Steel plates, components, and methods for manufacturing them.
A tailored steel composition and manufacturing process enhance the yield ratio, ductility, and delayed fracture resistance of high-strength steel sheets, addressing the limitations of existing technologies for automotive structural components.
Patent Information
- Application Number
- JP2026521073
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2025-01-24
- Filing Date
- 2025-12-08
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-12-08
AI Technical Summary
Existing high-strength steel sheets for automobiles lack sufficient yield ratio, ductility, and delayed fracture resistance in the bending compression section, especially in corrosive environments, which are critical for structural components like floor cross members.
A steel composition with specific element ranges and microstructural controls, including high tempered martensite content, limited retained austenite and ferrite-bainitic ferrite fractions, and controlled dislocation distribution, along with a manufacturing process involving annealing and tempering, to achieve tensile strength of 1180 MPa, yield ratio of 65%, and excellent ductility and delayed fracture resistance.
The steel sheets exhibit enhanced mechanical properties, enabling weight reduction in vehicles, improved collision resistance, and increased fuel efficiency by maintaining structural integrity in corrosive conditions.
Smart Images

Figure 0007948494000007 
Figure 0007948494000008 
Figure 0007948494000001
Abstract
Description
[Technical Field]
[0001] This invention relates to steel sheets, components, and methods for manufacturing them, which exhibit excellent tensile strength, yield ratio, ductility, and delayed fracture resistance at the bending compression portion in corrosive environments. The steel sheets of this invention can be suitably used as structural components for automobile parts and the like. [Background technology]
[0002] To achieve both a reduction in CO2 emissions through vehicle weight reduction and improved collision resistance through vehicle weight reduction, the strength of thin steel sheets for automobiles is being increased, and new legal regulations are being introduced one after another. As a result, in order to increase the strength of the vehicle body, the application of high-strength steel sheets with a tensile strength of 1180 MPa or higher (TS) is increasing in major structural components that make up automobiles.
[0003] High-strength steel sheets used in automobiles are required to have excellent yield ratio, excellent ductility, and excellent delayed fracture resistance in the bent compression section in corrosive environments. For example, in structural components such as floor cross members of automobiles, it is preferable to use steel sheets with excellent ductility from the viewpoint of formability. Furthermore, from the viewpoint of component performance, excellent yield ratio and excellent delayed fracture resistance in the bent compression section in corrosive environments are required.
[0004] Patent Document 1 discloses a high-strength steel sheet with a yield ratio of 1180 MPa or higher, excellent flatness in the width direction, and resistance to work-induced embrittlement, and a method for manufacturing the same. However, the technology described in Patent Document 1 does not take into account the delayed fracture resistance of the bending compression section in a corrosive environment.
[0005] Patent Document 2 discloses a high-strength steel sheet with excellent ductility and shear end face resistance to bending cracks, and a high yield ratio of 1180 MPa or higher, as well as a method for manufacturing the same. However, the technology described in Patent Document 2 does not take into account the delayed fracture resistance of the bending compression portion in a corrosive environment.
[0006] Patent Document 3 discloses a method for manufacturing high-strength steel sheets with excellent ductility, elongation flangeability, and mechanical stability, with a strength of 980 MPa or higher. However, the technology described in Patent Document 3 does not take into account the yield ratio and the delayed fracture resistance of the bending compression section in a corrosive environment. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Patent No. 7323093 [Patent Document 2] Patent No. 7298647 [Patent Document 3] Patent No. 5333298 [Overview of the project] [Problems that the invention aims to solve]
[0008] The present invention was developed in view of these circumstances, and aims to provide steel plates, components, and methods for manufacturing them, which have a tensile strength TS of 1180 MPa or higher, a yield ratio YR of 65% or higher, and excellent ductility and delayed fracture resistance at the bending compression portion in a corrosive environment.
[0009] Here, the tensile strength TS (hereinafter also simply referred to as TS) and the yield ratio YR (hereinafter also simply referred to as YR) can be measured in accordance with JIS Z 2241 (2022). Excellent ductility means that the TS × El, as determined by the measurement method according to JIS Z 2241 (2022), is 14,000 MPa·% or higher. Excellent delayed fracture resistance in a bent compression section in a corrosive environment means that, for a V-bend test specimen that has undergone a baking treatment of being held at 170°C for 20 minutes after V-bending, the R / t (represented by the relationship between the plate thickness t and the radius of curvature R of the bending process) is 3.5, and the number of days to crack in a delayed fracture test in a corrosive environment is 63 days or more. [Means for solving the problem]
[0010] In order to achieve the above-mentioned objectives, the inventors conducted extensive research and, as a result, discovered the following: (1) By setting the area fraction of tempered martensite to 83% or more, a total stress point (TS) of 1180 MPa or higher can be achieved. (2) By making the total area fraction of ferrite and bainitic ferrite 5% or more, excellent ductility can be achieved. (3) By keeping the volume fraction of retained austenite to less than 3% and the total area fraction of ferrite and bainitic ferrite to less than 15%, a YR of 65% or more can be achieved. (4) By setting {C(B)-C(A)} to 3.5 at% or more for the average carbon concentration (at%) within the grains of tempered martensite (C(A)) and the carbon concentration (at%) at the prior austenite grain boundaries (C(B)), and by setting the M value, which represents the distribution state of dislocations in tempered martensite, to 1.5 or less, excellent delayed fracture resistance in the bending compression section in a corrosive environment can be achieved.
[0011] This invention is based on the above findings. Specifically, the gist of this invention is as follows: [1] In mass%, C: 0.030% or more and 0.500% or less, Si: 0.010% or more and 2.500% or less, Mn: 0.10% or more and 5.00% or less, P: 0.100% or less, S: 0.0200% or less, Al: 1.000% or less, N: 0.0100% or less, and, O: 0.0100% or less It contains, with the remainder being Fe and unavoidable impurities, and has a component composition. At the point where the plate thickness is 1 / 4, Area fraction of tempered martensite: 83% or more. Volume fraction of retained austenite: less than 3%, The total area fraction of ferrite and bainitic ferrite is 5% or more and less than 15%, The M value representing the dislocation distribution state of the tempered martensite is 1.5 or less, A steel sheet having a steel microstructure that satisfies the following formula (1). {C(B)-C(A)}≧ 3.5at% ···(1) In formula (1), C(A): the average carbon concentration (at%) within the grains of the tempered martensite, C(B): the carbon concentration (at%) at the prior austenite grain boundaries. [2] The steel sheet according to the above [1], wherein the component composition further contains, in mass%, Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less, Ni: 1.00% or less, Co: 0.010% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, Bi: 0.200% or less, The steel sheet according to the above [1], containing at least one element selected from the group consisting of the above elements. [3] The steel sheet according to the above [1] or [2], having a plating layer on the surface of the steel sheet. [4] A member formed using the steel sheet according to any one of the above [1] to [3]. [5] A cold-rolled sheet made by hot-rolling, pickling and cold-rolling a steel having the component composition described in [1] or [2] above, Annealing temperature T1: 750℃ or higher and 850℃ or lower. Holding time t1 at annealing temperature T1: 10 seconds or more. An annealing process in which heating is performed under conditions of an average tensile stress S1 of 5 MPa or more at an annealing temperature T1, Average cooling rate CR1 at 700-500℃: less than 50℃ / s. Average tensile stress S2 from annealing temperature T1 to cooling stop temperature T2: 10 MPa or more. A cooling process in which cooling is performed under the condition that the cooling stop temperature T2 is 80℃ or lower, Tempering temperature T3: 100℃ or higher, Average tensile stress S3 during tempering treatment: 20 MPa or more. A method for manufacturing a steel sheet, comprising a tempering step in which the steel sheet is heated under the condition that the holding time t3 at a tempering temperature T3 is between 10 seconds and 10,000 seconds. [6] A method for manufacturing a steel sheet according to [5], wherein a plating treatment is applied. [7] A method for manufacturing a component, comprising the step of forming and joining a steel plate according to any one of [1] to [3] above to form a component. [Effects of the Invention]
[0012] According to the present invention, a steel sheet can be obtained that has a TS of 1180 MPa or higher, a YR of 65% or higher, and excellent ductility and delayed fracture resistance at the bending compression section in corrosive environments. Furthermore, by applying the steel sheet of the present invention to, for example, automotive structural members, it is possible to improve fuel efficiency by reducing the weight of the vehicle body. Therefore, its industrial utility is extremely large. [Brief explanation of the drawing]
[0013] [Figure 1] Figure 1 is a schematic diagram illustrating the method for evaluating the delayed fracture characteristics of a test specimen (HeTsAce). [Figure 2] Figure 2 schematically shows how the spray liquid in the atmosphere re-adheses to the evaluation surface when the distance between the shielding material and the evaluation surface of the test specimen is changed. [Modes for carrying out the invention]
[0014] Embodiments of the present invention will be described below. [Steel plate] The steel sheet of the present invention has a composition in mass%, containing C: 0.030% to 0.500%, Si: 0.010% to 2.500%, Mn: 0.10% to 5.00%, P: 0.100% or less, S: 0.0200% or less, Al: 1.000% or less, N: 0.0100% or less, and O: 0.0100% or less, with the remainder being Fe and unavoidable impurities. At the 1 / 4 position of the sheet thickness, the area fraction of tempered martensite is 83% or more, the volume fraction of retained austenite is less than 3%, the total area fraction of ferrite and bainitic ferrite is 5% or more and less than 15%, the M value representing the distribution state of dislocations in tempered martensite is 1.5 or less, and the steel structure satisfies the following formula (1). {C(B)-C(A)}≧ 3.5at% ···(1) In formula (1), C(A): Average carbon concentration within the grains of tempered martensite (at%) C(B): Carbon concentration (at%) at the prior austenite grain boundary.
