Battery separator and coating process thereof, coating system and battery

The described coating process for lithium ion battery separators addresses issues of heat resistance and moisture resistance by using synchronized heat setting and online coating, resulting in improved battery performance and reduced production costs.

JP7595754B2Active Publication Date: 2024-12-06SHANGHAI ENERGY NEW MATERIALS TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023516546
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-02
Filing Date
2021-09-14
Publication Date
2024-12-06
Estimated Expiration
2041-09-14

AI Technical Summary

Technical Problem

Conventional lithium ion battery separators face issues with heat resistance, moisture resistance, porosity, thickness uniformity, and high internal resistance, leading to poor battery performance and increased production costs due to complex processes and low pass rates.

Method used

A battery separator coating process involving initial heat setting of a polyolefin film, online coating with a polyolefin film, and heat setting of the coated film, utilizing a multi-stage oven system with synchronized tension and temperature control to improve heat resistance and adhesion, and a coating system with multiple coating devices to simplify the process.

Benefits of technology

The process enhances heat resistance, moisture content, porosity, and uniformity of the separator, improving battery safety and cycle performance while reducing production costs and increasing the pass rate, thus enhancing lithium ion battery performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595754000002
    Figure 0007595754000002
  • Figure 0007595754000003
    Figure 0007595754000003
  • Figure 0007595754000004
    Figure 0007595754000004
Patent Text Reader

Abstract

The present invention relates to the field of lithium battery separators, and aims to provide a battery separator, a coating process thereof, a coating system, and a battery. [Solution] The coating process includes initial heat setting of the polyolefin film, online coating of the polyolefin film, and heat setting of the coated film. The coating system includes multi-stage ovens installed along the path of heat setting of the polyolefin film, with coating devices installed at intervals between adjacent ovens for applying coating slurry to the polyolefin film. By installing the online coating flow at a stage before the end of heat setting of the polyolefin film, the temperature of the polyolefin film heat setting oven is fully utilized to dry the polyolefin base film and coating slurry, and by ensuring intimate contact between the coating layer and the polyolefin film, the heat resistance of the coated film is effectively improved and the moisture content of the coated film is reduced. Compared to conventional process flows, this process is simpler and the pass rate for splitting is significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of lithium battery separators, and in particular to battery separators and their coating process, coating system and batteries. [Background technology]

[0002] A lithium ion battery is generally composed of a positive electrode, a negative electrode, a separator, an electrolyte, and a battery housing. In the structure of a lithium ion battery, the separator is one of the important inner layer assemblies. As the lithium ion battery develops in the trend of high energy density, high capacity, and high power density, the demand for high performance separators becomes more and more urgent.

[0003] For the single-layer coated separator, the heat resistance, moisture resistance, and other properties of the separator of the battery manufactured by the conventional process need to be further improved, so as to ensure the safety of the battery. In addition, the conventional separator has a porosity of about 40%, and the thickness uniformity is poor. Due to the characteristics of the low porosity and poor flatness of the separator, the internal resistance of the separator increases, and as a result, the performance of the battery such as cycle and high rate discharge is seriously affected. In addition, due to the complexity of the conventional process and the characteristics of the separator itself such as poor flatness, the final split pass rate is low, and the cost is greatly increased.

[0004] Combining a ceramic coating layer with an adhesive polymer coating film can increase the heat shrinkage resistance of the separator and improve the liquid absorption and retention capabilities of the separator, thereby improving the cycle performance of the battery to a certain extent and improving the safety of the battery. However, each coating layer of such a composite coating product needs to go through the steps of painting, drying, winding, and unwinding, which lengthens the production line, increases the processing cost, and reduces the pass rate of the product due to the complicated process. In addition, a coated separator in which two types of coating layers are combined generally does not achieve the desired performance in terms of heat resistance, moisture, porosity, adhesive ability, and uniformity. On the other hand, when the heat resistance and adhesive performance are improved by increasing the coating amount of the composite coating layer in the conventional technology, the internal resistance of the separator always increases too much, and safety performance and electrochemical performance cannot be achieved at the same time. Summary of the Invention [Problem to be solved by the invention]

[0005] SUMMARY OF THE PRESENT EMBODIMENT The present invention aims to overcome the deficiencies of the prior art and provide a coated battery separator having high adhesion and high heat resistance. [Means for solving the problem]

[0006] In order to achieve the above object, the technical solution of the present invention is as follows:

[0007] A battery separator coating process, comprising the steps of initial heat setting of a polyolefin film, online coating of a polyolefin film, and heat setting of the coated film.

