Carburized two-phase steel
A carburized duplex steel with a martensite single-phase and two-phase ferrite structure, optimized with aluminum and niobium, addresses distortion and strength issues in existing treatments, offering low strain and high fatigue strength for mechanical elements.
Patent Information
- Application Number
- JP2022101454
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-06-23
AI Technical Summary
Existing carburizing and quenching treatments for steel materials result in significant distortion and are not suitable for thick mechanical elements, while alternative treatments like soft nitriding and nitriding do not provide sufficient fatigue strength.
A carburized duplex steel with a martensite single-phase structure and a non-carburized two-phase structure of martensite and ferrite, optimized with specific elements like aluminum and niobium, to enhance fatigue strength and reduce distortion.
The proposed steel composition achieves low distortion, high fatigue strength, and ease of manufacturing, suitable for thick mechanical elements.
Smart Images

Figure 0007947765000003 
Figure 0007947765000004 
Figure 0007947765000005
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a low-distortion steel material comprising a carburized layer having a martensite single-phase structure, and a non-carburized layer having a two-phase structure of a martensite structure and a ferrite structure. BACKGROUND ART
[0002] For example, mechanical devices manufactured using steel materials, such as automotive gears, have conventionally been required to improve the quietness of mechanical noise generated during their operation. Particularly in the automotive field, in recent years, along with the electrification of prime movers, the demand for improved quietness of drive train mechanical devices has been further increasing.
[0003] The improvement of mechanical noise quietness can be realized, for example, by reducing the distortion of the steel material constituting mechanical elements such as gears, increasing the fatigue strength of the steel material, and enhancing the design accuracy thereof. The "distortion of steel material" herein means the distortion caused by stress generated during surface processing by heat treatment performed in the steel material manufacturing process, as described in Patent Documents 1 to 3 below.
[0004] As a heat treatment for steel materials, for example, carburizing and quenching treatment is known. However, since this carburizing and quenching treatment involves martensitic transformation, large distortion may occur inside the steel material due to the stress caused by the formation of martensite.
[0005] As other heat treatments, for example, soft nitriding treatment and nitriding treatment are known. Since soft nitriding treatment and nitriding treatment do not involve martensitic transformation, the occurrence of distortion in the steel material due to such treatments can be suppressed. However, since the thickness of the hardened layer obtained by soft nitriding treatment or nitriding treatment is about 0.2 mm from the surface layer of the steel material, it is not suitable for steel materials constituting thick mechanical elements, and sufficient fatigue strength required for mechanical elements such as gears may not be obtained.
[0006] As a heat treatment that can ensure the thickness of the hardened layer on the surface of the steel material and reduce internal strain, for example, there is carburizing two-phase quenching as disclosed in the following Patent Documents 1 and 2. Carburizing two-phase quenching makes it possible to obtain carburized two-phase quenched steel in which the surface layer is a single phase of martensitic structure and the interior is a two-phase structure of ferrite and martensitic structure. Carburized two-phase quenched steel makes it possible to increase fatigue strength by forming a thick hardened layer on the surface and to suppress the occurrence of strain caused by martensitic transformation inside the material. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 9-111405 [Patent Document 2] Japanese Patent Publication No. 2001-32036 [Patent Document 3] Japanese Patent Publication No. 2012-001774 [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] However, the technology described in Patent Document 1 employs a method of adding an excess of silicon (Si) to obtain carburized duplex steel. Si promotes grain boundary oxidation, which can significantly reduce the fatigue strength of carburized duplex steel. Therefore, the technology in Patent Document 1 makes it difficult to achieve both strength and strain reduction. Furthermore, the carburized duplex steel described in Patent Document 2 has complex conditions for the content ratio of each element, resulting in extremely low design flexibility, and its manufacture is by no means easy. Thus, sufficient research has not been conducted on the composition of carburized duplex steel that is suitable for carburized duplex quenching, exhibits low strain, and has high fatigue strength, and there is still room for improvement. [Means for solving the problem]
[0009] The inventors of the present invention have diligently researched a simpler method for manufacturing carburized duplex steel, which comprises a carburized layer with a single-phase martensitic structure and a non-carburized layer with a two-phase structure of martensitic and ferritic structures, and which exhibits low strain and high fatigue strength. As a result, the inventors have found that by adjusting the aluminum (Al) content, the two-phase region including the martensitic and ferritic structures can be expanded, and the carburized duplex quenching process for obtaining carburized duplex steel can be facilitated. Furthermore, the inventors have found that by including niobium (Nb) together with Al in a predetermined proportion, the fatigue strength of carburized duplex steel can be effectively increased. Based on these findings, the inventors have succeeded in manufacturing carburized duplex steel, which has a simple chemical composition that is easy to manufacture, exhibits low strain, and has high fatigue strength, as shown in the following embodiment.
