.
[0097] Furthermore, from Figures 14 and 15, it can be seen that for the samples corresponding to the plots of open triangles, open squares, and filled squares, by setting the Al composition ratio of the top well layer to be 28% or more and 36% or less, the light output is improved and the full width at half maximum is narrowed.
[0098] 12 and 14, it can be seen that the light output of the light-emitting device including the active layer having four well layers is relatively low. Therefore, the configuration of the third embodiment preferably has two or three well layers.
[0099] FIG. 16 is a diagram showing the relationship between the Al composition ratio q of the n-type semiconductor layer and the thickness d [μm] of the n-type semiconductor layer for the samples related to the open triangle plots and the filled square plots in FIG. 12 to FIG. 15. All of these samples have high light output, and FIG. 15 shows the relationship between the Al composition ratio q of the n-type semiconductor layer and the thickness d of the n-type semiconductor layer for increasing the light output. These samples are three types of samples with Al composition ratios q of 55%, 65%, and 75%. The vertical axis in the graph of FIG. 16 shows the average thickness of the n-type semiconductor layer in the samples having each Al composition ratio. In FIG. 16, the approximation line of the three plots is also shown. This approximation line is a line expressed by d=4.1q-0.3. That is, in a light-emitting device having an emission wavelength of 265 nm or more and less than 300 nm, an active layer having a multiple quantum well structure, and an n-type semiconductor layer having a coherent growth mode, the Al composition ratio q of the n-type semiconductor layer and the thickness d of the n-type semiconductor layer preferably satisfy the relationship d=4.1q-0.3 or a relationship close to this. For example, it is preferable to satisfy 4.1q-0.6≦d≦4.1q, which is within the range of plus or minus 0.3 of d=4.1q-0.3.
[0100] (Summary of the embodiment) Next, the technical ideas grasped from the above-described embodiment will be described by using the reference numerals and the like in the embodiment. However, the reference numerals and the like in the following description do not limit the components in the claims to the members and the like specifically shown in the embodiment.
[0101] [1] A first embodiment of the present invention is a nitride semiconductor light-emitting device (1) that includes a substrate (2) having a growth surface (21) that is a c-plane, and a nitride semiconductor layer (3) that is laminated on the growth surface (21) of the substrate (2), and that emits ultraviolet light having a center wavelength of more than 320 nm and not more than 365 nm, wherein the nitride semiconductor layer (3) includes an n-type semiconductor layer (32) containing Al, Ga, and N, and a nitride semiconductor layer (33) that is formed on the side of the n-type semiconductor layer (32) opposite to the substrate (2), and that contains Al, Ga, and N. The nitride semiconductor light-emitting element (1) comprises: an active layer (33) of a single quantum well structure having one well layer (332) containing N; and a p-type semiconductor layer (35) formed on the active layer (33) opposite the substrate (2), wherein the n-type semiconductor layer (32) has an Al composition ratio of 50% or less and a thickness of more than 2 μm, and a composition difference obtained by subtracting the Al composition ratio of the well layer (332) from the Al composition ratio of the n-type semiconductor layer (32) is 22% or more. This makes it possible to provide a nitride semiconductor light emitting device (1) capable of improving the optical output in a specific range of emission wavelengths.
[0102] [2] A second embodiment of the present invention is the first embodiment, in which the composition difference is 28% or more and 34% or less. This improves the optical output of the nitride semiconductor light emitting device (1) and also improves productivity.
[0103] [3] A third embodiment of the present invention is the first or second embodiment, wherein the substrate (2) is a sapphire substrate, the nitride semiconductor layer (3) further comprises a buffer layer (31) having an AlN layer formed between the substrate (2) and the n-type semiconductor layer (32), and the buffer layer (31) has a thickness of 1 μm or more and 4 μm or less. This further improves the optical output of the nitride semiconductor light emitting device (1).
[0104] [4] A fourth embodiment of the present invention is a nitride semiconductor light-emitting device (1) that includes a substrate (2) having a growth surface (21) that is a c-plane, and a nitride semiconductor layer (3) that is laminated on the growth surface (21) of the substrate (2), and that emits ultraviolet light having a center wavelength of 300 nm or more and 320 nm or less, wherein the nitride semiconductor layer (3) includes an n-type semiconductor layer (32) containing Al, Ga, and N, and a single well (34) containing Al, Ga, and N that is formed on the side of the n-type semiconductor layer (32) opposite to the substrate (2). The nitride semiconductor light-emitting element (1) includes an active layer (33) of a single quantum well structure having a well layer (332) and a p-type semiconductor layer (35) formed on the active layer (33) opposite the substrate (2), the active layer (33) including, in order from the n-type semiconductor layer (32) side, a first barrier layer (331a) containing Al and N, a second barrier layer (331b) containing Al, Ga, and N and having a smaller Al composition ratio than the first barrier layer (331a), and the well layer (332). This makes it possible to provide a nitride semiconductor light emitting device (1) capable of improving the optical output in a specific range of emission wavelengths.
[0105] [5] A fifth embodiment of the present invention is the fourth embodiment, in which a composition difference obtained by subtracting the Al composition ratio of the well layer (332) from the Al composition ratio of the n-type semiconductor layer (32) is 28% or more and 41% or less. This further improves the optical output of the nitride semiconductor light emitting device (1).
[0106] [6] A sixth embodiment of the present invention is the fifth embodiment, wherein the n-type semiconductor layer (32) satisfies at least one of an Al composition ratio of more than 50% and a film thickness of 2 μm or less, and the composition difference is 30% or more and 40% or less. This makes it possible to narrow the full width at half maximum in the emission spectrum of the nitride semiconductor light emitting device (1).