[0015] First, we will explain the appropriate range of the steel sheet's composition and the reasons for its limitations. In the following explanation, the "%" used to represent the content of the steel's constituent elements means "mass percent" unless otherwise specified.
[0016] C: 0.030% or more and 0.500% or less Carbon (C) is one of the important basic components of steel, and in particular in this invention, it is an important element that affects the area fraction of tempered martensite and the delayed fracture resistance of the bending compression section in a corrosive environment. If the C content is less than 0.030%, the total area fraction of ferrite and bainitic ferrite increases, and the area fraction of tempered martensite decreases, making it difficult to achieve a YR of 65% or more and a TS of 1180 MPa or more. On the other hand, if the C content exceeds 0.500%, the tempered martensite becomes brittle, making it difficult to obtain excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the C content should be between 0.030% and 0.500%. Preferably, the C content should be 0.050% or more. More preferably, the C content should be 0.100% or more. Also, preferably, the C content should be 0.400% or less. More preferably, the C content should be 0.350% or less.
[0017] Si: 0.010% or more and 2.500% or less Si is one of the important basic components of steel, and in this invention in particular, it is an important element that affects the volume fraction of retained austenite because it suppresses carbide formation during continuous annealing and promotes the formation of retained austenite. It is also an important element that affects TS. If the Si content is less than 0.010%, it becomes difficult to achieve a TS of 1180 MPa or higher. On the other hand, if the Si content exceeds 2,500%, the amount of retained austenite increases excessively, making it difficult to achieve YR ≥ 65%. Therefore, the Si content should be between 0.010% and 2,500%. Preferably, the Si content should be 0.050% or more. More preferably, the Si content should be 0.100% or more. Also, preferably, the Si content should be 2,000% or less. More preferably, the Si content should be 1,200% or less.
[0018] Mn: 0.10% or more and 5.00% or less Mn is one of the important basic components of steel, and in particular in this invention, it is an important element that affects the area fraction of tempered martensite and the delayed fracture resistance in corrosive environments. If the Mn content is less than 0.10%, the total area fraction of ferrite and bainitic ferrite increases, and the area fraction of tempered martensite decreases, making it difficult to achieve a YR of 65% or more and a TS of 1180 MPa or more. On the other hand, if the Mn content exceeds 5.00%, corrosion of the steel plate is accelerated, and hydrogen generation associated with corrosion is also accelerated, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the Mn content should be between 0.10% and 5.00%. Preferably, the Mn content should be 0.50% or more. More preferably, the Mn content should be 0.80% or more. Furthermore, preferably, the Mn content should be 4.50% or less. More preferably, the Mn content should be 4.00% or less.
[0019] P:0.100% or less Since phosphorus (P) segregates at prior austenite grain boundaries and embrittles them, if its content exceeds 0.100%, it becomes difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the P content must be 0.100% or less. Preferably, the P content is 0.070% or less. Although there is no specific lower limit for the P content, since P is a solid solution strengthening element and can increase the strength of the steel sheet, it is preferable that the P content be 0.001% or more. More preferably, the P content is 0.002% or more.
[0020] S: 0.0200% or less S exists as a sulfide, and if its content exceeds 0.0200%, it embrittles the steel plate, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the S content must be 0.0200% or less. Preferably, the S content is 0.0050% or less. Although there is no specific lower limit for the sulfur content, due to production technology constraints, it is preferable that the sulfur content be 0.0001% or more. More preferably, the sulfur content is 0.0002% or more.
[0021] Al: 1.000% or less Al exists as an oxide, and if its content exceeds 1,000%, it embrittles the steel sheet, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the Al content must be 1,000% or less. Accordingly, the Al content should be 1,000% or less. Preferably, the Al content should be 0.500% or less. Although there is no specific lower limit for the Al content, due to production technology constraints, it is preferable that the Al content be 0.001% or higher. More preferably, the Al content should be 0.002% or higher.
[0022] N: 0.0100% or less N exists as a nitride, and if its content exceeds 0.0100%, it embrittles the steel sheet, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the N content must be 0.0100% or less. Preferably, the N content is 0.0050% or less. Although there is no specific lower limit for the N content, due to production technology constraints, it is preferable that the N content be 0.0001% or higher.
[0023] O: 0.0100% or less O exists as an oxide, and if its content exceeds 0.0100%, it embrittles the steel plate, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the O content must be 0.0100% or less. Accordingly, the O content should be 0.0100% or less. Preferably, the O content should be 0.0050% or less. Although there is no specific lower limit for the O content, due to production technology constraints, it is preferable that the O content be 0.0001% or higher.
[0024] A steel sheet according to one embodiment of the present invention has a composition containing the above components, with the remainder being Fe and unavoidable impurities. A steel sheet according to one embodiment of the present invention may have a composition containing the above components, with the remainder being Fe and unavoidable impurities. Examples of unavoidable impurities include Zn, Pb, As, Ge, Sr, and Cs. These impurities may be present in a total amount of 0.100% or less.
[0025] In addition to the above component composition, the steel sheet of the present invention may further contain, by mass%, at least one element selected from Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less, Ni: 1.00% or less, Co: 0.010% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, and Bi: 0.200% or less, either alone or in combination.
[0026] Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less If Ti, Nb, and V are present in amounts of 0.200% or less, large amounts of coarse precipitates and inclusions will not be generated, and the steel sheet will not become brittle, thus preventing a decrease in the delayed fracture resistance of the bending compression section in a corrosive environment. Therefore, when at least one of Ti, Nb, and V is included, the content of Ti, Nb, and V should be 0.200% or less each. Preferably, the content of each is 0.100% or less. There is no particular lower limit for the content of Ti, Nb, and V, but since the strength of the steel sheet is increased by forming fine carbides, nitrides, or carbonitrides during hot rolling or continuous annealing, it is preferable that the content of Ti, Nb, and V be 0.001% or more each. More preferably, the content of each is 0.002% or more, and even more preferably 0.003% or more.