[0010] The present invention can be realized, for example, in the following forms.
[0011] [First Form] The first form is provided as a carburized duplex steel having a chemical composition comprising, by mass%, 0.10% to 0.35% carbon (C), greater than 0% to 2.00% silicon (Si), 0.4% to 2.0% manganese (Mn), less than 0.03% phosphorus (P), less than 0.05% sulfur (S), greater than 0% to 2.00% chromium (Cr), 0.015% to 2.000% aluminum (Al), 0.005% to 0.100% niobium (Nb), and 0.001% to 0.100% nitrogen (N), with the remainder being iron (Fe) and unavoidable impurities, and comprising a carburized layer having a single-phase martensite structure and a non-carburized layer having a two-phase structure of martensite and ferrite structures.
[0012] [Second form] The carburized duplex steel according to the first form, having a chemical composition further comprising, by mass%, at least one of copper (Cu) at a concentration of 0.01% to 1.00% or nickel (Ni) at a concentration of 0.01% to 2.00%.
[0013] [Third form] A carburized duplex steel according to the first or second form, having a chemical composition further containing 0.01% to 1.00% by mass of molybdenum (Mo).
[0014] [Fourth form] A carburized duplex steel according to any one of the first, second, and third forms, further comprising, by mass%, at least one of vanadium (V) in an amount of 0.01% or more and 0.50% or less, or titanium (Ti) in an amount of 0.005% or more and 0.200% or less.
[0015] [Fifth form] A carburized duplex steel according to any one of the first, second, third, and fourth forms, having a chemical composition further containing 5 ppm to 30 ppm of boron (B) by mass.
[0016] [Sixth Form] A carburized duplex steel according to any one of the first, second, third, fourth, and fifth forms, wherein the grain size number of the prior austenite grains is 7 or higher.
[0017] [Seventh form] A carburized duplex steel according to any one of the first, second, third, fourth, fifth, and sixth forms, wherein the area ratio of ferrite in the non-carburized layer is 15% or more and 70% or less. [Effects of the Invention]
[0018] According to the present invention, a carburized duplex steel can be obtained that has low distortion, high fatigue strength, and is easy to manufacture.
[0019] The present invention can be realized in various forms other than carburized duplex steel. For example, it can be realized in the form of a method for manufacturing carburized duplex steel, a method for carburizing duplex quenching to manufacture carburized duplex steel, metal parts such as gears and screws made from carburized duplex steel, and machines, devices, and equipment using such metal parts. [Brief explanation of the drawing]
[0020] [Figure 1]Schematic diagram showing a rod-shaped steel piece constituting a test material for fatigue testing. [Figure 2] Schematic diagram showing an annular steel piece constituting a test material for deformation rate measurement. [Figure 3] Explanatory diagram showing an example of a phase diagram of carburized dual-phase steel. [Figure 4] Explanatory diagram showing an example of a phase diagram of a steel material of a comparative example. [Figure 5] Explanatory diagram showing the relationship between ferrite area fraction and deformation rate. [Mode for Carrying Out the Invention]
[0021] Hereinafter, embodiments of the carburized dual-phase steel according to the present invention will be described.
[0022] 1. Chemical composition of carburized dual-phase steel: The carburized dual-phase steel of the present embodiment includes a carburized layer having a martensite single-phase structure, and a non-carburized layer having a dual-phase structure of a martensite structure and a ferrite structure. Further, the carburized dual-phase steel of the present embodiment has a chemical composition containing C, Si, Mn, P, S, Cr, Al, Nb, and N, with the balance being Fe and unavoidable impurities.
[0023] The reasons for limiting each chemical component in the carburized dual-phase steel of the present embodiment are described in detail below. In the following description, unless otherwise specified, "%" means "mass %", and "ppm" means "mass ppm".
[0024] C: 0.10% or more and 0.35% or less Carbon (C) is an effective element for ensuring the hardness and strength of steel materials. By including carbon, the internal (core) hardness of carburized parts can be increased, thereby improving fatigue strength. By including 0.10% or more carbon, the required strength for steel materials can be obtained, resulting in high fatigue strength. It is more preferable that the carbon content be 0.12% or more. This allows for more stable acquisition of high fatigue strength. However, the carbon content in carburized duplex steel should be 0.35% or less. This is because if the carbon content exceeds 0.35%, the machinability of carburized duplex steel may be significantly reduced. It is more preferable that the carbon content be 0.30% or less. This allows for better machinability of carburized duplex steel.
