Polymer, its production method, and resist resin composition
A polymer with p-hydroxystyrene and acetal-protected carboxylic acid units is produced using controlled deprotection, addressing sensitivity and resolution challenges in semiconductor lithography while ensuring storage stability.
Patent Information
- Application Number
- JP2021539241
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-09
- Filing Date
- 2020-08-06
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-08-06
AI Technical Summary
Existing polymers used in semiconductor lithography face challenges in achieving high sensitivity and resolution while maintaining storage stability, particularly when using p-hydroxystyrene units due to issues like polymerization during storage and unwanted changes in solubility and film loss during development.
A polymer containing structural units derived from p-hydroxystyrene and carboxylic acid protected with an acetal group is produced through a deprotection reaction at controlled temperatures using specific bases with a pKa of 12 or more, ensuring minimal migration of the acetal group and maintaining polymer stability.
The resulting polymer exhibits high sensitivity, resolution, and improved storage stability, suitable for chemically amplified resists, with controlled acetal group elimination to prevent unwanted by-products.
Smart Images

Figure 0007596275000001 
Figure 0007596275000002 
Figure 0007596275000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer and a method for producing the same. More specifically, the present invention relates to a polymer containing a structural unit derived from p-hydroxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group, and a method for producing the same. Furthermore, the present invention relates to a resist resin composition containing the polymer. [Background technology]
[0002] Conventionally, in the manufacturing process of semiconductor devices such as ICs and LSIs, microfabrication is carried out by lithography using a photoresist composition. In recent years, with the increasing integration of integrated circuits, there has been a demand for the formation of ultrafine patterns in the submicron and quarter-micron regions, and exposure light sources have shifted from g-line and i-line to KrF excimer lasers and ArF excimer lasers with shorter wavelengths in the mass production of semiconductors. Furthermore, the development of lithography techniques using electron beams, X-rays, or extreme ultraviolet rays (EUV) is currently underway.
[0003] Lithography using electron beams, X-rays, or EUV is considered to be the next-generation or next-next-generation pattern formation technology, and resist compositions with high sensitivity and high resolution are desired. In particular, increasing the sensitivity of resists is a very important issue in order to shorten wafer processing time, but there is a trade-off between sensitivity and resolution, and there is a strong demand for the development of resist compositions that simultaneously satisfy both of these characteristics.
[0004] Patent Document 1 proposes a polymer containing a structural unit having a phenolic hydroxyl group and a structural unit having a structure in which a carboxylic acid is protected by an acetal group as a resist polymer for lithography using an electron beam or EUV. The polymer is synthesized by directly polymerizing a monomer having a phenolic hydroxyl group (e.g., p-hydroxystyrene or 4-hydroxyphenyl methacrylate) and a monomer having a structure in which a carboxylic acid is protected by an acetal group. However, it is known that p-hydroxystyrene has low stability and can cause problems such as polymerization during storage (Non-Patent Document 1), making industrial-scale production by the above method difficult.
[0005] Other known methods for producing polymers having p-hydroxystyrene units include a method in which tert-butoxystyrene or acetoxystyrene, instead of p-hydroxystyrene, is used as a raw material for polymerization, and then the tert-butyl group or acetyl group is eliminated (Patent Document 2 and Patent Document 3).
[0006] In general, base resins for chemically amplified resists have a structure in which acidic groups such as carboxyl groups are protected with a protecting group that is released by the action of acid (hereinafter referred to as an acid-removable group). As described above, when synthesizing a copolymer containing p-hydroxystyrene units and structural units having an acid-removable group using tertiary butoxystyrene or acetoxystyrene as a starting material, it is necessary to remove only the protecting group of the hydroxystyrene in the deprotection step after polymerization, while maintaining the other structures having the acid-removable group. If the acid-leaving group is eliminated, the portion in which the solubility of the resin in the developer changes due to exposure will decrease, and the development contrast between the exposed and unexposed portions will become smaller, and strong acids such as carboxylic acids will be generated in the polymer due to the elimination of the acid-leaving group, which may cause problems such as a large film loss in the unexposed portions during alkaline development. In addition, there is a concern that the storage stability of the polymer will deteriorate due to the carboxylic acids generated in the polymer.
[0007] Patent Document 4 discloses a method for removing the acyl group in a shorter time in a deprotection reaction of a polymer containing a unit structure having a phenolic hydroxyl group protected by an acyl group while preserving other partial structures, in which a deprotection reagent selected from primary or secondary amine compounds having a ClogP value of 1.00 or less (with the proviso that in the secondary amine compound, neither of the two carbon atoms bonded to the nitrogen atom of the amino group is tertiary) is used. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent Publication No. 2014-41328 [Patent Document 2] Japanese Patent Publication No. 04-211258 [Patent Document 3] Japanese Patent Application Publication No. 10-186665 [Patent Document 4] Patent Publication No. 2011-102386 [Non-patent literature]
[0009] [Non-Patent Document 1] Vinylphenol Basics and Applications (by Maruzen Petrochemical Co., Ltd.) Summary of the Invention [Problem to be solved by the invention]
[0010] However, the deprotection method described in Patent Document 4 has been confirmed to be effective for polymers in which the structure of an acid-leaving group is an ester structure derived from an aliphatic alcohol, and the method of Patent Document 4 is not sufficient for polymers containing a unit structure having an acetal-type acid-leaving group which has a lower activation energy in the elimination reaction and is more likely to be eliminated.