[0027] Ta: 0.10% or less, W: 0.10% or less If the content of Ta and W is 0.10% or less, large amounts of coarse precipitates and inclusions will not be generated, and the steel sheet will not become brittle, thus preventing a decrease in the delayed fracture resistance of the bending compression section in a corrosive environment. For this reason, when at least one of Ta and W is included, the content of Ta and W should be 0.10% or less each. Preferably, the content of each is 0.08% or less. There is no particular lower limit for the content of Ta and W, but since the strength of the steel sheet is increased by forming fine carbides, nitrides, or carbonitrides during hot rolling or continuous annealing, it is preferable that the content of Ta and W be 0.01% or more each. More preferably, the content of each is 0.02% or more, and even more preferably 0.03% or more.
[0028] B: 0.0100% or less If B is present in a concentration of 0.0100% or less, it does not cause cracks to form inside the steel sheet during casting or hot rolling, and does not embrittle the steel sheet, thus preventing a decrease in the delayed fracture resistance of the bending compression section in a corrosive environment. For this reason, when B is included, its content should be 0.0100% or less. Preferably, the B content should be 0.0080% or less. Although there is no specific lower limit for the B content, it is preferable that the B content be 0.0003% or more, as it is an element that segregates at the austenite grain boundaries during annealing and improves hardenability.
[0029] Cr: 1.00% or less, Mo: 1.00% or less, Ni: 1.00% or less If the content of Cr, Mo, and Ni is 1.00% or less, the amount of coarse precipitates and inclusions will not increase, and the steel sheet will not become brittle, thus not reducing the delayed fracture resistance of the bending compression section in a corrosive environment. For this reason, when at least one of Cr, Mo, and Ni is included, the content of Cr, Mo, and Ni should be 1.00% or less each. Preferably, the content of each is 0.80% or less. More preferably, the content of each is 0.75% or less, and even more preferably 0.70% or less. There is no particular lower limit for the content of Cr, Mo, and Ni, but since they are elements that improve hardenability, it is preferable that the content of Cr, Mo, and Ni be 0.01% or more each. More preferably, the content of each is 0.02% or more.
[0030] Co:0.010% or less If the Co content is 0.010% or less, it does not increase coarse precipitates or inclusions and does not embrittle the steel plate, thus not reducing the delayed fracture resistance of the bending compression section in a corrosive environment. For this reason, when Co is included, the Co content should be 0.010% or less. Preferably, the Co content should be 0.008% or less. More preferably, the Co content should be 0.007% or less. There is no particular lower limit for the Co content, but since it is an element that improves hardenability, it is preferable that the Co content be 0.001% or more.
[0031] Cu:1.00% or less If the Cu content is 1.00% or less, it does not increase coarse precipitates or inclusions and does not embrittle the steel plate, thus not reducing the delayed fracture resistance of the bending compression section in a corrosive environment. For this reason, when Cu is included, the Cu content should be 1.00% or less. Preferably, the Cu content should be 0.80% or less. There is no specific lower limit for the Cu content, but since Cu is an element that improves hardenability, it is preferable that the Cu content be 0.01% or more.
[0032] Sn: 0.200% or less If the Sn content is 0.200% or less, it does not cause cracks to form inside the steel sheet during casting or hot rolling, and does not embrittle the steel sheet, so the delayed fracture resistance of the bending compression section in a corrosive environment does not decrease. For this reason, when Sn is included, the Sn content should be 0.200% or less. Preferably, the Sn content should be 0.150% or less. There is no particular lower limit for the Sn content, but since Sn is an element that improves hardenability (generally an element that improves corrosion resistance), it is preferable that the Sn content be 0.001% or more. More preferably, the Sn content should be 0.002% or more.
[0033] Sb: 0.200% or less If the Sb content is 0.200% or less, the amount of coarse precipitates and inclusions does not increase, and the steel plate does not become brittle, so the delayed fracture resistance of the bending compression section in a corrosive environment does not decrease. For this reason, when Sb is included, the Sb content should be 0.200% or less. Preferably, the Sb content should be 0.150% or less. More preferably, the Sb content should be 0.100% or less. There is no particular lower limit for the Sb content, but since it is an element that controls the surface softening thickness and allows for strength adjustment, it is preferable that the Sb content be 0.001% or more. More preferably, the Sb content should be 0.002% or more.
[0034] Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less If Ca, Mg, and REM are present in amounts of 0.0100% or less, the amount of coarse precipitates and inclusions does not increase, and the steel sheet does not become brittle, thus preventing a decrease in the delayed fracture resistance of the bending compression section in a corrosive environment. Therefore, when at least one of Ca, Mg, and REM is included, the content of Ca, Mg, and REM should be 0.0100% or less each. Preferably, the content of each is 0.0050% or less. Although there is no specific lower limit for the content of Ca, Mg, and REM, it is preferable that the content of Ca, Mg, and REM be 0.0001% or more each, since these elements spheroidize the shape of nitrides and sulfides and improve the delayed fracture resistance of the bending compression section in a corrosive environment. More preferably, the content of each is 0.0002% or more, and even more preferably 0.0005% or more.
[0035] Zr: 0.100% or less, Te: 0.100% or less If the content of Zr and Te is 0.100% or less, the amount of coarse precipitates and inclusions does not increase, and the steel sheet does not become brittle, so the delayed fracture resistance of the bending compression section in a corrosive environment does not decrease. For this reason, when at least one of Zr and Te is included, the content of Zr and Te should be 0.100% or less. Preferably, the content of each is 0.080% or less. There is no particular lower limit for the content of Zr and Te, but since these elements spheroidize the shape of nitrides and sulfides and improve the delayed fracture resistance of the bending compression section in a corrosive environment, it is preferable that the content of Zr and Te be 0.001% or more. More preferably, the content of each is 0.002% or more, and even more preferably 0.003% or more.
[0036] Hf: 0.10% or less If Hf is present at a concentration of 0.10% or less, it does not increase the amount of coarse precipitates or inclusions, and does not embrittle the steel sheet, thus preventing a decrease in the delayed fracture resistance of the bending compression section in a corrosive environment. For this reason, when Hf is included, the Hf content should be 0.10% or less. Preferably, the Hf content should be 0.09% or less. More preferably, the Hf content should be 0.08% or less, and even more preferably, 0.07% or less. There is no specific lower limit for the Hf content, but since Hf is an element that spheroidizes the shape of nitrides and sulfides and improves the delayed fracture resistance of the bending compression section in a corrosive environment, it is preferable that the Hf content be 0.01% or more.
[0037] Bi:0.200% or less If the Bi content is 0.200% or less, it does not increase coarse precipitates or inclusions and does not embrittle the steel plate, thus not reducing the delayed fracture resistance of the bending compression section in a corrosive environment. For this reason, when Bi is included, the Bi content should be 0.200% or less. Preferably, the Bi content should be 0.190% or less. There is no particular lower limit for the Bi content, but since it is an element that reduces segregation, it is preferable that the Bi content be 0.001% or more. More preferably, the Bi content should be 0.002% or more, and even more preferably 0.003% or more.
[0038] Furthermore, regarding the above-mentioned Ti, Nb, V, Ta, W, B, Cr, Mo, Ni, Co, Cu, Sn, Sb, Ca, Mg, REM, Zr, Te, Hf, and Bi, if their respective contents are below the preferred lower limit, they will not impair the effects of the present invention and will therefore be included as unavoidable impurities.
[0039] Next, the structural framework of the steel sheet of the present invention will be described.
[0040] Tempered martensite: 83% or more by area fraction In this invention, tempered martensite is one of the important constituent elements. By using tempered martensite as the main phase, it is possible to achieve a total stress point (TS) of 1180 MPa or higher. In order to obtain this effect, the area fraction of tempered martensite must be 83% or more. Therefore, the area fraction of tempered martensite is set to 83% or more. Preferably, the area fraction of tempered martensite is 84% or more. Furthermore, the area fraction of tempered martensite may be 95% or less, and is preferably 94% or less.