[0025] Si: Greater than 0% and less than or equal to 2.0% Si is an effective element for improving the hardenability of carburized duplex steel. Si is also effective as a deoxidizing element. By including more than 0% Si, the hardenability of carburized duplex steel can be effectively improved. However, the Si content in carburized duplex steel should be 2.0% or less. This is because a Si content exceeding 2.0% can promote intergranular oxidation, reducing fatigue strength and potentially significantly decreasing cold forgeability and machinability. A Si content of 1.5% or less is more preferable. This more reliably suppresses the decrease in machinability of carburized duplex steel.
[0026] Mn: 0.4% or more and 2.0% or less Mn is an effective element for improving the hardenability and increasing the strength of carburized duplex steel. By including 0.4% or more Mn, the formation of sulfides by sulfur can be suppressed. It is more preferable that the Mn content be 0.5% or more. This can more reliably suppress defects caused by the presence of sulfur. However, the Mn content in carburized duplex steel should be 2.0% or less. If the Mn content exceeds 2.0%, the machinability and workability of the carburized duplex steel may be significantly reduced. In addition, bainite may be formed, which can significantly reduce the toughness of the carburized duplex steel. It is more preferable that the Mn content in carburized duplex steel be 1.8% or less. This can more reliably suppress the decrease in machinability, workability, and toughness of the carburized duplex steel.
[0027] P: Less than 0.03% Since phosphorus (P) can cause embrittlement due to grain boundary segregation, its content should be kept as low as possible. The upper limit for the P content should be less than 0.03%. This makes it possible to suppress the occurrence of embrittlement due to grain boundary segregation in carburized duplex steel.
[0028] S: Less than 0.05% Similar to phosphorus (P), sulfur (S) can cause embrittlement due to grain boundary segregation; therefore, a lower S content is preferable. The upper limit for S content should be less than 0.05%. This suppresses the occurrence of embrittlement due to grain boundary segregation in carburized duplex steel.
[0029] Cr: Greater than 0% and less than or equal to 2.0% Cr is preferable to be present in amounts exceeding 0% because it has the effect of improving the hardenability of carburized duplex steel. A Cr content of 0.2% or more is more preferable. This allows for a more reliable improvement in the hardenability of carburized duplex steel. However, the Cr content should be 2.0% or less. This is because if the Cr content exceeds 2.0%, the machinability and workability of the carburized duplex steel may be significantly reduced. A Cr content of 1.50% or less is more preferable. This further suppresses the reduction in the machinability and workability of the carburized duplex steel.
[0030] Al: 0.015% or more and 2.000% or less As will be explained in the embodiments described later, by adding Al to the carburized duplex steel and adjusting the Al content ratio, the duplex region containing the martensitic and ferrite structures can be expanded, and carburized duplex quenching can be facilitated. If the Al content ratio is 0.015% or more, it is possible to make the uncarburized layer into a duplex, and the ferrite area ratio in the uncarburized layer can be increased, thereby suppressing the occurrence of strain. If the Al content ratio is 2.000% or less, it is possible to suppress the duplex formation of the uncarburized layer along with the carburized layer. Therefore, if the Al content ratio is 0.015% or more and 2.000% or less, carburized duplex steel with low strain can be easily obtained. It is more preferable that the Al content ratio be 0.035% or more. This makes carburized duplex quenching easier and further suppresses the occurrence of strain.
[0031] Furthermore, in carburized duplex steel, the higher the Al content, the greater the deoxidation effect. Therefore, from the viewpoint of obtaining a deoxidation effect, it is more preferable for carburized duplex steel to contain 0.50% or more Al, and even more preferable for it to contain 0.80% or more.
[0032] However, from the viewpoint of suppressing the formation of coarse inclusions, a low Al content is preferable. The formation of coarse inclusions can reduce the fatigue strength of carburized duplex steel. From the viewpoint of suppressing the formation of coarse inclusions, the Al content is preferably 1.50% or less, and more preferably 1.2% or less. The Al content is even more preferably 1.1% or less.
[0033] Nb: 0.005% or more and 0.100% or less Nb promotes the formation of carbonitrides and suppresses abnormal grain growth caused by the addition of Al. Therefore, by including Nb together with Al, the fatigue strength of carburized duplex steel can be improved.
