Method for producing water- and oil-repellent film-forming liquid composition
A liquid composition with perfluoroether-structured metal oxide particles and silica sol-gel addresses film hardness and fingerprint issues, providing enhanced oil repellency and durability.
Patent Information
- Application Number
- JP2020050796
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-23
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-03-23
AI Technical Summary
Existing film-forming compositions exhibit insufficient hardness, abrasion strength, and are prone to showing fingerprints, with fluorine-containing compounds having perfluoroamine structures not effectively repelling oil and adhering fingerprints.
A liquid composition comprising metal oxide particles with a perfluoroether structure bonded to silicon alkoxide, mixed with silica sol-gel, enhances film hardness and abrasion strength while reducing fingerprint visibility.
The composition achieves high oil repellency, improved film durability, and reduced fingerprint visibility by using perfluoroether structures and metal oxide particles bonded with silica sol-gel, ensuring strong adhesion to substrates.
Smart Images

Figure 0007596074000017 
Figure 0007596074000018 
Figure 0007596074000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid composition for forming a water- and oil-repellent film having water and oil repellency, and a method for producing the same, and more particularly to a liquid composition for forming a water- and oil-repellent film containing metal oxide particles, and a method for producing the same. [Background technology]
[0002] The applicant has proposed a film-forming liquid composition having water- and oil-repellency and a method for producing the same, which comprises a component mainly consisting of silica sol-gel and a solvent, and is characterized in that, when the silica sol-gel is taken as 100 mass%, the silica sol-gel contains 0.5 mass % to 10 mass % of a fluorine-containing functional group component (F) having a perfluoroamine structure represented by the following general formula (28) and 0.5 mass % to 20 mass % of an alkylene group component (G) having 2 to 7 carbon atoms, and the solvent is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of an alcohol having 1 to 4 carbon atoms and an organic solvent other than the alcohol (see Patent Document 1 (Claim 1 and Claim 2)).
[0003] This patent document 1 describes a process for producing a liquid mixture comprising: (a) mixing tetramethoxysilane or tetraethoxysilane as silicon alkoxide (A), an epoxy group-containing silane (B), an alcohol having 1 to 4 carbon atoms and having a boiling point of less than 120° C., and water; (b) mixing the liquid mixture with a catalyst made of an organic acid, an inorganic acid, or a titanium compound to hydrolyze the silicon alkoxide (A) and the epoxy group-containing silane (B) to produce a liquid containing a first hydrolyzate (C); and (c) and a step of mixing a fluorine-containing silane (D) represented by the following general formula (28) and an alcohol having 1 to 4 carbon atoms or a mixed solvent of an alcohol having 1 to 4 carbon atoms and an organic solvent other than the alcohol with a liquid containing the first hydrolyzate (C) to hydrolyze the fluorine-containing silane (D) to produce a film-forming liquid composition containing a second hydrolyzate, silica sol-gel (E), characterized in that in the step (a), the epoxy group-containing silane (B) is mixed so as to contain 1 to 40 mass% based on the total mass of the silicon alkoxide (A) and the epoxy group-containing silane (B), and in the step (c), the fluorine-containing silane (D) is mixed in a proportion of 0.6 to 12 mass% based on the silica sol-gel (E).
[0004] [ka]
[0005] On the other hand, the present applicant has proposed a method for producing fluorine-containing nanocomposite particles, the method including: a first step of dispersing hydrophilic calcium carbonate having an average particle size of 5 to 200 nm in an organic solvent to prepare a dispersion; and a second step of adding a carboxylic acid having a nitrogen-containing perfluoroalkyl group represented by the following general formula (29) or a fluorine compound which is a halide thereof to the dispersion to synthesize a nanocomposite material of the calcium carbonate and the fluorine compound (Patent Document 2 (Claim 1, Claim 5, Claim 6, Paragraph
[0006] See paragraphs
[0017] and
[0061] to
[0065] .) Patent Document 2 discloses that in the second step, a silane coupling agent such as trialkoxysilane represented by the chemical formula [R1Si(OR2)3] may be added to the dispersion liquid of the inorganic compound.
[0006] [ka] [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6609382 [Patent Document 2] JP 2018-39987 A Summary of the Invention [Problem to be solved by the invention]
[0008] The film-forming liquid composition and its manufacturing method disclosed in Patent Document 1 have the features of being excellent in film-forming properties, having good adhesion to a substrate, being strong, and being capable of forming a film that does not produce rainbow-colored interference fringes, but when the film is formed, the hardness and abrasion resistance of the film are insufficient. Also, since the film is formed smoothly, fingerprints are easily noticeable on the film surface after being attached thereto, and further improvements are required for the invention of Patent Document 1.
[0009] In addition, Patent Document 2 describes a material that utilizes the hydrophilicity, durability, and surface structure forming ability of inorganic compounds and the excellent water-repellent, oil-repellent, and antifouling properties of fluorine compounds, and provides a novel fluorine-containing nanocomposite particle having high water-repellent and oil-repellent properties or hydrophilic and oil-repellent properties, and a method for producing the same, which is made from a low molecular weight fluorine compound as a raw material, and also describes that in the second step, a silane coupling agent such as trialkoxysilane is added to the dispersion liquid of the inorganic compound. However, when the silane coupling agent is added in the second step, the silane coupling agent is mainly used to bond with the inorganic compound, and is not used as a binder to adhere the film to the substrate. Therefore, the hardness and abrasion resistance of the film are less sufficient than those of the invention of Patent Document 1, and the invention of Patent Document 2 was also required to be improved.
[0010] Furthermore, the fluorine-containing functional group component (F) shown in Patent Document 1 and the fluorine compound shown in Patent Document 2 both have a perfluoroamine structure, and the perfluoro group is bonded to nitrogen at the center, so they tend to have a rigid structure. Therefore, even if the fluorine content in the liquid composition is increased, when oil adheres to the film, the oil may not slide off well, and from the viewpoint of oil repellency, the inventions of Patent Document 1 and Patent Document 2 still have room for improvement.
[0011] An object of the present invention is to provide a liquid composition for forming a water- and oil-repellent film which forms a film with high oil repellency, improved film hardness and abrasion resistance, and makes fingerprints less noticeable on the film surface, and a method for producing the same. [Means for solving the problem]
[0012] The present inventors have arrived at the present invention by noting that a perfluoroether structure is more likely to have a flexible structure than a perfluoroamine structure, that a fluorine-based compound containing a fluorine-based functional group component of a perfluoroether structure has good oil sliding properties when oil adheres to a film even if the fluorine content is low, and that when a film is formed by binding metal oxide particles together with silica sol-gel, the hardness and abrasion resistance of the film are improved, and unevenness is formed on the film surface, improving fingerprint resistance.
