Method for manufacturing superabsorbent resin
By controlling the surface tension of the surface crosslinking solution with an epoxy-based agent, a solvent, and a dispersant, the method enhances the liquid permeability and gel bed permeability of superabsorbent resins, overcoming the limitations of previous production techniques.
Patent Information
- Application Number
- JP2025525361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-11-06
- Filing Date
- 2023-11-07
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-11-07
AI Technical Summary
Existing methods for producing superabsorbent polymers face challenges in achieving both sufficient gel strength and liquid permeability, as crosslinking processes often result in decreased crosslinking density, hindering optimal absorption performance.
A method involving the use of a surface crosslinking solution with a controlled surface tension of 36 mN/m to 50 mN/m, comprising an epoxy-based surface crosslinking agent, a monohydric alcohol solvent, and a hydrophobic dispersant, applied during the surface crosslinking step to enhance gel bed permeability and absorption rate.
This approach produces superabsorbent resins with improved liquid permeability and gel bed permeability (GBP) by ensuring uniform application of the surface crosslinking solution, addressing the limitations of previous methods.
Smart Images

Figure 0007948695000001 
Figure 0007948695000002
Abstract
Description
[Technical Field]
[0001] [Cross-reference of related applications] This application claims priority rights based on Korean Patent Application No. 10-2022-0154686 dated November 17, 2022, and Korean Patent Application No. 10-2023-0152074 dated November 6, 2023, and all content disclosed in the documents of said Korean Patent Applications is incorporated herein by reference.
[0002] The present invention relates to a method for producing superabsorbent polymers, and more specifically, to a method for producing superabsorbent polymers that have excellent absorption performance, in particular, appropriate gel bed permeability (GBP), by controlling the surface tension of the surface crosslinked solution to a specific range in the surface crosslinking step. [Background technology]
[0003] Superabsorbent polymers (SAPs) are synthetic polymers capable of absorbing approximately 500 to 1,000 times their own weight in water. Each developing company names them differently, such as SAM (Super Absorbency Material) or AGM (Absorbent Gel Material). Superabsorbent polymers have begun to be used in sanitary products and are now widely used not only in hygiene products such as children's diapers, but also in horticultural soil water retention agents, waterproofing materials for civil engineering and construction, seedling sheets, freshness preservatives in food distribution, and materials for poultices.
[0004] In most cases, such superabsorbent polymers are widely used in hygiene products such as diapers and sanitary napkins. For these applications, they need to exhibit high absorbency of moisture, have excellent pressure absorption performance so that absorbed moisture does not escape even under external pressure, and maintain their shape well and exhibit excellent permeability even when swollen (expanded) from absorbing water.
[0005] In addition, when the superabsorbent polymer is incorporated into sanitary materials such as diapers, it needs to diffuse urine and other liquids as widely as possible, even in environments where it is pressurized by the user's weight. This allows for the overall utilization of the superabsorbent polymer particles contained in the entire surface area of the sanitary material's absorbent layer, thereby further improving the absorption performance and absorption rate of the sanitary material. Furthermore, due to this characteristic of diffusion under pressure, the rewetting properties of the diaper can be further improved, preventing urine and other liquids absorbed by the superabsorbent polymer from seeping out again, and simultaneously improving the leakage suppression properties of the diaper.
[0006] Previously, attempts were made to improve the diffusion properties of urine and other liquids by changing the design of sanitary materials such as diapers. For example, methods were attempted to improve the diffusion properties of urine and other liquids by introducing ADL (Acquisition Distribution Layer) into the sanitary material or by utilizing absorption channels. However, such improvements in diffusion properties through changes in the design of the sanitary material itself were not sufficient.
[0007] On the other hand, in order to improve the physical properties of superabsorbent polymers, such as absorption capacity, liquid permeability, and absorption rate, various post-treatment processes such as surface crosslinking and foaming are performed, or various additives are used. However, in the process of forming such absorption capacity, there was a problem in that the crosslinking density of the resin decreased, making it impossible to achieve sufficient gel strength.
[0008] Therefore, there is a need for research on the production of superabsorbent polymers that can achieve appropriate liquid permeability and gel strength while maintaining the existing absorbent properties well. [Overview of the Initiative] [Problems that the invention aims to solve]
[0009] Therefore, the present invention relates to a method for producing superabsorbent polymers, and more specifically, aims to produce superabsorbent polymers with excellent absorption performance more productively by controlling the surface tension of a surface crosslinked solution containing specific components in a surface crosslinking step. [Means for solving the problem]
[0010] To solve the aforementioned problems, the present invention provides: A step of forming a hydrated gel polymer containing a crosslinked polymer obtained by crosslinking an acrylic acid monomer having at least a portion of its acidic groups neutralized in the presence of an internal crosslinking agent, The steps include drying, grinding, and classifying the aforementioned water-containing gel polymer to form a base resin powder, The step of crosslinking the surface of a base resin powder in the presence of a surface crosslinking solution comprising an epoxy surface crosslinking agent, a monohydric alcohol solvent, and a hydrophobic dispersant, having a surface tension of 36 mN / m to 50 mN / m, This invention provides a method for producing superabsorbent polymers. [Effects of the Invention]
[0011] The present invention provides a method for producing superabsorbent resins that allows for the more productive production of superabsorbent resins having excellent liquid permeability and appropriate gel bed permeability (GBP) by controlling the surface tension of a surface crosslinked solution containing specific components in the surface crosslinking step. [Modes for carrying out the invention]
[0012] The terms used herein are used solely to illustrate exemplary embodiments and are not intended to limit the invention.