[0107] [7] A seventh embodiment of the present invention is any one of the fourth to sixth embodiments, wherein the film thickness of the first barrier layer (331a) is smaller than the film thickness of the second barrier layer (331b). This makes it possible to reduce the overall electrical resistance of the nitride semiconductor light emitting device (1).
[0108] [8] An eighth embodiment of the present invention is a nitride semiconductor light-emitting element (1) comprising a substrate (2) whose growth surface (21) is a c-plane, and a nitride semiconductor layer (3) laminated on the growth surface (21) of the substrate (2), and emitting ultraviolet light having a central wavelength of 265 nm or more and less than 300 nm, in which the nitride semiconductor layer (3) comprises an n-type semiconductor layer (32) containing Al, Ga, and N, an active layer (33) of a multiple quantum well structure formed on the side of the n-type semiconductor layer (32) opposite to the substrate (2) and having a plurality of well layers (332a to 332c) containing Al, Ga, and N, and a p-type semiconductor layer (35) formed on the side of the active layer (33) opposite to the substrate (2), and an Al composition ratio of the n-type semiconductor layer (32) is more than 50% and not more than 70%. This makes it possible to provide a nitride semiconductor light emitting device (1) capable of improving the optical output in a specific range of emission wavelengths.
[0109] [9] A ninth embodiment of the present invention is the eighth embodiment, wherein an Al composition ratio q of the n-type semiconductor layer (32) and a film thickness d [μm] of the n-type semiconductor layer (32) satisfy a relationship of 4.1q-0.6≦d≦4.1q. This further improves the optical output of the nitride semiconductor light emitting device (1).
[0110]
[10] A tenth embodiment of the present invention is the eighth or ninth embodiment, in which a composition difference obtained by subtracting an Al composition ratio of an uppermost well layer (332c), which is a well layer among the plurality of well layers (332a to 332c) located closest to the p-type semiconductor layer (35) from an Al composition ratio of the n-type semiconductor layer (32) is not less than 15% and not more than 31%. This further improves the optical output of the nitride semiconductor light emitting device (1).
[0111]
[11] An eleventh embodiment of the present invention is any one of the eighth to tenth embodiments, wherein the substrate (2) is a sapphire substrate, the nitride semiconductor layer (3) further comprises a buffer layer (31) having a layer made of AlN formed between the substrate (2) and the n-type semiconductor layer (32), and the thickness of the buffer layer (31) is 1 μm or more and 4 μm or less. This further improves the optical output of the nitride semiconductor light emitting device (1).
[0112] (Additional Note) Although the embodiment of the present invention has been described above, the invention according to the claims is not limited to the above embodiment. It should be noted that not all of the combinations of features described in the embodiment are essential to the means for solving the problems of the invention. The present invention can be modified appropriately without departing from the spirit of the invention. [Explanation of symbols]
[0113] 1...Nitride semiconductor light emitting device 2...Substrate 21…Growth aspect 3...Nitride semiconductor layer 31...Buffer layer 32...n-type semiconductor layer 33…Active layer 331a...first barrier layer 331b…Second barrier layer 332...Well layer 332a…Lowest well layer 332b...Middle well layer 332c…Top well layer 35...p-type semiconductor layer
Claims
1. A nitride semiconductor light emitting device comprising: a substrate having a c-plane as a growth surface; and a nitride semiconductor layer laminated on the growth surface of the substrate, the nitride semiconductor light emitting device emitting ultraviolet light having a central wavelength of 265 nm or more and less than 300 nm, The nitride semiconductor layer is an n-type semiconductor layer containing Al, Ga, and N; an active layer having a multiple quantum well structure, the active layer being formed on the n-type semiconductor layer on the opposite side to the substrate and having a plurality of well layers containing Al, Ga, and N; a p-type semiconductor layer formed on the active layer opposite the substrate; The Al composition ratio of the n-type semiconductor layer is more than 50% and not more than 70%, when the well layer closest to the n-type semiconductor layer among the plurality of well layers is defined as a bottom well layer, the film thickness of the bottom well layer is larger than the film thickness of each of the well layers other than the bottom well layer, an Al composition ratio q of the n-type semiconductor layer and a film thickness d [μm] of the n-type semiconductor layer satisfy a relationship of 4.1q-0.6≦d≦4.1q, a composition difference obtained by subtracting an Al composition ratio of an uppermost well layer, which is a well layer among the plurality of well layers located closest to the p-type semiconductor layer, from an Al composition ratio of the n-type semiconductor layer is 15% or more and 31% or less. Nitride semiconductor light emitting element.
2. the substrate is a sapphire substrate; the nitride semiconductor layer further includes a buffer layer having an AlN layer formed between the substrate and the n-type semiconductor layer, The thickness of the buffer layer is 1 μm or more and 4 μm or less. The nitride semiconductor light emitting device according to claim 1 .
Citation Information
Patent Citations
Method of manufacturing nitride semiconductor layer, method of manufacturing nitride semiconductor light emitting device, and nitride semiconductor light emitting device
JP2010258097A
Wafer for nitride semiconductor element formation, manufacturing method of wafer for nitride semiconductor element formation, nitride semiconductor element and nitride semiconductor element manufacturing method
JP2013187296A
Ultraviolet light-emitting device
JP2015119108A
Semiconductor light-emitting element and manufacturing method of the same
JP2018163941A
Group iii nitride semiconductor light-emitting device and manufacturing method thereof
JP2020077874A