[0034] By including 0.005% or more of Nb, grain refinement through the formation of carbonitrides can be promoted. Therefore, the fatigue strength of the carburized duplex steel can be increased. It is more preferable that the Nb content be 0.01% or more. This further increases the fatigue strength of the carburized duplex steel. However, the Nb content should be 0.100% or less. This is because if the Nb content exceeds 0.100%, the strength may decrease due to the formation of coarse nitrides. It is more preferable that the Nb content be 0.05% or less. This further suppresses the decrease in strength caused by the formation of coarse nitrides.
[0035] N: 0.001% or more and 0.100% or less The strength of carburized duplex steel can be increased by incorporating nitrogen (N). By including 0.001% or more N, grain refinement is promoted through the formation of carbonitrides, thereby increasing the strength of the carburized duplex steel. However, the N content should be 0.100% or less. If the N content exceeds 0.100%, the strength may decrease due to nitride formation.
[0036] Inevitable impurities include, for example, oxygen (O). In the carburized duplex steel of this embodiment, the O content is less than 0.002%. This suppresses the reduction in strength of the carburized duplex steel due to the formation of coarse oxides.
[0037] The carburized duplex steel of this embodiment may further optionally contain the following elements.
[0038] Cu: 0.01% or more and 1.00% or less By including 0.01% or more of Cu, the corrosion resistance of carburized duplex steel can be improved. It is more preferable that the Cu content be 0.03% or more. This further improves the corrosion resistance of carburized duplex steel. However, from the viewpoint of suppressing a decrease in the hot workability of carburized duplex steel, the Cu content is preferably 1.00% or less, and more preferably 0.50% or less.
[0039] Ni: 0.01% or more and 2.00% or less By including 0.01% or more Ni, the ductility and corrosion resistance of the carburized duplex steel can be improved. It is more preferable that the Ni content be 0.10% or more. This further improves the ductility and corrosion resistance. However, from the viewpoint of suppressing bainite formation, the Ni content is preferably 2.00% or less, and more preferably 1.50% or less. It is even more preferable that the Ni content is 1.00% or less.
[0040] Mo: 0.01% or more and 1.00% or less By including 0.01% or more of Mo, the hardenability of the carburized duplex steel can be improved, and the hardness after tempering can be increased. It is more preferable that the Mo content be 0.10% or more. This further improves the hardenability of the carburized duplex steel and further increases the hardness after tempering. However, the Mo content is preferably 1.00% or less, and more preferably 0.80% or less. This suppresses the decrease in workability and machinability of the carburized duplex steel caused by excessive addition of Mo.
[0041] V: 0.01% or more and 0.50% or less By including 0.01% or more of V, the crystal grains of the carburized duplex steel can be made finer, and the hardness after tempering can be increased. However, the V content is preferably 0.50% or less, and more preferably 0.30% or less. This makes it possible to suppress the decrease in workability and machinability of the carburized duplex steel caused by excessive addition of V.
[0042] Ti: 0.005% or more and 0.200% or less By including 0.005% or more of Ti, the formation of carbonitrides is promoted, the crystal grains can be refined, and the strength of the carburized duplex steel can be increased. The Ti content is preferably 0.200% or less, and more preferably 0.100% or less. This suppresses the promotion of coarse TiN formation due to excessive Ti addition, which can lead to a decrease in the strength of the carburized duplex steel.
[0043] B: 5ppm or more and 30ppm or less It is preferable that the B content be 5 ppm or more. This prevents P and S from segregating at the grain boundaries and improves fatigue strength. It is preferable that the B content be 30 ppm or less. This suppresses the reduction in toughness of the carburized duplex steel caused by excessive addition of B, which promotes the formation of B nitrides.
[0044] 2. Microstructure of carburized duplex steel: In the carburized duplex steel having the above chemical composition, it is preferable that the grain size number of the prior austenite grains is 7 or higher. This helps to suppress a significant decrease in the fatigue strength of the carburized duplex steel.
[0045] In carburized duplex steel having the above chemical composition, the area ratio of ferrite in the non-carburized layer is preferably 15% or more. This suppresses the increase in strain of the carburized duplex steel. The area ratio of ferrite in the non-carburized layer is preferably 70% or less. This suppresses a significant decrease in the fatigue strength of the carburized duplex steel.
