Oil sorbent sheet made of biodegradable fibers

A biodegradable cellulose-based oil adsorbent with silicone treatment and optional nonwoven laminates addresses the lack of strength and buoyancy in existing materials, providing effective oil absorption and reducing marine pollution.

JP7596120B2Active Publication Date: 2024-12-09ASAHI KASEI ADVANCE CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020184314
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-04
Publication Date
2024-12-09
Estimated Expiration
2040-11-04

AI Technical Summary

Technical Problem

Conventional sheet-like oil absorbing materials are not made from 100% biodegradable fibers, lack strength and buoyancy, and often contain synthetic fibers that contribute to marine pollution, posing an environmental burden throughout their life cycle.

Method used

A sheet-like oil adsorbent made of recycled cellulose fibers treated with a silicone water-repellent agent and optionally laminated with biodegradable nonwoven fabric, ensuring high oil adsorption capacity and buoyancy without synthetic materials.

Benefits of technology

The adsorbent effectively adsorbs oil, maintains buoyancy, and minimizes environmental impact by being fully biodegradable, addressing marine pollution concerns and reducing microplastic contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596120000001
    Figure 0007596120000001
Patent Text Reader

Abstract

To provide an oil adsorbent which does not cause a microplastic problem in marine environment, is few in load on environment in the whole life cycle from production to disposal and contributes to environment conservation.SOLUTION: A sheet-like oil adsorbent comprising a biodegradable fiber is characterized in that when inserting a test piece in a fresh water-charged container in a precipitation test based on the acceptance test standard of National Land and transportation Ministry, and applying to the container, a horizontal oscillation of 120 times reciprocation per minute with 4 cm amplitude for 60 hours, a part of the test piece exists on a water level; and when calculating how many times of the dead weight of the test piece is adsorbed by the oil adsorption amount obtained by subtracting the dead weight of the test piece from the weight thereof by: floating the test piece on the oil levels in the baths filled with salad oil, machine oil and diesel oil, respectively in an oil adsorption performance test based on the above acceptance test standard; standing the test piece for 5 minutes; and placing the test piece taken out of the oil on a mesh and standing for 5 minutes, the oil adsorption amount is 8 g or more, and the oil of 6 times or more of the test piece dead weight is adsorbed.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet-shaped oil sorbent made of biodegradable fibers that floats on water and has high oil adsorption performance. More specifically, the present invention relates to a sheet-shaped oil sorbent made of remnants of cellulose fibers, preferably cellulose fiber, having a buoyancy component attached to the surface of the fibers. [Background technology]

[0002] In recent years, as petroleum consumption increases, serious marine pollution accidents caused by oil are becoming more and more prevalent, and oil spills caused by floods, earthquakes, tsunamis, etc. are becoming more frequent. In addition, as the amount of suspended oil in industrial wastewater increases, it is becoming more difficult to technically treat wastewater such as activated sludge. Under these circumstances, a wide variety of sheet-shaped (harbor) oil sorbents are commercially available. These oil sorbents are made of a mixture of natural cotton, kapok fiber, polyester fiber, polypropylene fiber, etc. as the main material, and are generally 4mm to 8mm thick, 37 to 75cm x 50 to 65cm in size per sheet, and 1.1 to 4.0L (per sheet) in oil absorption capacity. However, the main material of these commercially available sheet-type oil adsorbents is not made of 100% biodegradable fibers, nor are they made of 100% unused fibers.

[0003] The following Patent Document 1 discloses a sheet-shaped oil sorbent consisting of kapok fiber, cotton fiber, and polypropylene or polyester heat-melting fiber, the kapok fiber and cotton fiber being bonded and fixed by the heat-melting fiber. The purpose of the sheet-shaped oil sorbent disclosed in Patent Document 1 is to provide a sheet-shaped oil sorbent that is inexpensive, does not scatter kapok fiber, and has sufficient strength after use, in a situation where serious marine pollution by oil continues to expand with the increase in petroleum consumption, and where the technical treatment of wastewater such as activated sludge is becoming difficult with the increase in suspended oil in industrial wastewater, especially food and livestock wastewater. Although kapok fiber has excellent oil absorption, it is difficult to process and has no stiffness, which makes it inconvenient to use, so inexpensive cotton fiber with a fiber length of 20 to 40 mm is used, and the kapok fiber and cotton fiber are bonded and fixed with heat-melting fiber so that the fiber entanglement is good and the adsorption amount does not decrease even if the needle punching process is omitted, and the heat-melting fiber is attached to the front and back surfaces of the sheet-like oil adsorbent, and the front and back surfaces are sewn around and diagonally with cotton thread, etc. Patent Document 1 recommends that the surface of polyester fiber is generally hydrophilic and therefore that it be rendered lipophilic by a water-repellent treatment, but does not disclose the water-repellent treatment of kapok fiber or cotton fiber, which are natural fibers.