[0041] The measurement method for tempered martensite is as follows: After polishing the L-section of the steel plate, it is etched with 1 vol.% nital, and 1 / 4 of the plate thickness (a position corresponding to 1 / 4 of the plate thickness in the depth direction from the surface of the steel plate) is observed using a SEM at 2000x magnification with a field of view of 30 μm × 30 μm for 10 fields. In the above microstructure image, tempered martensite is a structure with fine irregularities inside and contains carbides. The tempered martensite can be determined from the average value of these values.
[0042] Retained austenite: Less than 3% by volume fraction This is one of the important constituent elements of the present invention. When the volume fraction of retained austenite is 3% or more, it becomes difficult to achieve YR ≥ 65%. The reason why it becomes difficult to achieve YR ≥ 65% is that the retained austenite transforms into martensite during the tensile test, causing a decrease in YS. Therefore, the volume fraction of retained austenite should be less than 3%. Preferably, the volume fraction of retained austenite should be 1% or less. The lower limit of retained austenite is not particularly limited and may be 0%.
[0043] The method for measuring retained austenite is as follows: After polishing a steel plate to a surface that is 1 / 4 of its thickness, the surface is further polished by 0.1 mm using chemical polishing. Using an X-ray diffractometer with CoKα rays, the integral intensity ratios of the diffraction peaks of the {200}, {220}, and {311} planes of fcc iron and the {200}, {211}, and {220} planes of bcc iron are measured, and the retained austenite is determined by averaging the nine (=3×3) integral intensity ratios for the three planes of each crystal structure.
[0044] Total of ferrite and bainitic ferrite: 5% or more but less than 15% in area fraction In this invention, this is one of the important constituent elements of the invention. When the total amount of ferrite and bainitic ferrite is 15% or more, it becomes difficult to achieve YR ≥ 65%. On the other hand, if the total area fraction of ferrite and bainitic ferrite falls below 5%, it becomes difficult to achieve excellent ductility. Therefore, the total area fraction of ferrite and bainitic ferrite should be 5% or more and less than 15%. Preferably, the total area fraction of these materials should be 6% or more. Preferably, the total area fraction of these materials should be 13% or less.
[0045] The method for measuring the total amount of ferrite and bainitic ferrite is as follows: After polishing the L-section of the steel plate, it is etched with 1 vol.% nital, and 1 / 4 of the plate thickness (a position corresponding to 1 / 4 of the plate thickness in the depth direction from the surface of the steel plate) is observed using a SEM at 2000x magnification with a field of view of 30 μm × 30 μm for 10 fields. In the above microstructure image, ferrite and bainitic ferrite are structures with a flat interior in the recesses and do not contain carbides. The total amount of ferrite and bainitic ferrite can be determined from the average value of these values.
[0046] The steel structure of the steel sheet of the present invention may consist of tempered martensite, retained austenite, ferrite, and bainitic ferrite, but other structures such as pearlite, fresh martensite, and acicular ferrite can also be considered. These structures may be included as long as they are within a range of 5% or less, as they do not affect the properties.
[0047] M value representing the distribution state of dislocations in tempered martensite: 1.5 or less In this invention, the distribution of dislocations in tempered martensite is one of the important constituent elements. The distribution of dislocations in tempered martensite affects the delayed fracture resistance of the bending and compression section in a corrosive environment. As described in Non-Patent Literature 1 (Iron and Steel, Vol. 93, No. 459, pp. 159-456), the distribution of dislocations in tempered martensite is known to be random immediately after martensitic transformation. Furthermore, by analyzing the X-ray diffraction peaks obtained from XRD (X-Ray Diffraction) using the modified Williamson-Hall / Warren-Averbach method (mWH / WA method) described in Non-Patent Literature 2 (Plasticity and Processing, Vol. 58, No. 682, pp. 1004-1008), it is possible to evaluate the M value representing the distribution of dislocations. When the M value is large, it can be evaluated that the dislocations are randomly distributed, and when the M value is small, it can be evaluated that the dislocations take on a stable arrangement such as dislocation cells. As a result of diligent research, the inventors have found that by changing the distribution state of dislocations in tempered martensite to a stable arrangement such as dislocation cells, specifically by setting the M value to 1.5 or less, random dislocations that embrittle steel due to interaction with hydrogen in corrosive environments can be reduced, thereby improving the delayed fracture resistance of the bending compression section in corrosive environments. Therefore, the M value representing the distribution state of dislocations in tempered martensite should be 1.5 or less. Preferably, this M value should be 1.3 or less. Furthermore, there is no particular limit to the lower limit of the M value, which represents the distribution state of dislocations in tempered martensite. In the inventors' investigation, the minimum value of the M value was 0.1. Therefore, the M value representing the distribution state of dislocations in tempered martensite is preferably 0.1 or higher, but it is not necessary to limit it to this.
[0048] The M-value, which represents the dislocation distribution state of tempered martensite, was evaluated by analyzing the X-ray diffraction peaks obtained from XRD. First, a specimen for XRD was taken from a steel plate. Next, the taken specimen was mechanically ground down to 1 / 4 of the plate thickness (a position corresponding to 1 / 4 of the plate thickness in the depth direction from the surface of the steel plate). Then, to remove the strain effect of grinding, the ground surface was chemically polished with oxalic acid to remove 100 μm of the ground surface. XRD measurements were then performed on the sample using Cu-Kα1 as the X-ray source and α-Fe(110), (200), (211), and (310) as the measurement surfaces. From the obtained X-ray diffraction peaks, the dislocation density and the M-value, which is the dislocation arrangement parameter, were analyzed based on the modified Williamson-Hall / Warren-Averbach method (mWH / WA method). In this invention, the modified Williamson-Hall / Warren-Averbach method (mWH / WA method) used for measuring the M value is a data analysis technique obtained by XRD, and was calculated using the methods described in Participating Reference 1 and Reference 2 below. The following data input values were used in the calculation. Diffraction planes used for analysis: {100}, {200}, {211}{310} planes of bcc iron. Standard sample for instrument constant correction: pure iron Instrument constant correction method: Stokes method Numerical value of the constant term in the analysis method: C h00 S =0.298, C h00 E =0.262, q S =2.652, q E =1.372 [Reference 1] D.Akama, T.Tsuchiyama and S.Takaki: ISIJ Int., 56(2016), 1675. [Reference 2] Takuro Masumura, Setsuo Takagi, and Satoshi Tsuchiyama: Iron and Steel, 106(2020), 183.
[0049] {C(B)-C(A)}≧ 3.5at% ···(1) In formula (1), C(A): Average carbon concentration within the grains of tempered martensite (at%) C(B): Carbon concentration (at%) at prior austenite grain boundaries In this invention, C(B)-C(A) is one of the important constituent elements. The difference between C(B) and C(A) affects the delayed fracture resistance of the bending compression section in a corrosive environment. If {C(B)-C(A)} ≥ 3.5 at% is not satisfied, it means that the bonding force of the prior austenite grain boundaries is low compared to the strength within the prior austenite grains, and the initiation and propagation of cracks at the prior austenite grain boundaries are promoted. Therefore, {C(B)-C(A)} should be 3.5 at% or more. Preferably, {C(B)-C(A)} should be 7.0 at% or more. However, there is no particular upper limit to {C(B)-C(A)}. In the inventors' investigation, the maximum value of {C(B)-C(A)} was 22.0 at%. Therefore, {C(B)-C(A)} is preferably 22.0 at% or less, but it is not necessary to limit it to this.
[0050] Here, the measurement method for C(B)-C(A) is as follows. First, a specimen for scanning transmission electron microscopy (STEM) observation is prepared from a steel plate by focused ion beam (FIB) processing, and elemental analysis is performed by energy dispersive X-ray spectroscopy (STEM-EDS, hereafter also referred to as STEM / EDS). For sampling with the FIB instrument, the crystal orientation of the martensite is measured in advance by electron backscatter diffraction (EBSD), and a STEM sample containing prior austenite grain boundaries is taken out and thinned. In measuring the carbon content in steel using STEM-EDS, it is necessary to consider the strong influence of carbon, which is the main component of contamination. In this invention, a line profile perpendicular to the grain interface is obtained, and the carbon concentration (at%) at the prior austenite grain boundary (C(B)) and the average carbon concentration (at%) within the tempered martensite grains surrounding it (C(A)) are evaluated. This analysis is performed on 10 or more prior austenite grain boundaries and the surrounding tempered martensite grains, and the average value of the difference is taken as C(B)-C(A).
