Ultra-water-repellent surface structure and method for manufacturing a mold

A surface structure mimicking proboscis termite wings using needle-shaped diarylethene crystals efficiently collects microdroplets by adsorbing small droplets and repelling larger ones, addressing the challenges of replicating the termite wing surface structure and improving fog collection efficiency.

JP7595980B2Active Publication Date: 2024-12-09RYUKOKU UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023178233
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2024-12-09
Estimated Expiration
2040-03-30

AI Technical Summary

Technical Problem

Existing technologies struggle to efficiently collect microdroplets from fog due to the difficulty in replicating the fine surface structure of proboscis termite wings, which are several millimeters in size, and the high cost and complexity of photolithography methods.

Method used

A surface structure is developed that mimics the proboscis termite wing surface by forming two types of needle-shaped crystals of diarylethene derivatives with different sizes, controlled by light irradiation, and a mold is created using electroforming to replicate this structure, allowing for efficient microdroplet collection.

Benefits of technology

The surface structure effectively adsorbs small droplets while repelling larger ones, enabling efficient collection of microdroplets, such as mist droplets, by imitating the proboscis termite wing surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595980000019
    Figure 0007595980000019
  • Figure 0007595980000020
    Figure 0007595980000020
  • Figure 0007595980000001
    Figure 0007595980000001
Patent Text Reader

Abstract

To imitate the surface structure of a wing of termites of Nasutitermitinae and provide a surface structure that can efficiently recover fine droplets.SOLUTION: A surface structure has, on a base material, a first acicular structure with a length of 1.5-30 μm and a diameter of 1-6 μm and a second acicular structure with a length of 1-5 μm and a diameter of 0.05-1 μm, the first acicular structure and second acicular structure being composed of metal or resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface structure and a method for recovering droplets using the same. [Background technology]

[0002] As a result of global warming, arid regions are expanding, and solutions to water shortages are being sought. While groundwater sources are limited in arid regions, fog sometimes forms in the air, and if fog could be efficiently collected, it could become a valuable water source. Fog droplets are small in weight and therefore easily adhere to material surfaces, but because they have a large surface area relative to their volume, they tend to evaporate quickly, making collection difficult.

[0003] Nastotermes, native to Australia, fly in the rainy season to build nests. The surface of the wings of these termites has the function of attaching mist particles, turning them into large water droplets, and then expelling them from the surface (Non-Patent Document 1). If this surface structure could be imitated to efficiently collect mist particles and convert them into droplets, it would be an effective measure to combat water shortages in arid regions. However, the wings of Nastotermes are only a few millimeters in size, and it is difficult to faithfully reproduce the microstructure of their surface using a 3D printer or other device. Such a microstructure can be reproduced using photolithography, which is used in the manufacture of semiconductor integrated circuits, but photolithography requires large-scale equipment and many steps, and a technology for more easily manufacturing microstructures is needed.

[0004] On the other hand, diarylethene derivatives 1o and 2o [ka] [ka] When the microcrystalline film of 1c was irradiated with ultraviolet light, the closed ring forms 1c and 2c were formed on the surface of the microcrystalline film. [ka] [ka] It was known to grow as needle-like crystals.

[0005] In addition, a surface having needle-like crystals of diarylethene derivative 1c repels stationary water droplets but adsorbs falling water droplets, and has low adsorption power for mist particles (Non-Patent Document 2). On the other hand, a surface having needle-like crystals of diarylethene derivative 2c has the property of repelling both large water droplets and small mist particles (Patent Document 1). However, a method for using the structure of these needle-like crystals to collect mist particles was not known. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-34583 A [Non-patent literature]

[0007] [Non-Patent Document 1] ACS Nano 2010,4,1,129-136 [Non-Patent Document 2] Angew.Chem.Int.Ed.2006,45,6470-6473 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a surface structure that mimics the surface structure of the wings of Nasturtium termites and is capable of efficiently collecting microdroplets. [Means for solving the problem]

[0009] The present inventors have found that a surface structure that mimics the surface structure of the wing of Nasturtium termites can be formed by growing needle-like crystals of two diarylethene derivatives with different sizes that can be controlled by irradiation with light on the surface of a material. Furthermore, they have found that a template onto which the surface structure is transferred can be created by electroforming, and that a surface structure that mimics the surface structure of the wing of Nasturtium termites can be manufactured by using this template, thus completing the present invention.