[0004] The following Patent Document 2 discloses a sheet-like hybrid adsorbent for recovering oil and radioactive substances contained in contaminated water, which comprises a radioactive substance adsorption layer containing activated carbon and / or zeolite and adsorbing radioactive substances in contaminated water, a surface nonwoven fabric covering the surface of the radioactive substance adsorption layer and containing absorbent cotton for absorbing contaminated water, and a back nonwoven fabric covering the back side of the radioactive substance adsorption layer and containing wool for absorbing oil in the contaminated water. It also discloses that the surface of the surface nonwoven fabric is further covered with a PP nonwoven fabric. The sheet-type hybrid adsorbent disclosed in Patent Document 2 has a problem that when radioactive materials from contaminated water containing oil are adsorbed onto an adsorbent, if the adsorbent containing activated carbon is exposed, the oil in the contaminated water blocks the adsorption holes in the adsorbent sheet, preventing the contaminated water from passing through to the adsorbent. Even if the activated carbon layer is covered with a liquid-permeable layer made of hydrophobic fibers such as polyethylene or polypropylene, the oil contained in the contaminated water blocks the passage holes in the liquid-permeable layer, preventing the contaminated water from passing through to the activated carbon layer located inside the liquid-permeable layer. To solve this problem, three types have been proposed depending on the amount of oil that has spilled onto the sea surface.

[0005] The first type is a type in which the surface nonwoven fabric is made of absorbent cotton and PP nonwoven fabric, and the back nonwoven fabric is made of wool nonwoven fabric. When almost no oil is found on the surface of the contaminated water, absorbent cotton has high water absorption, wool has excellent breathability and low specific gravity, and can float on the water surface for a long time even after absorbing a small amount of oil. Therefore, when no oil film is found on the surface of the contaminated water, the surface nonwoven fabric made of absorbent cotton is dropped into the contaminated water with the surface nonwoven fabric facing down, and the contaminated water is instantly absorbed by the surface nonwoven fabric, and the radioactive material in the contaminated water is adsorbed by the radioactive material absorption layer. Also, when a very small amount of oil film is found on the surface of the contaminated water, the back nonwoven fabric made of wool nonwoven fabric is dropped into the contaminated water with the back nonwoven fabric facing down, and the oil in the contaminated water is removed by the back nonwoven fabric, and then the contaminated water is passed through the radioactive material absorption layer (i.e., only the contaminated water from which the oil has been removed is brought into contact with the radioactive material adsorption layer). It is also stated that absorbent cotton has a much faster water absorption rate than wool, and that wool is harder and more water repellent than absorbent cotton. The second type has both the front and back nonwoven fabrics made of wool, and is suitable for cases where oil has been found on the surface of the contaminated water. The third type has both the front and back nonwoven fabrics made primarily of kapok fiber, and is suitable for cases where a large amount of oil has been found on the surface of the contaminated water. Patent Document 2 also states that kapok fiber is a fiber derived from the Bombaceae ( Bombaceae It is a seed fiber of a plant belonging to the family Polysaccharides, and contains cellulose, lignin, and pentosan. Kapok fiber itself is composed of one cell, and since the cell wall is thin but the lumen is thick, it has air bubbles inside, so its specific gravity is extremely light, for example, 0.038 for kapok fiber from Java and 0.05 for kapok fiber from India, and it is described that it can float on the water surface even if it is increased to 20 to 40 times its own weight, and has a high oil absorption capacity of about 50 times per gram of material. By covering the radioactive material layer with kapok fiber, which has such a light specific gravity and high oil absorption capacity, the hybrid adsorbent sheet can be made to float on the surface of the contaminated water for a long time and can adsorb a large amount of oil in the contaminated water.

[0006] Patent Document 2 describes a method in which activated carbon is spread on a back nonwoven fabric, a front nonwoven fabric is placed on top of that, and the fibers are then entangled with each other using a needle punching device to integrally entangle the front nonwoven fabric, back nonwoven fabric, and radioactive substance adsorption layer. Patent Document 2 does not disclose the water repellent treatment of natural fibers such as absorbent cotton, wool, and kapok fiber.

[0007] In recent years, marine pollution by microplastics has become a global social issue, and under the circumstances where there are concerns about the impact on ecosystems, synthetic fiber waste is considered to be one of the sources of microplastics. Therefore, from the viewpoint of environmental conservation, there is a demand for oil adsorbents that do not contain synthetic fibers.

[0008] Under these circumstances, there is still a need to provide an oil sorbent with high oil absorption performance that does not cause the microplastic problem in marine pollution, imposes little burden on the environment throughout its entire life cycle from "production" to "disposal," and is useful for environmental conservation. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 4-161289 [Patent Document 2] Patent No. 5759265 Summary of the Invention [Problem to be solved by the invention]

[0010] As a sheet-like oil absorbent of the prior art, there is a commercially available product using cotton fiber. Generally, the fiber length of cotton is classified into short fiber cotton (21 mm or less), medium fiber cotton (21 mm to less than 28 mm), long fiber cotton (28 mm or more), and extra long fiber cotton (35 mm or more). These commercially available products use cotton with a short fiber length of 21 mm to 28 mm, which is difficult to tangle. If you try to obtain reeled cotton using only short fiber lengths like this, it will be difficult to maintain the cohesion when made into a sheet, so it is necessary to mix synthetic fibers such as polyester fiber and polypropylene (PP) fiber, which are not biodegradable fibers, or to press the front and back with nonwoven fabrics made of these synthetic fibers. On the other hand, if extra long fiber cotton (35 mm or more) is used, it may be possible to obtain reeled cotton, but the cost will be high. Therefore, for example, the product manufactured by Hashimoto Cross Co., Ltd. used in Comparative Example 4 described below is a sheet made of a blend of rayon and polyester short fiber. Also, there are some that have a structure in which cotton fiber batting is sandwiched between polyester or PP nonwoven fabric that can provide buoyancy and binding power. However, it seems that there are no sheet-type oil sorbents made of 100% biodegradable fibers on the market at present. Even if a sheet-type oil sorbent made of 100% biodegradable fibers is known, it is likely that the strength of the sheet-type oil sorbent will be insufficient, and if a water repellent or oil agent is not added as a buoyancy component, it will sink in water and will not be able to float on the water surface, and therefore it is considered that it would not function as a sheet-type oil sorbent. In view of the above-mentioned state of the art, the problem that the present invention aims to solve is to provide an oil sorbent that does not cause the microplastic problem in marine pollution, imposes little burden on the environment throughout its entire life cycle from "production" to "disposal," and is useful for environmental conservation. [Means for solving the problem]