[0013] A first aspect of the present invention is a liquid composition for forming a water-repellent and oil-repellent film, comprising: Any one of equations (19) to (27) Fluorine-based compounds containing a perfluoroether structure represented by the formula: compound (A) is bonded to metal oxide particles (B) having an average particle size of 2 nm to 90 nm; It is a hydrolyzate of silicon alkoxide. The silica sol-gel (C) and the solvent (D) are contained, and when the amount of all components excluding the solvent (D) is taken as 100 mass %, the fluorine-based compound The content of (A) is 1% by mass to 30% by mass, and the fluorine-based compound The total content of (A) and the metal oxide particles (B) is 5% by mass to 80% by mass, and the ratio of the fluorine-based compound The water- and oil-repellent film-forming liquid composition is characterized in that the mass ratio (A / B) of (A) is in the range of 0.05 to 0.80.
[0014] [ka] [ka]
[0015] the above In formulas (19) to (27), R is a methyl group or an ethyl group. It is.
[0017] A second aspect of the present invention is the invention based on the first aspect, wherein the metal oxide particles (B) are oxide particles of one or two metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.
[0018] A third aspect of the present invention is the invention based on the first aspect, wherein the silica sol-gel (C) is a water- and oil-repellent film-forming liquid composition containing 0.5% by mass to 20% by mass of an alkylene group component having 2 to 7 carbon atoms, when the silica sol-gel is taken as 100% by mass.
[0019] A fourth aspect of the present invention is the invention based on the first aspect, and relates to a water- and oil-repellent film-forming liquid composition according to claim 1, wherein the solvent (D) is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms, and an organic solvent other than the alcohol.
[0020] A fifth aspect of the present invention is A method for producing a water- and oil-repellent film-forming liquid composition according to the first to fourth aspects, comprising: A dispersion of fluorine-containing metal oxide particles and a silica sol-gel liquid are mixed to produce a liquid composition for forming a water- and oil-repellent film. Water- and oil-repellent film-forming liquid composition Manufacturing method.
[0021] A sixth aspect of the present invention is the invention based on the fifth aspect, wherein the dispersion liquid of the fluorine-containing metal oxide particles is The above metal oxide particles (B) Fluorine-based compound in the dispersion liquid (A) and then adding and mixing water and a catalyst to the mixture to prepare the water- and oil-repellent film-forming liquid composition according to claim 5.
[0023] The present invention 7 The third aspect is an invention based on the fifth aspect, which is a method for producing a liquid composition for forming a water- and oil-repellent film, in which the silica sol-gel liquid is prepared by adding a catalyst to a mixed liquid of silicon alkoxide, alcohol, and water. Effect of the Invention
[0024] The water- and oil-repellent film-forming liquid composition according to the first aspect of the present invention is Any one of equations (19) to (27) Shown in 、 Fluorine-based compounds containing perfluoroether structures compound (A) is bonded to metal oxide particles (B) having an average particle size of 2 nm to 90 nm; It is a hydrolyzate of silicon alkoxide. The silica sol-gel (C) and the solvent (D) are contained, and when the amount of all components excluding the solvent (D) is taken as 100 mass %, the fluorine-based compound The content of (A) is 1% by mass to 30% by mass, and the fluorine-based compound The total content of (A) and the metal oxide particles (B) is 5% by mass to 80% by mass, and the ratio of the fluorine-based compound The mass ratio (A / B) of (A) is in the range of 0.05 to 0.80. When the liquid composition is formed into a film, the fluorine-based compound Since the film contains metal oxide particles (B) bonded to (A), the oil repellency of the film is high. In addition, when the film is formed, the metal oxide particles (B) with an average particle size of 2 nm to 90 nm are bonded to each other in the film by the silica sol-gel (C), which improves the hardness and abrasion resistance of the film. Since the surface of the film formed is not smooth, fingerprints are less noticeable on the film surface after they are applied to the film surface.
[0025] In the liquid composition of the second aspect of the present invention, the metal oxide particles are one or two types of metal oxide particles selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr, and therefore it is possible to include metal oxide particles suitable for the application or usage environment of the film to be formed from among many types of metal oxide particles.
[0026] In the liquid composition according to the third aspect of the present invention, the silica sol-gel contains 0.5% by mass to 20% by mass of an alkylene group component having 2 to 7 carbon atoms, and therefore the water- and oil-repellent film adheres well to the substrate on which it is formed, and the thickness of the water- and oil-repellent film becomes uniform, thereby imparting even more excellent oil repellency to the water- and oil-repellent film.
[0027] In the liquid composition according to the fourth aspect of the present invention, the solvent (D) is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms, and an organic solvent other than this alcohol, so that the drying speed of the liquid composition is improved and the viscosity of the liquid composition is reduced. Therefore, this liquid composition is easy to handle and has excellent film-forming properties on a substrate.
[0028] In a method for producing a liquid composition according to a fifth aspect of the present invention, A method for producing a water- and oil-repellent film-forming liquid composition according to the first to fourth aspects, comprising: As shown in Fig. 1, a liquid composition for forming a water- and oil-repellent film is produced by mixing a dispersion of fluorine-containing metal oxide particles with a silica sol-gel liquid. As a result, metal oxide particles having water- and oil-repellent particle surfaces are present in the silica sol-gel, and when the liquid composition is formed into a film, the film retains water- and oil-repellent properties.
[0029] In the method for producing a liquid composition according to the sixth aspect of the present invention, metal oxide particles (B) Fluorine-based compound in the dispersion liquid (A) To this mixture, water and a catalyst are added and mixed, so that a dispersion in which the fluorine-containing metal oxide particles are uniformly dispersed is obtained.
[0031] The present invention 7 In the method for producing a liquid composition from this viewpoint, a silica sol-gel liquid prepared by adding a catalyst to a mixed liquid of silicon alkoxide, alcohol and water acts as a binder for fluorine-containing metal oxide particles, and when the liquid composition is formed into a film on a substrate surface, the film can be firmly bound to the substrate surface.