[0011] The present invention provides a polymer that contains a structural unit derived from p-hydroxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group, and in which the amount of structural units generated during the production process due to elimination or migration of the acetal group is extremely small, and a production method for the polymer. [Means for solving the problem]
[0012] As a result of intensive research to solve the above-mentioned problems, the present inventors have found that by subjecting a polymer containing a structural unit derived from p-acetoxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group to a deprotection reaction in an organic solvent in the presence of a base whose conjugated acid has a pKa of 12 or more at a temperature of 0°C to 50°C, it is possible to deprotect only the acyl group of the acetoxystyrene unit while suppressing elimination or migration of the acetal group, and have completed the present invention.
[0013] That is, according to the present invention, the following inventions are provided. [1] A method for producing a polymer containing a structural unit derived from p-hydroxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group, comprising the steps of: The production method is characterized in that a polymer containing a structural unit derived from p-acetoxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group is subjected to a deprotection reaction in an organic solvent in the presence of a base whose conjugated acid has a pKa of 12 or more at a temperature in the range of 0°C to 50°C, thereby converting the structural unit derived from p-acetoxystyrene in the polymer into a structural unit derived from p-hydroxystyrene. [2] The structural unit having a structure in which a carboxylic acid is protected with an acetal group is represented by the formula (II): [ka] (In formula (II), R 1 represents a hydrogen atom or a methyl group, and R 2 R represents an alkyl group having 1 to 10 carbon atoms. 3represents an alkyl group having 1 to 15 carbon atoms, a saturated aliphatic cyclic group having 5 to 15 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkylaryl group having 7 to 15 carbon atoms, or an aralkyl group having 7 to 15 carbon atoms. 2 and R 3 is combined with R 3 may form a 5- to 8-membered heterocyclic group together with the oxygen atom to which it is bonded. [3] The method for producing a polymer according to [1] or [2], wherein the base having a pKa of 12 or more is at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, sodium methoxide, potassium methoxide, and diazabicycloundecene. [4] The method for producing a polymer according to any one of [1] to [3], wherein the organic solvent used in the deprotection reaction is at least one selected from the group consisting of methanol, ethanol, isopropanol, propylene glycol monomethyl ether, methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, methyl propionate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, and propylene glycol monomethyl ether acetate. [5] The method for producing a polymer according to any one of [1] to [4], wherein the deprotection reaction is carried out at a temperature within the range of 20°C to 50°C. [6] Formula (I): [ka] and structural units represented by formula (II): [ka] (In formula (II), R 1 represents a hydrogen atom or a methyl group, and R 2 R represents an alkyl group having 1 to 10 carbon atoms. 3 represents an alkyl group having 1 to 15 carbon atoms, a saturated aliphatic cyclic group having 5 to 15 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkylaryl group having 7 to 15 carbon atoms, or an aralkyl group having 7 to 15 carbon atoms. 2 and R 3is combined with R 3 may form a 5- to 8-membered heterocyclic group together with the oxygen atom to which it is bonded. [ka] (In formula (III), R 1 is R of formula (II) 1 (IV): [ka] (In formula (IV), R 2 and R 3 is R of formula (II) 2 and R 3 (1) is 1 mol % or less relative to 100 mol % of the total of all structural units. [7] A resin composition for a resist comprising the polymer according to [6]. Effect of the Invention
[0014] According to the present invention, it is possible to produce a polymer that contains a structural unit derived from p-hydroxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group, and has an extremely small amount of structural units generated by elimination and migration of the acetal group. Furthermore, the polymer is useful as a polymer for a chemically amplified resist having high sensitivity, high resolution, and good storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] [Method of producing polymer] The polymer produced by the production method of the present invention is a polymer containing a structural unit derived from p-hydroxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group.
[0016] The structural unit derived from p-hydroxystyrene is represented by the following formula (I). [ka]
[0017] The proportion of the structural unit represented by formula (I) contained in the polymer is preferably 1 mol % or more and 99 mol % or less, more preferably 10 mol % or more and 90 mol % or less, and even more preferably more than 30 mol % and 70 mol % or less, relative to 100 mol % in total of all structural units.
[0018] The structural unit having a structure in which a carboxylic acid is protected by an acetal group is not particularly limited, and examples thereof include structural units generated by vinyl addition polymerization of a monomer in which a carboxyl group, such as acrylic acid, methacrylic acid, or 5-norbornene-2-carboxylic acid, is protected by an acetal. A structural unit derived from an acetalized product of acrylic acid or methacrylic acid is preferred. In particular, a structural unit represented by the following formula (II) is preferred.