[0008] There is also provided a battery separator coating system, which includes multiple ovens arranged in a path of progress for thermal fixing of a polyolefin film, and a coating device for coating the polyolefin film with a coating slurry is provided at an interval between adjacent ovens.

[0009] There is further provided a coated battery separator comprising a polyolefin substrate, a heat-resistant coating on at least one side of the polyolefin substrate, and a spray coating on at least one side of the polyolefin substrate or on the heat-resistant coating. Effect of the Invention

[0010] The present invention has the following beneficial effects over the prior art: For the separator of a coated battery, multiple coating processes are alternately inserted during the heat fixing of the polyolefin substrate, so that the coating layer and the polyolefin base film and the multi-layer composite coating layer are in close contact with each other, so that the heat resistance performance of the coated battery separator is effectively improved and the separator powder falling phenomenon caused by the traditional spraying is avoided. The composite coated battery separator made by the online coating method has significantly improved heat resistance, moisture, porosity and uniformity compared with the traditional coating method, and finally, the safety, cycle performance, high-rate discharge performance and other electrochemical performance of the battery are effectively improved, the process flow is more simplified than the traditional process flow, and the split pass rate is also significantly improved.

[0011] In addition, in the online coating process of the separator of the composite coated battery, multiple types of coating layers can be coated online at one time, which significantly simplifies the process flow, reduces production costs, simplifies the process, reduces unstable factors in separator production, and effectively improves the production pass rate of the separator. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a flow chart of a coating process according to the first embodiment of the present invention.

[0013] [Diagram 2] FIG. 2 is a schematic diagram of a coating system according to the first embodiment of the present invention.

[0014] [Diagram 3] FIG. 3 is a structural schematic diagram of a separator of a composite coated battery according to Example 2 of the present invention.

[0015] [Figure 4] FIG. 4 is a flow chart of the coating process of the composite coating layer according to the second embodiment of the present invention.

[0016] [Diagram 5] FIG. 5 is a schematic diagram of a composite coating application system according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the preferred embodiment of the present invention will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terms used in the specification and the accompanying claims should not be interpreted limited to their general dictionary meanings, but should be interpreted based on the principle of appropriately limiting terms as best interpreted by the inventor, and the meaning and concept corresponding to the technology of the present invention. Therefore, the description provided herein is merely a preferred example for the purpose of illustrating the invention, and does not limit the scope of the present invention, and therefore it should be understood that other equivalents and modifications can be made without departing from the spirit and scope of the present invention.

[0018] The coating process for the separator of the battery according to the present invention comprises, in order, initial heat setting of the polyolefin film, on-line coating of the polyolefin film, and heat setting of the coated film.

[0019] In the present invention, a coating process step is placed in the process of heat fixing to the polyolefin film, Easy to control tension and temperature in online coating and heat fixing to synchronize; Avoid the accumulation and uneven distribution of internal stress in the base film caused by multiple processing, thereby optimizing the flatness of the product coating film; The subsequent coating film split pass rate can be guaranteed to be ≥ 90%. In addition, the polyolefin substrate can eliminate the internal stress of the substrate film after one heat setting, and during the drying process after coating, another high temperature is applied to further eliminate the internal stress caused by tension during the coating process and the mismatch between the substrate and the coating layer, thus achieving two-stage fixing, which can adjust the drying and heat setting mutually and improve the thickness, porosity and conformity of the coating film produced.

[0020] It also helps to achieve good alignment between the coating layer and the polyolefin film, and the permeability between the polyolefin film and the coating layer is greatly increased, so that the air permeability value of the separator is reduced; the smaller the air permeability value, the correspondingly smaller the internal resistance of the separator, making the transmission of lithium ions easier, which is beneficial to the cycle and high-rate charge / discharge performance of the lithium battery.