[0010] That is, the present invention relates to a surface structure having, on a substrate, first needle-like structures having a length of 1.5 to 30 μm and a diameter of 1 to 6 μm, and second needle-like structures having a length of 1 to 5 μm and a diameter of 0.05 to 1 μm, the first needle-like structures and second needle-like structures made of metal or resin.

[0011] The present invention also relates to a method for recovering microdroplets, comprising a first step of adsorbing microdroplets onto the surface structure, and a second step of recovering the adsorbed microdroplets.

[0012] The present invention also provides a method for producing a polymerizable compound having the following structural formula (3c): [ka] Needle crystals of a closed-ring diarylethene compound represented by the formula: The following structural formula (4c): [ka] The present invention relates to an ultrawater-repellent surface structure having needle-shaped crystals of a diarylethene ring-closed product represented by the following formula: (In structural formulas (3c) and (4c), R A , and R B each independently represents a methyl group, an ethyl group, a propyl group, an isopropyl group, a methoxy group, an ethoxy group, or a cyano group; R E , and R F each independently represents a methyl group, an ethyl group, a propyl group, or an isopropyl group; R C , R D , RG , and R H each independently represents a trimethylsilyl group, a t-butyl group, a neopentyl group, or an isopropyl group; R1 to R8 each independently represent a hydrogen atom, an optionally substituted chain or cyclic alkyl group, or a halogen atom.

[0013] A diarylethene ring-closed product represented by structural formula (3c) is represented by the following structural formula (1c): [ka] A compound represented by the formula: The diarylethene ring-closed product represented by structural formula (4c) is represented by the following structural formula (2c): [ka] It is preferable that the compound is represented by the following formula:

[0014] It is preferred that the length of the needle-like crystals of the diarylethene closed-ring product represented by structural formula (3c) is at least 8 times the length of the needle-like crystals of the diarylethene closed-ring product represented by structural formula (4c), and that the diameter of the needle-like crystals of the diarylethene closed-ring product represented by structural formula (3c) is at least 7 times the diameter of the needle-like crystals of the diarylethene closed-ring product represented by structural formula (4c).

[0015] It is preferable that a layer containing needle-like crystals of a diarylethene closed-ring product represented by structural formula (3c) and needle-like crystals of a diarylethene closed-ring product represented by structural formula (4c) is formed on the surface of a substrate to a thickness within a range of 1 to 10 μm.

[0016] The present invention also relates to a method for producing a mold, comprising the steps of: (a) forming a metal film on the surface of the ultrawater-repellent surface structure; (b) performing electroplating on the metal film; and (c) peeling off the metal film from the electroplating. Effect of the Invention

[0017] The surface structure of the present invention exhibits super-water repellency due to the presence of first and second needle-like structures of different sizes. When microdroplets are dropped onto this surface structure, the small droplets adhere to the surface, but the large droplets are repelled and move away. By adsorbing microdroplets in the air to the surface structure, the microdroplets present in the gas can be efficiently collected. [Brief description of the drawings]

[0018] [Figure 1] The SEM image and schematic diagram of the surface structure are shown. [Diagram 2] The adhesion of a water droplet to a surface structure is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] <<Surface structure>> The surface structure of the present invention is characterized in that it has, on a substrate, first needle-like structures having a length of 1.5 to 30 μm and a diameter of 1 to 6 μm, and second needle-like structures having a length of 1 to 5 μm and a diameter of 0.05 to 1 μm, and the first needle-like structures and second needle-like structures are made of metal or resin.

[0020] The length of the first needle-like structure is 1.5 to 30 μm, preferably 10 to 30 μm, and more preferably 15 to 20 μm. The diameter of the first needle-like structure is 1 to 6 μm, preferably 1 to 3 μm, more preferably 1 to 2 μm, and even more preferably 1.5 to 2 μm. The length of the second needle-like structure is 1 to 5 μm, preferably 1.5 to 2 μm, and more preferably 1.8 to 2 μm. The diameter of the second needle-like structure is 0.05 to 1 μm, preferably 0.1 to 0.5 μm, more preferably 0.1 to 0.3 μm, and even more preferably 0.1 to 0.2 μm. In a surface structure in which the sizes of the first and second needle-like structures are within the above ranges, small droplets adhere to the surface, but large droplets are repelled and moved.

