Optical films and display devices

The optical film with a colored layer and functional layer addresses display quality issues in self-emissive displays by enhancing lightfastness and heat resistance, ensuring long-term high display quality without a gas barrier layer.

JP7947934B2Active Publication Date: 2026-11-11TOPPAN HOLDINGS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022185784
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-21
Publication Date
2026-11-11
Estimated Expiration
2042-11-21

AI Technical Summary

Technical Problem

Existing display devices, particularly self-emissive displays like organic light-emitting displays, suffer from reduced display quality due to external light reflection, which is exacerbated by the use of polarizers and phase delay plates that lead to light loss and potential dye deterioration, and the addition of colorfastness inhibitors and gas barrier layers increases thickness and cost.

Method used

An optical film comprising a transparent substrate with a colored layer and a functional layer, where the colored layer contains specific dyes and energy-ray curable compounds, along with a radical scavenger, to enhance lightfastness and heat resistance without requiring a gas barrier layer.

Benefits of technology

The optical film maintains high display quality over time by effectively suppressing external light reflection and improving color purity, while avoiding the need for a gas barrier layer, thus extending the lifespan and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007947934000017
    Figure 0007947934000017
  • Figure 0007947934000018
    Figure 0007947934000018
  • Figure 0007947934000019
    Figure 0007947934000019
Patent Text Reader

Abstract

To provide an optical film with which it is possible to maintain high display quality, even for use over a long period, without requiring a gas barrier layer.SOLUTION: Provided is an optical film 1 comprising a transparent substrate 20, a colored layer 10, and a function layer 30. The ultraviolet ray shield rate of at least one of the transparent substrate and the function layer is 85% or higher. The colored layer is composed of a cured product containing a pigment (A), an energy-ray curable compound (B), a photoinitiator (C), and a radical scavenger (D). The pigment (A) contains at least one of a first colorant, a second colorant, and a third colorant. The energy-ray curable compound (B) contains 20 weight% or more of a compound that has only two (meth)acryloyl groups including an alicyclic skeleton. In a simultaneous thermogravimetry and calorie measurement under 200 ml / minute gas flow rate and 10°C / minute heat-up temperature conditions, the difference between 50% weight reduction temperature under a nitrogen atmosphere and 50% weight reduction temperature under an air atmosphere of the colored layer is 60°C or below.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to an optical film. A display device using this optical film is also mentioned. [Background technology]

[0002] Display devices are often used in environments where ambient light is present, both indoors and outdoors. Ambient light entering a display device is reflected by its surface, causing a decrease in display quality. Self-emissive display devices, such as organic light-emitting displays, have a problem where electrodes and many other metal wirings strongly reflect ambient light, easily leading to a decrease in display quality. However, they are expected to be next-generation display devices because they excel in miniaturization and possess high-quality characteristics such as low power consumption, high brightness, and high response speed.

[0003] To solve the problem of reduced display quality due to external light reflection, there is a configuration in which polarizing plates and phase delay plates are placed on the display surface side to suppress external light reflection. However, in methods using polarizers and phase delay plates, a significant portion of the light emitted from the display device is lost when it passes through the polarizer and phase delay plate and is emitted to the outside, which tends to lead to a decrease in the lifespan of the device.

[0004] Patent Document 1 proposes an organic light-emitting display device comprising a display substrate containing an organic light-emitting element and a sealing substrate spaced apart from the display substrate, wherein a filler is embedded in the space between the display substrate and the sealing substrate to selectively absorb external light in each wavelength band and adjust the transmittance. According to the invention of Patent Document 1, visibility is improved by suppressing external light reflection, and color purity is also improved by selectively absorbing light in wavelength bands that particularly degrade color purity among the light emitted from the display device.

[0005] Regarding the improvement of color purity, Patent Document 2 discloses a configuration that includes a dye having an absorption maximum wavelength in at least the wavelength regions of 480-510 nm and 580-610 nm. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] Patent No. 5673713 [Patent Document 2] Japanese Patent Publication No. 2019-56865 [Patent Document 3] International Publication No. 2021 / 066082 [Overview of the project] [Problems that the invention aims to solve]

[0007] Many wavelength-selective absorption dyes have poor lightfastness and heat resistance, and their function may deteriorate over time, preventing them from fully exhibiting their color purity-enhancing effect. In relation to this problem, Patent Document 3 shows a configuration in which a predetermined compound is added to the dye as a colorfastness inhibitor and a gas barrier layer is provided. However, the addition of a gas barrier layer results in a thicker film and increased costs, and there is a possibility that the dye may deteriorate from defects in the gas barrier layer. Furthermore, in the inventors' studies, they found that when only the colorfastness inhibitor was added without a gas barrier layer, an improvement in lightfastness was observed, but conversely, a decrease in heat resistance occurred.

[0008] Based on the circumstances described above, the present invention aims to provide an optical film that can maintain high display quality even after long-term use without requiring a gas barrier layer. Another object of the present invention is to provide a display device that can maintain high display quality even after long-term use without requiring a gas barrier layer. [Means for solving the problem]

[0009] A first aspect of the present invention is an optical film comprising a sheet-like transparent substrate, a colored layer formed on the first surface of the transparent substrate, and a functional layer formed on the second surface of the transparent substrate opposite to the first surface, or on the colored layer. At least one of the transparent substrate and the functional layer has an ultraviolet shielding rate of 85% or more as measured in accordance with JIS L1925. The colored layer is composed of a cured product containing a colorant (A), an energy ray-curable compound (B), a photopolymerization initiator (C), and a radical scavenger (D). The colorant (A) contains at least one of a first color material, a second color material, and a third color material. The first color material has an absorption maximum wavelength in the range of 470 to 530 nm, and a half-value width of the absorption spectrum of 15 to 45 nm. The second color material has an absorption maximum wavelength in the range of 560 to 620 nm, and a half-value width of the absorption spectrum of 15 to 55 nm. The third color material has a wavelength with the lowest transmittance in the wavelength range of 380 to 780 nm within the range of 650 to 780 nm. The energy ray-curable compound (B) contains 20% by weight or more of a compound having only two (meth)acryloyl groups containing an alicyclic skeleton. In the simultaneous thermogravimetry and calorimetry measurement under the conditions of a gas flow rate of 200 ml / min and a temperature increase rate of 10°C / min, the difference between the 50% weight reduction temperature in a nitrogen atmosphere and the 50% weight reduction temperature in an air atmosphere of the colored layer is 60°C or less.

[0010] A second aspect of the present invention is a display device comprising the optical film according to the first aspect. [Advantageous Effects of the Invention]

[0011] According to the present invention, it is possible to provide an optical film that can maintain high display quality even after long-term use without requiring a gas barrier layer. [Brief Description of the Drawings]

[0012] [Figure 1] It is a cross-sectional view of an optical film according to one embodiment of the present invention. [Figure 2] It is a cross-sectional view of an optical film according to another embodiment of the present invention. [Figure 3] It is a cross-sectional view of an optical film according to still another embodiment of the present invention. [Figure 4]This is a cross-sectional view of an optical film according to another embodiment of the present invention. [Figure 5] This is a cross-sectional view of an optical film according to another embodiment of the present invention. [Figure 6] This is a cross-sectional view of an optical film according to another embodiment of the present invention. [Figure 7] This graph shows the spectrum of the white display output through the organic EL light source and color filter in the example. [Figure 8] These are graphs of the spectra output through the organic EL light source and color filter in the example, for red, green, and blue displays. [Modes for carrying out the invention]

[0013] Embodiments of the present invention will be described below with reference to the accompanying drawings. In all drawings, even if the embodiments differ, the same or corresponding components will be denoted by the same reference numerals, and common descriptions will be omitted.

[0014] [Optical film] An optical film according to one embodiment of the present invention will be described in detail below with reference to Figure 1.

[0015] As shown in Figure 1, the optical film 1 has a colored layer 10, a transparent substrate 20, and a functional layer 30. The functional layer 30 has a low refractive index layer 31 and a hard coat layer 32. In other words, the optical film 1 has a transparent substrate 20 located on one side of the colored layer 10, and is a laminate in which the colored layer 10, transparent substrate 20, hard coat layer 32, and low refractive index layer 31 are laminated in this order.

[0016] The thickness of the optical film 1 is preferably, for example, 10 to 140 μm, more preferably 15 to 120 μm, and even more preferably 20 to 100 μm. If the thickness of the optical film 1 is above the lower limit, the strength of the optical film 1 can be further increased. If the thickness of the optical film 1 is below the upper limit, not only can the optical film 1 be made lighter, but it is also advantageous for making the display device thinner. The following describes each layer that makes up the optical film 1.