[0021] In order to improve the heat shrinkage performance of the coated film prepared by the above process, it is more preferable to control the shrinkage of the coated film after online coating of the polyolefin film, i.e., simultaneously with online coating of the polyolefin film, control the synchronous shrinkage of the coating slurry in a liquid state, thereby making the contact between the coating slurry and the surface of the base film closer, and effectively improving the heat shrinkage performance of the coated film.

[0022] Specifically, the polyolefin film can shrink 0.1-10% in the MD direction while the coating slurry is in a liquid state, which results in closer contact between the coating slurry and the surface of the polyolefin film, and significantly improves the peel strength after coating. Good peel strength can withstand the tendency of the coating film to shrink at high temperatures and improve the heat resistance of the coating film, and a small thermal shrinkage rate can significantly reduce the risk of explosion due to the contraction of the coating film caused by abnormal operation at high temperatures or the contact short circuit between the positive and negative electrodes of the lithium ion battery.

[0023] The polyolefin film is not limited to a specific type, and may be any type that is common in the art, including but not limited to at least one copolymer or mixture of polyethylene, polypropylene, polybutene, polypentene, polyhexene, and polyoctene. When the polyolefin film is ultra-high molecular weight PE, the molecular weight of the ultra-high molecular weight PE is preferably between 300,000 and 2,000,000. Preferably, the film-forming process of the polyolefin substrate is a wet process, and the appropriate amount of volatilization of the solvent extracted from the substrate promotes the formation of through-holes in the coating and base film, avoids the occurrence of the pore clogging phenomenon, reduces the breathability of the coating film, and is conducive to the transmission of lithium ions.

[0024] After the material of the polyolefin film is determined, the initial heat setting temperature of the polyolefin film in the corresponding coating process and the heat setting temperature of the coated film are also limited. The initial heat setting temperature of the polyolefin film is limited to the melting point of the corresponding polyolefin film material. During the heat setting of the coated film after coating, most of the moisture in the coated film can be removed, which helps to obtain a low-moisture separator during subsequent drying. The upper limit of the heat setting temperature of the coated film is limited to the temperature that increases the melting point of the polyolefin film material by 10°C. That is, when the polyolefin film is an ultra-high molecular weight PE with a molecular weight of 300,000 to 2 million, the initial heat setting temperature of the polyolefin film is controlled to 70°C to 120°C, and the heat setting temperature of the coated film is controlled to 70°C to 130°C.

[0025] The coating film layer is not limited to a particular type, and may be any type that is conventional in the art, including, but not limited to, a ceramic coating, a PVDF coating, a polyacrylic acid-based coating, and a composite of any one or more of an aramid coating.

[0026] In addition, the coating method for the online coating of the polyolefin film of each coating layer is not limited, and it is sufficient that the slurry is coated on the polyolefin film, and may be any one or a combination of a plurality of methods such as spraying, knife coating, gravure coating (intaglio coating), wire rod coating (line coating), slit coating, extrusion coating, and dip coating.

[0027] When the coating layer of the coating film is a multi-layer composite coating layer, the coating is performed after the polyolefin substrate in the present invention is slightly dried and fixed at the beginning, compared with the conventional coating process, so that the coating slurry can better wet the substrate, and the composite coating layer contacts when it is not completely dried, and the slurries at the interface have enough time to penetrate each other, and after synchronous drying, the bonding strength at the interface is much greater than that of the conventional coating process. The better the interface bonding of the ceramic coating layer with heat resistance with the base film, the greater the peel strength of the coating, and the more obvious the improvement of the heat resistance performance to the substrate. The spray coating layer is discontinuous, so it is easy to fall off with irregular distribution, and when the coating layer peels off and collects on the roller, a lot of granules are generated on the surface of the film, which results in a lower pass rate. The online coating technology effectively avoids this phenomenon because the coating is tightly bonded between the coatings.

[0028] In the present invention, the polyolefin substrate and the composite coating are dried synchronously, and since the polyolefin substrate is a completely heat-set type, the internal stress remaining in the extraction cooling during the stretch extraction is released, so the separator shrinks to a certain extent, and this process occurs synchronously with the volume change caused by the drying of the composite coating, effectively avoiding the curling phenomenon that is likely to occur in separators coated on one side. In addition, since the slurry and the substrate shrink synchronously, the coating is folded more densely and the contact between the coating and the base film is tighter, so that the heat shrink performance of the coating film is effectively improved.