[0021] The length of the needle crystals of the first needle structure is preferably 8 times or more, more preferably 9 times or more, the length of the needle crystals of the second needle structure. The diameter of the first needle structure is preferably 7 times or more, more preferably 8 times or more, the diameter of the second needle structure. Since the first needle structure is preferably longer than the second needle structure, it is preferable that a layer consisting of two needle structures is formed on the surface of the substrate with a thickness of 1.5 to 20 μm.

[0022] The first needle-like structure and the second needle-like structure each preferably have an inclination of 60° to 90° with respect to the substrate.

[0023] The density of the first needle-like structures on the substrate is 1 mm 2 The density of the second needle-like structures is preferably 50,000 to 80,000 per mm, more preferably 60,000 to 70,000 per mm, and even more preferably 65,000 to 70,000 per mm. 2 Preferably, the number of fibers per unit area is 600,000 to 900,000, and more preferably 700,000 to 800,000.

[0024] The surface structure of the present invention mimics the surface structure of the wing of the Nasturtium termite, but since the two needle-like structures are made of metal or resin, they can be produced inexpensively by using a mold described below. Examples of metals include nickel. Examples of resins include polystyrene, polydimethylsiloxane, polymethyl methacrylate (PMMA), poly(n-butyl methacrylate), poly(methyl acrylate), polyolefin, and cycloolefin polymer (Zeonex polymer). Among these, polystyrene and polydimethylsiloxane are particularly preferred. The constituent materials of the two needle-like structures do not need to be the same, but it is preferable that they are the same from the viewpoint of manufacturing costs.

[0025] The contact angle of a water droplet with respect to the surface of the superhydrophobic surface structure of the present invention is preferably 90° or more, and more preferably 100° or more. In general, a surface with a contact angle of a water droplet dropped thereon that is less than 90° is considered hydrophilic, whereas a surface with a contact angle of 90° or more is considered water repellent. Furthermore, a surface with a contact angle of more than 150° is said to be superhydrophobic. A typical example of such a surface having superhydrophobicity is the surface of a lotus leaf, and thus the superhydrophobicity is sometimes called the "lotus effect."

[0026] The material of the substrate supporting the first and second needle-like structures is not particularly limited, and examples thereof include metal, resin, glass, etc. From the viewpoint of manufacturing costs, it is preferable that the substrate is made of the same material as the first and / or second needle-like structures. When the surface structure of the present invention is used for collecting fog particles as described below, the surface structure of the present invention may be supported on a support such as a net or a plate.

[0027] The surface structure of the present invention may have any surface structure in addition to the first and second needle-like structures, such as a surface structure in which plate-like crystals are laid out vertically.

[0028] The method for producing the surface structure of the present invention is not particularly limited, but examples thereof include a method using a template, which will be described later.

[0029] <<How to collect microdroplets>> The method for recovering microdroplets of the present invention includes a first step of adsorbing microdroplets to the surface structure, and a second step of recovering the adsorbed microdroplets.

[0030] The surface structure mimics the surface structure of the wings of the Nasu-go-termite, and therefore has the property of adsorbing microdroplets in the same manner as the wings of the Nasu-go-termite. The size of the microdroplets adsorbed to the surface structure in the first step is preferably 1 to 200 μm, more preferably 10 to 180 μm. Microdroplets exceeding 200 μm tend to be repelled by the surface structure. Water is preferable as the microdroplets. A specific example is mist droplets. The space in which the microdroplets exist is not particularly limited as long as it contains gas and is not a vacuum, but is preferably a space in which air exists.

[0031] Methods for adsorbing microdroplets include a method of spraying a gas containing microdroplets onto the surface structure, and a method of supporting the surface structure in a space in which a gas containing microdroplets exists. For example, by placing the surface structure of the present invention in a space in which mist is generated, mist particles can be adsorbed onto the surface of the surface structure.

[0032] In the second step, the specific recovery method is not particularly limited as long as the microdroplets adsorbed in the first step can be recovered, and for example, the microdroplets can be recovered by being allowed to flow by gravity by tilting the surface structure. If the microdroplets adsorbed in the first step are too small, the microdroplets may be brought into contact with each other to form larger droplets, and then recovered.