[0017] ≪Colored layer≫ The colored layer 10 is a cured product of the colored layer forming composition and contains a dye (A), an active energy ray curable resin (B), a photopolymerization initiator (C), and a radical scavenger (D).

[0018] The thickness of the colored layer 10 is preferably, for example, 0.5 to 10 μm. If the thickness of the colored layer 10 is greater than or equal to the lower limit, the dye can be contained without causing any abnormalities in the appearance of the colored layer 10, and the light absorption properties of the dye can improve the reflection characteristics and color reproduction. If the thickness of the colored layer 10 is less than or equal to the upper limit, it is advantageous for making the display device thinner. The thickness of the colored layer 10 can be determined by observing a cross-section of the optical film 1 in the thickness direction using a microscope or the like.

[0019] <Pigment (A)> The pigment (A) contains at least one of the following colorants: the first colorant, the second colorant, and the third colorant. The absorption maximum wavelength of the first colorant is within the range of 470 nm to 530 nm, and the full width at half maximum of the absorption spectrum is 15 to 45 nm. If the absorption maximum wavelength is below the lower limit, it tends to decrease the luminance efficiency of blue emission, and if it exceeds the upper limit, it tends to decrease the luminance efficiency of green emission. If the full width at half maximum of the absorption spectrum is below the lower limit, the effect of suppressing the reflection characteristics to ambient light is small, and if it exceeds the upper limit, the reflection characteristics to ambient light tend to improve, but the luminance efficiency tends to decrease.

[0020] The absorption maximum wavelength of the second colorant is within the range of 560 nm to 620 nm, and the full width at half maximum of the absorption spectrum is 15 to 55 nm. If the absorption maximum wavelength is below the lower limit, it tends to decrease the brightness efficiency of green emission, and if it exceeds the upper limit, it tends to decrease the brightness efficiency of red emission. If the full width at half maximum of the absorption spectrum is below the lower limit, the effect of suppressing the reflection characteristics to ambient light is small, and if it exceeds the upper limit, the reflection characteristics to ambient light tend to improve, but the brightness efficiency tends to decrease.

[0021] The third colorant has a wavelength range of 380-780 nm at which the wavelength with the lowest transmittance is between 650 and 780 nm. If the wavelength with the lowest transmittance in the 380-780 nm range of the third colorant is below the lower limit, it tends to reduce the luminance efficiency of red emission, and if it exceeds the upper limit, the suppression effect on the reflection characteristics to ambient light becomes smaller.

[0022] The dye (A) preferably contains a compound having one of the following structures: porphyrin, merocyanine, phthalocyanine, azo, cyanine, squarylium, coumarin, polyene, quinone, tetradiporphyrin, pyromethene, or indigo, or a metal complex thereof. In particular, the use of a metal complex having a porphyrin, pyromethene, or phthalocyanine structure, or a compound having a squarylium structure, is more preferable due to its superior reliability. The dye (A) may contain one of these compounds or their metal complexes alone, or two or more of them. These compounds or their metal complexes may be contained in the first colorant, the second colorant, the third colorant, or two or more of these colorants.

[0023] <Energy ray curable compound (B)> Energy-ray curable compound (B) is a resin that polymerizes and hardens upon irradiation with active energy rays such as ultraviolet light or electron beams. For example, monofunctional, bifunctional, or trifunctional (meth)acrylate monomers, urethane (meth)acrylates, etc., can be used. Here, "(meth)acrylate" means both or either "acrylate" and "methacrylate".

[0024] Examples of monofunctional (meth)acrylate compounds that can be included in energy-ray curable compound (B) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfluryl acrylate, cyclohexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. Acrylate, isobornyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phosphate (meth)acrylate, ethylene oxide-modified phosphate (meth)acrylate, phenoxy (meth)acrylate, ethylene oxide-modified phenoxy (meth)acrylate )Acrylate, Propylene oxide-modified phenoxy(meth)acrylate, Nonylphenol(meth)acrylate, Ethylene oxide-modified nonylphenol(meth)acrylate, Propylene oxide-modified nonylphenol(meth)acrylate, Methoxydiethylene glycol(meth)acrylate, Methoxypolyethylene glycol(meth)acrylate, Methoxypropylene glycol(meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl(meth) )Acrylate, 2-(meth)acryloyloxyethyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hexahydrohydrogen phthalate, 2-(meth)acryloyloxypropyl tetrahydrohydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate,Examples include adamantane derivative mono(meth)acrylates such as adamantyl acrylate, which has a monovalent mono(meth)acrylate derived from 2-adamantane and adamantanediol. Here, "(meth)acryloyl" means both or either "acryloyl" and "methacryloyl."

[0025] Examples of difunctional (meth)acrylate compounds that can be included in energy-ray curable compound (B) include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate, and other di(meth)acrylates.

[0026] Examples of trifunctional or more (meth)acrylate compounds that can be included in energy-ray curable compound (B) include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris-2-hydroxyethyl isocyanurate tri(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, etc. Examples include meth)acrylate compounds, polyfunctional (meth)acrylate compounds with three or more functions, such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ditrimethylolpropane hexa(meth)acrylate, as well as polyfunctional (meth)acrylate compounds in which some of these (meth)acrylates are substituted with alkyl groups or ε-caprolactone.

[0027] In addition, urethane (meth)acrylate can also be used as a resin that can be included in energy-ray curable compound (B). Examples of urethane (meth)acrylate include those obtained by reacting a product obtained by reacting a polyester polyol with an isocyanate monomer or prepolymer with a (meth)acrylate monomer having a hydroxyl group.

[0028] Examples of urethane (meth)acrylates include pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate toluene diisocyanate urethane prepolymer, pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, and dipentaerythritol pentaacrylate isophorone diisocyanate urethane prepolymer.

[0029] The monofunctional, bifunctional, or trifunctional (meth)acrylate monomers, urethane (meth)acrylates, etc., that can be included in the above-mentioned other energy-ray curable compound (B) may be used individually or in combination of two or more. They may also be oligomers in which a portion has been polymerized.

[0030] The content of the energy ray-curable compound (B) is preferably 20 to 80% by mass, and more preferably 30 to 70% by mass, relative to the total mass of the colored layer-forming composition. If the content of the energy ray-curable compound (B) is above the lower limit, the fade-inhibiting effect can be further enhanced. If the content of the energy ray-curable compound (B) is below the upper limit, the handling of the colored layer-forming composition can be further enhanced.

[0031] <Photopolymerization initiator (C)> A photopolymerization initiator (C) is, for example, one that generates radicals when ultraviolet light is used as the active energy ray, when ultraviolet light is irradiated onto it. Examples of photopolymerization initiators (C) include benzoins (benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and other benzoin alkyl ethers), phenyl ketones [e.g., acetophenones (e.g., acetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, etc.), alkyl phenyl ketones such as 2-hydroxy-2-methylpropiophenone; cycloalkyl phenyl ketones such as 1-hydroxycyclohexyl phenyl ketone, etc.], and aminoacetophenones {2-methyl-1-[4-(methylthio)pheni Examples include photopolymerization initiators such as 2-2-morpholinoaminopropanone-1, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, anthraquinones (anthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 1-chloroanthraquinone, etc.), thioxanthones (2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone, etc.), ketals (acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.), benzophenones (benzophenone, etc.), xanthones, and phosphine oxides (e.g., 2,4,6-trimethylbenzoyldiphenylphosphine oxide, etc.). These photopolymerization initiators may be used individually or in combination of two or more.

[0032] The content of the photopolymerization initiator (C) is preferably 0.01 to 20% by mass, and more preferably 0.01 to 5% by mass, relative to the solid content of the colored layer forming composition. If the content of the photopolymerization initiator (C) is below the lower limit, the curability will be insufficient. If the content of the photopolymerization initiator (C) exceeds the upper limit, unreacted photopolymerization initiator (C) will remain, and the reliability, such as heat resistance, will deteriorate.

[0033] <Radical scavenger (D)> Examples of radical scavengers (D) include resins having an amine structure. Here, "amine structure" refers to a structure in which a hydrogen atom of ammonia is replaced by a hydrocarbon group or an aromatic group. Examples of amine structures include primary amines, secondary amines, and tertiary amines, and may also be quaternary ammonium cations.

[0034] The radical scavenger (D) works by capturing radicals that occur when the dye (A) undergoes oxidative degradation, thereby suppressing auto-oxidation and inhibiting dye degradation (fading). Examples of resins having an amine structure that can be used as a radical scavenger (D) include resins having a hindered amine structure with a molecular weight of 2000 or more. A high fading suppression effect can be obtained when the molecular weight of the resin having a hindered amine structure is 2000 or more. This is thought to be because a large number of molecules remain within the colored layer 10, resulting in a sufficient fading suppression effect. The molecular weight of a resin having a hindered amine structure is, for example, around 200,000, but there is no particular upper limit. In this specification, "molecular weight" means "mass-average molecular weight" measured using gel permeation chromatography (GPC) with polystyrene as the standard substance.