[0019] [ka]
[0020] In formula (II), R 1 represents a hydrogen atom or a methyl group. R 2 represents an alkyl group having 1 to 10 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group. R 3 represents an alkyl group having 1 to 15 carbon atoms, an aliphatic cyclic group having 5 to 15 carbon atoms, an aryl group having 6 to 15 carbon atoms, or an aralkyl group having 7 to 15 carbon atoms. 2 and R 3 are combined together to form R 3 may form a 5- to 8-membered heterocyclic group together with the oxygen atom to which it is bonded. The alkyl group preferably has 2 to 10 carbon atoms, more preferably 2 to 6 carbon atoms, and may be linear or branched. The aliphatic cyclic group preferably has 5 to 12 carbon atoms, and more preferably 5 to 10 carbon atoms. Specific examples of the aliphatic cyclic group include monocyclic groups such as a cyclopentyl group, a cyclohexyl group, and a cyclooctyl group, and groups in which one hydrogen atom has been removed from a polycyclic aliphatic compound such as norbornane, bicyclo[4.3.0]nonane, decalin, and adamantane. The aryl group preferably has 6 to 12 carbon atoms, more preferably 6 to 10 carbon atoms, and specific examples thereof include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and an anthracenyl group. The aralkyl group preferably has 7 to 13 carbon atoms, and more preferably has 7 to 11 carbon atoms. Specific examples thereof include a benzyl group, a phenylethyl group, a 2-phenyl-2-propyl group, a naphthylmethyl group, a naphthylethyl group, and a 2-naphthyl-2-propyl group. Also, R 2 and R 3 Specific examples of the heterocyclic group formed by bonding together include a tetrahydrofuranyl group, a tetrahydropyranyl group, an oxepanyl group, and an oxocanyl group.
[0021] The proportion of the structural unit represented by formula (II) contained in the polymer is preferably 1 mol % or more and 99 mol % or less, more preferably 10 mol % or more and 90 mol % or less, and even more preferably 30 mol % or more and less than 70 mol %, relative to 100 mol % in total of all structural units.
[0022] When the acetal moiety of the structural unit represented by formula (II) is eliminated, a structural unit represented by formula (III) is by-produced in the polymer. [ka]
[0023] In formula (III), R 1 is the same as in formula (II).
[0024] Furthermore, the eliminated acetal may bond with a phenolic hydroxyl group of a p-hydroxystyrene unit, resulting in the formation of a structural unit represented by formula (IV) as a by-product in the polymer. [ka]
[0025] In formula (IV), R 2 , R 3 The definition and preferred embodiments are the same as those of formula (II).
[0026] If the structural units represented by formula (III) or formula (IV) are produced as by-products in the polymer, the resist performance such as the development speed may deviate from the desired values. In addition, the elimination of the acetal-type protective group of the formula (II) unit may be further promoted under the influence of the carboxylic acid, which may impair the storage stability of the polymer, so the by-production of formula (III) or formula (IV) must be suppressed as much as possible. Preferably, the total proportion of the structural units represented by formula (III) or formula (IV) contained in the polymer is 1 mol% or less, more preferably 0.5 mol% or less, and even more preferably 0.1 mol% or less, relative to 100 mol% of the total of all structural units.
[0027] The method for producing a polymer of the present invention involves subjecting a structural unit derived from p-acetoxystyrene in a polymer containing a structural unit derived from p-acetoxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group to a deprotection reaction to convert the structural unit derived from p-acetoxystyrene to a structural unit derived from p-hydroxystyrene.
[0028] In the present invention, the polymer containing a structural unit derived from p-acetoxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group can also be obtained by polymerizing a monomer that is copolymerizable with at least p-acetoxystyrene and has a structure in which a carboxylic acid is protected with an acetal group. Examples of the monomer having a structure in which a carboxylic acid is protected with an acetal group include those represented by the following (ii).
[0029] [ka]
[0030] Formula (ii) is a monomer that provides the structural unit represented by formula (II), and in formula (ii), R 1 , R 2 , R 3 The definition and preferred embodiments are the same as those of formula (II).
[0031] The polymer of the present invention may also contain other structures. As a monomer that provides other structural units, various monomers used in known resist polymers can be used to adjust the solubility in resist solvents and lithography developers, etching resistance, substrate adhesion, etc. For example, styrene-based monomers derived from styrene, vinylnaphthalene, vinylanthracene, etc.; various (meth)acrylic acid ester-based monomers derived from acrylic acid and methacrylic acid; norbornene-based monomers derived from norbornene, tricyclodecene, tetracyclododecene, etc. Indene, acenaphthylene, etc. can also be copolymerized.
[0032] The weight average molecular weight (Mw) and dispersity (Mw / Mn) of the polymer of the present invention can be appropriately set according to the application, and are not particularly limited. For example, the weight average molecular weight (Mw) is preferably 1,000 to 100,000, more preferably 2,000 to 50,000, even more preferably 3,000 to 30,000, and even more preferably 5,000 to 15,000 from the viewpoint of expressing the polymeric property. Moreover, the dispersity (Mw / Mn) is preferably 1.1 to 2.0, more preferably 1.2 to 1.80, and even more preferably 1.3 to 1.7 from the viewpoint of uniforming the properties of the polymer. In the present invention, the weight average molecular weight (Mw) and dispersity (Mw / Mn) of the polymer are values measured by GPC (gel permeation chromatography) under the measurement conditions described below.
[0033] (Polymerization reaction) The polymerization reaction in the production method of the present invention is not particularly limited, and any conventionally known polymerization method such as radical polymerization, cationic polymerization, and living anionic polymerization can be used.