[0046] In the carburized duplex steel having the above chemical composition, it is more preferable that the grain size number of the prior austenite grains is 7 or higher, and that the area ratio of ferrite in the non-carburized layer is 15% to 70%. This makes it possible to increase the fatigue strength of the carburized duplex steel while reducing the strain of the carburized duplex steel.
[0047] 3. Method for manufacturing carburized duplex steel: The method for producing the carburized duplex steel of this embodiment will now be described. First, steel within the range of chemical composition described above is melted, for example, in a high-frequency induction furnace. Subsequently, the resulting steel ingot is formed by hot rolling or hot forging, and the resulting formed steel material is subjected to a normalizing treatment. The normalizing treatment is carried out by heating the steel material to a temperature of, for example, 800 to 1000°C, and then air-cooling it for a predetermined time. After that, the normalized steel material is subjected to a carburizing treatment.
[0048] In this embodiment, gas carburizing is performed. In gas carburizing, a gas carburizing furnace is used, and propane gas, for example, is supplied as the carburizing gas. In gas carburizing, the steel material is heated in the gas carburizing furnace at a temperature of, for example, 900 to 960°C for about 1 to 3 hours, and then cooled to a temperature of, for example, 800 to 900°C, and held at that temperature for a predetermined time. This causes the uncarburized layer to become two-phase. In addition to gas carburizing, gas carbonitriding, vacuum carburizing, vacuum carbonitriding, etc., may be performed in the carburizing process. Subsequently, in the carburizing process, oil quenching is performed, followed by tempering. Through the above steps, the carburized two-phase steel of this embodiment is obtained.
[0049] 4. Summary of the embodiments: The carburized duplex steel of this embodiment contains at least Al within the preferred content range described above, making carburized duplex quenching easy and reducing strain. Furthermore, the carburized duplex steel of this embodiment contains Nb along with Al within a preferred content range, achieving both strain reduction and improved fatigue strength. In addition, by containing the above-mentioned elements in preferred content ratios, it is possible to improve various other properties as described above. [Examples]
[0050] Next, an example of the carburized duplex steel according to the present invention will be described.
[0051] A. Chemical composition As examples and comparative examples of the carburized duplex steel according to the present invention, test specimens having the chemical compositions shown in Table 1 below were prepared. In Table 1, test specimens within the range of chemical compositions of the embodiments described above are shown as Examples 1 to 14, and test specimens outside that range are shown as Comparative Examples 1 to 7. Note that the test specimens for each of Examples 1 to 14 and each of Comparative Examples 1 to 7 were prepared with different dimensions and shapes according to the purpose of evaluation and testing described later.
[0052] [Table 1]
[0053] <Manufacturing conditions of the test material> The test materials for evaluation and testing were manufactured using the following process.
[0054] [Step 1] Steel having the chemical composition shown in Table 1 was melted in a high-frequency induction path, and the resulting steel ingot was formed by hot rolling or hot forging to produce round steel bars with a circular cross-sectional shape having the dimensions described below according to the purpose of evaluation and testing. [Step 2] The round steel bar was subjected to a normalizing treatment to produce steel pieces with the shape and dimensions described below, according to the purpose of evaluation and testing. In the normalizing treatment, the bar was heated at 900°C for 1 hour, followed by air cooling. [Step 3] The steel pieces were subjected to a carburizing treatment to obtain test specimens having the shape and dimensions described below, according to the purpose of evaluation and testing. In the carburizing treatment, a gas carburizing furnace was used, propane gas was supplied as the carburizing gas, and the pieces were heated at 930°C for 120 minutes, after which they were cooled to 850°C, the quenching start temperature, and held at that temperature. After that, oil quenching was performed, followed by tempering at 180°C for 120 minutes. The carbon potential (CP) during the carburizing treatment was controlled to 0.8 by adjusting the partial pressures of carbon monoxide and carbon dioxide.
[0055] B. Evaluation and Testing Table 2 summarizes the evaluation results for Examples 1-14 and Comparative Examples 1-7. Table 2 shows the results of observing the cross-sections of the test materials for Examples 1-14 and Comparative Examples 1-7 to confirm the structure of the carburized and uncarburized layers, the measurement results of the ferrite area ratio of the uncarburized layer, and the evaluation results of the grain size of the test materials. Table 2 also shows the measurement results of the deformation rate before and after carburizing treatment for the test materials of Examples 1-14 and Comparative Examples 1-7, as well as the test results of fatigue tests to evaluate fatigue strength.