[0051] C(B)-C(A) is measured using energy-dispersive X-ray spectroscopy (EDS) with a scanning transmission electron microscope (STEM), as described above. For this measurement, it is important to efficiently select and measure the prior austenite grain boundaries. First, the sample surface is polished, and crystal orientation information is obtained by EBSD (Electron Backscatter Diffraction) measurement of the sample surface. By reconstructing the prior austenite grains from the crystal orientation of the martensite, the prior austenite grain boundaries are identified. The Nishiyama-Wassermann (NW) relationship is used as the correspondence between martensite and austenite. From the reconstructed orientation information, locations that can be considered grain boundaries are selected, and thin sections for STEM measurement are cut out by focused ion beam (FIB) processing.
[0052] Crystal orientation information of the thin section sample is obtained by transmission EBSD measurement of the thin section sample for STEM measurement. By reconstructing the prior austenite grains from the crystal orientation of the martensite, the prior austenite grain boundaries are identified. The Nishiyama-Wassermann (NW) relationship was used as the correspondence between martensite and austenite. From the reconstructed orientation information, locations that can be considered grain boundaries are selected and STEM / EDS measurements are performed.
[0053] When measuring grain boundaries using STEM / EDS, it is crucial that the grain interface is parallel to the transmission direction, as electrons pass through the sample. If the grain interface is tilted relative to the transmission direction, the peak shape of the element corresponding to the grain boundary will be broader than the actual peak shape when obtaining an elemental profile perpendicular to the grain interface. In other words, the maximum peak value will be underestimated, making it impossible to accurately measure the grain boundary concentration. Therefore, the tilt angle of the sample is adjusted so that the grain interface is horizontal to the transmission direction. The relevant grain boundary is identified using the STEM image, and the sample is subjected to STEM / EDS measurement at the tilt angle that minimizes the width of the defect recognizable as a grain boundary when the tilt angle of the sample is systematically changed.
[0054] Compositional analysis will be performed using STEM / EDS. In STEM / EDS analysis, the amount of characteristic X-ray absorption differs depending on the thickness of the thin section sample, which particularly affects the quantitative values of light elements. Therefore, the thickness of each thin section sample will be adjusted to be in the range of 90 nm to 110 nm. The thickness will be measured by first measuring the relative thickness using electron energy loss spectroscopy (EELS), and then calculating the product of the mean free paths of iron calculated using Iakoubovskii's formula. The magnification for STEM / EDS analysis will be 640,000x, and the pixel size will be 0.4 nm. Multiple line profiles crossing the prior austenite grain boundary will be obtained, and the average profile will be used as the line profile for that grain boundary. In STEM / EDS measurements, it is necessary to consider that the measurement is strongly influenced by carbon, which is the main component of contamination. The carbon concentration (at%) of the prior austenite grain boundary: C(B) will be the value of the peak top of the line profile. The average carbon concentration (at%) within the grains of tempered martensite, C(A), is defined as the average value of the line profile at a position 10 nm or more away from the peak top.
[0055] The STEM / EDS analysis results are used to determine whether the grain boundaries measured by STEM / EDS are prior austenite grain boundaries. Since phosphorus (P) segregates at grain boundaries in the austenite state before quenching, grain boundaries where P segregation can be confirmed are considered candidates. Here, confirmation of P segregation is achieved by obtaining a map of P across the grain boundary, ensuring that the grain boundary is recognizable as a line. In addition, it is determined whether the channeling contribution in the obtained profile is small and whether it is suitable for measuring the carbon (C) grain boundary concentration. In the carbon concentration profile across the grain boundary, it is confirmed that the average carbon concentration in each of the two matrix phases adjacent to the grain boundary is similar. If the difference in average carbon concentration is greater than 0.01 mass%, the STEM / EDS measurement result for that grain boundary is excluded.
[0056] When evaluating C(A) and C(B), the analysis data of the prior austenite grain boundaries will be used for evaluation if the following conditions are met for the thin film sample after pickup: reconstruction in transmission EBSD confirms that it is a prior martensite grain boundary, P segregates in STEM / EDS, and the difference in average carbon concentration within each grain of tempered martensite adjacent to the grain boundary is small (0.01 mass% or less). Ten or more grain boundaries that satisfy these conditions will be analyzed. The C(B)-C(A) of each grain boundary will be evaluated, and the average value will be taken as the C(B)-C(A) of the material.
[0057] The steel sheet of the present invention may have a plating layer on its surface. Examples of plating layers include zinc plating layers such as hot-dip galvanized layers, alloyed hot-dip galvanized layers, and electroplated zinc plating layers. Examples of plating layers other than zinc plating layers include aluminum plating layers and alloy plating layers. Examples of alloy plating layers include hot-dip zinc-aluminum-magnesium alloy plating layers and Zn-Ni electroalloy plating layers.
[0058] The thickness of the steel plate of the present invention is preferably 0.5 mm or more. Furthermore, the thickness is preferably 3.0 mm or less.
[0059] [Method of manufacturing steel plates] Next, the method for manufacturing steel sheets according to the present invention will be described. The present invention provides a method for manufacturing a steel sheet, comprising: an annealing step in which a cold-rolled sheet, prepared by hot-rolling, pickling, and cold-rolling a steel having the aforementioned component composition, is heated under the conditions of annealing temperature T1: 750°C to 850°C, holding time t1 at annealing temperature T1: 10 seconds or more, and average tensile stress S1 at annealing temperature T1: 5 MPa or more; a cooling step in which the sheet is cooled under the conditions of average cooling rate CR1: less than 50°C / s at 700 to 500°C, average tensile stress S2 from annealing temperature T1 to cooling stop temperature T2: 10 MPa or more, and cooling stop temperature T2: 80°C or less; and a tempering step in which the sheet is heated under the conditions of tempering temperature T3: 100°C or more, average tensile stress S3 during tempering: 20 MPa or more, and holding time t3 at tempering temperature T3: 10 seconds to 10,000 seconds. In the steel sheet manufacturing method of the present invention, each of the above temperatures refers to the surface temperature of the steel sheet or steel.
[0060] In this invention, the method for melting the steel material (steel slab) is not particularly limited, and any known melting method, such as a converter or electric furnace, is suitable. The steel slab (slab) is preferably manufactured by a continuous casting method to prevent macrosegregation.
[0061] In the present invention, the slab heating temperature, slab soaking time, and coiling temperature in hot rolling are not particularly limited. Methods for hot rolling a steel slab include a method of heating the slab before rolling, a method of directly rolling a slab after continuous casting without heating it, and a method of subjecting a slab after continuous casting to a short-time heat treatment before rolling. The slab heating temperature, slab soaking time, finish rolling temperature, and coiling temperature in hot rolling are not particularly limited, but the slab heating temperature is preferably 1100°C or higher. The slab heating temperature is preferably 1300°C or lower. A slab heating time of 30 minutes or more is preferable. A slab heating time of 250 minutes or less is preferable. The finishing rolling temperature is preferably above the Ar3 transformation point. Furthermore, a winding temperature of 350°C or higher is preferable. Also, a winding temperature of 650°C or lower is preferable.
[0062] The hot-rolled steel sheets produced in this manner are then pickled. Pickling is important for ensuring good chemical conversion treatment properties and plating quality in the final high-strength steel sheet product because it removes oxides from the surface of the steel sheet. Pickling may be performed once or in multiple stages. Furthermore, the hot-rolled and pickled sheets may be cold-rolled immediately, or they may be cold-rolled after heat treatment.