[0032] For comparison, as shown in Comparative Example 4 described later, when a liquid composition for forming a water- and oil-repellent film is produced by a method different from that of the present invention shown in FIG. 1, in which a dispersion of metal oxide particles is added to a sol-gel liquid obtained by adding a catalyst to a mixture of silicon alkoxide, fluorine-containing silane, alcohol, and water, the essential oil-repellent properties cannot be imparted to the film when the liquid composition is formed into a film. 7 In the method for producing a liquid composition according to any one of the above aspects, when the liquid composition is formed on the surface of a substrate, the water- and oil-repellent film contains metal oxide particles to which a fluorine-based functional group component is bonded, so that the water- and oil-repellent film can be imparted with sufficient oil repellency.Furthermore, the metal oxide particles bonded with silica sol-gel can improve the hardness and abrasion resistance of the film. [Brief description of the drawings]
[0033] [Figure 1] FIG. 2 is a flow diagram for producing the water- and oil-repellent film-forming liquid composition of the present embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a water- and oil-repellent film formed on a substrate according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Next, an embodiment of the present invention will be described with reference to the drawings.
[0035] [Method for producing water- and oil-repellent film-forming liquid composition] The water- and oil-repellent film-forming liquid composition is generally produced by the following method. As shown in Fig. 1, metal oxide particles 11 and an organic solvent 12 are mixed to prepare a metal oxide particle dispersion 13. A fluorine-based compound 14 containing a fluorine-based functional group component (B) is mixed with this dispersion 13, and water 15 and a catalyst 16 are further mixed to prepare a fluorine-containing metal oxide particle dispersion 17. Meanwhile, a silicon alkoxide 21, an alcohol 22, water 23, and optionally an alkylene group component 24 are mixed, and a catalyst 25 is added to this mixture to prepare a silica sol-gel liquid 26. The silica sol-gel liquid 26 is mixed with alcohol 27, and this mixture is then mixed with the above-mentioned dispersion liquid 17 of fluorine-containing metal oxide particles to produce a water- and oil-repellent film-forming liquid composition 30. Each step will be described in detail below.
[0036] [Preparation of Metal Oxide Particle Dispersion] First, a dispersion liquid of metal oxide particles is prepared by dispersing metal oxide particles in an organic solvent. The metal oxide particles have an average particle size of 2 nm to 90 nm, preferably 2 nm to 85 nm. If the average particle size is less than 2 nm, the metal oxide particles are likely to aggregate and are difficult to disperse in the medium. If the average particle size exceeds 90 nm, the metal oxide particles will fall off from the water-repellent and oil-repellent film when the liquid composition is formed into a film. Examples of metal oxide particles include particles of SiO2, Al2O3, MgO, CaO, TiO2, ZnO, and ZrO2, mixed particles of these, and composite oxide particles such as MgAl2O4. Examples of organic solvents include methanol, ethanol, isopropanol (hereinafter sometimes referred to as IPA), tetrahydrofuran, hexane, chloroform, toluene, ethyl acetate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), acetone, and fluorine-based solvents. Among these, alcohols such as methanol, ethanol, and isopropanol, which have a boiling point of less than 120° C. and a carbon number of 1 to 4, are preferred. In this specification, the average particle size of metal oxide particles refers to the average value of particle sizes measured by image analysis at 200 points among particle shapes observed with a transmission electron microscope (TEM).
[0037] [Preparation of Fluorine-Containing Metal Oxide Particle Dispersion] Next, a fluorine-based compound containing a fluorine-based functional group component represented by the above formula (1) or (2) is added to the prepared dispersion of metal oxide particles to synthesize a nanocomposite material of the metal oxide particles and the fluorine-based functional group component. To further promote the reaction, water and a catalyst are added. In this way, a dispersion of fluorine-containing metal oxide particles is prepared.
[0038] The catalyst may be an organic acid, an inorganic acid, or a titanium compound, and examples of the organic acid include formic acid and oxalic acid, examples of the inorganic acid include hydrochloric acid, nitric acid, and phosphoric acid, and examples of the titanium compound include tetrapropoxytitanium, tetrabutoxytitanium, tetraisopropoxytitanium, and titanium lactate. The catalyst is not limited to the above. As the water, it is preferable to use ion-exchanged water or pure water to prevent the inclusion of impurities.
[0039] The fluorine-based compound containing a fluorine-based functional group component is represented by the following general formula (3) or formula (4). More specifically, the perfluoroether group in the formula (3) or formula (4) may include the perfluoroether structures represented by the following formulae (5) to (13).
[0040] [ka]
[0041] [ka]
[0042] [ka]
[0043] Examples of X in the above formulae (3) and (4) include structures represented by the following formulae (14) to (18). Note that the following formula (14) shows an example containing an ether bond, the following formula (15) an ester bond, the following formula (16) an amide bond, the following formula (17) a urethane bond, and the following formula (18) a sulfonamide bond.
[0044] [ka]
[0045] In the above formulas (14) to (18), R 2 and R 3 is a hydrocarbon group with 0 to 10 carbon atoms, R 4 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 3 Examples of the hydrocarbon group include alkylene groups such as methylene and ethylene groups. 4 Examples of the hydrocarbon group include alkyl groups such as methyl and ethyl groups, as well as phenyl groups.
[0046] In addition, in the above formula (3) and formula (4), R 1 Examples of the alkyl group include a methoxy group and an ethoxy group.
[0047] In addition, in the above formula (3) and formula (4), Z is not particularly limited as long as it is a hydrolyzable group that can be hydrolyzed to form a Si-O-Si bond. Specific examples of such hydrolyzable groups include alkoxy groups such as methoxy, ethoxy, propoxy, and butoxy groups, aryloxy groups such as phenoxy and naphthoxy groups, aralkyloxy groups such as benzyloxy and phenethyloxy groups, and acyloxy groups such as acetoxy, propionyloxy, butyryloxy, valeryloxy, pivaloyloxy, and benzoyloxy groups. Among these, it is preferable to apply a methoxy group or an ethoxy group.
[0048] Specific examples of the fluorine-based compound containing a fluorine-based functional group component having a perfluoroether structure represented by the above formula (3) or (4) include structures represented by the following formulas (19) to (27), in which R is a methyl group or an ethyl group.
[0049] [ka]
[0050] [ka]
[0051] As described above, the fluorine-based compound contained in the water- and oil-repellent film-forming liquid composition of the present embodiment has a perfluoroether group in which a plurality of short-chain perfluoroalkyl groups and perfluoroalkylene groups each having 6 or less carbon atoms are bonded to an oxygen atom in the molecule, and since the fluorine content in the molecule is high, it is possible to impart excellent water- and oil-repellency to the formed film.