[0035] In this embodiment, the radical scavenger (D) is a polymer containing an amine structure that has radical scavenging ability, and includes a structural unit represented by the following formula (i).

[0036] [ka]

[0037] In the above equation (i), R 12R represents a hydrogen atom, halogen atom, carboxyl group, sulfo group, cyano group, hydroxyl group, alkyl group having 10 or fewer carbon atoms, alkoxycarbonyl group having 10 or fewer carbon atoms, alkylsulfonylaminocarbonyl group having 10 or fewer carbon atoms, arylsulfonylaminocarbonyl group, alkylsulfonyl group, arylsulfonyl group, acylaminosulfonyl group having 10 or fewer carbon atoms, alkoxy group having 10 or fewer carbon atoms, alkylthio group having 10 or fewer carbon atoms, aryloxy group having 10 or fewer carbon atoms, nitro group, alkoxycarbonyloxy group, aryloxycarbonyloxy group, acyloxy group having 10 or fewer carbon atoms, acyl group having 10 or fewer carbon atoms, carbamoyl group, sulfamoyl group, aryl group having 10 or fewer carbon atoms, substituted amino group, substituted ureido group, substituted phosphono group, or heterocyclic group. 13 X represents a hydrogen atom or an alkyl group having 30 or fewer carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or fewer carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by a combination thereof, and all of these may contain a spirodioxane ring.

[0038] R 12 Preferred elements include hydrogen atoms, hydroxyl groups, and alkyl groups having 10 or fewer carbon atoms. The alkyl group preferably has 1 to 6 carbon atoms, and more preferably 1 to 3 carbon atoms. R 13 Preferably, the alkyl group consists of a hydrogen atom or an alkyl group having 10 or fewer carbon atoms. The alkyl group preferably has 1 to 6 carbon atoms, and more preferably 1 to 3 carbon atoms. X is preferably a single bond or an aliphatic alkyl chain having 30 or fewer carbon atoms. The number of carbon atoms in the aliphatic alkyl chain is preferably 10 or less, preferably 1 to 6, and more preferably 2 to 4.

[0039] In this embodiment, the radical scavenger (D) may be mainly composed of a copolymer of a structural unit represented by formula (i) above and a copolymer component having one of the repeating units described below (the component that makes up the largest mass % of the components). Being a copolymer allows for control of compatibility with other components.

[0040] Examples of repeating units include (meth)acrylate-based repeating units, olefin-based repeating units, halogen atom-containing repeating units, styrene-based repeating units, vinyl acetate-based repeating units, vinyl alcohol-based repeating units, and the like.

[0041] Examples of (meth)acrylate repeating units include repeating units derived from (meth)acrylate monomers having a linear or branched alkyl group as a side chain, and repeating units derived from (meth)acrylate monomers having a hydroxyl group as a side chain.

[0042] Examples of repeating units derived from (meth)acrylate monomers having the above-mentioned linear or branched alkyl group as a side chain include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, and isopropyl (meth)acrylate. Examples of monomer-derived components include octyl, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, myristyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, and octadecyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above, repeating (meth)acrylate units having a linear or branched alkyl group with 1 to 4 carbon atoms as a side chain are preferably used.

[0043] Examples of repeating units derived from (meth)acrylic monomers having a hydroxyl group in the side chain include monomer-derived components such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and hydroxyphenyl (meth)acrylate. These may be used individually or in combination of two or more.

[0044] Examples of olefinic repeating units include components derived from olefinic monomers such as ethylene, propylene, isoprene, and butadiene. These may be used individually or in combination of two or more.

[0045] Examples of halogen atom-containing repeating units include monomer-derived components such as vinyl chloride and vinylidene chloride. These may be used individually or in combination of two or more.

[0046] Examples of styrene-based repeating units include styrene, α-methylstyrene, vinyltoluene, and other styrene monomer-derived components. These may be used individually or in combination of two or more types. Examples of vinyl acetate repeating units include esters of saturated carboxylic acids such as vinyl acetate and vinyl propionate with vinyl alcohols. These may be used individually or in combination of two or more. Examples of vinyl alcohol repeating units include vinyl alcohol, which may have 1,2-glycol bonds in its side chains.

[0047] The copolymer may have any of the following structures: random copolymer, alternating copolymer, block copolymer, or graft copolymer. If the copolymer has a random copolymer structure, the manufacturing process and preparation with other components are easy. For this reason, random copolymers are preferred over other copolymers.

[0048] Radical polymerization can be used as a polymerization method to obtain copolymers. Radical polymerization is preferred because it facilitates industrial production. Radical polymerization may be carried out by solution polymerization, emulsion polymerization, bulk polymerization, and suspension polymerization. Solution polymerization is preferred for radical polymerization. By using solution polymerization, it is easy to control the molecular weight in the copolymer.

[0049] In radical polymerization, the monomers described above may be diluted with a polymerization solvent, and then a polymerization initiator may be added to carry out the polymerization of the monomers. The polymerization solvent may be, for example, an ester solvent, an alcohol ether solvent, a ketone solvent, an aromatic solvent, an amide solvent, or an alcohol solvent. Ester solvents may be, for example, methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, t-butyl acetate, methyl lactate, and ethyl lactate. Alcohol ether solvents may be, for example, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, 3-methoxy-1-butanol, and 3-methoxy-3-methyl-1-butanol. Ketone solvents may be, for example, acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. Aromatic solvents may be, for example, benzene, toluene, and xylene. Amide solvents may be, for example, formamide and dimethylformamide. The alcohol-based solvent may be, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, s-butanol, t-butanol, diacetone alcohol, and 2-methyl-2-butanol. Note that one of the polymerization solvents described above may be used alone, or two or more may be used in combination.

[0050] The radical polymerization initiator may be, for example, a peroxide and an azo compound. The peroxide may be, for example, benzoyl peroxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, and di-t-butyl peroxide. The azo compound may be, for example, azobisisobutyronitrile, azobisamidinopropane salt, azobiscyanovaleric acid (salt), and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide].

[0051] The amount of radical polymerization initiator used is preferably 0.0001 parts by mass or more and 20 parts by mass or less, more preferably 0.001 parts by mass or more and 15 parts by mass or less, and even more preferably 0.005 parts by mass or more and 10 parts by mass or less, when the total amount of monomers is set to 100 parts by mass. The radical polymerization initiator may be added to the monomers and polymerization solvent before polymerization begins, or it may be added dropwise into the polymerization reaction system. Adding the radical polymerization initiator dropwise to the monomers and polymerization solvent into the polymerization reaction system is preferable because it can suppress the exothermic reaction caused by polymerization.

[0052] The reaction temperature for radical polymerization is appropriately selected depending on the type of radical polymerization initiator and polymerization solvent. From the viewpoint of ease of manufacture and reaction controllability, the reaction temperature is preferably between 60°C and 110°C.

[0053] When the radical scavenger (D) is a polymer containing a structural unit represented by formula (i), the content of the structural unit represented by formula (i) is preferably 1 to 95 mol%, and more preferably 10 to 90 mol%, relative to the total molar amount of monomers constituting the energy ray curable compound (B). When the content of the structural unit represented by formula (i) is within the above numerical range, the light resistance and heat resistance of the dye (A) are improved, and fading is easily suppressed.

[0054] The radical scavenger (D) according to the present invention is not limited to the polymer described above, and hindered amine-based light stabilizers and the like can also be used.

[0055] The colored layer 10 may contain a solvent (E) and an additive (F). Details of these are described below. <Solvent (E)> Solvent (E) is necessary for the formation of the colored layer. Although much of it disappears from the colored layer due to evaporation during drying after coating, some remains in the colored layer, so its components are described below. Examples of solvents (E) include ethers, ketones, esters, and cellosolves. Examples of ethers include dibutyl ether, dimethoxymethane, dimethoxyethane, diethoxyethane, propylene oxide, 1,4-dioxane, 1,3-dioxolane, 1,3,5-trioxane, tetrahydrofuran, anisole, or phenetol. Examples of ketones include acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, or ethylcyclohexanone. Examples of esters include ethyl formate, propyl formate, n-pentyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, n-pentyl acetate, or γ-butyrolactone. Examples of cellosolves include methyl cellosolve, cellosolve (ethyl cellosolve), butyl cellosolve, or cellosolve acetate. Solvent (E) may be used alone or in combination of two or more.