[0056] [Table 2]
[0057] 1. Methods for observing and evaluating cross-sectional tissue a. About the test material In step 1 above, the steel ingot obtained by melting was formed into a round bar shape with a cross-sectional diameter of 105 mm by hot rolling or hot forging, and then further hot forged to produce a round steel bar material with a cross-sectional diameter of 30 mm. After the normalizing treatment in step 2 above was performed on this round steel bar material, the cross-sectional area was 25 mm². 2 Next, a round bar-shaped steel piece with a length of 100 mm was cut out, and the carburizing treatment described in step 3 above was performed on the steel piece to obtain a test material for observation and evaluation of its structure.
[0058] b. Method for observing the cross-sectional structure of the test specimen The test specimen was divided in half along its central axis to create a semicircular cross-section. The cut surface was then embedded in resin and mirror-polished, and the microstructure of the carburized and uncarburized layers was observed. In Table 2, the single-phase martensite structure is denoted by "M," and the two-phase structure of martensite and ferrite is denoted by "M+α."
[0059] The ferrite area ratio of the non-carburized layer was measured by etching the test material with Nital and taking images at a magnification of 400x at a position half the radius R from the central axis of the test material. The values in Table 2 are the average values of the ferrite area ratio measured in 10 randomly selected images.
[0060] For grain size determination, the test material was polished and etched with a saturated picric acid solution to expose the prior austenite grain boundaries. Grain size was then determined by observing approximately 10 fields of view at a magnification of 400x, in accordance with JIS G 0511.
[0061] 2. Method for measuring fatigue intensity a. About the test material In step 1 above, the steel ingot obtained by melting was formed into a round bar shape with a cross-sectional diameter of 105 mm by hot rolling or hot forging, and then further hot forged to produce a round steel bar with a cross-sectional diameter of 25 mm. After the normalizing treatment in step 2 above was performed on the round steel bar, a cross-sectional area of 18 mm was obtained from the round steel bar. 2 A 210 mm long round bar was cut out, and the central part along its central axis was processed to obtain the rod-shaped steel piece 10 shown in Figure 1. The carburizing treatment described in step 3 above was performed on this rod-shaped steel piece 10 to prepare it as a test material for fatigue testing.
[0062] As shown in Figure 1, the rod-shaped steel piece 10 has cylindrical portions 11 with a uniform diameter located at both ends in the direction of the central axis, and a reduced-diameter portion 12 located in the central part between the two cylindrical portions 11, with a smaller diameter than the cylindrical portions 11. The reduced-diameter portion 12 includes a first reduced-diameter portion 12a and a second reduced-diameter portion 12b. The first reduced-diameter portion 12a is a notched portion formed by cutting out the center of the reduced-diameter portion 12 in the direction of the central axis, and is the portion with the smallest diameter in the rod-shaped steel piece 10. The second reduced-diameter portion 12b is provided on both sides of the first reduced-diameter portion 12a in the direction of the central axis, and is a portion with a larger diameter than the first reduced-diameter portion 12a and with a uniform diameter. In the rod-shaped steel piece 10, the lengths La of the two cylindrical portions 11 were 80 mm each, and the length Lb of the reduced-diameter portion 12 was 50 mm. Furthermore, the diameter φa of the first reduced diameter section 12a was 10 mm, and its notch bottom was 1R, while the diameter φb of the second reduced diameter section 12b was 15 mm.
[0063] b. Method of fatigue testing The fatigue strength of the test specimen, which was composed of the above-mentioned rod-shaped steel pieces 10, was measured by performing an Ono-type rotary bending fatigue test in accordance with JIS Z 2274 (test conditions: rotation speed 3500 rpm, test temperature room temperature). The fatigue strength value was 10 7 This refers to the fatigue limit, which is the maximum stress at which fracture does not occur within a given number of cycles. The fatigue strengths in Table 2 are the ratios of the measured fatigue strengths of Examples 1-14 and Comparative Examples 1-6 to the reference value 1, where the measured fatigue strength of Comparative Example 7, which consists only of a single-phase martensite structure, is set as the reference value 1. In Table 2, a higher value indicates greater fatigue strength.
[0064] 3. Method for measuring deformation rate a. About the test material In step 1 above, the steel ingot obtained by melting was formed into a round bar shape with a cross-sectional diameter of 105 mm by hot rolling or hot forging, and the normalizing treatment in step 2 above was performed on the round bar steel material. The round bar steel material after the normalizing treatment was processed to obtain an annular steel piece 20 having the annular shape shown in Figure 2. The shape of the cross-section perpendicular to the circumferential direction of the annular steel piece 20 is approximately quadrilateral. The annular steel piece 20 had an outer diameter Ra of 100 mm, an inner diameter Rb of 90 mm, and a thickness T of 20 mm. The carburizing treatment in step 3 above was performed on this annular steel piece 20 to prepare it as a test material for deformation rate measurement.