[0052] [Preparation of Silica Sol-Gel Liquid] First, a mixed solution is prepared by mixing tetramethoxysilane or tetraethoxysilane as silicon alkoxide, alcohol having 1 to 4 carbon atoms and a boiling point of less than 120°C, and water. At this time, an epoxy group-containing silane as an alkylene group component may be mixed together. Specific examples of this silicon alkoxide include tetramethoxysilane and its oligomers, and tetraethoxysilane and its oligomers. For example, in order to obtain a highly durable water- and oil-repellent film, it is preferable to use tetramethoxysilane, while in order to avoid methanol generated during hydrolysis, it is preferable to use tetraethoxysilane.
[0053] Specific examples of the epoxy group-containing silane that is the alkylene group component include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and polyfunctional epoxysilane. The alkylene group component is contained in an amount of 1% by mass to 40% by mass, preferably 2.5% by mass to 20% by mass, based on the total mass of the silicon alkoxide and the alkylene group component. If the alkylene group component is less than the lower limit of 1% by mass, when a film is formed on a substrate that does not contain a hydroxyl group, the adhesion to the substrate becomes insufficient. If the alkylene group component exceeds the upper limit of 40% by mass, the durability of the formed film decreases. If the epoxy group-containing silane is contained so that the alkylene group component is in the above range of 1% by mass to 40% by mass, the epoxy group also opens in the hydrolysis polymerization process and contributes to polymerization, which improves leveling during the drying process and makes the film thickness uniform. When the substrate contains a hydrophilic group such as glass, the content of the alkylene group component may be very small or may be zero.On the other hand, when the substrate does not contain a hydrophilic group, the content of the alkylene group component in the silica sol-gel (C) is preferably 0.5% by mass to 20% by mass.
[0054] Examples of the alcohol having 1 to 4 carbon atoms and a boiling point of less than 120°C include the above-mentioned alcohols. In particular, methanol or ethanol are preferred. This is because these alcohols are easily mixed with silicon alkoxide. As the water, it is preferable to use ion-exchanged water or pure water to prevent the inclusion of impurities. A mixed solution is prepared by adding an alcohol having 1 to 4 carbon atoms and water to silicon alkoxide, or to silicon alkoxide and epoxy group-containing silane, and stirring the mixture at a temperature of 10°C to 30°C for 5 to 20 minutes.
[0055] A catalyst is added to the mixed liquid prepared above. Examples of the catalyst include organic acids, inorganic acids, and titanium compounds. At this time, the liquid temperature is preferably kept at 30°C to 80°C, and the mixture is stirred for preferably 1 hour to 24 hours. This prepares a silica sol-gel liquid. For the next step, an alcohol is added to the silica sol-gel liquid and mixed.
[0056] The silica sol-gel liquid to which the alcohol is added contains 2% by mass to 50% by mass of silicon alkoxide, 20% by mass to 98% by mass of alcohol having 1 to 4 carbon atoms, 0.1% by mass to 40% by mass of water, and 0.01% by mass to 5% by mass of catalyst. When an epoxy group-containing silane, which is an alkylene group component, is mixed, the epoxy group-containing silane can be contained up to a maximum of 30% by mass.
[0057] The reason why the proportion of the alcohol having 1 to 4 carbon atoms is limited to the above range is that if the proportion of alcohol is less than the lower limit, silicon alkoxide does not dissolve in the solution and separates, and the reaction solution is easily gelled during the hydrolysis reaction of silicon alkoxide; on the other hand, if it exceeds the upper limit, the amount of water and catalyst required for hydrolysis is relatively small, so the reactivity of hydrolysis decreases, polymerization does not proceed, and the adhesion of the film decreases.The reason why the proportion of water is limited to the above range is that if it is less than the lower limit, the hydrolysis rate slows down, polymerization does not proceed, and the adhesion of the water-repellent and oil-repellent film becomes insufficient; on the other hand, if it exceeds the upper limit, the reaction solution gels during the hydrolysis reaction, and the silicon alkoxide compound does not dissolve in the alcohol aqueous solution due to the excessive water, causing the problem of separation.
[0058] The SiO2 concentration (SiO2 content) in the silica sol-gel is preferably 1% by mass to 40% by mass. If the SiO2 concentration is less than the lower limit, polymerization is insufficient, and the adhesion of the film is reduced and cracks are likely to occur, while if the SiO2 concentration exceeds the upper limit, the proportion of water becomes relatively high, silicon alkoxide does not dissolve, and the reaction solution gels.
[0059] The organic acid, inorganic acid or titanium compound functions as a catalyst for promoting the hydrolysis reaction. Examples of organic acids include formic acid and oxalic acid, examples of inorganic acids include hydrochloric acid, nitric acid and phosphoric acid, and examples of titanium compounds include tetrapropoxytitanium, tetrabutoxytitanium, tetraisopropoxytitanium, and titanium lactate. The catalyst is not limited to the above. The reason why the proportion of the catalyst is limited to the above range is that if it is less than the lower limit, the reactivity is poor and polymerization is insufficient, so that a film is not formed, while if it exceeds the upper limit, there is no effect on reactivity, but the substrate on which the film is formed is easily corroded by the remaining acid.
[0060] [Water- and oil-repellent film-forming liquid composition] The water- and oil-repellent film-forming liquid composition of the present embodiment is produced by the above-mentioned production method, and contains the metal oxide particles (B) to which the fluorine-based functional group component (A) is bonded, the silica sol-gel (C), and the solvent (D). The fluorine-based functional group component has a perfluoroether structure represented by the above-mentioned general formula (1) or formula (2), and is contained in the liquid composition in an amount of 1% by mass to 30% by mass when the total amount of components excluding the solvent (D) is taken as 100% by mass. If the fluorine-based functional group component is less than 1% by mass, the formed film cannot be imparted with oil repellency, and if it exceeds 30% by mass, the film repels, etc., and the film-forming property is poor. The preferred content ratio of the fluorine-based functional group component is 2% by mass to 28% by mass. The total content ratio of the fluorine-based functional group component (A) and the metal oxide particles (B) is 5% by mass to 80% by mass, preferably 7% by mass to 75% by mass, when the total amount of components excluding the solvent (D) is taken as 100% by mass. Furthermore, the mass ratio (A / B) of the fluorine-based functional group component (A) to the metal oxide particles (B) is in the range of 0.05 to 0.80, preferably 0.07 to 0.70.