[0011] As a result of intensive research and repeated experiments to solve the above-mentioned problems, the inventors unexpectedly discovered that the above-mentioned problems can be solved, preferably by needle punching cellulose fiber wool to form a nonwoven fabric of a predetermined thickness, and then immersing this in a water-repellent solution of a predetermined concentration to form a sheet-shaped oil adsorbent, and thus completed the present invention.

[0012] That is, the present invention is as follows. [1] A sheet-like oil sorbent made of biodegradable fibers, characterized in that in a sedimentation test conforming to the Ministry of Land, Infrastructure, Transport and Tourism's type approval test standards, when a 5 cm square test piece is placed in a container containing 300 mL of clean water and horizontally vibrated at 120 reciprocations per minute with an amplitude of 4 cm for 60 minutes, a part of the test piece is above the water surface, and in an oil adsorption performance test conforming to the Ministry of Land, Infrastructure, Transport and Tourism's type approval test standards, a 10 cm square test piece is floated on the oil surface of a bath filled with salad oil, machine oil, and light oil, respectively, and left to stand for 5 minutes, then removed, placed on a wire mesh, and left for 5 minutes, the oil adsorption amount is calculated by subtracting the test piece's own weight from the weight of the test piece, and when calculating how many times the test piece's own weight the test piece has adsorbed, the oil adsorption amount is 8 g or more for each of the above test oils and is at least 6 times its own weight. [2] The sheet-shaped oil adsorbent according to [1], wherein the biodegradable fibers are cellulose fibers. [3] The sheet-shaped oil adsorbent according to [1] or [2], wherein a buoyancy component is attached to the surface of the biodegradable fiber. [4] The sheet-like oil adsorbent material according to any one of [1] to [3] above, which is made of cellulose fiber pulp that has been treated to be water repellent with a silicone-based water repellent agent. [5] The sheet-shaped oil adsorbent according to [4], wherein the water repellent is a silicone-based water repellent. [6] The sheet-shaped oil adsorbent material according to [4] or [5], wherein the cellulose fiber ream is a ream derived from a cellulose nonwoven fabric and cellulose yarn. [7] The sheet-like oil adsorbent material according to [6], wherein the ream of cotton derived from the cellulose nonwoven fabric and cellulose yarn is obtained by reaming cellulose nonwoven fabric and cellulose yarn (cellulose nonwoven fabric:cellulose yarn) in a weight ratio of 10:90 to 60:40. [8] The sheet-shaped oil adsorbent according to any one of the above [2] to [7], wherein the cellulose fibers are mixed with vegetable fibers. [9] 250g / m 2 More than 450g / m 2 The sheet-like oil adsorbent according to any one of the above [1] to [8], having a basis weight of 3.5 mm or more and a thickness of 3.5 mm or more and 6.5 mm or less.

[10] A sheet-like oil adsorbent according to any one of [1] to [9], wherein in measuring the single fiber length of the biodegradable fibers constituting the oil adsorbent, 30% or more and less than 90% of the total number of fibers used in the measurement are fibers having a single fiber length of 50 mm or more.

[11] The sheet-like oil adsorbent material according to any one of [2] to

[10] , wherein the front and back surfaces of the sheet made of cellulose fiber batting are laminated with biodegradable nonwoven fabric.

[12] The process of: A step of defatting the cellulose nonwoven fabric and the cellulose yarn in a weight ratio of cellulose nonwoven fabric:cellulose yarn=10:90 to 60:40 to obtain defatted cotton; A step of needle punching the obtained recycled cotton into a nonwoven fabric of a predetermined thickness; A step of dipping the obtained nonwoven fabric into a water repellent solution of a predetermined concentration and then drying it to form a sheet-like product; and If desired, a step of laminating a biodegradable nonwoven fabric on both sides of the obtained sheet-like material; A method for producing the sheet-shaped oil adsorbent according to any one of the above [7] to

[11] , comprising: Effect of the Invention

[0013] The sheet-shaped oil sorbent of the present invention is an oil sorbent that does not cause the microplastics problem in marine pollution, imposes little burden on the environment throughout its entire life cycle from "production" to "disposal," and is useful for environmental conservation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail. Note that the present invention is not limited to the following embodiment, and can be practiced in various modifications within the scope of the present invention.