[0065] b. Method for measuring deformation ratio The deformation rate was measured as the amount of strain in the inner diameter Rb of the annular steel piece 20 before and after the carburizing treatment in step 3 described above. The deformation rate is the ratio of the strain amounts of each of Examples 1 to 14 and Comparative Examples 1 to 6 to the reference strain amount 1, with the strain amount of Comparative Example 7, which has only a single-phase martensite structure, being set as the reference strain amount 1. The deformation rate corresponds to an index that shows the magnitude of the strain of the steel material before and after surface treatment. In Table 2, a smaller value for the deformation rate indicates less strain.
[0066] 4. Evaluation Results and Test Results 4-1. Facilitation of two-phase carburizing quenching with Al Figure 3 shows an example of an phase diagram for a carburized duplex steel corresponding to Example 1, and Figure 4 shows an example of an phase diagram for the steel material of Comparative Example 7. In the phase diagrams of Figures 3 and 4, the vertical axis is temperature, and the horizontal axis is the percentage of carbon (mass%) in the steel material. In the phase diagrams of Figures 3 and 4, point P1, which corresponds to the central region of the carburized layer at 850°C, and point P2, which corresponds to the central region of the non-carburized layer, are shown. Also, for convenience, in the phase diagrams of Figures 3 and 4, hatching of different concentrations is applied to the single-phase microstructure region γ of the ferrite structure and the duplex microstructure region α+γ of the martensitic and ferrite structures, respectively.
[0067] As shown in Table 1, the Al content in Comparative Example 7 is 0.010%, while the Al content in Example 1 is 1.010%. Comparing the phase diagrams in Figures 3 and 4, it can be seen that increasing the amount of Al added allows the two-phase region α+γ of the martensitic and ferrite structures to extend into the high-temperature region. This indicates that increasing the Al content facilitates two-phase quenching.
[0068] In Comparative Example 2, the Al content was less than 0.015%. Furthermore, in Comparative Example 2, the carburized layer had a single-phase martensite structure, while the uncarburized layer had a two-phase structure of martensite and ferrite. The deformation rate was less than 1, indicating less strain than in Comparative Example 7. However, in Comparative Example 2, the ferrite area ratio was smaller than in the other Examples 1-14 and Comparative Examples 1,3-6, where the uncarburized layer was two-phase, resulting in the largest deformation rate. This suggests that strain can be reduced by increasing the Al content to 0.015% or more.
[0069] In Comparative Example 6, where the Al content was greater than 2.000%, both the carburized and uncarburized layers exhibited a two-phase structure of martensitic and ferrite. In contrast, in Examples 1-14 and Comparative Examples 1-5, where the Al content was 2.000% or less, the carburized layer exhibited a single-phase martensite structure, while the uncarburized layer exhibited a two-phase structure of martensitic and ferrite. This indicates that by limiting the Al content to 2.000% or less, it is easy to create a single-phase martensite structure in the carburized layer and a two-phase structure of martensitic and ferrite in the uncarburized layer.
[0070] In all of Examples 1 to 14, the Al content was between 0.015% and 2.000%, and the fatigue strength was high and the strain was low.
[0071] 4-2. Improvement of fatigue strength by Nb Examples 1 to 14, in which the Nb content was between 0.005% and 0.100%, all achieved high fatigue strength. In Comparative Example 5, the Nb content was less than 0.005%, and both the grain size and fatigue strength were significantly lower compared to Examples 1 to 14. This is thought to be because, in Comparative Example 5, the insufficient Nb content prevented the suppression of abnormal grain growth due to the addition of Al, resulting in a decrease in fatigue strength. In Comparative Example 3, the Nb content exceeded 0.100%, and both the grain size and fatigue strength were significantly lower compared to Examples 1 to 14. This is thought to be because, in Comparative Example 3, the high Nb content promoted the formation of coarse nitrides, leading to a decrease in fatigue strength.