[0056] The content of solvent (E) is preferably 20 to 80% by mass, and more preferably 30 to 70% by mass, based on the total mass of the colored layer-forming composition containing (A) to (D) above. If the content of solvent (E) is above the lower limit, the handling properties of the colored layer-forming composition can be further improved. If the content of solvent (E) is below the upper limit, the time required to form the colored layer can be shortened.

[0057] <Additive (F)> Examples of additive (F) include compounds having a structure represented by at least the following formula (ii) (hereinafter referred to as "compound A") and sulfur-based antioxidants.

[0058]

Chemical Formula

[0059] In formula (ii), R 1 is each independently any one selected from an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, a group represented by R 9 CO-, a group represented by R 10 SO2-, and a group represented by R 11 NHCO- (R 9 , R 10 , and R 11 are each independently any one selected from an alkyl group, an alkenyl group, an aryl group, and a heterocyclic group.). R 2 and R 3 are each independently any one selected from a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, and an alkenyloxy group. R 4 to R 8 are each independently any one selected from a hydrogen atom, an alkyl group, an alkenyl group, and an aryl group.

[0060] Examples of the sulfur-based antioxidant include dialkyl dithiophosphates, dialkyl dithiocarbamates, benzenedithiols, and transition metal complexes thereof.

[0061] When the colored layer contains the aforementioned Compound A and the sulfur-based antioxidant, the light resistance and heat resistance of the dye (A) can be improved.

[0062] The additive (F) may further contain other additives such as leveling agents, antifoaming agents, antioxidants, ultraviolet absorbers, light stabilizers, photosensitizers, and conductive materials.

[0063] By containing the composition for forming a colored layer of the present invention, the colored layer 10 can achieve improved light resistance and heat resistance without requiring a gas barrier layer, can achieve both reflection suppression and luminance efficiency, can improve display quality, can extend the service life of light-emitting elements, and can improve color reproducibility.

[0064] ≪Transparent base material≫ The transparent substrate 20 is a sheet-like member located on one side of the colored layer 10 and forms the optical film 1. A light-transmitting resin film can be used as the material for the transparent substrate 20. Transparent resins and inorganic glass can be used as the forming material for the transparent substrate 20. Examples of transparent resins include polyolefins, polyesters, polyacrylates, polyamides, polyimides, polyarylates, polycarbonates, triacetylcellulose, polyvinyl alcohol, polyvinyl chloride, cycloolefin copolymers, norbornene-containing resins, polyethersulfones, and polysulfones. Examples of polyolefins include polyethylene and polypropylene. Examples of polyesters include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyacrylates include polymethyl methacrylate. Examples of polyamides include nylon 6 and nylon 66. Among these, films made of polyethylene terephthalate (PET), films made of triacetylcellulose (TAC), films made of polymethyl methacrylate (PMMA), and films made of polyesters other than PET can be suitably used. The thickness of the transparent substrate 20 is not particularly limited, but for example, 10 to 100 μm is preferred. The transmittance of the transparent substrate 20 is preferably 90% or more.

[0065] The transparent substrate 20 may be given ultraviolet absorption capabilities. By adding an ultraviolet absorber to the resin that is the raw material for the transparent substrate 20, ultraviolet absorption capabilities can be imparted to the transparent substrate 20.

[0066] Examples of UV absorbers include salicylate ester-based UV absorbers, benzophenone-based UV absorbers, benzotriazole-based UV absorbers, benzotriazine-based UV absorbers, and cyanoacrylate-based UV absorbers. These UV absorbers may be used individually or in combination of two or more types.

[0067] When imparting ultraviolet absorption ability to the transparent substrate 20, it is preferable that the ultraviolet shielding rate is 85% or higher. Here, the ultraviolet shielding rate is a value measured in accordance with JIS L1925 and is calculated by the following formula. UV shielding rate (%) = 100 - Average transmittance of UV light with wavelengths of 290-400 nm (%) If the UV shielding rate is less than 85%, the fade-preventing effect of the lightfastness of pigment (A) will be reduced.

[0068] Functional Layer The functional layer 30 is located on one or the other surface of the colored layer 10. The optical film can exhibit various functions by having the functional layer 30. The functions of the functional layer 30 include anti-reflective function, anti-glare function, anti-static function, anti-fouling function, strengthening function, and ultraviolet absorption function (ultraviolet absorption capacity). The functional layer 30 may be a single layer or multiple layers. The functional layer 30 may have one type of function or two or more types of functions.

[0069] If the optical film 1 has an anti-reflective function, the functional layer 30 functions as an anti-reflective layer. Examples of anti-reflective layers include the hard coat layer 32 and anti-glare layer 34 described later, and a low refractive index layer 31 that exhibits a lower refractive index than the transparent substrate 20. The low refractive index layer 31 can be formed by using a material with a lower refractive index than the material of the hard coat layer 32, anti-glare layer 34, and transparent substrate 20 in the functional layer. To adjust the refractive index of the low refractive index layer 31, fine particles of lithium fluoride (LiF), magnesium fluoride (MgF2), sodium hexafluoroaluminum (crylite, cryolite, 3NaF·AlF3, Na3AlF6), aluminum fluoride (AlF3), or silica fine particles may be added. As for the silica fine particles, using porous silica fine particles or hollow silica fine particles that have voids inside the particles is effective in lowering the refractive index of the low refractive index layer 31. In addition, the composition for forming the low refractive index layer 31 (composition for forming the low refractive index layer) may appropriately contain the photopolymerization initiator (C), solvent (E), and additive (F) described in the colored layer 10. The refractive index of the low refractive index layer 31 is preferably 1.20 to 1.55. The thickness of the low refractive index layer 31 is not particularly limited, but is preferably, for example, 40 nm to 1 μm.

[0070] When the optical film 1 has an anti-glare function, the functional layer 30 functions as an anti-glare layer 34. The anti-glare layer 34 has fine irregularities on its surface, which scatter external light and suppress reflections, thereby improving display quality. When combined with the low refractive index layer 31, the low refractive index layer 31 and the anti-glare layer 34 form an anti-reflective layer. The anti-glare layer 34 contains one or more organic and inorganic fine particles as needed. The organic fine particles are materials that form fine irregularities on the surface and provide the function of scattering ambient light. Examples of organic fine particles include resin particles made of light-transmitting resin materials such as acrylic resin, polystyrene resin, styrene-(meth)acrylic acid ester copolymer, polyethylene resin, epoxy resin, silicone resin, polyvinylidene fluoride, and polyfluoroethylene resin. To adjust the refractive index and the dispersibility of the resin particles, two or more types of resin particles with different materials (refractive index) may be mixed and used. Inorganic microparticles are materials that regulate the sedimentation and aggregation of organic microparticles. Examples of inorganic microparticles include silica microparticles, metal oxide microparticles, and various mineral microparticles. Examples of silica microparticles include colloidal silica and silica microparticles surface-modified with reactive functional groups such as (meth)acryloyl groups. Examples of metal oxide microparticles include alumina (aluminum oxide), zinc oxide, tin oxide, antimony oxide, indium oxide, titania (titanium dioxide), and zirconia (zirconium dioxide). Examples of mineral microparticles include mica, synthetic mica, vermiculite, montmorillonite, iron montmorillonite, bentonite, byderite, saponite, hectorite, stevensite, nontronite, magadiite, islarite, kanemite, layered titanate, smectite, and synthetic smectite. Mineral microparticles may be natural products or synthetic products (including substituted and derivative products), and mixtures of both may be used. Among mineral microparticles, layered organic clay is more preferred. Layered organic clay refers to a material in which organic onium ions are introduced between the layers of a swellable clay. The organic onium ions are not limited as long as they can be organicated by utilizing the cation exchange properties of the swellable clay. When layered organic clay minerals are used as mineral microparticles, the synthetic smectite described above can be suitably used. Synthetic smectite has the function of increasing the viscosity of the coating liquid for forming the anti-glare layer, suppressing the settling of resin particles and inorganic microparticles, and adjusting the uneven surface shape of the anti-glare layer 34 (functional layer 30).

[0071] If the optical film 1 has an antistatic function, the functional layer 30 functions as an antistatic layer. Examples of antistatic layers include metal oxide fine particles such as antimony-doped tin oxide (ATO) and tin-doped indium oxide (ITO), polymer-type conductive compositions, and layers containing antistatic agents such as quaternary ammonium salts. The antistatic layer may be provided on the outermost surface of the functional layer 30, or it may be provided between the functional layer 30 and the transparent substrate 20. Alternatively, the antistatic layer may be formed by incorporating an antistatic agent into any of the layers constituting the functional layer 30 as described above. When an antistatic layer is provided, the surface resistance of the optical film is 1.0 × 10⁻⁶. 6 ~1.0×10 12 (Ω / cm) is preferable.