[0033] <<Super water-repellent surface structures>> The superwater-repellent surface structure of the present invention has, on a substrate, a compound represented by the following structural formula (3c): [ka] Needle crystals of a closed-ring diarylethene compound represented by the formula: The following structural formula (4c): [ka] The compound is characterized in that it has needle-shaped crystals of a closed-ring diarylethene compound represented by the following formula:

[0034] In structural formulas (3c) and (4c), R A , and R BR each independently represents a methyl group, an ethyl group, a propyl group, an isopropyl group, a methoxy group, an ethoxy group, or a cyano group. E , and R F Each of R independently represents a methyl group, an ethyl group, a propyl group, or an isopropyl group. A , and R B are each independently preferably a methoxy group or a methyl group, and R E , and R F are each independently preferably a methyl group or an ethyl group.

[0035] R C , R D , R G , and R H each independently represents a trimethylsilyl group, a t-butyl group, a neopentyl group, or an isopropyl group, with a trimethylsilyl group being more preferred.

[0036] R1 to R8 each independently represent a hydrogen atom, an optionally substituted chain or cyclic alkyl group, or a halogen atom. The alkyl group preferably has 1 to 4 carbon atoms. Examples of the substituent of the alkyl group include a hydrogen atom, a methyl group, a trimethylsilyl group, an ethyl group, an isopropyl group, a tertiary butyl group, a methoxy group, and an ethoxy group. Examples of the halogen atom include fluorine, iodine, and chlorine. Among the above, R1 to R8 are preferably a hydrogen atom, a methyl group, a trimethylsilyl group, an ethyl group, an isopropyl group, a tertiary butyl group, and a methoxy group.

[0037] The diarylethene ring-closed product represented by structural formula (3c) is represented by the following structural formula (1c): [ka] The diarylethene ring-closed product represented by the structural formula (4c) is preferably a compound represented by the following structural formula (2c): [ka] It is preferable that the compound is represented by the following formula:

[0038] The needle-shaped crystals of the diarylethene ring-closed compound represented by structural formula (3c) were formed by coating a substrate with a compound represented by structural formula (3o): [ka] Similarly, needle-shaped crystals of a diarylethene ring-closed compound represented by structural formula (4c) can be formed by applying a compound of structural formula (4o): [ka] The needle-like crystals of (3c) and (4c) grow epitaxially regardless of the type of substrate.

[0039] (3o), (3c), (4o), and (4c) are all photoresponsive, and when the open-ring form (3o) is irradiated with ultraviolet light, it becomes the closed-ring form (3c), and when the closed-ring form (3c) is irradiated with visible light, it becomes the open-ring form (3o). Similarly, when the open-ring form (4o) is irradiated with ultraviolet light, it becomes the closed-ring form (4c), and when the closed-ring form (4c) is irradiated with visible light, it becomes the open-ring form (4o).

[0040] In the superhydrophobic surface structure of the present invention, a change in crystal structure occurs with a change in molecular structure due to light irradiation, and the change in crystal structure enables a reversible change in water repellency. The surface on which the microcrystals of the ring-opened form of structural formulas (3o) and (4o) are present on the substrate is smooth. When this surface is irradiated with ultraviolet light, the ring-opened form changes to the ring-closed form of structural formulas (3c) and (4c), needle-shaped crystals grow from the surface of the layer, and the smooth crystal face disappears. When visible light is irradiated onto the layer surface on which the needle-shaped crystals have grown, the ring-closed form changes to the ring-opened form, the needle-shaped crystals disappear, and the original smooth crystal face is restored. The wavelength of the visible light irradiated to burn off the needle-shaped crystals is not particularly limited, and may be, for example, 360 to 830 nm. Since the needle-shaped crystals of structural formulas (3c) and (4c) are generated from the microcrystals of structural formulas (3o) and (4o), it is preferable that the needle-shaped crystals are formed on the microcrystals of structural formulas (3o) and (4o) on the substrate.

[0041] More specifically, the length of the needle crystal of structural formula (3c) is preferably 1.5 to 30 μm, more preferably 10 to 30 μm, and more preferably 15 to 20 μm. The diameter of the needle crystal of structural formula (3c) is preferably 1 to 6 μm, more preferably 1 to 3 μm, even more preferably 1 to 2 μm, and even more preferably 1.5 to 2 μm. The length of the needle crystal of structural formula (4c) is preferably 1 to 5 μm, more preferably 1.5 to 2 μm, and even more preferably 1.8 to 2 μm. The diameter of the needle crystal of structural formula (4c) is preferably 0.05 to 1 μm, more preferably 0.1 to 0.5 μm, even more preferably 0.1 to 0.3 μm, and even more preferably 0.1 to 0.2 μm.