[0015] One embodiment of the present invention is a sheet-like oil adsorbent made of biodegradable fibers, characterized in that in a sedimentation test conforming to the Ministry of Land, Infrastructure, Transport and Tourism type approval test standard, when a 5 cm square test piece is placed in a container containing 300 mL of clean water and horizontal vibration is applied at 120 reciprocations per minute with an amplitude of 4 cm for 60 minutes, a part of the test piece is above the water surface, and in an oil adsorption performance test conforming to the Ministry of Land, Infrastructure, Transport and Tourism type approval test standard, a 10 cm square test piece is floated on the oil surface of a bath filled with salad oil, machine oil, and light oil, respectively, and left to stand for 5 minutes, and then removed and placed on a wire mesh and left for 5 minutes, the weight of the test piece is subtracted from its own weight to determine the oil adsorption amount, and when calculating how many times the own weight of the test piece has been adsorbed, the oil adsorption amount for each of the above test oils is 8 g / g or more and is 6 times or more of its own weight. In the above-mentioned sedimentation test, it is preferable that a part of the test piece remains above the water surface even when the test piece is subjected to continuous vibration for 24 hours.

[0016] A preferred aspect of this embodiment is the sheet-like oil adsorbent using cellulose fibers as the biodegradable fibers and having a buoyancy component attached to the surface thereof, and more preferably, the sheet-like oil adsorbent is made of regenerated cellulose fiber pulp that has been treated for water repellency with a silicone-based water repellent agent. The cellulose fibers are preferably pulp, and the cellulose fiber pulp is more preferably pulp derived from a cellulose nonwoven fabric and cellulose yarn.

[0017] In this specification, the term "cellulose fibers" includes plant fibers such as cotton, bast, banana, and kapok, and "regenerated cellulose fibers" (rayon, polynosic, cupra, tencel, lyocell, etc.) artificially produced by dissolving natural cellulose such as trees, pulp, and cotton linters, and further includes semi-synthetic fibers (acetate, etc.) made from cellulose as a raw material. In this embodiment, the cellulose fibers may be mixed with vegetable fibers.

[0018] Cotton linters are the downy hairs around cotton seeds and are unused fibers that are not used for cotton thread. After washing, they are repeatedly steamed and filtered to remove impurities, producing refined linters. These are then refined and dissolved in a cuprammonium solution (Schweitzer solution, which turns a deep blue due to the cuprammonium complex) made by adding sodium hydroxide to an aqueous solution of copper sulfate to cause precipitation of copper hydroxide (II), and then adding aqueous ammonia to dissolve cellulose, to produce a liquid (undiluted solution). This is then extruded into acidic water to spin (regenerate) the cellulose, and the cellulose is transformed into 100% regenerated fiber, to produce cupra yarn (Bemberg (registered trademark), long fiber, short fiber) and cupra long fiber nonwoven fabric (Bemliese (registered trademark)). Bemberg (registered trademark) is a clothing fiber that has a nearly perfectly circular cross section and a smooth surface, which means it is less irritating to the skin, reduces friction and allows for smoother body movement, and has beautiful colors, luster and a unique texture.In addition, compared to cotton fiber, it has a large amount of amorphous parts that absorb moisture easily and release it easily, making it an excellent moisture absorbing and releasing fiber, creating a comfortable clothing environment. The water absorption rate of cupra yarn is approximately 11 times its own weight.

[0019] In addition, Bemliese (registered trademark) is used in face masks and puffs, gauze and disinfectant wet wipes, industrial wipes, greening materials, tea bags, hand towels, etc. due to its low dust generation (lint-free), excellent liquid absorption, heat resistance, wiping ability and low impurity content. As mentioned above, these cupra yarns and cupra long fiber and / or short fiber nonwoven fabrics are made from naturally derived cotton linters, and therefore are made of biodegradable fibers that decompose through natural processes even after being discarded after use. For example, if buried in the soil under summer conditions (temperature 35°C, humidity 80%), the weight of the raw fabric will be reduced to half in about two months, and even if burned, almost no harmful substances are produced. On the other hand, there is almost no weight change in polyester raw fabric.

[0020] In this specification, the term "regenerated cellulose fiber" includes rayon and lyocell in addition to the above-mentioned cupra. Rayon is a regenerated fiber made to resemble silk, and was formerly known as rayon (artificial silk thread). It is produced by dissolving cellulose such as pulp or cotton linters in alkali such as sodium hydroxide and carbon disulfide to turn it into viscose, which is then spun in acid (wet spinning). Unlike chemical fibers made from petroleum such as polyester, rayon itself is considered a fiber that does not put a strain on the environment, as it will return to the soil if buried after processing. However, problems such as the toxicity of carbon disulfide used in production and its low strength have been raised, and in Japan production has been discontinued because softwood pulp is used as raw material.

[0021] Lyocell is also a type of regenerated cellulose fiber, and is obtained by spinning a solution of cellulose itself dissolved in a solvent, without going through a process of derivatization like acetate fiber. Like rayon, the raw material is pulp from wood (such as eucalyptus). These are dissolved in an aqueous solution of N-methylmorpholine N-oxide to make a spinning solution (dope), which is then extruded into a dilute solution of N-methylmorpholine N-oxide to make fibers. Unlike the viscose method, which uses carbon disulfide, a completely closed system can be constructed, so the environmental impact is relatively low. Since Lyocell does not go through a process such as derivatization, there is little decrease in the degree of polymerization of the cellulose molecules, and it is excellent in terms of strength, but since the molecules are highly aligned in the long axis direction of the fiber during spinning, it is prone to the disadvantage of the fibers tearing (fibrillation) like string cheese.

[0022] The Eco Mark project is a project carried out by the Japan Environment Association, a public interest incorporated foundation, in accordance with the International Organization for Standardization's standards ISO14020 (Environmental labels and declarations, general principles) and ISO14024 (Environmental labels and declarations, Type I environmental labeling, principles and procedures). The Eco Mark is an environmental label given to products (goods and services) that are recognized as having low environmental impact throughout their entire life cycle, from "production" to "disposal," and as being useful for environmental conservation.