[0072] If the optical film 1 has an antifouling function, the functional layer 30 functions as an antifouling layer. The antifouling layer enhances antifouling properties by providing both or either water repellency and oil repellency. Examples of antifouling layers include layers containing antifouling agents such as silicon oxides, fluorine-containing silane compounds, fluoroalkylsilazanes, fluoroalkylsilanes, fluorine-containing silicon compounds, and perfluoropolyether group-containing silane coupling agents. The antifouling layer may be provided on the outermost surface of the functional layer 30, or the antifouling layer may be formed by incorporating an antifouling agent into the outermost layer of the functional layer 30 as described above.

[0073] If the optical film 1 has a strengthening function, the functional layer 30 functions as a strengthening layer. The strengthening layer is a layer that increases the strength of the optical film. An example of a strengthening layer is a hard coat layer 32. An example of a hard coat layer 32 is a layer formed of a hard coat agent containing monofunctional, bifunctional, or trifunctional or more (meth)acrylate or urethane (meth)acrylate.

[0074] If the optical film 1 has ultraviolet absorption ability, the functional layer 30 functions as an ultraviolet absorption layer. Examples of ultraviolet absorption layers include layers containing triazine-based ultraviolet absorbers such as 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxyphenol, and benzotriazole-based ultraviolet absorbers such as 2-(2H-benzotriazole-2-yl)-4-methylphenol. The amount of UV absorber is preferably 0.1 to 5% by mass relative to the total mass of the material forming the UV absorption layer. If the amount of UV absorber is above the lower limit, sufficient UV absorption capacity can be imparted to the functional layer 30. If the amount of UV absorber is below the upper limit, insufficient hardness due to a decrease in the curing component can be avoided.

[0075] In the optical film 1, one or both of the transparent substrate 20 and the functional layer 30 have an ultraviolet shielding rate of 85% or more, preferably 90% or more, more preferably 95% or more, and may be 100%. If the ultraviolet shielding rate is above the lower limit of the above value, light resistance and heat resistance can be further improved. The ultraviolet shielding rate can be measured in accordance with the method described in JIS L1925. The UV shielding rate can be adjusted by imparting UV absorption capabilities to one or both of the transparent substrate 20 and the functional layer 30.

[0076] The thickness of the functional layer 30 is preferably, for example, 0.04 to 25 μm, more preferably 0.1 to 20 μm, and even more preferably 0.2 to 15 μm. If the thickness of the functional layer 30 is above the lower limit, it is easier to impart various functions to the optical film 1. If the thickness of the functional layer 30 is below the upper limit, it is advantageous for making the display device thinner.

[0077] [Method for manufacturing optical films] The optical film 1 of this embodiment can be manufactured by conventionally known methods. For example, a colored layer 10 is obtained by applying a colored layer-forming composition to one side of a transparent substrate 20 and curing the colored layer-forming composition by irradiating it with active energy rays. The light source used to cure the colored layer-forming composition by irradiating it with active energy rays and to form the colored layer 10 can be any light source that generates active energy rays without restriction. As active energy rays, light energy rays such as radiation (gamma rays, X-rays, etc.), ultraviolet rays, visible light, and electron beams (EB) can be used, and ultraviolet rays and electron beams are the most common. For example, low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, electrodeless discharge tubes, etc., can be used as lamps that emit ultraviolet rays. The ultraviolet irradiation dose is typically 100-1000 mJ / cm². 2 That is the case.

[0078] Next, a hard coat agent is applied to the other side of the transparent substrate 20, and the hard coat agent is cured by irradiation with active energy rays in the same manner as the colored layer 10 to obtain a hard coat layer 32.

[0079] By forming a low refractive index layer 31 on the hard coat layer 32, an optical film 1 is obtained in which the functional layer 30 is located on the other side of the transparent substrate 20. There are no restrictions on the method for forming the low refractive index layer 31. Methods such as applying a low refractive index layer-forming composition to the hard coat layer 32 and curing it by irradiation with active energy rays, vacuum deposition, sputtering, ion plating, ion beam, and plasma vapor deposition can be used.

[0080] [Other embodiments] As shown in Figure 2, the optical film may have a transparent substrate 20 located on one side of the colored layer 10, and the optical film 3 may be formed by laminating the colored layer 10, the transparent substrate 20, and the anti-glare layer 34 in this order. In the optical film 3, the anti-glare layer 34 constitutes the functional layer 30. The optical film 3 of this embodiment has an anti-glare layer 34, and therefore exhibits excellent reflection suppression.

[0081] As shown in Figure 3, the optical film may have a transparent substrate 20 located on one side of the colored layer 10, and the optical film 4 may be formed by laminating the colored layer 10, the transparent substrate 20, the anti-glare layer 34, and the low refractive index layer 31 in this order. In the optical film 4, the anti-glare layer 34 and the low refractive index layer 31 constitute the functional layer 30. The optical film 4 of this embodiment has a low refractive index layer 31 and an anti-glare layer 34, and therefore exhibits superior reflection suppression.

[0082] As shown in Figure 4, the optical film may have a transparent substrate 20 located on one side of the colored layer 10 and a functional layer 30 located on the other side of the colored layer 10, and the optical film 5 may be formed by laminating the transparent substrate 20, the colored layer 10, the hard coat layer 32, and the low refractive index layer 31 in this order. In the optical film 5, the hard coat layer 32 and the low refractive index layer 31 constitute the functional layer 30. The optical film 5 of this embodiment has a colored layer 10 and a functional layer 30 having ultraviolet absorption and anti-reflective properties on one side of a transparent substrate 20. The ultraviolet absorption property may be provided to any of the layers constituting the functional layer.

[0083] As shown in Figure 5, the optical film may have a transparent substrate 20 located on one side of the colored layer 10 and an anti-glare layer 34 located on the other side of the colored layer 10, and the optical film 7 may be formed by laminating the transparent substrate 20, the colored layer 10, and the anti-glare layer 34 in this order. In the optical film 7, the anti-glare layer 34 constitutes the functional layer 30. The optical film 7 of this embodiment has an anti-glare layer 34, and therefore exhibits excellent reflection suppression. In the optical film 7, it is preferable to provide the anti-glare layer 34 with an ultraviolet absorption function.

[0084] As shown in Figure 6, the optical film may have a transparent substrate 20 located on one side of the colored layer 10 and a functional layer 30 located on the other side of the colored layer 10, and the optical film 8 may be formed by laminating the transparent substrate 20, the colored layer 10, the anti-glare layer 34, and the low refractive index layer 31 in this order. In the optical film 8, the anti-glare layer 34 and the low refractive index layer 31 constitute the functional layer 30. The optical film 8 of this embodiment has a low refractive index layer 31 and an anti-glare layer 34, and therefore exhibits superior reflection suppression. In the optical film 8, it is preferable to impart an ultraviolet absorption function to one of the layers constituting the functional layer 30.

[0085] [Display device] The display device of the present invention comprises the optical film of the present invention. Specific examples of display devices include, for example, televisions, monitors, mobile phones, portable game devices, personal information terminals, personal computers, e-books, video cameras, digital still cameras, head-mounted displays, navigation systems, sound playback devices (car audio, digital audio players, etc.), photocopiers, facsimile machines, printers, printer-multifunction devices, vending machines, automated teller machines (ATMs), personal authentication devices, optical communication devices, IC cards, etc. In particular, it is preferably used in display devices equipped with self-emissive elements such as LEDs, organic ELs, inorganic phosphors, and quantum dots, which are susceptible to external light reflection due to metal electrodes and wiring.

[0086] In the optical films according to each of the embodiments described above, the transparent substrate or functional layer located closer to ambient light than the colored layer has a certain level of UV shielding ability, and the colored layer contains a radical scavenger (D). As a result, light resistance and heat resistance can be improved without providing a gas barrier layer, and both reflection suppression and brightness efficiency can be achieved.

[0087] The colored layer according to this embodiment was found to exhibit properties such as those shown in formula (1) below, with oxidative degradation caused by high heat and light being suitably suppressed. AB ≤ 60 (℃) …(1) In equation (1) above, A is the temperature at which the colored layer loses 50% of its weight when thermogravimetric and calorific values ​​are simultaneously measured under a nitrogen atmosphere with a gas flow rate of 200 ml / min and a heating temperature of 10°C / min. B is the temperature at which the colored layer loses 50% of its weight when thermogravimetric and calorific values ​​are simultaneously measured under an air atmosphere with a gas flow rate of 200 ml / min and a heating temperature of 10°C / min. The value of A indicates resistance to thermal decomposition, and the value of B indicates resistance to thermal decomposition and oxidative degradation. However, by taking the difference between A and B, resistance to oxidative degradation can be accurately evaluated. The inventors' studies have found that even if the value of B is high, if the difference in A is large, the resistance to oxidative degradation may not necessarily be high. In this embodiment, the colored layer is effectively protected from oxidative degradation caused by high heat and light, resulting in a higher 50% weight loss temperature under air conditions and a smaller difference between this temperature and the 50% weight loss temperature under nitrogen conditions. The ability to evaluate light resistance based on the difference between the 50% weight loss temperature under nitrogen conditions and the 50% weight loss temperature under air conditions is a discovery made for the first time in this invention.