[0061] In the liquid composition excluding the solvent, if the total amount of the components (A) and the particles (B) is less than 5% by mass, the oil repellency of the water- and oil-repellent film is reduced. If the total amount exceeds 80% by mass, the content of the silica sol-gel (C) is relatively low, and when the liquid composition is formed on a substrate, the water- and oil-repellent film is not firmly attached to the substrate surface. If the mass ratio (A / B) is less than 0.05, the water- and oil-repellent film has poor oil repellency, and if it exceeds 0.80, the adhesion of the water- and oil-repellent film to the substrate surface is reduced.
[0062] 1, the solvent (D) contains an organic solvent 12, water 15, an alcohol 22, water 23, and an alcohol 27. That is, it is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms, and an organic solvent other than the above alcohol. Specific examples of the perfluoroether structure include the structures represented by the above formulas (19) to (27).
[0063] Since the water- and oil-repellent film-forming liquid composition of the present embodiment contains a silica sol-gel liquid as a main component, when the water- and oil-repellent film is formed on the surface of a substrate, the water- and oil-repellent film has excellent adhesion to the substrate surface, and is difficult to peel off, resulting in a high-strength water- and oil-repellent film.In addition, since the water- and oil-repellent film-forming liquid composition contains a fluorine-based functional group component having a perfluoroether structure represented by the above general formula (1) or formula (2), it has an oil-repellent effect.
[0064] [Method of forming a water-repellent and oil-repellent film on a substrate surface] To form the water-repellent and oil-repellent film on the surface of a substrate, the water-repellent and oil-repellent film-forming liquid composition is applied to the substrate, and then dried at room temperature in the air to harden the liquid composition. The substrate is not particularly limited, but may be metal plates such as stainless steel (SUS), aluminum, and iron, glass such as window glass and mirrors, tiles, plastics such as polyvinyl chloride (PVC), or polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. The coating method of the liquid composition may be screen printing, bar coating, die coating, doctor blade, spin coating, brush coating, etc.
[0065] As shown in FIG. 2, the water- and oil-repellent film 2 formed on the surface of the substrate 1 is composed of a large number of metal oxide particles 3 whose particle surfaces are covered with fluorine-based functional group components bound together by silica sol-gel 4 as a binder. The water- and oil-repellent film 2 contains metal oxide particles 3 bound to fluorine-based functional group components, so the oil-repellent performance of the film is maintained. In addition, the metal oxide particles 3 with an average particle size of 2 nm to 90 nm are bound together in the film 2 by the silica sol-gel 4, so the hardness and abrasion resistance of the film 2 can be improved. In addition, the presence of the metal oxide particles 3 makes the film surface uneven, which has the advantage that fingerprints are less noticeable on the film surface after they are attached to the film 2 surface. The film thickness can be controlled by changing the particle size of the metal oxide particles and the content ratio of the metal oxide particles in the film components. EXAMPLES
[0066] Next, examples of the present invention will be described in detail together with comparative examples. First, Synthesis Examples 1 to 9 and Comparative Synthesis Examples 1 to 3 for preparing a dispersion liquid of metal oxide particles will be described, and then Examples 1 to 9 and Comparative Examples 1 to 7 for producing a water- and oil-repellent film-forming liquid composition using these Synthesis Examples and Comparative Synthesis Examples will be described.
[0067] [Synthesis Examples 1 to 9 for preparing metal oxide particle dispersion liquid, and Comparative Synthesis Examples 1 to 3] <Synthesis Example 1> 9.75 g of the fluorine-based compound represented by the above formula (19) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of silicon dioxide with an average particle size of 12 nm (IPA-ST, Nissan Chemical Co., Ltd., SiO2 concentration 30%). Next, 3.51 g of water was added and mixed. Furthermore, 0.031 g of nitric acid was added and mixed at 40°C for 2 hours to obtain a dispersion of silicon dioxide (silica) particles in which the fluorine-based compound is bonded to the silicon dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to the silicon dioxide, which is the metal oxide particle (B), was 0.61.
[0068] <Synthesis Example 2> 1.50 g of the fluorine-based compound represented by the above formula (20) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 45 nm (IPA-ST-L, manufactured by Nissan Chemical Industries, Ltd., SiO2 concentration 30%). Next, 0.54 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.09.
[0069] <Synthesis Example 3> 0.75 g of the fluorine-based compound represented by the above formula (21) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 80 nm (IPA-ST-ZL, manufactured by Nissan Chemical Industries, Ltd., SiO2 concentration 30%). Next, 0.27 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.05.
[0070] <Synthesis Example 4> 2.25 g of the fluorine-based compound represented by the above formula (22) was added and mixed into a beaker containing 50.0 g of the same silicon dioxide IPA dispersion as in Synthesis Example 1. Next, 0.81 g of water was added and mixed. Furthermore, 0.010 g of nitric acid was added, and the rest of the procedure was the same as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.14.
[0071] <Synthesis Example 5> A dispersion of silicon dioxide (silica) particles was obtained in the same manner as in Synthesis Example 4, except that the fluorine-based compound used in Synthesis Example 4 was replaced with the fluorine-based compound represented by the above formula (27). The mass ratio (A / B) was 0.14.
[0072] <Synthesis Example 6> 11.25 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of a methanol dispersion of zirconium dioxide having an average particle size of 3 nm (SZR-M, manufactured by Sakai Chemical Industry Co., Ltd., ZrO2 concentration 30%). Next, 4.05 g of water was added and mixed. Furthermore, 0.035 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of zirconium dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to zirconium dioxide, which is the metal oxide particle (B), was 0.71.
[0073] <Synthesis Example 7> 2.70 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of titanium dioxide having an average particle size of 6 nm (TKD-701, manufactured by Teika Co., Ltd., TiO2 concentration 18%). Next, 0.97 g of water was added and mixed. Furthermore, 0.010 g of nitric acid was added, and the rest of the procedure was the same as in Synthesis Example 1 to obtain a dispersion of titanium dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to titanium dioxide, which is the metal oxide particle (B), was 0.28.
[0074] <Synthesis Example 8> 0.25 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of alumina and silicon dioxide with an average particle size of 60 nm (Baylal AS-L10, manufactured by Taki Chemical Industry Co., Ltd., 3Al2O3·2SiO2 concentration 10%). Next, 0.09 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the rest of the procedure was the same as in Synthesis Example 1 to obtain a dispersion of alumina and silicon dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to the alumina and silicon dioxide, which are the metal oxide particles (B), was 0.05.