[0042] The length of the needle crystals of structural formula (3c) is preferably 8 times or more, more preferably 9 times or more, the length of the needle crystals of structural formula (4c). The diameter of the needle crystals of the diarylethene closed ring product represented by structural formula (3c) is preferably 7 times or more, more preferably 8 times or more, the diameter of the needle crystals of the diarylethene closed ring product represented by structural formula (4c). Since the needle crystals of structural formula (3c) are preferably longer than those of structural formula (4c), a layer of the needle crystals of the diarylethene closed ring product is preferably formed on the surface of the substrate with a thickness of 1 to 3 μm, more preferably 1 to 2 μm.

[0043] The contact angle of a water droplet with respect to the surface of the superwater-repellent surface structure of the present invention is preferably at least 120°, and more preferably at least 150°. Furthermore, when the superwater-repellent surface structure of the present invention is irradiated with visible light, the water repellency decreases, and the contact angle of a water droplet decreases to 110° to 120°.

[0044] The material of the substrate supporting the needle-shaped crystals is not limited as long as the needle-shaped crystals of the diarylethene ring-closed compound can be grown thereon, and examples thereof include glass, metal, and resin. Metals include nickel, iron, stainless steel, and aluminum. Resins include polystyrene, polydimethylsiloxane, polymethyl methacrylate (PMMA), polyolefin, polycarbonate, melamine resin, and epoxy resin.

[0045] The superwater-repellent surface structure of the present invention may have any surface structure in addition to the needle-like crystals of structural formulas (3c) and (4c), so long as it has the desired superwater-repellency. Such a surface structure may include a surface structure in which plate-like crystals are laid out vertically.

[0046] <<Method of manufacturing ultra-water-repellent surface structures>> The superhydrophobic surface structure can be produced by (a) applying a solution containing microcrystals of a diarylethene ring-opened product represented by structural formula (3o) and microcrystals of a diarylethene ring-opened product represented by structural formula (4o) onto a substrate, and (b) irradiating the applied surface with ultraviolet light to form needle-like crystals of a diarylethene ring-closed product represented by structural formula (3c) and needle-like crystals of a diarylethene ring-closed product represented by structural formula (4c).

[0047] Examples of the solvent for the solution used in step (a) include chloroform, dichloromethane, benzene, toluene, THF, etc. In the solution, the molar ratio (3o:4o) of the compound of structural formula (3o) to the compound of structural formula (4o) is preferably 80:120 to 120:80, more preferably 95:105 to 105:95, and most preferably an equimolar ratio. In addition, the concentrations of the microcrystals of structural formula (3o) and the microcrystals of structural formula (4o) are preferably 100 to 500 mg / mL, respectively.

[0048] In step (a), after the solution containing the microcrystals is applied, it is preferable to dry the solvent. The drying conditions are not particularly limited, and may be at room temperature under normal pressure.

[0049] The wavelength of the ultraviolet light irradiated in step (b) is preferably 254 to 313 nm. The energy of the ultraviolet light irradiated is preferably 5 to 30 W. After irradiation with ultraviolet light, the material is preferably kept at a temperature in the range of 30 to 40°C for about 24 hours to 1 week, which can promote the growth of the needle-like crystals. The needle-like crystals of structural formulae (3c) and (4c) tend to grow in size and have a reduced super-water-repellent effect when the temperature is increased, so the material is preferably kept at a temperature in the range.

[0050] <<Method for manufacturing a mold and method for manufacturing a surface structure using the mold>> When the above-mentioned surface structure is composed of needle-like crystals of a diarylethene ring-closed compound, the diarylethene ring-closed compound is converted into an open-ring compound by exposure to visible light, and the needle-like structure is lost. Therefore, when the surface structure is used in an environment exposed to visible light, it is preferable to compose the surface structure from a material such as a resin or metal that is not sensitive to visible light other than the diarylethene ring-closed compound. As a method for producing such a fine surface structure from a material such as a resin or metal, a method using a template can be mentioned.