[0088] Furthermore, the inventors' studies have shown that if the energy-ray curable compound (B) contains 20% by weight or more of a compound having only two (meth)acryloyl groups containing an alicyclic skeleton, it is even more preferable because it suppresses the excessive amount of double bonds in the structure of the colored layer, thereby suppressing the generation of radicals that degrade the functional colorant when light strikes the double bonds. With such a configuration, a certain amount of double bonds is ensured in the structure of the colored layer, so sufficient hardness is imparted to the colored layer, and the pencil hardness at a 500g load on the surface of the colored layer can be H or higher.

[0089] A display device equipped with the optical film of this embodiment having the characteristics described above can improve display quality and extend the lifespan of the light-emitting element.

[0090] Although each embodiment of the present invention has been described in detail above with reference to the drawings, the specific configuration is not limited to these embodiments, and modifications and combinations of the configuration are also included without departing from the spirit of the present invention.

[0091] For example, although each of the optical films described above has one colored layer, the number of colored layers may be two or more. In the optical film according to each embodiment, the ultraviolet absorption ability may be provided to the transparent substrate 20 or to the functional layer 30 such as the hard coat layer 32. The important thing is to provide the ultraviolet absorption ability to a layer that is closer to the screen viewed by the user than the colored layer 10 when attached to a display device (i.e., the layer that the ambient light incident on the display device passes through before it enters the colored layer). [Examples]

[0092] The present invention will be described in more detail below using examples. The technical scope of the present invention is not limited in any way based solely on the specific details of these examples.

[0093] [Examples 1-9, Comparative Examples 1-8] In the following examples and comparative examples, optical films 1 to 17 with the layer configurations shown in Tables 1 and 2 were prepared. In the tables, "-" indicates the absence of that layer.

[0094] [Table 1]

[0095] [Table 2]

[0096] <<Production of optical films>> The following describes the formation methods for each layer.

[0097] [Formation of a colored layer] (Materials used for colored layer forming composition) The composition of the colored layer in the example is shown in Table 3, and the composition of the colored layer in the comparative example is shown in Table 4. The following materials were used. Note that the absorption maximum wavelength, full width at half maximum, and minimum transmittance wavelength within the specified wavelength range of the colorant are characteristic values ​​for the cured coating film.

[0098] <Pigment (A)> ·First color material Dye-1: Pyrromethene cobalt complex dye (maximum absorption wavelength 493 nm, half-width 26 nm) <Production Example of Dye-1> Ethyl 5-formyl-2,4-dimethyl-1H-pyrrole-3-carboxylate (2.5 g) was charged into a reaction vessel, dissolved in methanol (50 mL), then 47% hydrobromic acid (45 g) was added, and the mixture was refluxed for 1 hour. The precipitated solid was filtered off to obtain 3,3',5,5'-tetramethyl-4,4'-di-ethoxycarbonyl-2,2'-dipyrromethene hydrobromide (2.6 g). 3,3',5,5'-Tetramethyl-4,4'-di-ethoxycarbonyl-2,2'-dipyrromethene hydrobromide (0.6 g) was charged into a reaction vessel, methanol (5 mL), triethylamine (0.17 g), and cobalt acetate tetrahydrate (0.18 g) were added, and the mixture was refluxed for 2 hours. The precipitated solid was filtered off to obtain Dye-1 (0.42 g). ·Second color material Dye-2: Tetraazaporphyrin copper complex dye (manufactured by Yamada Chemical Co., Ltd., FDG-007, maximum absorption wavelength 595 nm, half-width 22 nm) Dye-3: Dye FDG-003 (manufactured by Yamada Chemical Co., Ltd., FDG-003, maximum absorption wavelength 545 nm, half-width 79 nm) Note that Dye-3 is a comparison target used only in comparative examples, and does not correspond to the second color material in the present application because its half-width is large. ·Third color material Dye-4: Phthalocyanine copper complex dye (manufactured by Yamada Chemical Co., Ltd., FDN-002, wavelength at minimum transmittance in 400 to 780 nm: 780 nm)

[0099] <Active energy ray-curable resin (B)> ·DCPA: Tricyclodecane dimethanol diacrylate (containing only 2 (meth)acryloyl groups including an alicyclic skeleton: A-DCP manufactured by Shin-Nakamura Chemical Co., Ltd.) • 510H: Dipentaerythritol hexaacrylate, hexamethylene diisocyanate, urethane prepolymer (manufactured by Kyoeisha Chemical Co., Ltd., UA-510H) • NPA: Neopentyl glycol diacrylate (contains only two (meth)acryloyl groups that do not contain an alicyclic skeleton: manufactured by Shin-Nakamura Chemical Industry Co., Ltd., A-NPG) • BP4EAL: EO-modified bisphenol A diacrylate (contains only two (meth)acryloyl groups without an alicyclic skeleton: manufactured by Kyoeisha Chemical Co., Ltd., Light Acrylate BP-4EAL) • PE3A: Pentaerythritol triacrylate (manufactured by Kyoeisha Chemical Co., Ltd., Light Acrylate PE-3A) • DPHA: Dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Chemical Industry Co., Ltd., A-DPH)

[0100] <Photopolymerization initiator (C)> • Omnirad TPO: Acylphosphine oxide-based photopolymerization initiator (manufactured by IGM Resins BV)

[0101] <Radical scavenger (D)> • LA-63P: Hindered amine-based light stabilizer Adeka Stab LA-63P (manufactured by Adeka Co., Ltd.) • Resin 1: A polymer containing the structural unit represented by the above formula (i).

[0102] <Example of resin 1 manufacturing> 2.4 g of 1,2,2,6,6-pentamethyl-4-piperidyl methacrylic acid (FA-711MM, manufactured by Showa Denko Materials Co., Ltd.), 5.6 g of methyl methacrylate (manufactured by Kanto Chemical Co., Ltd.), 31 g of cyclohexanone (manufactured by Kanto Chemical Co., Ltd.), and 0.11 g of 2,2'-azobis(isobutyronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed in a reaction vessel and heated and stirred at 70°C for 8 hours under a nitrogen gas atmosphere. Subsequently, the mixture was heated and stirred at 100°C for 1 hour to obtain a polymer solution. This polymer solution was poured into 400 mL of methanol (manufactured by Kanto Chemical Co., Ltd.), and the precipitate that formed was filtered and dried to obtain resin 1 copolymerized with 1,2,2,6,6-pentamethyl-4-piperidyl methacrylic acid and methyl methacrylate in a ratio of 15:85 [mol%].

[0103] By performing an additional heating and stirring at 100°C for one hour, the initiator 2,2'-azobis(isobutyronitrile) can be completely decomposed, thereby suppressing the degradation of the optical film due to residual initiator. Furthermore, by pouring the polymer solution into methanol, unreacted monomers, polymerization solvents, and initiator decomposition products can be removed, thereby suppressing the degradation of the optical film.

[0104] <Solvent (E)> • MEK: Methyl ethyl ketone Methyl acetate

[0105] <Additive (F)> Compound A: Browning inhibitor T1477 having the structure shown in formula (ii) above. Note that R in the structural formula 1 It is C3H7, and R 2 ~R 8 H is H. • D1781: Singlet oxygen quencher (bis(dibutyldithiocarbamate)nickel(II), manufactured by Tokyo Chemical Industry Co., Ltd.)

[0106] <Other> • UV absorber: Tinuvin 479: Hydroxyphenyl triazine-based UV absorber, Tinuvin® 479 (manufactured by BASF Japan Ltd.).