[0075] <Synthesis Example 9> 1.50 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of an IPA dispersion of zinc oxide having an average particle size of 25 nm (MZ-500, manufactured by Teika Co., Ltd., ZnO concentration 30%). Next, 0.54 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the following procedure was repeated in the same manner as in Synthesis Example 1 to obtain a dispersion of zinc oxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to zinc oxide, which is the metal oxide particle (B), was 0.09.
[0076] <Comparative Synthesis Example 1> To a beaker containing 50.0 g of an IPA dispersion of titanium dioxide having an average particle size of 230 nm (R32, Sakai Chemical Industry Co., Ltd., TiO2 concentration 30%), 1.50 g of the fluorine-based compound represented by the above formula (27) was added and mixed. Next, 0.54 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the rest of the procedure was the same as in Synthesis Example 1 to obtain a dispersion of titanium dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to titanium dioxide, which is the metal oxide particle (B), was 0.09.
[0077] <Comparative Synthesis Example 2> 0.45 g of the fluorine-based compound represented by the above formula (27) was added and mixed into a beaker containing 50.0 g of the same silicon dioxide IPA dispersion as in Synthesis Example 1. Next, 0.16 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the rest of the procedure was the same as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.03.
[0078] <Comparative Synthesis Example 3> In a beaker containing 50.0 g of the same silicon dioxide IPA dispersion as in Synthesis Example 1, 15.00 g of the fluorine-based compound represented by the above formula (27) was added and mixed. Next, 5.40 g of water was added and mixed. Furthermore, 0.047 g of nitric acid was added, and the rest was the same as in Synthesis Example 1 to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.95.
[0079] Table 1 below shows the contents of the dispersions of fluorine-containing metal oxide particles in Synthesis Examples 1 to 9 and Comparative Synthesis Examples 1 to 3. In Table 1, all of the Rs in the fluorine-containing silanes represented by formulas (19) to (22) and (27) as fluorine-based compounds are ethyl groups.
[0080] [Table 1]
[0081] [Examples 1 to 9 and Comparative Examples 1 to 4 for the production of water- and oil-repellent film-forming liquid compositions] <Example 1> After mixing 30g of orthoethyl silicate, 60g of ethanol, and 10g of water, 1g of nitric acid was added and mixed at 30°C for 3 hours to obtain a silica sol-gel liquid. After adding and mixing 72.18g of industrial alcohol (AP-7, manufactured by Nippon Alcohol Industry Co., Ltd.), 1.70g of diacetone alcohol, and 11.04g of isopropyl glycol to 10.00g of the obtained silica sol-gel liquid, 11.51g of the dispersion of metal oxide particles of Synthesis Example 1 was added and mixed to prepare a liquid composition for forming a water- and oil-repellent film. The contents are shown in Table 2 below. Table 2 also shows the content ratio of the fluorine-based functional group component (A) in the liquid composition excluding the solvent and the total content ratio of the fluorine-based functional group component (A) and the metal oxide particles (B) in the liquid composition excluding the solvent. The content (%) of the fluorine-based functional group component (A) in the liquid composition excluding the solvent, when expressed taking into account the content of the metal oxide particles (C), is the percentage [(A) / [(A)+(B)+(C)]], and the total content (%) of the fluorine-based functional group component (A) and the metal oxide particles (B) in the liquid composition excluding the solvent, when expressed taking into account the content of the metal oxide particles (C), is the percentage [[(A)+(B)] / [(A)+(B)+(C)]].
[0082] [Table 2]
[0083] <Examples 2 to 9 and Comparative Examples 1 to 3> For Examples 2 to 9 and Comparative Examples 1 to 3, the type and amount of the dispersion liquid of the fluorine-containing metal oxide particles, the amount of the silica sol-gel liquid, and the amounts of the same industrial alcohol, diacetone alcohol, and isopropyl glycol as in Example 1 were determined as shown in Table 2, and the water- and oil-repellent film-forming liquid compositions of Examples 2 to 9 and Comparative Examples 1 to 3 were prepared. Regarding the silica sol-gel liquid, in Examples 2 to 9 and Comparative Examples 1 to 3, 28.50 g of trimer to pentamer of tetramethoxysilane (TMOS) (manufactured by Mitsubishi Chemical Corporation, product name: MKC Silicate MS51) and 1.50 g of 3-glycidoxypropyltrimethoxysilane (GPTMS: manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-403) were used as an epoxy group-containing silane serving as an alkylene group component, instead of the orthosilicate used in Example 1. Otherwise, the same operations as in Example 1 were performed.
[0084] <Comparative Example 4> In Comparative Example 4, a water- and oil-repellent film-forming liquid composition was prepared by a method different from that of the above-mentioned Examples 1 to 9 and Comparative Examples 1 to 3. That is, 8.52 g of trimer to pentamer of tetramethoxysilane (TMOS) (manufactured by Mitsubishi Chemical Corporation, product name: MKC silicate MS51) as silicon alkoxide, 0.48 g of 3-glycidoxypropyltrimethoxysilane (GPTMS: manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-403) as an epoxy group-containing silane that is an alkylene group component, 0.24 g of fluorine-containing silane (R: ethyl group) represented by formula (27) as a fluorine-based compound, and 17.34 g of ethanol (EtOH) (boiling point 78.3°C) as an organic solvent were mixed, and 3.37 g of ion-exchanged water was further added, and the mixture was stirred at a temperature of 25°C for 5 minutes in a separable flask to prepare a mixed liquid. To this mixture, 0.05 g of hydrochloric acid with a concentration of 35% by mass was added as a catalyst, and the mixture was stirred at 40° C. for 2 hours to obtain a fluorine-containing silica sol-gel liquid. 90 g of the same industrial alcohol as in Example 1, 2 g of diacetone alcohol, and 13 g of isopropyl glycol were mixed with 10 g of this silica sol-gel liquid, and 10 g of the same IPA dispersion of silicon dioxide with an average particle size of 12 nm as in Synthesis Example 1 was added and mixed as a dispersion of metal oxide particles to prepare a water- and oil-repellent film-forming liquid composition.
[0085] <Comparative Example 5> In Comparative Example 4, 90 g of the same industrial alcohol as in Example 1, 2 g of diacetone alcohol, and 13 g of isopropyl glycol were mixed with 10 g of the silica sol-gel liquid obtained in Comparative Example 4, respectively, and then a water- and oil-repellent film-forming liquid composition was prepared without adding the IPA dispersion of silicon dioxide having an average particle size of 12 nm, which is the same as in Synthesis Example 1, which is a dispersion of metal oxide particles.