[0034] In the case of the radical polymerization method, the raw material monomer, the radical polymerization initiator, and if necessary, the chain transfer agent, etc. are dissolved in a solvent, and the mixture is heated and stirred, preferably under an inert gas atmosphere such as nitrogen. For example, the so-called batch polymerization method in which all raw materials such as the monomer, the polymerization initiator, the chain transfer agent, etc. are dissolved in a solvent and heated to the polymerization temperature, the method in which the monomer is dissolved in a solvent and heated to the polymerization temperature, and then the polymerization initiator, etc. are added, or the so-called drop polymerization method in which a solution in which the monomer and the polymerization initiator are dissolved in a solvent is dropped into a solvent heated to the polymerization temperature, can be carried out. Among them, the drop polymerization method is preferred because of its high reproducibility for each production lot, and the so-called independent drop method in which the monomer and the polymerization initiator, which is a radical generating source, are dropped separately is particularly preferred. The monomer, the polymerization initiator, the chain transfer agent, etc. can each be supplied in part in advance to the polymerization system. In the drop method, the monomer concentration and the radical concentration in the polymerization system can be adjusted by changing the composition of the monomer solution to be supplied and the supply speed of the monomer solution and the polymerization initiator, thereby controlling the dispersion degree and composition distribution of the copolymer to be produced.
[0035] The radical polymerization initiator may be a conventional one, for example, an azo-based polymerization initiator or a peroxide-based polymerization initiator. Specific examples of the azo-based polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 1,1'-azobis(cyclohexane-1-carbonitrile), and 4,4'-azobis(4-cyanovaleric acid). Azo-based compound polymerization initiators are preferred because they are safe to handle. Specific examples of peroxide-based polymerization initiators include decanoyl peroxide, lauroyl peroxide, benzoyl peroxide, bis(3,5,5-trimethylhexanoyl) peroxide, succinic acid peroxide, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxypivalate, and 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate. These polymerization initiators can be used alone or in combination. The amount of polymerization initiator used can be selected depending on the target molecular weight, the type of monomer, polymerization initiator, chain transfer agent, solvent, etc., the structural unit composition, the polymerization temperature, the dropping speed, etc.
[0036] The chain transfer agent may be any known chain transfer agent, as required. Among them, thiol compounds are preferred, and a wide range of known thiol compounds may be selected. Specific examples include t-dodecyl mercaptan, mercaptoethanol, mercaptoacetic acid, and mercaptopropionic acid. In addition, thiol compounds having a structure in which a 2-hydroxy-1,1,1,3,3,3-hexafluoro-2-propyl group is bonded to a saturated aliphatic hydrocarbon are particularly preferred because they have the effect of suppressing roughness and defects in lithography patterns. The amount of the chain transfer agent used may be selected according to the target molecular weight, the types of monomers, polymerization initiators, chain transfer agents, and solvents, the structural unit composition, the polymerization temperature, the dropping speed, and the like.
[0037] The solvent used in the polymerization reaction is not particularly limited as long as it is a solvent capable of stably dissolving the raw material monomers, the polymerization initiator, the chain transfer agent, and the polymerization reaction product. Specific examples of the polymerization solvent include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl isoamyl ketone, methyl amyl ketone, and cyclohexanone; alcohols such as methanol, ethanol, and isopropanol; ether alcohols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; esters such as methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, butyl acetate, methyl propionate, methyl lactate, and ethyl lactate; ether esters such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; ethers such as tetrahydrofuran, 1,4-dioxane, and ethylene glycol dimethyl ether; aromatic hydrocarbons such as toluene and xylene; N,N-dimethylformamide, and acetonitrile.
[0038] These may be used alone or in combination of two or more. In addition, compounds having a high boiling point and high solubility for monomers, polymerization initiators, chain transfer agents, and polymerization reaction products, such as ethylene glycol monobutyl ether, 3-methoxy-3-methyl-1-butanol, 3-methoxy-3-methyl-1-butyl acetate, ethyl 3-ethoxypropionate, γ-butyrolactone, diethylene glycol dimethyl ether, N-methylpyrrolidone, and dimethyl sulfoxide, may be used in combination.
[0039] There is no particular limit to the amount of the polymerization solvent used, but if the amount of the solvent used is too small, the monomer may precipitate or the viscosity may become too high, making it difficult to maintain the polymerization system uniform, while if the amount of the solvent used is too large, the conversion rate of the monomer may be insufficient or the molecular weight of the copolymer may not be increased to the desired value. Usually, the amount of the solvent is 0.5 to 20 parts by weight, preferably 1 to 10 parts by weight, per part by weight of the monomer.
[0040] In the dropping polymerization method, the amount of the solvent (hereinafter sometimes referred to as the initially charged solvent) charged in advance into the reaction tank may be equal to or greater than the minimum amount that allows stirring, but if it is greater than necessary, the amount of monomer solution that can be supplied decreases, which is undesirable since it reduces production efficiency. Usually, the volume ratio is selected from, for example, 1 / 30 or more, preferably 1 / 20 to 1 / 2, and particularly preferably 1 / 10 to 1 / 3, relative to the final charge amount (i.e., the total amount of the initially charged solvent, the monomer solution to be dropped, and the initiator solution). Note that a part of the monomer may be mixed in advance with the initially charged solvent.
[0041] In the dropping polymerization method, if the dropping time is short, the degree of dispersion tends to become broad, and a large amount of solution is dropped at once, which causes a drop in the temperature of the polymerization solution, and is therefore undesirable. Conversely, if the dropping time is long, the copolymer is subjected to more heat than necessary, and the productivity decreases, which is also undesirable. Therefore, the dropping time is usually selected from the range of 0.5 to 24 hours, preferably 1 to 12 hours, and particularly preferably 2 to 8 hours.