[0029] In the present invention, after the heat setting of the coated film, the steps of online winding, online division, unwinding and drying are successively carried out to obtain the finished coated film, so that the suitable and wide finished film can be obtained by only one division by online division, and the waste of raw materials caused by multiple divisions in the conventional process can be avoided. The online winding tension can be controlled at 10-20N, the winding speed at 40m / min, the online division tension at 3-5N, and the division speed at 70-90m / min.

[0030] In contrast, the coating process corresponds to a coating system for a battery separator, which includes a multi-stage oven provided in the path of progress of the thermal fixation of the polyolefin film, and a coating device for applying a coating slurry to the polyolefin film is provided at the interval between adjacent ovens.

[0031] Specifically, one group or multiple groups installed in series are provided along the progression path of the heat setting of the polyolefin film, and each group includes a coating device, an initial heat setting oven located upstream of the coating device for initially drying the uncoated polyolefin film, and a coating heat setting oven located downstream of the coating device for drying the coated coated film.

[0032] Alternatively, a plurality of coating devices are provided in series at intervals between adjacent ovens, and the coating methods of the coating devices include gravure coating, wire rod coating or extrusion coating, high-pressure atomization spraying such as high-speed centrifugal dispersion.

[0033] The coating device is equipped with a variety of conventional devices selectable in this field, such as a coating head, a wire rod, etc., and the coating speed of the coating device is controlled at 30-90 m / min. When the thickness of the coating layer needs to be changed, the coating speed can be adjusted accordingly.

[0034] In order to improve the heat shrinkage performance of the coated film produced by the above system, a shrinkage control device for controlling the shrinkage of the coated film may be provided downstream of the coating device in the group along the progress path of the heat setting of the polyolefin film, and the device can shrink the polyolefin film after the slurry is applied to the polyolefin film by the coating device and when the slurry is in a liquid state, preferably, the device for controlling the shrinkage of the coated film can shrink the slurry in the liquid state in the MD direction by 0.1 to 10%, and the coated slurry shrinks together with the polyolefin film and is heated and dried in the subsequent coated heat setting oven, thereby achieving synchronous heat setting.

[0035] The peel strength after coating is greatly improved. Good peel strength makes it possible to withstand the tendency of the coating film to shrink at high temperatures and improve the heat resistance of the coating film. A small thermal shrinkage rate can greatly reduce the risk of explosion due to shrinkage of the coating film caused by abnormal operation of lithium-ion batteries at high temperatures or short circuit of the positive and negative electrodes.

[0036] For example, between the coating device and the initial heat-setting oven and between the coating heat-setting oven and the coating heat-setting oven, suction wheels are respectively provided, which are pressed against the surface of the polyolefin film. The main function of the two suction rollers is to control the tension change of the polyolefin film during the coating process, thereby ensuring the stability of the coating.

[0037] A relay tank for relaying the coating slurry and a filter may be further arranged near the coating device, and during the preparation of the slurry before coating the polyolefin film with the coating device, the coating slurry enters the 40μ magnetic filter through the relay tank, and the 40μ magnetic filter filters foreign matter such as large granules and metal impurities in the coating slurry, thereby effectively preventing the short circuit phenomenon of the battery core circulation caused by the metal foreign matter present in the separator, and improving the cycle stability. In addition, in order to avoid a decrease in the separator production rate due to frequent stoppage and cleaning of the magnetic filter, a 40μ filter is simultaneously installed at the relay tank, which avoids the occurrence of multiple filter stoppages and cleaning, thereby improving the separator production rate.

[0038] An online thickness gauge and a defect meter may further be arranged next to the coating device, the thickness gauge mainly monitors the thickness of the base film and the coating film in real time, and the defect meter can detect abnormalities in the separator, so as to improve the quality of the finished coating film.

[0039] At the end of the multi-stage oven, an online winding device, an online dividing device, and then an unwinding / drying device may be provided.

[0040] Depending on the above coating process and coating device, a separator for a composite coated battery can be produced, which comprises a polyolefin substrate 13, a heat-resistant coating layer 14 on at least one side of the polyolefin substrate 13, and a spray coating layer 15 on at least one side of the polyolefin substrate 13 or on the heat-resistant coating layer 14.