[0023] As mentioned above, cupra is made from the downy fuzz around cotton seeds, and is made from unused fibers that are not used for cotton yarn, so it has a smaller impact on the environment than rayon or lyocell.

[0024] In addition, the type approval system by the Ministry of Land, Infrastructure, Transport and Tourism is a system for streamlining inspections based on the provisions of the Ship Safety Act and the Act on Prevention of Marine Pollution and Maritime Disasters, and when identical types of objects are mass-produced, the system allows inspections to be conducted more efficiently by obtaining type approval. By obtaining type approval, manufacturers of oil sorbents undergo inspections (tests) to confirm that the objects they have manufactured are the same as the objects that have obtained type approval, and if they pass this, inspections for the items that have passed the test are omitted. If a material meets the test standards for performance testing under the type approval system set by the Ministry of Land, Infrastructure, Transport and Tourism, it can be said to have sufficient oil absorption properties and seat performance that can withstand practical use.

[0025] In order to achieve the desired performance, it is important that the sheet-type oil sorbent has oil adsorption capacity, buoyancy capacity, and strength. In a strength test based on the Ministry of Land, Infrastructure, Transport and Tourism type approval test standards, the strength is judged by hanging the oil sorbent from a hook with a diameter of 8 mm at a position 10 cm from any one end of the oil sorbent, and applying a load of 2.5 times the maximum unit weight calculated by a weight test to one point in the vertical direction. The criterion for judgment is whether or not the oil sorbent breaks after 3 minutes. It is preferable that the sheet-type oil sorbent of this embodiment satisfies this standard.

[0026] In the biodegradable fibers constituting the sheet-like oil sorbent of this embodiment, it is preferable that in the measurement of the monofilament length of the biodegradable fibers, 30% or more but less than 90% of the total number of fibers used in the measurement are fibers with a monofilament length of 50 mm or more. By mixing monofilaments with relatively long fiber lengths in this manner, a sheet-like material with excellent strength and buoyancy can be obtained. It is preferable that 40% or more of the total have a monofilament length of 50 mm or more, and more preferable that 50% or more of the total have a monofilament length of 50 mm or more, but it is not preferable from the viewpoint of the sheet molding process if 90% or more of the total have a monofilament length of 50 mm or more.

[0027] Furthermore, in the sheet-shaped oil sorbent made of biodegradable fibers of this embodiment, the cellulose fibers can be mixed with plant fibers, and it is preferable to use kapok fibers as at least one of the plant fibers. Kapok is a tree of the Bombacaceae family that grows widely, mainly in Southeast Asia, and is widely cultivated for the purpose of utilizing the fiber (fluff) extracted from its seeds. Kapok fiber is a plant fiber with a small environmental impact, with a single filament length of about 2 mm to 7 mm, and is characterized by being extremely light and dense, as well as having a highly hollow structure with a hollow ratio of about 80%. However, since the single filament length is short, the sheet processability and sheet strength are poor when used alone, and it is preferable to use it in a mixture with the above-mentioned fiber having a single filament length of 50 mm or more. The mixing ratio is not particularly limited, and it is sufficient that 50% or more of the total in the obtained sheet is made of fibers having a single filament length of 50 mm or more.

[0028] In the sheet-shaped oil adsorbent made of biodegradable fibers of this embodiment, it is preferable that a buoyancy component is attached to the surface of the biodegradable fibers. For example, it is difficult to obtain the necessary buoyancy with a sheet made of defatted cotton. Examples of the buoyancy component include oils and fats derived from plant fibers, oil components attached during spinning of regenerated fibers, etc., and water-repellent components attached during sheet formation or in a subsequent processing step. Examples of the water-repellent component include water-repellent agents, such as known fluorine-based water-repellent agents, silicone-based water-repellent agents, and acrylic-based water-repellent agents.

[0029] The sheet-shaped oil adsorbent of this embodiment can be obtained by forming a plant fiber with oil derived from a plant, for example, a cotton-like material made of undefatted cotton, into a sheet. As described above, in order to increase the ratio of fibers with a long single filament length, it is preferable to use special extra-long fiber cotton or to mix it with cellulose fibers other than cotton with a long single filament length, and these materials are obtained by forming them into a sheet shape by needle punching, chemical bonding, etc. If the buoyancy or strength is insufficient, it is preferable to further attach a buoyancy component or to attach another nonwoven fabric made of biodegradable fibers to the front and back of the sheet. However, from the viewpoint of oil adsorption performance, it is preferable to use a single-layer sheet without laminating nonwoven fabric on the front and back.

[0030] The sheet-like oil adsorbent of this embodiment can be obtained by forming the cellulose fibers into a sheet from the pulp obtained by pulping the cellulose fibers. The cellulose fibers may be either vegetable fibers or regenerated cellulose fibers, or a mixture of these may be used. The shape of the cellulose fibers may be spun or spun yarn, or may be a fiber structure such as a nonwoven fabric or a woven or knitted fabric, or may be a mixture of these. In addition, it is also possible to reuse defective products or scraps generated in the manufacturing process, such as fiber manufacturing, spinning, and nonwoven fabric or woven or knitted fabric manufacturing, and if the material is derived from such materials, it is particularly preferable in terms of environmental load.