[0042] After the dropwise addition is completed and after the temperature is raised to the polymerization temperature in the batch heating method, it is preferable to maintain the temperature for a certain period of time or to further raise the temperature to perform aging, thereby reacting the remaining unreacted monomers. If the aging time is too long, the production efficiency per unit time decreases and the copolymer is subjected to more heat history than necessary, which is not preferable. Therefore, the aging time is usually selected within 12 hours, preferably within 6 hours, and particularly preferably within the range of 1 to 4 hours.
[0043] The polymerization temperature can be appropriately selected depending on the boiling points of the solvent, monomer, chain transfer agent, etc., the half-life temperature of the polymerization initiator, etc. At low temperatures, the polymerization does not proceed easily, which causes problems in productivity, and if the temperature is set higher than necessary, there is a problem in terms of the stability of the monomer and copolymer. Therefore, the polymerization temperature is preferably selected within the range of 40 to 160°C, and particularly preferably 60 to 120°C. The polymerization temperature has a large effect on the molecular weight and copolymer composition of the copolymer, so it needs to be precisely controlled. On the other hand, since the polymerization reaction is generally an exothermic reaction, the polymerization temperature tends to rise, so it is difficult to control it to a constant temperature. For this reason, in the present invention, it is preferable to contain at least one compound having a boiling point close to the target polymerization temperature as the polymerization solvent, and to set the polymerization temperature to be equal to or higher than the initial boiling point of the compound at the polymerization pressure. According to this method, the increase in the polymerization temperature can be suppressed by the latent heat of vaporization of the polymerization solvent.
[0044] The polymerization pressure is not particularly limited, and may be normal pressure, pressurized or reduced pressure, but is usually normal pressure. In the case of radical polymerization, when radicals are generated from an initiator, nitrogen gas is generated in the case of an azo system, and oxygen gas is generated in the case of a peroxide system, so that it is preferable to make the polymerization system an open system and perform the polymerization at near atmospheric pressure in order to suppress fluctuations in the polymerization pressure.
[0045] (purification) When the polymer used in the present invention contains impurities such as a solvent, unreacted monomers, oligomers, reaction by-products, etc., it may be further purified in order to remove these impurities or to obtain a polymer having a desired dispersity.
[0046] Specifically, the method is carried out by diluting a solution containing a polymer by adding a good solvent as necessary, and then contacting the solution with a poor solvent to precipitate the polymer and extract the impurities into the liquid phase (hereinafter referred to as precipitation purification), or by extracting the polymer into a liquid-liquid two-phase phase and the impurities into a poor solvent phase.
[0047] In the precipitation purification, the precipitated solid may be subjected to solid-liquid separation by a method such as filtration or decantation, and the solid may be further washed with a poor solvent, etc. The purification may be performed before or after the deprotection reaction.
[0048] The types and amounts of the poor solvent and good solvent used for purification are not particularly limited as long as the polymer can be separated from low molecular weight compounds, and can be appropriately selected depending on the solubility of the polymer in the poor solvent, the type and amount of the solvent used in the polymerization, the type and amount of impurities, etc.
[0049] The temperature during purification must be strictly controlled, since it greatly affects the molecular weight and dispersity of the polymer, and the removal rate of impurities such as residual monomers and initiator residues. If the purification temperature is too low, the solubility of impurities in the precipitation extraction treatment solvent and washing solvent will be insufficient, and the impurities will not be sufficiently removed, making it inefficient. Conversely, if the purification temperature is too high, the polymer will dissolve in the purification solvent, causing the composition balance in the low molecular weight region of the polymer to be lost and the yield to be reduced, which is not preferable. For this reason, purification is preferably carried out in the range of 0 to 80°C, preferably 0 to 60°C.
[0050] (Deprotection reaction) In the deprotection reaction of the present invention, it is essential that only the acetyl groups of the acetoxystyrene units in the copolymer are deprotected, while the acetal protecting groups of the units of formula (II) are not eliminated.
[0051] In the deprotection reaction of the present invention, a base with a conjugate acid pKa of 12 or more is used as a catalyst. The pKa here is basically a value in water at 25°C. The base with a conjugate acid pKa of 12 or more is not particularly limited, but specific examples thereof include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, alkali metal alkoxides such as sodium methoxide and potassium methoxide, diazabicycloundecene, diazabicyclononene, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 1,1,3,3-tetramethylguanidine. Among these, sodium hydroxide, potassium hydroxide, sodium methoxide, potassium methoxide, and diazabicycloundecene are preferred.
[0052] The amount of the base catalyst used varies depending on the type of base used and cannot be generally defined, but is usually 1 to 50 mol %, preferably 5 to 20 mol %, based on the number of moles of the acetyl group to be deprotected. If the amount of the base catalyst used is within the above range, a sufficient reaction rate is likely to be obtained.
[0053] The temperature of the deprotection reaction is in the range of 0 to 50° C., and preferably in the range of 20 to 50° C. If the reaction temperature is higher than this range, undesirable side reactions occur, such as elimination of the acetal group protecting the carboxylic acid and reaction of the eliminated acetal with the phenolic hydroxyl group of p-hydroxystyrene, while if the reaction temperature is lower than this range, the deprotection reaction takes a long time, which reduces productivity, and is therefore undesirable.