[0072] 4-3. Performance improvement due to the C content ratio Examples 1 to 14, in which the carbon content was between 0.01% and 0.35%, all achieved high fatigue strength and suppressed strain generation. In Comparative Example 1, the carbon content was less than 0.1%, and the fatigue strength was lower than that of Examples 1 to 16 and Comparative Examples 2 to 7. This is thought to be because the carbon content was insufficient, preventing the acquisition of sufficient strength. In Comparative Example 4, the carbon content was greater than 0.35%. In Comparative Example 4, the ferrite area ratio was lower than 15%, and the deformation rate was greater than that of all Examples 1 to 16, resulting in greater strain.
[0073] 4-4. Regarding the ferrite area ratio Figure 5 shows a graph plotting the evaluation results for each of Examples 1-16 and Comparative Examples 1-7 shown in Table 2, with the ferrite area ratio on the horizontal axis and the deformation ratio on the vertical axis. As is clear from this graph, when the ferrite area ratio was 15% or more, the deformation ratio could be kept below 0.3, and the generation of strain was effectively suppressed. In Examples 1-14, the ferrite area ratio was within the range of 15% to 70%, and good results were obtained for both fatigue strength and deformation ratio. In contrast, in Comparative Example 1, the ferrite area ratio exceeded 70%, and although the deformation ratio was significantly smaller, the fatigue strength was lower than the others. This decrease in fatigue strength is thought to be due to the amount of ferrite contained in the non-carburized layer being too large. In Comparative Examples 2 and 4, the ferrite area ratio was less than 15%, and in both cases the deformation ratio was larger than in Examples 1-14, indicating greater strain. This is thought to be because the amount of ferrite contained in the non-carburized layer was insufficient, and the generation of strain could not be sufficiently suppressed.
[0074] 4-5. About grain size Examples 1-14 all had a grain size of 7 or higher, and good results were obtained in both fatigue strength and deformation rate. In contrast, Comparative Examples 3, 5, and 6 all had a grain size smaller than 7, and all of them showed low fatigue strength. From this, it can be seen that if the grain size is 7 or higher, the grains are refined and high fatigue strength can be obtained.
[0075] 5. Summary As shown above in the examples and comparative examples, the preferred carburized duplex steel described in the above embodiments is suitable for carburized duplex quenching and can increase fatigue strength while reducing distortion.
[0076] The present invention is not limited to the above embodiments and examples, and various modifications are possible without departing from the spirit of the invention. [Explanation of symbols]
[0077] 10...Rod-shaped steel piece, 11...Cylindrical portion, 12...Reduced diameter portion, 12a...First reduced diameter portion, 12b...Second reduced diameter portion, 20...Annular steel piece
Claims
1. In mass percent, C: 0.10% or more and 0.35% or less, Si: Greater than 0% and less than or equal to 2.0% Mn: 0.4% or more and 2.0% or less, P: Less than 0.03% S: Less than 0.05% Cr: greater than 0% and less than or equal to 2.0% Al: 0.015% or more, 2.000% or less, Nb: 0.005% or more and 0.100% or less, N: 0.001% or more and 0.100% or less, It has a chemical composition that includes, with the remainder being Fe and unavoidable impurities. It comprises a carburized layer with a single-phase martensite structure and an uncarburized layer with a two-phase structure of martensite and ferrite structures. The grain size number of the old austenite grains is 7 or higher. A carburized duplex steel in which the area ratio of ferrite in the non-carburized layer is 15% or more and 70% or less.
2. In mass percent, Cu: 0.01% or more and 1.00% or less, Ni: 0.01% or more and 2.00% or less, The carburized duplex steel according to claim 1, further comprising a chemical composition containing at least one of the following.
3. In mass percent, Mo: 0.01% or more and 1.00% or less, The carburized duplex steel according to claim 1, further comprising a chemical composition containing the above.
4. In mass percent, V: 0.01% or more and 0.50% or less, Ti: 0.005% or more and 0.200% or less, The carburized duplex steel according to claim 1, further comprising a chemical composition containing at least one of the following.
5. In ppm mass, B: 5ppm or more and 30ppm or less The carburized duplex steel according to claim 1, further comprising a chemical composition containing the above.
Citation Information
Patent Citations
High-quality carburized gear steel for heavy truck and production method of high-quality carburized gear steel
CN113481442A
Method for carburizing heat treatment of high strength gear small in strain and the gear
JP1993070924A
Low strain type carburized and quenched steel stock for gear
JP1997111405A
Quenching method for case hardening steel capable of preventing heat treatment strain
JP1999036016A
Low distortion carburized and quenched steel for gear, excellent in machinability, and manufacture of gear using the steel
JP2001032036A