[0031] Another embodiment of the present invention is a method for producing a method for manufacturing a semiconductor device comprising the steps of: A step of defatting the cellulose nonwoven fabric and the cellulose yarn in a weight ratio of cellulose nonwoven fabric:cellulose yarn=10:90 to 60:40 to obtain defatted cotton; A step of needle punching the obtained recycled cotton into a nonwoven fabric of a predetermined thickness; A step of dipping the obtained nonwoven fabric into a water repellent solution of a predetermined concentration and then drying it to form a sheet-like product; and If desired, a step of laminating a biodegradable nonwoven fabric on both sides of the obtained sheet-like material; The method for producing the sheet-shaped oil adsorbent comprises the steps of:

[0032] De-foaming is a recycling technology that converts textile waste into recyclable resources. It is a process that returns various forms of textile waste (thread, string, cloth, etc.) and scraps to a cotton-like state. In order to process it into thread or nonwoven fabric (felt) and reuse it, textile waste, etc. must be returned to cotton (de-foaming). De-foaming is, so to speak, the reverse operation of the process of manufacturing thread. In general, the de-foaming process is a series of steps: (1) cutting the raw material to an appropriate size, (2) stacking the raw material to reduce the variation between materials, (3) passing it through a de-foaming machine 6 to 8 times to make cotton, and (4) stuffing the de-foaming into a bag called a donta. The de-foaming machine is equipped with rotating blades of various shapes, such as for rough beating, medium beating, tekain, and garnet, and the properties of the de-foaming (fiber length and entanglement) change greatly depending on the processing conditions. Depending on the final product, such as for thread, felt raw material, or stuffing, these are combined to process it into de-foaming that meets the required performance. Basically, it is important to make the fibers as long as possible, to disentangle them well, and to minimize damage to the fibers.

[0033] A needle punching device generally has a beam with needles with sharp hubs protruding from the periphery embedded in a needle board at a predetermined interval and density. This beam is moved up and down by a drive device, and the needles are inserted into the sheet of rolled cotton and brought close to a receiving plate. This needle insertion action causes the hubs formed on the needles to hook the fibers and entangle the fibers with each other, making it possible to produce a nonwoven fabric of a predetermined thickness in which the fibers are integrally entangled.

[0034] In this embodiment, the density of the needles is 40,000 pieces / m 2 It is preferable to set the needles to about 5 mm apart in the needle board, because, although a denser density is generally more suitable for maintaining the strength of the entire material, if the density is too high, the fibers of the cellulose nonwoven fabric are cut too short, which actually reduces the strength of the resulting nonwoven fabric.

[0035] From the standpoint of the strength, thickness and fiber damage of the nonwoven fabric obtained by needle punching, it is preferable that the remnant batting derived from the cellulose nonwoven fabric and cellulose yarn is remnant in a weight ratio of cellulose nonwoven fabric and cellulose yarn (cellulose nonwoven fabric:cellulose yarn) of 10:90 to 60:40, more preferably 30:70 to 50:50. The fibers constituting the cellulose nonwoven fabric are finely chopped in the de-pilling and needle punching processes, and the length of the fibers themselves becomes shorter, but fragments of fibers that remain entangled in the fiber width direction remain, so the strength of the sheet-like material can be ensured. On the other hand, the cellulose yarns remain in a relatively long state even after the de-pilling and needle punching processes, so they are effective in ensuring the strength of the sheet-like material. Therefore, if the weight of the cellulose nonwoven fabric is 10% or more, damage to the fibers and a decrease in the strength of the nonwoven fabric can be suppressed, while if the weight of the cellulose yarns is 40% or more, damage to the fibers and a decrease in the strength of the nonwoven fabric can be similarly suppressed.

[0036] For example, when the cellulose nonwoven fabric is a cupra nonwoven fabric and the cellulose yarn is a cupra yarn, the fiber diameter of the fiber derived from the cupra nonwoven fabric in the fluff is preferably about 10 μm to about 15 μm and the fiber length is preferably about 1 cm to about 2 cm. Also, the fiber diameter of the fiber derived from the cupra yarn in the remnant fluff is preferably about 10 μm to about 15 μm and the fiber length is preferably about 3 cm to about 10 cm on average. In needle punching, it is essential to minimize damage to the fibers in the piece.

[0037] The nonwoven fabric obtained by needle punching has a fiber thickness of 250 g / m2 from the viewpoint of oil adhesion and buoyancy. 2 More than 450g / m 2 and a thickness of 3.5 mm to 6.5 mm, and 2 More than 450g / m 2 It is more preferable that the fiber has a basis weight of 4.5 mm or more and a thickness of 4.5 mm or more and 5.5 mm or less.

[0038] In this specification, the term "silicone-based water repellent agent" refers to a silicone in which the main chemical bond structure is a siloxane bond (Si-O-Si), and is not particularly limited as long as it forms a coating (oil film or hardened coating) on ​​fibers and exhibits water repellency. For example, it can be emulsion-type POLON-MK-206, which has excellent washability and is manufactured by Shin-Etsu Silicones Co., Ltd.

[0039] As mentioned above, the water absorption rate of cupra yarn is approximately 11 times its own weight, but the inventors of the present application unexpectedly discovered that by treating it with the silicone-based water repellent agent, it becomes able to selectively absorb oil over water, and that it becomes able to float on water, and based on this discovery, they have completed the present invention. In the process of immersing (dipping) the nonwoven fabric obtained through needle punching in a silicone-based water-repellent solution of a predetermined concentration, the concentration of the silicone-based water-repellent agent is preferably 3% to 6% from the viewpoint of the balance between oil adsorption capacity and water repellency (the degree to which the cupra yarn does not absorb water). EXAMPLES

[0040] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Measurement values ​​in the examples were determined by the following measurement methods.