[0063] The reduction ratio (cumulative reduction ratio) in cold rolling and the thickness of the sheet after rolling are not particularly limited, but a reduction ratio of 30% or more is preferred. Furthermore, a reduction ratio of 80% or less is preferred. The effects of the present invention can be obtained without any particular limitations on the number of rolling passes or the reduction ratio of each pass.
[0064] Annealing process The cold-rolled sheet obtained as described above is then annealed. The annealing conditions are as follows:
[0065] Annealing temperature T1: 750℃ or higher and 850℃ or lower If the annealing temperature T1 is less than 750°C, the area fraction of tempered martensite decreases, making it difficult to achieve a YR of 65% or more and a TS of 1180 MPa or more. On the other hand, if the annealing temperature T1 exceeds 850°C, the total area fraction of ferrite and bainitic ferrite becomes less than 5%, making it difficult to achieve excellent ductility. Therefore, the annealing temperature T1 should be between 750°C and 850°C. The annealing temperature T1 is preferably 760°C or higher, and more preferably 770°C or higher. The annealing temperature T1 is preferably 840°C or lower, and more preferably 830°C or lower. The annealing temperature referred to here is the holding temperature during the annealing process. The annealing temperature may remain constant during holding. Furthermore, the annealing temperature does not need to be constantly constant during holding, as long as it is within the temperature range of 750°C to 850°C and the temperature fluctuation is within ±10°C of the set temperature.
[0066] Holding time at annealing temperature T1: 10 seconds or more If the holding time t1 at annealing temperature T1 is less than 10 seconds, the total area fraction of ferrite and bainitic ferrite increases, and the area fraction of tempered martensite decreases, making it difficult to achieve a YR of 65% or more and a TS of 1180 MPa or more. Therefore, the holding time t1 at annealing temperature T1 should be 10 seconds or more. Preferably, the holding time t1 is 30 seconds or more. There is no particular upper limit, but a holding time t1 of 1000 seconds or less is preferable.
[0067] Average tensile stress S1 at annealing temperature T1: 5 MPa or higher In this invention, the average tensile stress S1 at annealing temperature T1 affects the carbon diffusion rate and the degree of segregation at the prior austenite grain boundaries, and thus affects {C(B)-C(A)}. If the average tensile stress S1 at annealing temperature T1 is less than 5 MPa, {C(B)-C(A)} will be less than 3.5 at%, which promotes crack initiation and crack propagation at the prior austenite grain boundaries, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the average tensile stress S1 at annealing temperature T1 should be 5 MPa or higher. Preferably, the average tensile stress S1 is 100 MPa or higher. More preferably, the average tensile stress S1 is 200 MPa or higher. There is no particular upper limit, but it is preferable that the average tensile stress S1 is 500 MPa or lower. Here, the average tensile stress is the value obtained by dividing the load applied to the steel plate and steel strip by the width and thickness. The magnitude of the average tensile stress can be controlled by changing the feed speed of the plates at the entry and exit sides of the annealing process.
[0068] cooling process Average cooling rate CR1 at 700-500℃: less than 50℃ / s If the average cooling rate CR1 at 700-500°C exceeds 50°C / s, the total area fraction of ferrite and bainitic ferrite will be less than 5%, making it difficult to achieve excellent ductility. Therefore, the average cooling rate CR1 at 700-500°C should be less than 50°C / s. The average cooling rate CR1 is preferably 30°C / s or less. There is no particular need to limit the lower limit, but an average cooling rate CR1 of 2°C / s or more is preferable. Here, the average cooling rate CR1 is calculated as "(700°C - 500°C) / cooling time from 700°C to 500°C (s)". Specific examples of cooling at the average cooling rate CR1 include gas jet cooling and mist cooling.
[0069] Average tensile stress S2 from annealing temperature T1 to cooling stop temperature T2: 10 MPa or higher In this invention, the average tensile stress S2 between the annealing temperature T1 and the cooling stop temperature T2 affects the degree of segregation at the prior austenite grain boundaries and thus affects {C(B)-C(A)}. If the average tensile stress S2 between the annealing temperature T1 and the cooling stop temperature T2 is less than 10 MPa, {C(B)-C(A)} will be less than 3.5 at%, which promotes crack initiation and crack propagation at the prior austenite grain boundaries, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the average tensile stress S2 between the annealing temperature T1 and the cooling stop temperature T2 should be 10 MPa or higher. The average tensile stress S2 is preferably 100 MPa or higher. The average tensile stress S2 is more preferably 200 MPa or higher. There is no particular upper limit, but the average tensile stress S2 is preferably 500 MPa or lower. Here, the average tensile stress is the value obtained by dividing the load applied to the steel plate and steel strip by the width and thickness. The magnitude of the average tensile stress can be controlled by changing the plate passage speed at the entry and exit sides of the cooling process.
[0070] Cooling stop temperature T2: 80℃ or less If the cooling stop temperature T2 exceeds 80°C, the retained austenite will be 3% or more by volume fraction, making it difficult to achieve YR ≥ 65%. Therefore, the cooling stop temperature T2 should be 80°C or lower. Preferably, the cooling stop temperature T2 is 50°C or lower. There is no particular need to limit the lower limit, but it is preferable that the cooling stop temperature T2 is 0°C or higher.
[0071] Tempering process Tempering temperature T3: 100℃ or higher In this invention, tempered martensite refers to a structure obtained by heat treatment of martensite that has been heated to a tempering temperature of 100°C or higher and held for a holding time of 10 seconds or more, starting from 80°C or lower. The tempering temperature T3 affects the dislocation distribution state of the tempered martensite and thus affects the M value, which represents the dislocation distribution state of the tempered martensite. In the tempering process during the annealing process, if the tempering temperature T3 is less than 100°C, the martensite is not sufficiently tempered, the dislocations are randomly distributed, and the M value, which represents the dislocation distribution state of the tempered martensite, exceeds 1.5, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the tempering temperature T3 should be 100°C or higher. Preferably, the tempering temperature T3 should be 150°C or higher. There is no particular upper limit, but a tempering temperature T3 of 500°C or lower is preferable.
[0072] Holding time at tempering temperature T3: 10 seconds or more and 10,000 seconds or less In this invention, tempered martensite refers to a structure obtained by heat-treating martensite at a temperature of 80°C or lower to a tempering temperature of 100°C or higher and a holding time of 10 seconds or more. The holding time t3 at tempering temperature T3 affects the dislocation distribution state of the tempered martensite, and thus affects the M value, which represents the dislocation distribution state of the tempered martensite. If the holding time t3 at tempering temperature T3 is less than 10 seconds, the martensite is not sufficiently tempered, the dislocations are randomly distributed, and the M value, which represents the dislocation distribution state of the tempered martensite, exceeds 1.5, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the holding time t3 at tempering temperature T3 should be 10 seconds or more. Preferably, the holding time t3 at tempering temperature T3 should be 50 seconds or more. More preferably, the holding time t3 at tempering temperature T3 should be 100 seconds or more. The holding time t3 at tempering temperature T3 shall be 10,000 seconds or less. Preferably, the holding time t3 at tempering temperature T3 shall be 5,000 seconds or less, and more preferably 1,000 seconds or less.
[0073] Average tensile stress S3 during tempering: 20 MPa or higher In this invention, the average tensile stress S3 during tempering affects the distribution of dislocations in the tempered martensite, and thus affects the M value, which represents the distribution of dislocations in the tempered martensite. If the average tensile stress S3 during tempering is less than 20 MPa, dislocation movement within the martensite becomes difficult, making it difficult for dislocations to form stable arrangements such as dislocation cells. As a result, the M value, which represents the distribution of dislocations in the tempered martensite, exceeds 1.5, making it difficult to achieve excellent delayed fracture resistance in the bending compression section in a corrosive environment. Therefore, the average tensile stress S3 during tempering should be 20 MPa or higher. Preferably, the average tensile stress S3 during tempering is 200 MPa or higher. More preferably, the average tensile stress S3 during tempering is 400 MPa or higher. There is no particular upper limit, but it is preferable that the average tensile stress S3 during tempering is 800 MPa or lower. Here, the average tensile stress is the value obtained by dividing the load applied to the steel plate and steel strip by the width and thickness. The magnitude of the average tensile stress can be controlled by changing the feed speed of the steel plate at the entry and exit sides of the tempering process.