[0107] [Table 3]

[0108] [Table 4]

[0109] (Transparent base material) The following materials were used as the transparent substrate. • TAC: Triacetylcellulose film (manufactured by Fujifilm Corporation, TG60UL, substrate thickness 60 μm, UV shielding rate 92.9%) • PMMA: Polymethyl methacrylate film (manufactured by Sumitomo Chemical Co., Ltd., W002N80, substrate thickness 80 μm, UV shielding rate 13.9%)

[0110] (Formation of a colored layer) Colored layer-forming compositions, with the compositions shown in Tables 3 and 4, were applied to the transparent substrates shown in Tables 1 and 2, and dried in an 80°C oven for 60 seconds. Afterward, an ultraviolet irradiation device was used to irradiate the substrates at a dose of 150 mJ / cm². 2 The coating was cured by ultraviolet irradiation using a light source H bulb (manufactured by Fusion UV Systems Japan Co., Ltd.), forming a colored layer with a cured film thickness of 5.0 μm. The amount of additive is given as a mass ratio (mass%). In the table, "-" indicates that the component is not present.

[0111] [Formation of functional layer: Hard coat layer] (Materials used in hard coat layer formation composition) The following materials were used as the hard coat layer forming composition for forming the hard coat layer. • Active energy ray curable resin UA-306H: Pentaerythritol triacrylate, hexamethylene diisocyanate, urethane prepolymer (manufactured by Kyoeisha Chemical Co., Ltd., UA-306H) DPHA PE3A • Photopolymerization initiator Omnirad TPO: Acylphosphine oxide-based photopolymerization initiator (manufactured by IGM Resins BV) • Additives (ultraviolet (UV) absorbers) Tinuvin479 LA-36: Benzotriazole-based UV absorber, Adeka Stab (registered trademark) LA-36 (manufactured by Adeka Co., Ltd.) ·solvent MEK: Methyl ethyl ketone Methyl acetate Using these materials, two types of hard coat coating solutions were prepared, as shown in Table 5.

[0112] [Table 5]

[0113] (Formation of the hard coat layer) The corresponding hard coat coating solution was applied to the transparent substrate or colored layer shown in Tables 1 and 2, and dried in an 80°C oven for 60 seconds. Afterward, an ultraviolet irradiation device was used to administer an irradiation dose of 150 mJ / cm². 2 The coating film was cured by ultraviolet irradiation using a light source H bulb (manufactured by Fusion UV Systems Japan Co., Ltd.), forming a hard coat layer with a cured film thickness of 5.0 μm. Hard coat layer 1 does not have ultraviolet absorption ability, while hard coat layer 2 does.

[0114] [Formation of functional layer: Anti-glare layer] (Composition for forming anti-glare layer) The following composition was used as the anti-glare layer-forming composition for forming the anti-glare layer. • Active energy ray curable resin PE3A 43.7 parts by mass • Photopolymerization initiator Omnirad TPO (manufactured by IGM Resins BV) 4.55 parts by mass • Resin particles Styrene-methyl methacrylate copolymer particles (refractive index 1.515, average particle size 2.0 μm) 0.5 parts by mass ·Inorganic fine particles Synthetic smectite 0.25 parts by mass Alumina nanoparticles (average particle size 40nm) 1.0 parts by mass ·solvent Toluene 15 parts by mass Isopropyl alcohol 35 parts by mass

[0115] (Formation of an anti-glare layer) The above-mentioned anti-glare layer-forming composition was applied to the transparent substrate shown in Table 1 and dried in an 80°C oven for 60 seconds. Afterward, an ultraviolet irradiation device was used to irradiate the substrate at a dose of 150 mJ / cm². 2 The coating was cured by irradiating it with ultraviolet light using a light source H bulb (manufactured by Fusion UV Systems Japan Co., Ltd.), and an anti-glare layer was formed so that the film thickness after curing was 5.0 μm.

[0116] [Formation of functional layer: Low refractive index layer] (Composition for forming a low refractive index layer) The following composition was used to form the low refractive index layer. • Refractive index adjusting agent Porous silica microparticles (average particle size 75 nm, solid content 20%) methyl isobutyl ketone dispersion: 8.5 parts by mass • Antifouling agent Optool® AR-110 (manufactured by Daikin Industries, Ltd., solids content 15%, solvent: methyl isobutyl ketone) 5.6 parts by mass • Active energy ray curable resin PE3A 0.4 parts by mass • Photopolymerization initiator Omnirad TPO (manufactured by IGM Resins BV) 0.07 parts by mass • Leveling agent RS-77 (manufactured by DIC Corporation) 1.7 parts by mass ·solvent Methyl isobutyl ketone 83.73 parts by mass

[0117] (Formation of a low refractive index layer) The low refractive index layer-forming compositions shown in Tables 1 and 2 were applied to the hard coat layer or anti-glare layer and dried in an 80°C oven for 60 seconds. Afterward, an ultraviolet irradiation device was used to irradiate the area at a dose of 200 mJ / cm². 2 The coating was cured by irradiating it with ultraviolet light using a light source H-bulb (manufactured by Fusion UV Systems Japan Co., Ltd.), forming a low refractive index layer with a curing thickness of 100 nm.

[0118] The following evaluations were performed on the optical films related to each example. [Film characteristics evaluation] <UV protection rate on the colored layer> When a transparent substrate was located above the colored layer, the transmittance of the substrate was measured using an automatic spectrophotometer (Hitachi, Ltd., U-4100). When the colored layer was located above the substrate, the layer above the colored layer was peeled off using a transparent pressure-sensitive adhesive tape conforming to the JIS-K5600-5-6:1999 adhesion test, and the transmittance of the layer above the colored layer was measured using an automatic spectrophotometer (Hitachi, Ltd., U-4100) with the transparent pressure-sensitive adhesive tape as a reference. Using these transmittances, the average transmittance [%] in the ultraviolet region (290nm~400nm) was calculated, and the ultraviolet shielding rate [%] was calculated by subtracting the average transmittance [%] in the ultraviolet region (290nm~400nm) from 100%.

[0119] <Lightfastness Test> For the lightfastness test of the obtained optical film, a xenon weather meter (manufactured by Suga Test Instruments Co., Ltd., X75) was used, with a xenon lamp illuminance of 60 W / m². 2 The test was conducted for 120 hours under conditions of a test chamber temperature of 45°C and humidity of 50%RH in the wavelength range of 300nm to 400nm. Transmittance measurements were taken before and after the test using an automatic spectrophotometer (Hitachi, Ltd., U-4100). The difference in transmittance before and after the test was calculated as ΔTλ1 at wavelength λ1, which showed the minimum transmittance before the test in the wavelength range of 470nm to 530nm, and the difference in transmittance before and after the test was calculated as ΔTλ2 at wavelength λ2, which showed the minimum transmittance before the test in the wavelength range of 560nm to 620nm. A transmittance difference close to zero is preferable, with |ΔTλN| ≤ 15 (N=1 to 2) being preferable, and |ΔTλN| ≤ 10 (N=1 to 2) being even preferable. The evaluation was based on the following three levels, with anything other than an "X" being considered a pass. ◎(Excellent): |ΔTλN|≦10 〇 (Good): 10 < |ΔTλN| ≤ 15 ×(Bad):15<|ΔTλN|

[0120] <Heat resistance test> As a heat resistance test of the obtained optical film, it was tested at 90°C for 500 hours using an environmental testing machine (SU-221, manufactured by ESPEC Corporation), and transmittance measurements were taken before and after the test using an automatic spectrophotometer (U-4100, manufactured by Hitachi, Ltd.). The difference in transmittance before and after the test, ΔTλ1, was calculated at wavelength λ1, which shows the minimum transmittance before the test in the wavelength range of 470nm to 530nm, and the difference in transmittance before and after the test, ΔTλ2, was calculated at wavelength λ2, which shows the minimum transmittance before the test in the wavelength range of 560nm to 620nm. A transmittance difference close to zero is preferable, with |ΔTλN| ≤ 15 (N=1 to 2) being preferable, and |ΔTλN| ≤ 10 (N=1 to 2) being even preferable. The evaluation was based on the following three levels, with anything other than an "X" being considered a pass. ◎(Excellent): |ΔTλN|≦10 〇 (Good): 10 < |ΔTλN| ≤ 15 ×(Bad):15<|ΔTλN|

[0121] <Pencil Hardness Test> In accordance with JIS-K5400-1990, a pencil hardness test was performed on the surface of the colored layer for each example using a Clemens-type scratch hardness tester (HA-301, manufactured by Tester Sangyo Co., Ltd.) with a 500g load applied to a pencil (UNI, manufactured by Mitsubishi Pencil Co., Ltd.). The change in appearance due to scratches was evaluated visually, and if no scratches were observed, it was marked as "○ (pass)", and if scratches were observed, it was marked as "× (fail)".