[0041] [Oil adsorption performance test] In accordance with the test standards of the Ministry of Land, Infrastructure, Transport and Tourism's type approval system, performance tests of the sheet-type oil adsorbent were conducted using the following procedure. A 10cm square test piece is floated on the surface of a bath filled with each of the following test oils, left to stand for 5 minutes, then removed and placed on a wire mesh, left for 5 minutes, and then its weight is measured. Test piece: 10cm x 10cm / piece Test oil: salad oil (edible rapeseed oil), machine oil (ISO grade: 46), diesel (i) Measure the weight of one test piece (before absorbing oil). (ii) Place one test piece in the test oil and wait for 5 minutes. (iii) After that, take out the test piece and place it on a wire mesh, allowing the oil to drip off, for 5 minutes. (iv) Then, measure the weight (gross weight) of the test piece. The gross weight minus the weight of the test piece is the amount of oil adsorbed, and the number of times the weight of the test piece that the oil has been adsorbed is calculated. (v) Repeat the above three times (N=3). Products with an oil adsorption capacity of 8 g / l or more and absorbing more than six times their own weight were judged to pass.

[0042] [Sedimentation test] In accordance with the Ministry of Land, Infrastructure, Transport and Tourism's type approval test standards, the sedimentation test was carried out using the following procedure. A 5cm x 5cm test piece was placed in a reagent bottle containing 300mL of clean water and subjected to horizontal vibration at 120 strokes per minute with an amplitude of 4cm for 60 minutes, 24 hours, and 120 hours. If any part of the test piece was above the water surface, it was judged as passing (◯), i.e., floating on the water, and failing (×).

[0043] [Strength test] In accordance with the test standards of the Ministry of Land, Infrastructure, Transport and Tourism's type approval system, performance tests of the sheet-type oil adsorbent were conducted using the following procedure. An 8mm diameter hook was attached to any one end of the oil sorbent and hung 10cm from the hook, and a load of 2.5 times the maximum unit weight calculated by a weight test was applied to one point in the vertical direction. The criterion for judgment was whether or not there was any breakage after 3 minutes and 300 minutes. If there was no breakage, it was judged as "○", and if there was breakage, it was judged as "×". The maximum unit weight in this test was calculated as follows. A 10cm x 10cm test piece is immersed in heavy oil at 20 degrees Celsius for 5 minutes, and then left on a wire net for 5 minutes, after which its weight is measured and the total weight of the unit after absorbing oil is calculated. The same measurement is carried out for 3 samples, and the value of the sample with the heaviest weight is regarded as the maximum unit weight.

[0044] [Single yarn length measurement] Fibers were randomly extracted from an uncut area of ​​the sheet, attached to a mount so that they were almost straight, and their single-filament length was measured. 20 points were measured, and the percentage of single-filament lengths of 50 mm or more was calculated.

[0045] [Example 1] Commercially available, undegreased, medium-fiber cotton (single filament length 21-28 mm) was used and needle-punched to obtain a sheet-shaped nonwoven fabric with a thickness of 3 mm. A cellulose nonwoven fabric ("Benliese" manufactured by Asahi Kasei Corporation, thickness 1 mm, basis weight 28 g / m) that had been previously treated to be water repellent was used. 2 ) were stacked on top of each other, integrated by needle punching under the conditions below, and cut into 50 cm squares to obtain sheet-shaped oil adsorbents. Needle punch conditions: line speed 5 m / min, pre-punch rotation speed 450 rpm, double punch rotation speed 800 rpm.

[0046] [Example 2] Commercially available Tencel (LENZING, fineness 1.2 dtex) long fibers were roughly cut into average single fiber lengths of approximately 75 mm using a rotary blade cutter, and then charged into a mixing box and mixed with commercially available Kapok fibers in a weight ratio of 30:70 (Kapok:Tencel). The fibers were then turned into a cotton-like material using a wool recovery machine, and then made into sheets through carding and needle punching processes. The sheets were then cut into 50 cm square pieces to obtain sheet-form oil absorbents.

[0047] [Example 3] An oil adsorbent sheet was obtained in the same manner as in Example 2, except that the Tencel used in Example 2 was previously treated by immersing it in a commercially available silicone-based water repellent (5% solution) and then drying it.

[0048] [Example 4] Commercially available Bemberg yarn (manufactured by Asahi Kasei Corporation, fiber diameter 12 μm) and Bemliese nonwoven fabric (manufactured by Asahi Kasei Corporation, product number M-3II) were roughly cut into average single yarn lengths of approximately 75 mm using a rotary blade cutter, and then charged and mixed in a mixing box at a weight ratio of 50:50. The resulting mixture was then turned into a cotton-like material using a wool recovery machine, and then carded and needle-punched to form a sheet. The obtained sheet was immersed in a commercially available silicone-based water repellent (5% solution), dried, and then cut into a 50 cm square to obtain a sheet-like oil adsorbent.

[0049] [Example 5] A sheet-shaped oil adsorbent was obtained under the same conditions as in Example 4, except that in addition to Bemberg and Bemliese, commercially available kapok fiber was mixed so that the weight ratio of the three was 40:40:20.