[0074] Cooling after tempering does not need to be specifically defined and may be cooled to the desired temperature by any method. The desired temperature is preferably around room temperature (-50 to 50°C).
[0075] Furthermore, the above-mentioned steel plate (high-strength steel plate) may be processed under conditions that result in an equivalent plastic strain of 0.05% to 5.00%. In addition, after processing, it may be reheated again under conditions of 100°C to 400°C.
[0076] Furthermore, when steel plates (high-strength steel plates) are traded, they are usually cooled to room temperature before being traded.
[0077] Furthermore, the steel plate may optionally be plated. The plating treatment is not particularly limited. Examples of plating treatments include zinc plating treatments such as hot-dip galvanizing, alloyed hot-dip galvanizing, and electroplating. Examples of plating treatments other than zinc plating include aluminum plating and alloy plating. Examples of alloy plating treatments include hot-dip zinc-aluminum-magnesium alloy plating and Zn-Ni electroalloy plating. The treatment conditions in all cases should follow conventional methods. As mentioned above, it is preferable to perform the plating treatment during the cooling from the annealing temperature T1 to the cooling stop temperature T2, or after the tempering process. For example, hot-dip galvanizing and alloyed hot-dip galvanizing are preferable to perform during the cooling from the annealing temperature T1 to the cooling stop temperature T2. Also, it is preferable to perform electroplating and Zn-Ni electroalloy plating after the tempering process. Furthermore, in the case of hot-dip galvanizing and alloyed hot-dip galvanizing, from the viewpoint of productivity, it is preferable to perform the series of processes, including the heating, annealing, and plating processes, on a CGL (Continuous Galvanizing Line), which is a hot-dip galvanizing line. After hot-dip galvanizing, wiping is possible to adjust the plating thickness.
[0078] After annealing and plating, the material may be processed again under conditions that result in an equivalent plastic strain of 0.05% to 5.00%. Alternatively, after processing, it may be reheated again under conditions of 100°C to 400°C.
[0079] Other than the conditions mentioned above, there are no particular limitations, and conventional methods may be followed. According to the steel sheet manufacturing method of the embodiment described above, a steel sheet can be obtained in which the TS is 1180 MPa or higher, the YR is 65% or higher, and which has excellent ductility and delayed fracture resistance of the bending compression portion in a corrosive environment. The obtained steel sheet can be suitably used, for example, as a material for automobile parts.
[0080] [Components and methods for manufacturing components] Next, the component of the present invention and its manufacturing method will be described.
[0081] The component of the present invention is obtained by subjecting a steel sheet of the present invention to at least one of forming and joining processes. Furthermore, the method for manufacturing the component of the present invention includes the step of subjecting a steel sheet of the present invention to at least one of forming and joining processes to form the component.
[0082] The component of the present invention has the same component composition as the steel sheet of the present invention, and at least except for the corner portion after processing, it has the same steel structure and properties as the steel sheet of the present invention described above. Furthermore, when the component of the present invention is welded in a joining process, at least except for the heat-affected zone, it has the same steel structure and properties as the steel sheet of the present invention described above. The steel sheet of the present invention has a tensile strength of 1180 MPa or more, a YR of 65% or more, and excellent ductility and delayed fracture resistance in the bent compression section in a corrosive environment. Therefore, a component obtained using the steel sheet of the present invention also has a tensile strength of 1180 MPa or more, a YR of 65% or more, and excellent ductility and delayed fracture resistance in the bent compression section in a corrosive environment, at least except for the corners and heat-affected zone after processing. Weight reduction is possible by using the component of the present invention. Therefore, the component of the present invention can be suitably used, for example, in automotive structural components.
[0083] Forming processes can utilize general processing methods such as press working without restriction. Joining processes can utilize general welding methods such as spot welding and arc welding, as well as riveting and crimping without restriction. [Examples]
[0084] Steel having the component composition shown in Table 1 (Table 1-1, Table 1-2) (the remainder being Fe and unavoidable impurities) was melted in a converter and formed into steel slabs by continuous casting. The steel slabs were then heated. The steel slabs were then hot-rolled to form hot-rolled steel sheets. The hot-rolled steel sheets were then pickled. The hot-rolled steel sheets were then cold-rolled to form cold-rolled steel sheets. In this way, the raw steel sheets were prepared. The prepared raw steel sheets were then annealed under the conditions shown in Table 2 (Table 2-1, Table 2-2) to obtain the final product steel sheets (thickness: 0.5~3.0 mm). In addition, some of the steel sheets (those with type columns GI, GA, and EG in Table 2) were plated. Of these, those with type columns GI and GA in Table 2 were plated during the cooling from the annealing temperature T1 to the cooling stop temperature T2. Furthermore, for items with "EG" in the Type column of Table 2, plating was performed after the tempering process. Conditions not specified were governed by conventional methods.
[0085] [Table 1-1]
[0086] [Table 1-2]
[0087] [Table 2-1]
[0088] [Table 2-2]
[0089] The steel sheets (high-strength cold-rolled steel sheets) obtained as described above were used as test materials, and their tensile properties and delayed fracture resistance in the bending and compression sections under corrosive conditions were evaluated according to the following test methods.
[0090] (Tissue observation) Following the method described above, the total amount of tempered martensite (area fraction), retained austenite (volume fraction), ferrite, and bainitic ferrite (area fraction), as well as the M value representing the distribution of dislocations in the tempered martensite, were determined.
[0091] {C(B)-C(A)} Following the method described above, the carbon concentration at the prior austenite grain boundary (C(B)(at%)) and the average carbon concentration within the surrounding tempered martensite grains (C(A)(at%)) were evaluated. This analysis was performed on 10 or more prior austenite grain boundaries and the surrounding tempered martensite grains, and the average difference was calculated.
[0092] (Tensile test) For the tensile test, a JIS No. 5 test specimen (gauge length 50 mm, parallel section width 25 mm) was taken so that the longitudinal direction of the specimen was perpendicular to the rolling direction, and the test was performed according to JIS Z 2241 (2022). Crosshead speed: 1.67 × 10⁻⁶ -1 A tensile test was performed under conditions of mm / second, and the tensile strength TS was measured. In this invention, a TS of 1180 MPa or higher was considered acceptable. A yield ratio YR of 65% or higher was also considered acceptable. YR is calculated using the following formula (2). YR = 100 × YS / TS ... (2) Ductility was evaluated using TS × El, and a TS × El = 14000 MPa·% or higher was considered acceptable.
[0093] (Delayed fracture resistance characteristics of bending and compression joints in corrosive environments) A 30mm x 100mm test specimen was prepared from the obtained steel plate, with the longitudinal side perpendicular to the rolling direction. Then, V-bending was performed under conditions where R / t, which is the relationship between the steel plate thickness t and the radius of curvature R of the bending process, was 3.5. The inside of the test specimen, i.e., the compressed part, which springed back after V-bending, had residual tensile stress and was a part with a high risk of delayed fracture. In addition, a V-bent test specimen was prepared after being subjected to a baking treatment by holding it at 170°C for 20 minutes. A delayed fracture test was performed on this V-bent test specimen using the corrosion environment cycle described later.