[0041] That is, the separator of the composite coated battery may be Structure 1: heat-resistant coating 14-polyolefin substrate 13-sprayed coating 15, Structure 2 shown in FIG. 3: sprayed coating 15-heat-resistant coating 14-polyolefin substrate 13-heat-resistant coating 14-sprayed coating 15, or other combinations.

[0042] Based on the above coating process and coating equipment, in the online multi-layer composite coating process, drying and heat fixing is simultaneously performed on the composite coating layer when it is not dried or slightly dried. In order to avoid the multi-layer coating paints from excessively penetrating and fusing with each other during coating or drying and heat fixing, which may affect the physical properties of the separator of the composite coating layer, the present invention emphasizes that the particle diameter D1 of the heat-resistant coating layer 14 is smaller than the particle diameter D2 of the spray coating layer 15, and D1:D2<2 is satisfied.

[0043] Specifically, the heat-resistant coating layer 14 is a ceramic coating layer, and the ceramic coating layer includes inorganic granules having thermal inertness or lithium ion transmission, and the spray coating layer 15 includes polymer granules with adhesive function.

[0044] However, the ceramic coating includes water, a thickener, inorganic granules, an adhesive, and a wetting agent, the solid content of the slurry of the ceramic coating ranges from 30% to 40%, and the inorganic granules may be one or a combination of SrTiO3, SnO2, Mg(OH)2, MgO, Al(OH)3, Al2O3, SiO2, BaSO4, or TiO2.

[0045] The spray coating 15 includes high molecular weight polymer granules with adhesive function, dispersants, thickeners, adhesives, wetting agents, and defoamers, and the solid content of the slurry of the spray coating is between 5% and 80%.

[0046] The polymer granules are made of one or more of PVDF and its copolymers, and acrylate homopolymers or copolymers.

[0047] If the application of the ceramic coating layer and the spray coating layer 15 is performed online synchronously, the spray slurry and the ceramic slurry are fused together, and many polymeric polymer granules with adhesive function penetrate into the ceramic granules during drying, it may affect the adhesive performance of the separator of the composite coated battery. Therefore, more preferably, the particle size of the inorganic granules in the ceramic coating layer is 0.01 μm to 10 μm, preferably 0.02 μm to 2 μm, and the particle size of the polymeric polymer granules in the spray coating layer 15 is 0.5 μm to 10 μm, preferably 1 μm to 5 μm. By controlling the particle size of the inorganic granules and the particle size of the polymeric polymer granules, and using the particle size of the polymeric polymer granules with large granules, the particle size of the polymeric polymer granules can be effectively avoided from being completely embedded in the ceramic coating layer during application, which ensures that sufficient adhesive force is generated between the separator and the pole piece of the composite coated battery after the hot pressing process of the battery core. The present invention ensures that, with the same coating amount of the spray coating, the adhesive performance of the separator of the composite coated battery can be improved as much as possible, and the amount of polymer used can be reduced when the required adhesive strength is reached, so that the ionic resistance of the separator can be effectively reduced, and the cycle and rate performance of the battery can be effectively improved.

[0048] The coating method for coating the ceramic coating slurry on at least one surface of the polyolefin base film includes, for example, one of gravure coating, wire rod coating, extrusion coating, etc. The spray coating method for spraying the ceramic coating on at least one surface of the polyolefin base film includes high-pressure atomization spray methods such as high-speed centrifugal dispersion.

[0049] A battery, comprising the separator of the composite coated battery according to any one of the above solutions.

[0050] The present invention will be described in detail below with reference to examples to aid in understanding. However, it should be understood that the present invention may have multiple other forms and that the scope of the present invention is not limited to the following embodiments. The embodiments of the present invention are provided for those skilled in the art to which the present invention pertains to fully understand the present invention.

[0051] Example 1

[0052] The polyolefin film is a 2 million molecular weight ultra-high molecular weight PE-based film, the coating layer is a ceramic coating layer, and the ceramic coating layer is coated on one surface of the PE-based film. The ceramic slurry includes water, a thickener, ceramic granules, an adhesive, and a wetting agent, and has a solid content of 32%.

[0053] As shown in FIG. 1, the main process flow of this example is as follows: initial heat setting of polyolefin film--preparation of ceramic slurry--online coating of ceramic slurry--heat setting of coated film--shrinkage control--online winding--online division--unwinding and drying.