[0050] [Comparative Example 1] A commercially available oil adsorbent sheet made of rayon and polyester (HOC-5052, manufactured by Hashimoto Cloth Co., Ltd.) was evaluated. It has the necessary performance as an oil adsorbent but is not biodegradable, i.e., it was rated as "X."

[0051] [Comparative Example 2] In Example 1, the sheet obtained by needle punching was cut as it was to prepare a sheet-shaped oil adsorbent. The strength was low and the performance as an oil adsorbent was insufficient.

[0052] The performance evaluation results of the samples obtained in the Examples and Comparative Examples are shown in the following Table 1. The single fiber length in Example 1 is the value for the constituent fiber of the nonwoven fabric sandwiched between both outer nonwoven fabric layers.

[0053] [Table 1] [Industrial Applicability]

[0054] The sheet-shaped oil sorbent according to the present invention is made of biodegradable fibers that do not contain synthetic fibers, and does not cause the microplastic problem in marine pollution, so it can be suitably used as an oil sorbent used to prevent marine pollution due to oil spill accidents such as heavy oil tanker grounding, and is scheduled to obtain type approval from the Ministry of Land, Infrastructure, Transport and Tourism. In addition, the sheet-shaped oil sorbent according to the present invention is preferably manufactured by rending off scraps in the production process of cupra nonwoven fabric (Bemliese (registered trademark)) and cupra yarn (Bemberg (registered trademark)) manufactured using unused cotton linters as a raw material, so it can be suitably used as an oil absorbing mat used to prevent workers from falling when oil splashes and makes the floor slippery around kitchen fryers or at factory manufacturing sites, and to clean dirt on the soles of shoes, and is scheduled to obtain the Eco Mark.

Claims

1. A sheet-shaped oil sorbent made of biodegradable fibers, in which, in a sedimentation test conforming to the Ministry of Land, Infrastructure, Transport and Tourism type approval test standard, when a 5 cm square test piece is placed in a container containing 300 mL of fresh water and horizontal vibration is applied at 120 reciprocations per minute with an amplitude of 4 cm for 60 minutes, a part of the test piece is above the water surface, and in an oil adsorption performance test conforming to the Ministry of Land, Infrastructure, Transport and Tourism type approval test standard, a 10 cm square test piece is floated on the oil surface of a bath filled with salad oil, machine oil, and light oil, respectively, and left to stand for 5 minutes, then removed, placed on a wire mesh, and left for 5 minutes, the weight of the test piece is subtracted from its own weight to obtain the oil adsorption amount, and when calculating how many times the test piece's own weight the test piece has adsorbed, the oil adsorption amount for each of the above test oils is 8 g or more and adsorbs at least 6 times its own weight, and the oil adsorption amount is 250 g / m 2 or more and 450 g / m 2 or more. and a thickness of 3.5 mm or more and 6.5 mm or less, and wherein, in measuring the single fiber length of the biodegradable fibers constituting the oil adsorbent, 30% or more and less than 90% of the total number of fibers used in the measurement are fibers having a single fiber length of 50 mm or more.

2. 2. The sheet-shaped oil adsorbent according to claim 1, wherein the biodegradable fibers are cellulose fibers.

3. 3. The sheet-shaped oil adsorbent according to claim 1 or 2, wherein a buoyancy component is attached to the surface of the biodegradable fibers.

4. 4. The sheet-like oil adsorbent according to claim 1, which comprises cellulose fiber pulp that has been treated to be water repellent with a silicone-based water repellent agent.

5. 5. The oil adsorbent sheet according to claim 4, wherein the water repellent is a silicone-based water repellent.

6. 6. The sheet-like oil adsorbent according to claim 4 or 5, wherein the cellulose fiber scrap is a scrap derived from a cellulose nonwoven fabric and cellulose yarn.

7. The sheet-like oil adsorbent according to claim 6, wherein the remnant cotton derived from the cellulose nonwoven fabric and the cellulose yarn is produced by remnant fiber of the cellulose nonwoven fabric and the cellulose yarn (cellulose nonwoven fabric:cellulose yarn) in a weight ratio of 10:90 to 60:

40.

8. 3. The sheet-shaped oil adsorbent according to claim 2, wherein the cellulose fibers are mixed with vegetable fibers.

9. 3. The sheet-like oil adsorbent according to claim 2, wherein the front and back surfaces of the sheet made of the cellulose fiber scraps are laminated with biodegradable nonwoven fabric.

10. The following steps: A step of recovering the fiber from the cellulose nonwoven fabric and the cellulose yarn in a weight ratio of cellulose nonwoven fabric:cellulose yarn=10:90 to 60:40 to obtain recovered fiber; A step of needle punching the obtained recycled cotton into a nonwoven fabric of a predetermined thickness; A step of dipping the obtained nonwoven fabric into a water repellent solution of a predetermined concentration and then drying it to form a sheet-like product; and If desired, a step of laminating a biodegradable nonwoven fabric on both sides of the obtained sheet-like material; The method for producing the sheet-shaped oil adsorbent according to any one of claims 7 to 9, comprising:

Citation Information

Patent Citations

  • JP1977051335U

  • Calculating system for mean velue of irregular data

    JP1982059265A

  • Sheetlike oil-adsorbing material

    JP1992161289A

  • Oil-absorbing cellulose yarn

    JP1993321139A

  • Oil absorbent

    JP1994023267A