[0094] (Corrosion test cycle) The above-described test piece was subjected to treatments in a corrosion test cycle (corrosion test) composed of the following chloride adhesion step (A) and corrosion step (B), and a water washing step (C). FIG. 1 is a schematic diagram illustrating the method for evaluating the delayed fracture characteristics of a test piece (HeTsAce). FIG. 2 is a diagram schematically showing the state in which spray liquid in the atmosphere re-adheres to the evaluation surface when the distance between the shielding member and the evaluation surface of the test piece is varied. As shown in FIG. 1, in the chloride adhesion step (A), droplets 2 of the chloride-containing aqueous solution 1 were adhered such that the chloride adhesion amount (in terms of solid content) was 10000 mg / m 2 . The distance (X in FIG. 1) from the spray nozzle 3 to the evaluation surface 5 of the test piece 4 was set to 30 cm. The injection pressure of the spray nozzle 3 was set to 0.2 MPa. The salt water injection time was set to 5 seconds. The chloride adhesion amount was calculated by determining the mass difference of the test piece 4 before and after salt water injection, dividing the mass difference by the area of the evaluation surface of the test piece 4 to calculate the adhesion amount of the aqueous solution, and then calculating from the chloride concentration of the aqueous solution. In addition, the following conditions were adopted. Chloride-containing aqueous solution: 15 mass % NaCl aqueous solution sprayed by a spray method Distance between shielding member 6 and evaluation surface (Y in FIG. 2): 5 cm Temperature: 22°C, Relative humidity: 50% Distribution of droplets on evaluation surface Average contact area of droplets: 1.3 mm 2 , Standard deviation of contact area of droplets: 1.3 mm 2 , Total contact area ratio of droplets: 71%
[0095] Note that, in the second and subsequent chloride adhesion steps (A), chloride adhesion was performed under the same conditions as the first chloride adhesion step (A). The corrosion step (B) is a step in which a drying step (b1) → a transition step (b3) → a wetting step (b2) → a transition step (b4) are performed in order, and the case where the aforementioned four steps are performed is defined as one cycle. Note that, in the present example, the fluctuation range of the temperature in the corrosion step (B) was set within 30±5°C. Drying process (b1): A process of drying the metal material by holding it in an atmosphere with a relative humidity of 40% Hb1 for 2.0 hours. Wetting process (b2): A process of wetting a metal material by holding it in an atmosphere with 90% relative humidity Hb2 for 2.0 hours. Transition process (b3): A process of transitioning from an atmosphere with relative humidity Hb1 to an atmosphere with relative humidity Hb2 at a relative humidity change rate of 25% / h. Transition process (b4): A process of transitioning from an atmosphere with relative humidity Hb2 to an atmosphere with relative humidity Hb1 at a relative humidity change rate of 25% / h.
[0096] The water washing step (C) is a step in which the evaluation surface of the metal material is washed with water. The water washing method in the water washing step (C) involves spraying water onto the evaluation surface of the metal material from a spray nozzle to wash the evaluation surface. Furthermore, in this embodiment, the corrosion test cycle consisted of a chloride deposition process (A), followed by a corrosion process (B), and then a water washing process (C) before repeating the chloride deposition process (A). In other words, in this embodiment, the evaluation of delayed fracture characteristics was performed using the following corrosion test cycle. A cycle is repeated, consisting of a chloride deposition process (A) → corrosion process (B) → water washing process (C). In this embodiment, the period for evaluating delayed fracture resistance using a corrosion environment cycle was set to 63 days.
[0097] After the test, each test specimen was visually inspected for cracks. Then, the delayed fracture resistance in a corrosive environment was evaluated according to the following criteria. In this invention, a sample that showed no cracks when subjected to a stress equivalent to YS was judged to have excellent delayed fracture resistance in a corrosive environment. ◎ (Pass, particularly excellent): No cracks were observed in the V-bending test specimens, both those without and those with the heat treatment. ○ (Pass, Excellent): No cracks were found in the V-bending test specimen that had undergone heat treatment. × (Fail): Cracking was observed in both the V-bend test specimen without heat treatment and the V-bend test specimen with heat treatment.
[0098] The examples of the present invention shown in Table 3 (Tables 3-1 and 3-2) have a tensile strength TS of 1180 MPa or higher, a yield ratio YR of 65% or higher, and excellent ductility and delayed fracture resistance in the bending compression section in a corrosive environment, whereas the comparative examples were inferior in at least one of these aspects.
[0099] Furthermore, it was found that members obtained by forming and joining using the steel plate of the present invention example exhibited the same characteristics as the steel plate of the present invention: a tensile strength TS of 1180 MPa or higher, a yield ratio YR of 65% or higher, and excellent ductility and delayed fracture resistance in the bending compression section in a corrosive environment.
[0100] [Table 3-1]
[0101] [Table 3-2] [Explanation of Symbols]
[0102] 1. A chloride-containing aqueous solution that has been sprayed. 2. Droplets of chloride-containing aqueous solution 3. Spray nozzle 4 Test specimens 5. Evaluation 6 Shielding material
Claims
1. In mass percent, C: 0.030% or more and 0.500% or less, Si: 0.010% or more and 2.500% or less, Mn: 0.10% or more and 5.00% or less, P: 0.100% or less, S: 0.0200% or less, Al: 1.000% or less, N: 0.0100% or less, and, O: 0.0100% or less It contains, with the remainder being Fe and unavoidable impurities, and has a component composition. At the point where the plate thickness is 1 / 4, Area fraction of tempered martensite: 83% or more. Volume fraction of retained austenite: less than 3%, The total area fraction of ferrite and bainitic ferrite is 5% or more and less than 15%. The M value representing the distribution state of dislocations in the tempered martensite is 1.5 or less. A steel plate having a steel structure that satisfies the following formula (1). {C(B)-C(A)}≧3.5at%...(1) In formula (1), C(A): Average carbon concentration within the grains of tempered martensite (at%) C(B): This represents the carbon concentration (at%) at the prior austenite grain boundary.
2. The aforementioned component composition is further expressed in mass%, Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less Ni: 1.00% or less, Co: 0.010% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, Bi: 0.200% or less, The steel sheet according to claim 1, comprising at least one element selected from among the following.
3. The steel sheet according to claim 1, wherein the steel sheet surface has a plating layer.
4. The steel sheet according to claim 2, wherein the steel sheet surface has a plating layer.
5. A member made using the steel plate described in any one of claims 1 to 4.
6. A cold-rolled sheet is made by hot-rolling, pickling, and cold-rolling a steel having the component composition described in claim 1 or 2. Annealing temperature T1: 750°C or higher and 850°C or lower. Holding time t1 at annealing temperature T1: 10 seconds or more. An annealing process in which heating is performed under conditions of an average tensile stress S1 of 5 MPa or more at an annealing temperature T1, Average cooling rate CR1 at 700-500°C: less than 50°C / s. Average tensile stress S2 from annealing temperature T1 to cooling stop temperature T2: 10 MPa or more. A cooling process in which cooling is performed at a cooling stop temperature T2 of 80°C or lower, Tempering temperature T3: 100°C or higher. Average tensile stress S3 during tempering treatment: 20 MPa or more. A tempering process is included in which the heating is performed under the condition that the holding time t3 at the tempering temperature T3 is between 10 seconds and 10,000 seconds. At the point where the plate thickness is 1 / 4, Area fraction of tempered martensite: 83% or more. Volume fraction of retained austenite: less than 3%, The total area fraction of ferrite and bainitic ferrite is 5% or more and less than 15%. The M value representing the distribution state of dislocations in the tempered martensite is 1.5 or less. A method for manufacturing a steel plate having a steel structure that satisfies the following formula (1). {C(B)-C(A)}≧3.5at%...(1) In formula (1), C(A): Average carbon concentration within the grains of tempered martensite (at%) C(B): This represents the carbon concentration (at%) at the prior austenite grain boundary.
7. A method for manufacturing a steel sheet according to claim 6, wherein a plating treatment is applied.
8. A method for manufacturing a component, comprising the step of forming and joining a steel plate according to any one of claims 1 to 4 to form a component.
Citation Information
Patent Citations
Thermosetting resin composition
JP1978033298A
High strength steel plate and method for manufacturing the same
JP7298647B2
High strength steel plate and method for manufacturing the same
JP7323093B1
Thin steel sheet and production method therefor
WO2020026838A1
Steel sheet and method for manufacturing same
WO2024136299A1