[0054] As shown in FIG. 2 , the coating apparatus of this embodiment includes a defect meter 1, a thickness meter 2, an initial heat setting oven 3, a suction roller 4, a filter 5, a relay tank 6, a coating device 7, a shrinkage control device 8, a coating heat setting oven 9, an online winding device 10, an online dividing device 11, and an unwinding / drying device 12.

[0055] As shown in Figure 2, the PE film is made through the steps of material compounding, extrusion, filtration and weighing, die head extrusion, casting cooling and forming, biaxial stretching, and extraction and drying, which correspond to the steps before heat setting in the conventional wet separator process. The PE film travels in the direction shown in Figure 2, first through the defect meter 1 and thickness meter 2 for real-time quality monitoring, then enters the initial heat setting oven 3 to achieve initial heat setting. At this time, the PE film is not completely heat set, and the ceramic slurry placed in the filter 5 and relay tank 6 is applied to the PE film by the coating device 7, while the suction rollers 4 installed upstream and downstream of the coating device 7 control the change in tension during coating. When the ceramic slurry is in a liquid state, the shrinkage control device 8 causes shrinkage in the MD direction, making the contact between the coating slurry and the base film surface closer. After the shrinkage control is completed, the PE film coated with the ceramic slurry enters the coating heat setting oven 9 to complete the heat setting of the coating film, then passes through the online winding device 10, the online dividing device 11, and the unwinding and drying device 12 to obtain the finished ceramic coated film.

[0056] However, the dew point Td of the dry environment is -49°C, the humidity H is 0.31%, the moisture test of the coating film is 180°C / 5min, and the moisture is ≦800ppm. The present invention obtains a coating film with low moisture content by controlling the dry environment, reduces side reactions inside the battery, and effectively improves the battery performance.

[0057] When the ceramic coating layer is peeled off at a speed of 50 m / min, the peel strength is greater than 80 N / M. The greater peel strength is conducive to the adhesion between the coating layer and the base film and better resists the thermal shrinkage of the separator at high temperatures, thereby effectively improving the safety of the separator.

[0058] Example 2

[0059] This embodiment is a separator for a composite coated battery. As shown in FIG. 3, the separator for the composite coated battery includes a polyolefin substrate 13, a heat-resistant coating layer 14 applied to both surfaces of the polyolefin substrate 13, and a spray coating layer 15 sprayed on the heat-resistant coating layer 14, and the heat-resistant coating layer 14 is a ceramic coating layer.

[0060] As shown in FIG. 4, the main process flow of this embodiment is as follows: initial heat setting of polyolefin film--preparation of ceramic slurry--online coating of ceramic slurry--online spray coating--heat setting of coated film--shrinkage control--online winding--online division--unwinding and drying.

[0061] When the polyolefin film is not completely heat set, the ceramic coating is applied, and when the ceramic coating is not completely dried, the ceramic coating is spray applied.

[0062] However, the ceramic coating slurry has a solid content of 38.6%, and its specific components are 61.4% water, 0.5% sodium carboxymethylcellulose thickener, 0.1% polyether wetting agent, 35% aluminum oxide, and 3% acrylate adhesive. The slurry is prepared by dispersing and dissolving the thickener in water to obtain solution A, dispersing and grinding aluminum oxide in water to obtain dispersion B, mixing solution A and dispersion B, adding adhesive and wetting agent slurry, and thoroughly mixing to obtain ceramic slurry, and the average particle size of aluminum oxide in the finished slurry is 0.8 μm.

[0063] A spray coating slurry with a solid content of 10% is prepared, the specific components of which are 85% water, 13.5% PMMA granules, 1.3% acrylate adhesive, and 0.2% polyether dispersant. The PMMA emulsion containing adhesive and dispersant is dispersed in water to obtain a finished slurry, where the average particle size of PMMA in the slurry is 3 μm.

[0064] As shown in FIG. 5 , the coating apparatus of this embodiment includes a defect meter 1, a thickness meter 2, an initial heat setting oven 3, an adsorption roller 4, a filter 5, a relay tank 6, a coating device 7, a spray device 16, a shrinkage control device 8, a coating heat setting oven 9, an online winding device 10, an online dividing device 11, and an unwinding / drying device 12.