[0054] The solvent used in the deprotection reaction is not particularly limited as long as the copolymer before deprotection and the copolymer after deprotection are solvents. Specific examples of the solvent include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl isoamyl ketone, methyl amyl ketone, and cyclohexanone, alcohols such as methanol, ethanol, and isopropanol, ether alcohols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether, esters such as methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, butyl acetate, methyl propionate, methyl lactate, and ethyl lactate, ether esters such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate, ethers such as tetrahydrofuran, 1,4-dioxane, and ethylene glycol dimethyl ether, aromatic hydrocarbons such as toluene and xylene, N,N-dimethylformamide, and acetonitrile can be mentioned. Among these, methanol, ethanol, isopropanol, propylene glycol monomethyl ether, methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, methyl propionate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, and propylene glycol monomethyl ether acetate are preferred. These may be used alone or in combination of two or more.
[0055] After the deprotection reaction, an acid may be added to neutralize the base catalyst used in the deprotection reaction. However, attention must be paid to the type and amount of the acid added so that the acetal in the polymer is not eliminated. Specifically, a weak acid such as oxalic acid or acetic acid is used, and the amount added is 1 to 8 moles, preferably 2 to 3 moles, per mole of the base.
[0056] [Resin composition for resist] The polymer obtained by the manufacturing method of the present invention is useful as a base polymer for a resist resin composition. In addition to the polymer, the resist resin composition contains an acid generator, an acid diffusion inhibitor, and a solvent that dissolves them uniformly, and these may be conventionally known. Furthermore, the resist composition may contain, as necessary, compounds commonly used as resist additives, such as organic carboxylic acids and phosphorus oxo acids for preventing deterioration of the sensitivity of the acid generator and improving the shape and deposition stability of the resist pattern, additional resins for improving the performance of the resist film, surfactants for improving the coatability, dissolution inhibitors, plasticizers, stabilizers, colorants, antihalation agents, and dyes. EXAMPLES
[0057] Hereinafter, the present invention will be described in detail with reference to examples, but the present invention is not limited to these examples. In the following examples, parts are by weight unless otherwise specified.
[0058] The polymers in the present examples were analyzed as follows. [Weight average molecular weight / dispersity] The weight average molecular weight (Mw) and dispersity (Mw / Mn) of the polymer synthesized below were measured by GPC (gel permeation chromatography) using polystyrene as a standard. The analysis sample was prepared so that the solid content of the polymer was 2% by mass in tetrahydrofuran solution. The amount of sample injected into the apparatus was 50 μl. Measurement equipment: Tosoh HPLC-8220GPC Detector: Refractive index (RI) detector Column: Shodex GPC KF804 x 3 (Showa Denko) Eluent: Tetrahydrofuran Flow rate: 1.0mL / min Temperature: 40℃ Calibration curve: Created using polystyrene standard samples (manufactured by Tosoh)
[0059] [Polymer composition ratio (by-product content)] The composition ratio of the polymer synthesized below is 13 The polymer solution (2.0 g) after the deprotection reaction and the subsequent neutralization reaction and 0.1 g of Cr(III) acetylacetonate were dissolved in 1.0 g of deuterated acetone to prepare a sample for analysis. Equipment: Bruker "AVANCE400" Nuclide: 13 C Measurement method: Inverse gate decoupling Accumulation count: 6000 times Measurement tube diameter: 10mmφ
[0060] [Example 1] 71 parts of methyl ethyl ketone was charged into a reaction vessel equipped with a thermometer, a cooling tube, and a stirrer, and the mixture was heated to reflux. 72 parts of p-acetoxystyrene (hereinafter referred to as PACS), 83 parts of 1-(butoxy)ethyl methacrylate (hereinafter referred to as BEMA), 10 parts of dimethyl-2,2'-azobisisobutyrate, and 119 parts of methyl ethyl ketone were charged into a separate vessel to prepare a dropwise solution, which was dropped into the reaction vessel under reflux of methyl ethyl ketone over a period of 2 hours, and then reacted for 2 hours. A solution in which 3 parts of dimethyl-2,2'-azobisisobutyrate were dissolved in 10 parts of methyl ethyl ketone was added to the reaction solution, and the reaction was continued for another 2 hours, after which it was cooled. The polymerization liquid was dropped into 750 parts of hexane to precipitate a polymer, which was stirred for 30 minutes, allowed to stand, and then decanted. The obtained polymer was dissolved in 120 parts of acetone, dropped again into 750 parts of hexane to precipitate the polymer, stirred for 30 minutes, allowed to stand, and then decanted. The polymer was dissolved in 300 parts of propylene glycol monomethyl ether acetate (hereinafter referred to as PGMEA), concentrated at 40°C under reduced pressure, and adjusted so that the polymer concentration of the polymer solution was 45 wt%.
[0061] 0.1 parts of 28% by weight sodium methoxide / methanol solution was added to 11 parts of the obtained PACS / BEMA polymer solution, and the mixture was stirred at 40°C for 4 hours to deprotect the PACS units. The pKa of the conjugate acid of sodium methoxide is 15.5. After the deprotection reaction, the mixture was neutralized by adding 0.5 parts of 20% by weight acetic acid / PGMEA solution, and the polymer solution was subjected to GPC analysis and NMR analysis. The weight average molecular weight, polydispersity and structural unit composition of the resulting polymer were analyzed and the results are shown in Table 1.