[0086] <Comparative Example 6> A fluorine-based compound containing a fluorine-based functional group component having a perfluoroamine structure of the following formula (30) was used instead of the fluorine-based compound used in Example 1 to prepare the dispersion liquid of metal oxide particles of Synthesis Example 1. A water- and oil-repellent film-forming liquid composition was prepared in the same manner as in Example 1 except for the above.
[0087] [ka]
[0088] <Comparative Example 7> A silane coupling agent of methyltriethoxysilane was used instead of the silica sol-gel liquid prepared in Example 1. A water- and oil-repellent film-forming liquid composition was prepared in the same manner as in Example 1 except for the above.
[0089] <Comparative testing and evaluation> The 16 types of liquid compositions obtained in Examples 1 to 9 and Comparative Examples 1 to 7 were applied to a SUS304 substrate having a thickness of 2 mm, a length of 150 mm, and a width of 75 mm using a brush (Nylon Brush Meister manufactured by Suematsu Brush Co., Ltd.) so that the thickness after drying would be 1 to 3 μm, respectively, to form 16 types of coating films. All coating films were left to stand in an atmospheric atmosphere at room temperature for 3 hours, and the coating films were dried to obtain 16 types of films on the SUS304 substrate. For these films, the water wettability (water repellency), oil repellency, and appearance of the film were evaluated, and a film strength test, a cellophane tape peeling test, and a fingerprint resistance test were performed. The results are shown in Table 3. The fingerprint resistance of the film is a property in which fingerprints are not easily noticeable on the film surface after they are attached to the film, and fingerprints are easily wiped off when they are attached, as well as fingerprints are not easily attached to the film.
[0090] (1) Water repellency of the film surface (contact angle) Using a Dropmaster DM-700 manufactured by Kyowa Interface Science, ion-exchanged water at 22°C ± 1°C was prepared in a syringe, and a 2μL droplet was ejected from the tip of the needle of the syringe. The film on the SUS304 substrate to be evaluated was then brought close to the droplet, causing the droplet to adhere to the film. The contact angle of the adhered water was measured. The contact angle measured 1 second after the water touched the film surface in a stationary state was analyzed using the θ / 2 method, and this value was used to evaluate the water wettability (water repellency) of the film surface.
[0091] (2) Oil repellency of the film surface (contact angle) Using a Dropmaster DM-700 manufactured by Kyowa Interface Science, n-hexadecane (hereinafter referred to as oil) at 22°C ± 1°C was prepared in a syringe, and a 2μL droplet was ejected from the tip of the needle of the syringe. Next, the film on the SUS304 substrate to be evaluated was brought close to the droplet, and the droplet was attached to the film. The contact angle of the attached oil was measured. The contact angle 1 second after the oil touched the film surface in a stationary state was analyzed using the θ / 2 method, and the value was used to evaluate the oil repellency of the film surface.
[0092] (3) Appearance of the membrane The film on the SUS304 substrate to be evaluated was visually observed to check whether the film was transparent or not, and whether the film was cloudy or not. Films that were transparent were rated as "good", and films that were cloudy were rated as "poor cloudiness" or "slightly poor cloudiness" depending on the degree of cloudiness.
[0093] (4) Membrane strength test The contactor described below was applied with a specified load to the film on the SUS304 substrate to be evaluated, and after 10 reciprocating movements under the following conditions, the film on the substrate was visually inspected to see if it peeled off from the substrate. If the film did not peel off, it was judged as "passed", and if it peeled off, it was judged as "failed". (a) Measuring instrument: Static and dynamic friction measuring instrument TL201Tt (Trinity Lab Co., Ltd.) (b) Measurement conditions: ·Traveling distance: 30mm ·Vertical load: 500g weight ·Moving speed: 50mm / sec Contact: 5mm x 15mm neoprene rubber
[0094] (5) Cellophane tape peeling test of film A 1 mm wide cross-cut was made in a grid pattern on the film on the SUS304 substrate to be evaluated, and an adhesive tape (manufactured by Nichiban Co., Ltd., product name "Cellotape (registered trademark)") was applied to the grid-cut film, and a Cellotape (registered trademark) peeling test was performed in accordance with the grid tape method of JIS K5600-5-6 (cross-cut method). The denominator was the number of 100 cross-cut squares, and the numerator was the number of squares remaining on the substrate after the Cellotape (registered trademark) peeling test.
[0095] (6) Fingerprint resistance test of film A continuous cellulose fiber nonwoven fabric (manufactured by Asahi Kasei Corporation, product name: BEMCOT M-3II) was placed on the film on the SUS304 substrate to be evaluated, and 100 microliters of artificial fingerprint liquid (based on JIS K 2246) was dropped onto the nonwoven fabric. Black rubber No. 24 (mass 300 g) was placed on the nonwoven fabric, and a weight of 1 kg was placed on top and left to stand for 30 seconds to allow the fingerprint liquid to adhere to the film. The nonwoven fabric was then peeled off, and the fingerprint resistance of the film was visually observed. Films that did not have fingerprint liquid on the surface were rated as "good," and films that had fingerprint liquid on the surface were rated as "poor."
[0096] [Table 3]
[0097] As is clear from Table 3, in Comparative Example 1, a water- and oil-repellent film-forming liquid composition was prepared from the dispersion of titanium dioxide particles of Comparative Synthesis Example 1, which contains metal oxide (titanium dioxide) particles with an average particle diameter of 230 nm, and a film was formed using this liquid composition. Therefore, the average particle diameter of the metal oxide particles in the film was too large, and the metal oxide particles were difficult to bind to the substrate surface with the silica sol-gel, which is the binder component. As a result, the contact angles of water and n-hexadecane were poor, the film was cloudy, and the appearance of the film was poor. In addition, in the film strength test, the film peeled off from the substrate, and in the Cellotape (registered trademark) peel test, only 20 squares remained on the substrate, and most of them peeled off. Furthermore, the fingerprint resistance of the film was poor.
[0098] In Comparative Example 2, the ratio of "(A) / (B)" in the dispersion of fluorine-containing metal oxide particles was 0.03, the content of "fluorine-based functional group component (A)" in the liquid composition excluding solvent (D) was 0.1 mass%, and the content of "(A)+(B)" in the liquid composition excluding solvent (D) was 3 mass%, so the content of the fluorine-based functional group component in the film was too low. Therefore, although the appearance of the film was good and the film passed both the strength test and the Cellophane Tape (registered trademark) peeling test, the contact angles of water and n-hexadecane were poor, and the film's fingerprint resistance was poor.