[0051] The template can be manufactured based on the above-mentioned superhydrophobic surface structure, which is composed of needle-like crystals of a diarylethene ring-closed product. Electroforming is preferred because it can reduce the dimensional error with the master mold to about 100 mm ± 2.5 μm. In electroforming, the template can be manufactured by a method including the steps of (a) forming a metal film on the surface of the superhydrophobic surface structure, (b) electroplating the metal film, and (c) peeling off the metal film from the electroplating.

[0052] In step (a), a metal film is formed on the surface of the superwater-repellent surface structure to impart electrical conductivity. The superwater-repellent surface structure used is preferably one constituted by needle-shaped crystals of a diarylethene ring-closed body. Methods for forming the metal film include vapor deposition and sputtering. Metals constituting the film include gold, platinum, gold-palladium, etc. The thickness of the metal film is preferably 1 nm to 40 nm, more preferably 1 nm to 30 nm, and even more preferably 1 nm to 20 nm.

[0053] In step (b), electroplating is performed on the metal film formed in step (a). Examples of plating metals include zinc, chromium, nickel, etc. General conditions can be used for electroplating.

[0054] In step (c), the metal film is peeled off from the electroplating. The specific peeling method is not particularly limited as long as it can peel off the metal film without damaging the electroplating, and examples of the peeling method include triazine dithiol vapor deposition technology.

[0055] By the above method, a template is obtained in which the inverse shape of the ultrahydrophobic surface structure is transferred onto a thick plated metal film. By contacting the template with a metal, resin, or the like, the shape of the surface structure is transferred onto the metal. EXAMPLES

[0056] (Example 1) Superhydrophobic surface structure having needle-shaped crystals of structural formulas (1c) and (2c) The ring-opened structural formulae (1o) and (2o) were weighed out to an equimolar ratio (1o: 8.4 mg, 2o: 10.3 mg) and dissolved in 30 mL of chloroform. This solution was dropped onto a glass substrate cut into a 2 cm square and dried in a dark place at room temperature under normal pressure to create a mixed thin film containing microcrystals of structural formulae (1o) and (2o). The water contact angle of this thin film was 123°. This thin film was irradiated with ultraviolet light (wavelength 313 nm) for 5 minutes. It was then stored in a dark place at 30°C for 9 days to grow needle-shaped crystals, resulting in an ultrahydrophobic surface structure.

[0057] The obtained superhydrophobic surface structure was observed by SEM (scanning electron microscope). An SEM image of the surface is shown in Figure 1e, and an SEM image of the cross section is shown in Figure 1h. The needle-like crystals of structural formula (1c) had an average diameter of about 1.5 μm and a height of about 16 μm, while the needle-like crystals of structural formula (2c) had a diameter of about 0.2 μm and a height of about 1.9 μm. The density of the needle-like crystals of structural formula (1c) was about 1 mm 2 6.7 x 10 per 4 The structural formula (2c) is 1 mm 2 7.1 x 10 per 5 The contact angle of water on the obtained superhydrophobic surface structure was 164°. A schematic diagram of the obtained superhydrophobic surface structure is shown in Figure 1b.

[0058] (Comparative Example 1) Surface structure having needle-shaped crystals of structural formula (1c) A surface structure was obtained by the same procedure as in Example 1, except that only 8.4 mg of the ring-opened form of structural formula (1o) was dissolved in 30 mL of chloroform. An SEM image of the surface of the obtained surface structure is shown in Figure 1d, and an SEM image of the cross section is shown in Figure 1g. A schematic diagram of the obtained superhydrophobic surface structure is shown in Figure 1a.

[0059] (Comparative Example 2) Surface structure having needle-like crystals of structural formula (2c) A surface structure was obtained by the same procedure as in Example 1, except that only 10.3 mg of structural formula (2o), which is the ring-opened form, was dissolved in 30 mL of chloroform. An SEM image of the surface of the obtained surface structure is shown in Figure 1f, and an SEM image of the cross section is shown in Figure 1i. A schematic diagram of the obtained superhydrophobic surface structure is shown in Figure 1c.

[0060] The scale bars in Figures 1d to 1f and h indicate 5 µm, and the scale bars in Figures 1g and i indicate 10 µm.