[0062] [Example 2] The same procedures as in Example 1 were carried out except that the temperature of the deprotection reaction was set to 50° C. The results of analysis of the weight average molecular weight, dispersity and structural unit composition of the obtained polymer are shown in Table 1.
[0063] [Example 3] 0.4 parts of 10% by mass potassium hydroxide / methanol solution was added to 11 parts of the PACS / BEMA resin solution obtained in Example 1, and the mixture was stirred at 40° C. for 4 hours to deprotect the PACS units. The pKa of the conjugate acid of potassium hydroxide is 15.7. After the deprotection reaction, 0.5 parts of 20% by mass acetic acid / PGMEA solution was added to neutralize the mixture, and the polymer solution was subjected to GPC analysis and NMR analysis. The weight average molecular weight, polydispersity and structural unit composition of the resulting polymer were analyzed and the results are shown in Table 1.
[0064] [Example 4] 1.6 parts of 10% by mass diazabicycloundecene (hereinafter referred to as DBU) / methanol solution was added to 11 parts of the PACS / BEMA resin solution obtained in Example 1, and the mixture was stirred at 40°C for 4 hours to deprotect the PACS units. The pKa of the conjugate acid of DBU is 12.5. After the deprotection reaction, 2.2 parts of 20% by mass acetic acid / PGMEA solution was added to neutralize, and the polymer solution was subjected to GPC analysis and NMR analysis. The weight average molecular weight, polydispersity and structural unit composition of the resulting polymer were analyzed and the results are shown in Table 1.
[0065] [Example 5] 39 parts of methyl ethyl ketone was charged into a reaction vessel equipped with a thermometer, a cooling tube, and a stirrer, and heated to reflux. 37 parts of PACS, 48 parts of 1-(cyclohexyloxy)ethyl methacrylate (hereinafter referred to as CHEM), 5 parts of dimethyl-2,2'-azobisisobutyrate, and 64 parts of methyl ethyl ketone were charged into a separate vessel to prepare a dropwise solution, which was dropped into the reaction vessel under reflux of methyl ethyl ketone over 2 hours, and then reacted for 2 hours. A solution in which 1 part of dimethyl-2,2'-azobisisobutyrate was dissolved in 5 parts of methyl ethyl ketone was added to the reaction liquid, and the reaction was continued for another 2 hours, after which it was cooled. The polymerization liquid was dropped into 375 parts of hexane to precipitate a polymer, stirred for 30 minutes, allowed to stand, and then decanted. The obtained polymer was dissolved in 60 parts of acetone, dropped again into 375 parts of hexane to precipitate a polymer, stirred for 30 minutes, allowed to stand, and then decanted. The polymer was dissolved in 150 parts of PGMEA and concentrated under reduced pressure at 40° C., so that the polymer concentration of the polymer solution was adjusted to 45 wt %.
[0066] 0.1 parts of 28% by mass sodium methoxide / methanol solution was added to 13 parts of the obtained PACS / CHEMA polymer solution, and the mixture was stirred at 40°C for 4 hours to deprotect the PACS units. The pKa of the conjugate acid of sodium methoxide is 15.5. After the deprotection reaction, 0.5 parts of 20% by mass acetic acid / PGMEA solution was added to neutralize the mixture, and the polymer solution was subjected to GPC analysis and NMR analysis. The weight average molecular weight, polydispersity and structural unit composition of the resulting polymer were analyzed and the results are shown in Table 1.
[0067] [Example 6] 70 parts of methyl ethyl ketone was charged into a reaction vessel equipped with a thermometer, a cooling tube, and a stirrer, and heated to reflux. 37 parts of PACS, 78 parts of tetrahydropyranyl methacrylate (hereinafter referred to as THPMA), 11 parts of dimethyl-2,2'-azobisisobutyrate, and 117 parts of methyl ethyl ketone were charged into a separate vessel to prepare a dropwise solution, which was dropped into the reaction vessel under reflux of methyl ethyl ketone over a period of 2 hours, and then reacted for 2 hours. A solution of 3 parts of dimethyl-2,2'-azobisisobutyrate dissolved in 11 parts of methyl ethyl ketone was added to the reaction liquid, reacted for another 2 hours, and then cooled. The polymerization solution was dropped into 750 parts of hexane to precipitate the polymer, stirred for 30 minutes, allowed to stand, and then decanted. The obtained polymer was dissolved in 120 parts of acetone, dropped again into 75050 parts of hexane to precipitate the polymer, stirred for 30 minutes, allowed to stand, and then decanted. The polymer was dissolved in 300 parts of PGMEA, concentrated at 40°C under reduced pressure, and the polymer concentration of the polymer solution was adjusted to 45 wt%.
[0068] 0.6 parts of 28% by weight sodium methoxide / methanol solution was added to 50 parts of the obtained PACS / THPMA polymer solution, and the mixture was stirred at 40°C for 4 hours to deprotect the PACS units. The pKa of the conjugate acid of sodium methoxide is 15.5. After the deprotection reaction, 2.5 parts of 20% by weight acetic acid / PGMEA solution was added to neutralize the mixture, and the polymer solution was subjected to GPC analysis and NMR analysis. The weight average molecular weight, polydispersity and structural unit composition of the resulting polymer were analyzed and the results are shown in Table 1.