[0099] In Comparative Example 3, the ratio of "(A) / (B)" in the dispersion of fluorine-containing metal oxide particles was 0.95, the content of "fluorine-based functional group component (A)" in the liquid composition excluding the solvent (D) was 41.0% by mass, and the content of "(A)+(B)" in the liquid composition excluding the solvent (D) was 82% by mass, so the content of the fluorine-based functional group component in the film was too high. Therefore, although the contact angles of water and n-hexadecane were good and the Cellophane Tape (registered trademark) peeling test was passed, the fingerprint resistance of the film was poor, the film was slightly cloudy, the film surface was rough, and the appearance of the film was slightly poor. In addition, the film peeled off from the substrate and failed the strength test.
[0100] In Comparative Example 4, a water- and oil-repellent film-forming liquid composition was prepared by adding and mixing a dispersion of metal oxide particles to a fluorine-containing silica sol-gel liquid, and the oil-repellent performance was greatly deteriorated due to the presence of a large number of metal oxide particles with lipophilic particle surfaces in the film. As a result, the appearance of the film was good, and the film passed both the strength test and the Cellophane Tape (registered trademark) peeling test, but the contact angles of water and n-hexadecane were poor, and the film's fingerprint resistance was poor.
[0101] In Comparative Example 5, the water- and oil-repellent film-forming liquid composition was prepared without adding a dispersion of metal oxide particles to the fluorine-containing silica sol-gel liquid, so that the hydrophilic and oil-repellent metal oxide particles were not present in the film, and the oil-repellent performance was good. As a result, the contact angles of water and n-hexadecane and the appearance of the film were both good, and the Cellophane Tape (registered trademark) peeling test was passed, but the fingerprint resistance of the film was poor, and the film strength test was failed because the film peeled off from the substrate due to the absence of metal oxide particles.
[0102] In Comparative Example 6, the contact angles of water and n-hexadecane were slightly lower than those of the fluorine-based compound having a perfluoroamine structure of the above-mentioned formula (30). The appearance, adhesion test, and film strength test of the coating film were at the acceptable level, but the contact angles of water and n-hexadecane were low, so the fingerprint resistance of the film was poor.
[0103] In Comparative Example 7, instead of the silica sol-gel binder component, methyltriethoxysilane was used as a silane coupling agent, and the contact angles of water and n-hexadecane were not excellent, and the film had poor fingerprint resistance. The film also had a slightly cloudy appearance, and in a Cellophane Tape (registered trademark) peeling test, the film peeled off completely, showing poor adhesion. Furthermore, in the film strength test, the film peeled off easily after the first round trip, and failed.
[0104] In contrast, in Examples 1 to 9, the fluorine-based functional group component was of formula (1) or formula (2), the average particle size of the metal oxide particles was in the range of 2 nm to 90 nm, the content of the fluorine-based functional group component (A) in the liquid composition excluding the solvent (D) was 1 mass% to 30 mass%, the total content of the fluorine-based functional group component (A) and the metal oxide particles (B) in the liquid composition excluding the solvent (D) was 5 mass% to 80 mass%, and "(A) / (B)" was in the range of 0.05 to 0.80, which satisfied the scope of the invention according to the first aspect. Therefore, the contact angles with water and n-hexadecane and the appearance of the film were all good, and the film strength test, the Scotch tape peeling test, and the fingerprint resistance test were all passed. [Industrial Applicability]
[0105] The water- and oil-repellent film-forming liquid composition of the present invention is used in fields where oil stains need to be prevented in factories where machine oil is used, in kitchens where oil is scattered, and in range hoods, ventilation fans, refrigerator doors, and the like where oil vapor is present. [Explanation of symbols]
[0106] 1 Base material 2. Water- and oil-repellent film 3 Metal oxide particles 4. Silica sol-gel
Claims
1. A method for producing a water- and oil-repellent film-forming liquid composition, comprising the steps of: The present invention comprises metal oxide particles (B) having an average particle size of 2 nm to 90 nm and bonded to a fluorine-based compound (A) containing a perfluoroether structure, the metal oxide particles (B) being represented by any one of the following formulas (19) to (27), silica sol-gel (C) being a hydrolyzate of silicon alkoxide, and a solvent (D), When the amount of all components excluding the solvent (D) is taken as 100 mass%, the content of the fluorine-based compound (A) is 1 mass% to 30 mass%, and the total content of the fluorine-based compound (A) and the metal oxide particles (B) is 5 mass% to 80 mass%, a mass ratio (A / B) of the fluorine-based compound (A) to the metal oxide particles (B) is in the range of 0.05 to 0.80; A method for producing a water- and oil-repellent film-forming liquid composition, which is prepared by mixing a dispersion of fluorine-containing metal oxide particles with a silica sol-gel liquid. [C6] [C7] In the above formulas (19) to (27), R is a methyl group or an ethyl group.
2. 2. The method for producing a water- and oil-repellent film-forming liquid composition according to claim 1, wherein the metal oxide particles (B) are oxide particles of one or two metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.
3. 2. The method for producing a water- and oil-repellent film-forming liquid composition according to claim 1, wherein the silica sol-gel (C) contains 0.5% by mass to 20% by mass of an alkylene group component having 2 to 7 carbon atoms, when the silica sol-gel is taken as 100% by mass.
4. 2. The method for producing a water- and oil-repellent film-forming liquid composition according to claim 1, wherein the solvent (D) is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms, and an organic solvent other than the alcohol.
5. 2. The method for producing a water- and oil-repellent film-forming liquid composition according to claim 1, wherein the dispersion of the fluorine-containing metal oxide particles is prepared by adding and mixing a fluorine-based compound (A) to a dispersion of the metal oxide particles (B), and then adding and mixing water and a catalyst to the mixture.
6. 2. The method for producing a water- and oil-repellent film-forming liquid composition according to claim 1, wherein the silica sol-gel liquid is prepared by adding a catalyst to a mixture of silicon alkoxide, alcohol and water.
Citation Information
Patent Citations
Water-repellent film
JP2009154480A
Polyfluorine-containing siloxane coating
JP2016537484A
Fluoroalkylsilane and coatings derived therefrom
JP2016539085A
Fluorine-containing nanocomposite particle and method for producing the same, and coating agent, oil water separation film and resin composition containing the same