[0065] As shown in Figure 5, a 9μm PE separator is designed, and double-sided ceramic coating is performed online by a gravure roller. Double-sided spraying is performed by a high-speed centrifugal dispersion plate immediately after the ceramic coating head. However, the temperature of the pre-heat setting oven before coating is 80°C, and the coating heat setting oven 9 after coating is a three-stage oven with temperatures of 60°C / 80°C / 100°C respectively. The production line speed is 50m / min. The total thickness of the double-sided ceramic after drying is 4μm, and the loading amount of the double-sided spray coating layer is 0.8g / m 2 Let us assume that.

[0066] Comparative Example 1

[0067] The other steps are the same as those in Example 1, except that the average particle size of aluminum oxide in the ceramic coating slurry is 0.8 μm, and the average particle size of PMMA in the spray coating slurry is 0.3 μm.

[0068] A 9um PE separator is prepared, and a ceramic layer is applied on both sides by a gravure roller, the coating speed is 50m / min, and it is dried in a three-stage oven, with the oven temperatures being 60℃ / 65℃ / 70℃ respectively. The thickness of the completely dried separator is 13μm, and the thickness of the ceramic layer is 4μm. Then, the double-sided ceramic-coated film is sprayed on both sides by a high-speed centrifugal dispersion plate, and the loading amount of the double-sided spray coating is 0.8g / m2.

[0069] The characteristics tests were carried out for Example 2 and Comparative Example 1, and the data are shown in Table 1.

[0070] Table 1 JPEG0007595754000001.jpg33170

[0071] As can be seen from Table 1, the present invention and the comparative examples are coated with the same aluminum oxide slurry, and when the coating amount is the same, the examples have better heat shrinkage performance. When the coating amount of the spray coating is the same, the examples coated with larger granules online have better adhesion strength. Overall, the composite coating layer prepared by online coating has a smaller increase in air permeability, a smaller resistance value of the entire separator, and better heat resistance. As can be seen from this, the lithium ion battery prepared with the separator of the composite coating layer of the present invention is superior to the composite separator of the conventional lithium battery in many aspects such as safety, cycle rate, and other battery performance, and the integrated production by the process of the present invention has simple production steps and lower costs.

[0072] The above is only a preferred embodiment of the present invention, and those skilled in the art may further make some improvements and modifications without departing from the concept of the present invention, and these improvements and modifications should also be considered as within the protection scope of the present invention.

Claims

1. A method for coating a separator for a battery, comprising the steps of: an initial heat setting of the polyolefin film; performing an online coating on a polyolefin film; Simultaneously with the online coating of the polyolefin film, controlling the coating film to shrink by 0.1 to 10% in the MD direction while the coating slurry is in a liquid state; and a step of heat fixing the coated film.

1. A method for coating a battery separator, comprising:

2. In the initial heat setting process of the polyolefin film, the temperature is controlled at 70°C to 120°C. In the process of heat fixing the coated film, the temperature is controlled to 70°C to 130°C.

2. The method for coating a separator for a battery according to claim 1,

3. The coating layer of the coating film is a composite of one or more of a ceramic coating layer, a PVDF coating layer, a polyacrylic acid coating layer, and an aramid coating layer; 2. The method for coating a separator for a battery according to claim 1,

4. The coating method for online coating on the polyolefin film is any one or a combination of spray, knife coating, gravure coating, wire rod coating, slit coating, extrusion coating and dip coating; 2. The method for coating a separator for a battery according to claim 1,

5. A battery separator coating system, comprising: The path for heat fixing the polyolefin film is equipped with multiple ovens. Between the adjacent ovens, a coating device is provided for coating the polyolefin film with a coating slurry; A shrinkage control device is provided between the coating device and the oven to control shrinkage of the coating film. A battery separator coating system comprising:

Citation Information

Patent Citations

  • Preparation method for battery diaphragm containing coating layer and on-line coating system

    CN105702899A

  • Compression roller device of winding mechanism of coating machine

    CN105903648A

  • Novel lithium battery diaphragm spraying and coating production equipment

    CN111180640A

  • Separator for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and battery pack

    JP2008146963A

  • Manufacturing method of polyolefin-based multilayer composite porous film