[0061] (Measurement example) Adhesion of water droplets to each surface structure Pure water was sprayed onto the surfaces of the surface structures of Example 1 and Comparative Examples 1 and 2 using a commercially available sprayer, and the moment when the tiny water droplets collided with the surface was photographed using a high-speed camera (1000 fps). Figures 2a to 2d show the movement of the water droplets that were repelled by the surface structure over a period of 3 ms. The arrows indicate the direction of movement of the water droplets. The circles indicate the water droplets that were adsorbed onto the surface.

[0062] Figure 2 g The number of water droplets that were adsorbed on the surface of the surface structure of Example 1 and were not repelled (non-bouncing), the ... μ m) and the number of droplets that were ejected from the sprayer (Bouncing (Spr.1)) and bounced off the surface (Spr.2) 400~1000μ The figure shows the distribution of the number of water droplets (Bouncing (Spr.2)) that are ejected from the surface and bounced off the surface (generating microdroplets of 1.0 m each) and the diameter of the water droplets. e FIG. 2 shows the distribution of water droplets on the surface of the surface structure of Comparative Example 1. f 1 shows the distribution of water droplets on the surface of the surface structure of Comparative Example 2.

[0063] Figure 2 e and f As shown in FIG. 2, in the surface structures of Comparative Examples 1 and 2, the distributions of Non-bouncing and Bouncing (Spr. 1) overlapped greatly. gAs shown in Fig. 1, in the surface structure of Example 1, the overlap between the distributions of non-bouncing and bouncing (Spr. 1) was small, and water droplets with a diameter of approximately 100 µm or less tended to be adsorbed onto the surface, while larger water droplets were repelled.

Claims

1. On a substrate, a compound represented by the following structural formula (3c): [Case 1] Needle crystals of a closed-ring diarylethene compound represented by the formula: The following structural formula (4c): [Case 2] The superwater-repellent surface structure has needle-shaped crystals of a diarylethene ring-closed product represented by the formula: The length of the needle-like crystals of the diarylethene ring-closed product represented by structural formula (4c) is 1 to 5 μm; the length of the needle-like crystals of the diarylethene ring-closed product represented by structural formula (3c) is 8 times or more the length of the needle-like crystals of the diarylethene ring-closed product represented by structural formula (4c); The diameter of the needle-like crystals of the diarylethene ring-closed product represented by structural formula (4c) is 0.05 to 0.5 μm; A superhydrophobic surface structure, in which the diameter of needle-like crystals of a closed-ring diarylethene compound represented by structural formula (3c) is 7 times or more larger than the diameter of needle-like crystals of a closed-ring diarylethene compound represented by structural formula (4c). In structural formulas (3c) and (4c), R A , and R B each independently represents a methyl group, an ethyl group, a propyl group, an isopropyl group, a methoxy group, an ethoxy group, or a cyano group; R E , and R F each independently represents a methyl group, an ethyl group, a propyl group, or an isopropyl group; R C , R D , R G , and R H each independently represents a trimethylsilyl group, a t-butyl group, a neopentyl group, or an isopropyl group; R 1 ~R 8 each independently represents a hydrogen atom, an optionally substituted chain or cyclic alkyl group, or a halogen atom.

2. A diarylethene ring-closed product represented by structural formula (3c) is represented by the following structural formula (1c): [C3] A compound represented by the formula: A diarylethene ring-closed product represented by structural formula (4c) is represented by the following structural formula (2c): [C4] The compound represented by the formula: The ultra-water-repellent surface structure according to claim 1 .

3. 3. The superwater-repellent surface structure according to claim 1 or 2, characterized in that a layer containing needle-like crystals of a closed-ring diarylethene compound represented by structural formula (3c) and needle-like crystals of a closed-ring diarylethene compound represented by structural formula (4c) is formed on a surface of a substrate to a thickness of 1 to 10 μm.

4. (a) forming a metal film on the surface of the ultrawater-repellent surface structure according to any one of claims 1 to 3; (b) performing electroplating on the metal film; and (c) A step of peeling off the metal film from the electroplating A method for producing a mold, comprising:

Citation Information

Patent Citations

  • Thiophene derivative, its polymer and their production

    JP1996059651A

  • Optical memory element, and electrophotographic photoreceptor, electroluminescent element, liquid crystal display element and space light modulation element made by using it

    JP1998152679A

  • Water repellency-controlling agent and new diarylethene compound

    JP2007197502A

  • Extremely water-repelling surface structure and method of controlling water-repellency

    JP2014034583A

  • Electrolytic cell and method for manufacturing same

    JP2017031508A