[0069] [Comparative Example 1] The same procedures as in Example 1 were carried out except that the temperature of the deprotection reaction was set to 60° C. The results of analysis of the weight average molecular weight, dispersity and structural unit composition of the obtained polymer are shown in Table 1.
[0070] [Comparative Example 2] The same procedures as in Example 1 were carried out except that the temperature of the deprotection reaction was 80° C. The results of analysis of the weight average molecular weight, dispersity and structural unit composition of the obtained polymer are shown in Table 1.
[0071] [Comparative Example 3] 1.3 parts of 10% by weight triethylamine / methanol solution was added to 12 parts of the PACS / BEMA polymer solution obtained in Example 1, and the mixture was stirred at 50° C. for 40 hours to deprotect the PACS units. The pKa of the conjugate acid of triethylamine is 10.6. The results of analysis of the weight average molecular weight, dispersity, and structural unit composition of the obtained polymer are shown in Table 1.
[0072] [Comparative Example 4] A reaction vessel equipped with a thermometer, a cooling tube and a stirrer was charged with 16 parts of cyclohexanone and heated to 85°C. A separate vessel was charged with 4 parts of a 50% by mass p-hydroxystyrene / cyclohexanone solution (p-hydroxystyrene was synthesized according to the examples in JP-A-04-283529), 4 parts of BEMA, 0.4 parts of dimethyl-2,2'-azobisisobutyrate and 28 parts of cyclohexanone to prepare a dropwise solution, which was dropped into the reaction vessel over 2 hours, and then reacted for another 2 hours while maintaining the temperature at 85°C, and then cooled. The polymerization liquid was dropped into a mixed solvent of 360 parts of hexane and 40 parts of ethyl acetate to precipitate a polymer, which was stirred for 30 minutes and allowed to stand, and then filtered. A mixed solvent of 360 parts of hexane and 40 parts of ethyl acetate was added to the recovered polymer, and the slurry was stirred to wash the polymer, and then filtered. The recovered polymer was dried under reduced pressure at 40°C overnight. The weight average molecular weight, polydispersity and structural unit composition of the resulting polymer were analyzed and the results are shown in Table 1.
[0073] [Table 1]
[0074] [Storage stability test] The polymer solutions obtained in Example 1 and Comparative Example 1 were stored at 20° C., and the change in the total content of the structural unit (III) and the structural unit (IV) in the polymer was examined. The results are shown in Table 2.
[0075] [Table 2]
[0076] The polymer produced by the method of the present invention was one in which the formation of carboxylic acid structural units due to the elimination of acetal protecting groups and the formation of structural units resulting from the reaction of the eliminated acetal groups with phenolic hydroxyl groups of hydroxystyrene units were highly suppressed. Furthermore, the composition of such a polymer did not change even after storage at 20°C for 4 weeks, and the storage stability of the polymer was excellent. [Industrial Applicability]
[0077] The polymer of the present invention can be used as a highly sensitive resist resin composition.
Claims
1. A method for producing a polymer containing a structural unit derived from p-hydroxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group, comprising the steps of: The production method includes subjecting a polymer containing a structural unit derived from p-acetoxystyrene and a structural unit having a structure in which a carboxylic acid is protected with an acetal group to a deprotection reaction in an organic solvent in the presence of a base whose conjugated acid has a pKa of 12 or more at a temperature in the range of 0°C to 50°C, thereby converting the structural unit derived from p-acetoxystyrene in the polymer into a structural unit derived from p-hydroxystyrene; The method for producing a polymer, wherein the amount of the base having a pKa of 12 or more of the conjugate acid is 1 to 50 mol % based on the number of moles of the acetyl groups to be deprotected.
2. The structural unit having a structure in which a carboxylic acid is protected with an acetal group is represented by the formula (II): [Formula 1] (In formula (II), R 1 represents a hydrogen atom or a methyl group, R 2 R represents an alkyl group having 1 to 10 carbon atoms. 3 represents an alkyl group having 1 to 15 carbon atoms, a saturated aliphatic cyclic group having 5 to 15 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkylaryl group having 7 to 15 carbon atoms, or an aralkyl group having 7 to 15 carbon atoms. 2 and R 3 is combined to form R 3 may form a 5- to 8-membered heterocyclic group together with the oxygen atom to which it is bonded.
3. 3. The method for producing a polymer according to claim 1, wherein the base having a pKa of 12 or more for the conjugate acid is at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, sodium methoxide, potassium methoxide, and diazabicycloundecene.
4. The method for producing a polymer according to any one of claims 1 to 3, wherein the organic solvent used in the deprotection reaction is at least one selected from the group consisting of methanol, ethanol, isopropanol, propylene glycol monomethyl ether, methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, methyl propionate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, and propylene glycol monomethyl ether acetate.
5. The method for producing a polymer according to any one of claims 1 to 4, wherein the deprotection reaction is carried out at a temperature in the range of 20°C to 50°C.
Citation Information
Patent Citations
Preferential hydrolysis of copolymer of p-acetoxystyrene with allyl ester of ethylenically unsaturated acid
JP1990311505A
Chemical amplification type resist material
JP1992211258A
Novel copolymer and photoresist composition containing copolymer resin binder
JP1998186665A
Polymer for photoetching, photoetching composition containing the same and production of the same
JP1999310611A
Resist composition for electron beam or x-ray
JP2001281864A