[0122] <Simultaneous measurement of thermogravimetry and calorific value> Optical films (transparent substrate and colored layer) for each example before functional layer formation were cut to approximately the same size and set in a differential thermogravimetric analyzer (STA7200RV, Hitachi High-Tech Science Corporation). The temperature was raised to 550°C at a gas flow rate of 200 ml / min and a heating rate of 10°C / min, and measurements were taken. Air and nitrogen were used as the gas, and measurements were taken under both an air atmosphere and a nitrogen atmosphere. Since the weights of the set samples were not exactly the same, the weight at the start of heating was used as the reference, and the temperature at which the 50% weight loss occurred under each atmosphere was measured. The difference was adopted as the value of AB in the above formula. Except for Example 9, the transparent substrates were identical, and since they decompose faster than the colored layer after the start of measurement, it can be said that the difference in the measured values ​​in the above measurements depends solely on the difference in the colored layer.

[0123] [Display Device Characteristics Evaluation] <White display transmission characteristics> The transmittance of the obtained optical film was measured using an automatic spectrophotometer (Hitachi, Ltd., U-4100). Using this transmittance, the efficiency of the light transmitted through the optical film during white display was calculated and evaluated as the white display transmittance characteristic. As a baseline, the efficiency of the spectrum during white display, output through the white organic EL light source and color filter shown in Figure 7, was set to 100. The closer to 100, the higher the white display transmittance and the better the luminance efficiency. <Display device reflection characteristics> The transmittance T(λ) and surface reflectance R2(λ) of the obtained optical film were measured using an automatic spectrophotometer (U-4100). For the measurement of surface reflectance R2(λ), a matte black dye was applied to the surface of the transparent substrate where no colored or functional layers were formed to prevent reflection, and the spectral reflectance at an incident angle of 5° was measured to determine the surface reflectance R2(λ). Electrode reflectance R EAssuming (λ) is 100% for all wavelengths from 380 nm to 780 nm, and without considering interfacial and surface reflections in each layer, the relative reflection value for the display device against a D65 light source (CIE (International Commission on Illumination) standard light source D65) without an optical film was set to 100. The relative reflection value was calculated based on the following equations (1) to (4), and the surface reflectance R(λ) of the outermost layer on the observer side was evaluated as the display device reflection characteristic. A lower value for the display device reflection characteristic indicates that external light reflection can be reduced and the reflective properties are superior. In equations (1) to (4), R1(λ) is the internal reflection component, Y is one of the three stimulus values ​​at the white point of the D65 light source, and P D65 (λ) represents the spectrum of the D65 light source, and the overline y(λ) represents the CIE1931 color matching function.

[0124]

number

number

number

number

[0125] The results are shown in Tables 6 to 8. The results of the display device characteristic evaluation shown in Table 8 were performed for only some examples, and the white display transmission characteristics and display device reflection characteristics are also shown as a ratio with Comparative Example 8, which does not have a colored layer, as the baseline (100%).

[0126] [Table 6]

[0127] [Table 7]

[0128] [Table 8]

[0129] The optical films in the examples all satisfied formula (1) above and showed good light resistance and heat resistance even without a gas barrier layer. Furthermore, the colored layer contained an energy ray curable compound, resulting in sufficient hardness. The results of Example 9 demonstrate that when the colored layer and the functional layer are provided on the same side of the substrate, the light resistance and heat resistance of the optical film can be well maintained if the functional layer formed on the colored layer has sufficient ultraviolet shielding ability. On the other hand, Comparative Examples 1 to 4, which did not satisfy the above formula (1), generally had no problems in terms of hardness, but neither light resistance nor heat resistance was sufficient. Comparative Example 5 satisfied formula (1) above and had no problems with lightfastness and heat resistance, but because it did not contain any of the first, second, or third colorants in the colored layer, its color reproduction was insufficient. Comparative Example 6 also showed no significant problems in terms of hardness, but both its light resistance and heat resistance were insufficient. This was thought to be due to an insufficient amount of the compound containing only two (meth)acryloyl groups with an alicyclic skeleton in the energy ray curable compound. From the results of Comparative Example 7, it was considered that even if the colored layer satisfies formula (1) above, if the layer through which the incident ambient light passes before it reaches the colored layer does not have sufficient UV shielding ability, the light resistance of the optical film may not be sufficient. [Explanation of Symbols]

[0130] 1, 3, 4, 5, 7, 8 Optical film 10 Colored layer 20 Transparent base material 30 Functional Layers 31 Low refractive index layer 32 Hard Court Layers 34 Anti-glare layer

Claims

1. A sheet-like transparent substrate, A colored layer formed on the first surface side of the transparent substrate, In the transparent substrate, a functional layer formed on the second surface opposite to the first surface, or on the colored layer, Equipped with, At least one of the transparent substrate and the functional layer has an ultraviolet shielding rate of 85% or more, as measured in accordance with JIS L1925. The colored layer consists of a cured product containing a dye (A), an energy ray curable compound (B), a photopolymerization initiator (C), and a radical scavenger (D). The aforementioned pigment (A) contains at least one of the first colorant, the second colorant, and the third colorant. The first colorant has an absorption maximum wavelength in the range of 470 to 530 nm, and the full width at half maximum of its absorption spectrum is 15 to 45 nm. The second colorant has an absorption maximum wavelength in the range of 560 to 620 nm, and the full width at half maximum of its absorption spectrum is 15 to 55 nm. The third colorant has the lowest transmittance in the wavelength range of 400 to 780 nm, with the wavelength having the lowest transmittance being in the range of 650 to 780 nm. The energy ray curable compound (B) contains 20% by weight or more of a compound having only two (meth)acryloyl groups including an alicyclic skeleton. In simultaneous thermogravimetric and heat measurements under conditions of a gas flow rate of 200 ml / min and a heating rate of 10°C / min, the difference between the temperature at which the colored layer loses 50% of its weight under a nitrogen atmosphere and the temperature at which it loses 50% of its weight under an air atmosphere is 60°C or less. Optical film.

2. The radical scavenger (D) is a polymer containing a structural unit represented by the following formula (i). The optical film according to claim 1. 【Chemistry 1】 [In equation (i), R 12 R represents a hydrogen atom, halogen atom, carboxyl group, sulfo group, cyano group, hydroxyl group, alkyl group having 10 or fewer carbon atoms, alkoxycarbonyl group having 10 or fewer carbon atoms, alkylsulfonylaminocarbonyl group having 10 or fewer carbon atoms, arylsulfonylaminocarbonyl group, alkylsulfonyl group, arylsulfonyl group, acylaminosulfonyl group having 10 or fewer carbon atoms, alkoxy group having 10 or fewer carbon atoms, alkylthio group having 10 or fewer carbon atoms, aryloxy group having 10 or fewer carbon atoms, nitro group, alkoxycarbonyloxy group, aryloxycarbonyloxy group, acyloxy group having 10 or fewer carbon atoms, acyl group having 10 or fewer carbon atoms, carbamoyl group, sulfamoyl group, aryl group having 10 or fewer carbon atoms, substituted amino group, substituted ureido group, substituted phosphono group, or heterocyclic group. 13 X represents a hydrogen atom or an alkyl group having 30 or fewer carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or fewer carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by a combination thereof, all of which may contain a spirodioxane ring.

3. The colored layer contains any of the following: dialkyldithiophosphate, dialkyldithiocarbanate, benzenedithiol, and transition metal complexes thereof, as well as a compound represented by the following formula (ii). The optical film according to claim 1. 【Chemistry 2】 [In formula (ii), R 1 each independently represents an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, or a group represented by R 9 CO - , R 10 SO 2 - or R 11 NHCO - , and R 9 , R 10 and R 11 each independently represent an alkyl group, an alkenyl group, an aryl group, or a heterocyclic group. R 2 and R 3 each independently represent a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, or an alkenyloxy group, and R 4 to R 8 each independently represent a hydrogen atom, an alkyl group, an alkenyl group, or an aryl group.]

4. The dye (A) comprises one or more compounds selected from the group consisting of compounds having any of the following structures: porphyrin structure, merocyanine structure, phthalocyanine structure, azo structure, cyanine structure, squarylium structure, coumarin structure, polyene structure, quinone structure, tetradiporphyrin structure, pyromethene structure, and indigo structure, as well as metal complexes thereof. The optical film according to claim 1.

5. The pencil hardness of the surface of the colored layer under a 500g load is H or higher. The optical film according to claim 1.

6. The functional layer functions as at least one of an anti-reflective layer and an anti-glare layer. The optical film according to claim 1.

7. The functional layer has an antistatic layer or an antifouling layer. The optical film according to claim 1.

8. The optical film comprises the optical film described in claim 1. Display device.

Citation Information

Patent Citations

  • Prevention of freezing of marine structure

    JP1981073713A

  • Color filter and color liquid crystal display element

    JP2012155243A

  • Display optical filter and display having the same

    JP2019056865A

  • JPP7103544B

  • Optical filter for an organic electroluminescence device

    KR1020150039300A