[0013] A singular expression includes plural expressions unless the context clearly indicates otherwise. In this specification, terms such as “includes,” “equip,” or “possess” are intended to specify the existence of a feature, step, component, or combination thereof, and should not be understood to preemptively exclude the existence or possibility of adding one or more other features, steps, components, or combinations thereof.
[0014] The terms "first," "second," "third," etc., are used to describe various components, and are used solely for the purpose of distinguishing one component from others.
[0015] The present invention can be modified in various ways and may take many forms; therefore, specific embodiments are illustrated and described in detail below. However, this should not be understood as limiting the present invention to any particular form of disclosure, but rather as including any modifications, equivalents, or substitutions that fall within the spirit and technical scope of the present invention.
[0016] As used herein, the terms "polymer" or "polymer" refer to a state in which water-soluble ethylene-based unsaturated monomers have been polymerized, and can encompass all water content ranges or particle size ranges. Among the polymers, those in the state before drying after polymerization and with a water content (moisture content) of about 40% by weight or more may be called water-containing gel polymers, and particles obtained by grinding and drying such water-containing gel polymers may be called crosslinked polymers.
[0017] Furthermore, as used herein, the term "crosslinked polymer" means a water-soluble ethylene-based unsaturated monomer in which at least a portion of the acidic groups have been neutralized has been crosslinked, and the term "base resin powder" means a substance containing such a crosslinked polymer.
[0018] Furthermore, the term "superabsorbent resin" refers to a powdery base resin powder composed of a crosslinked polymer obtained by polymerizing a water-soluble ethylenically unsaturated monomer in which at least a portion of the acidic groups are neutralized, or superabsorbent resin particles obtained by pulverizing said crosslinked polymer, or is used to encompass all states obtained by subjecting said crosslinked polymer or said base resin to additional processes, such as surface crosslinking, fine powder regranulation, drying, pulverization, classification, and the like, to render them suitable for commercialization.
[0019] (Method for producing superabsorbent resin) A method for producing a superabsorbent resin according to one embodiment of the present invention comprises the step of forming a hydrogel polymer containing a crosslinked polymer obtained by crosslinking and polymerizing an acrylic monomer having acidic groups at least partially neutralized, in the presence of an internal crosslinking agent, the step of drying, pulverizing and classifying said hydrogel polymer to form a base resin powder, and the step of crosslinking the surface of the base resin powder in the presence of a surface crosslinking solution comprising an epoxy-based surface crosslinking agent, a monohydric alcohol-based solvent and a hydrophobic dispersant, and having a surface tension of 36 mN / m to 50 mN / m.
[0020] In order to improve the basic absorption capacity of superabsorbent resins, various post-treatment processes such as surface crosslinking and foaming are performed, or various additives are used. However, in such processes, the crosslinking density of the resin decreases, making it impossible to achieve sufficient gel strength, and there has been a problem that it is difficult to achieve the desired level of excellent liquid permeability.
[0021] Accordingly, the present inventors have found that when the surface tension of a surface crosslinking solution containing specific components is controlled in the surface crosslinking step, a superabsorbent resin having excellent liquid permeability and a further improved absorption rate can be produced more productively without the aforementioned problems, and thus the present invention has been completed.
[0022] In particular, by using a combination of an epoxy-based surface crosslinking agent, a monohydric alcohol-based solvent, and a hydrophobic dispersant in the surface crosslinking solution during the surface crosslinking step, the surface tension of the solution can be adjusted to the aforementioned range, thereby further slowing the diffusion rate of the surface crosslinking solution into the base resin and enabling uniform application of the surface crosslinking solution to the surface of the base resin particles. As a result, the absorbent properties of the final superabsorbent resin particles are improved, and in particular, the gel bed permeability (GBP) can be further enhanced.
[0023] The method for producing superabsorbent polymers will be described in more detail step by step below, with specific examples of the invention.
[0024] (Polymerization step) First, a method for producing a superabsorbent polymer according to one embodiment of the invention includes the step of forming a hydrated gel polymer containing a crosslinked polymer obtained by crosslinking an acrylic acid monomer having at least a portion of neutralized acidic groups in the presence of an internal crosslinking agent.
[0025] The polymerization step involves photopolymerizing and / or thermally polymerizing a monomer composition containing an acrylic acid monomer having at least a portion of neutralized acidic groups in the presence of an internal crosslinking agent to form a hydrated gel polymer.
[0026] The polymerization step may be carried out by crosslinking polymerization of a monomer composition containing components commonly used in the production of superabsorbent resins, in addition to the components mentioned above.
[0027] First, a monomer mixture is prepared containing an acrylic acid monomer having at least a portion of its acidic groups neutralized in the presence of an internal crosslinking agent. The monomer mixture may further contain a polymerization initiator for polymerization.
[0028] The acrylic acid monomer may be any monomer commonly used in the production of superabsorbent polymers. As a non-limiting example, the acrylic acid monomer may be a compound represented by the following chemical formula 1:
[0029] [Chemical formula 1] R1-COOM 1
[0030] In the aforementioned chemical formula 1, R1 is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond. M 1 This is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.
[0031] Preferably, the acrylic acid monomer may be one or more selected from the group consisting of acrylic acid, methacrylic acid, and monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts of these acids. Using an acrylic acid monomer in this way is advantageous because it allows for the acquisition of a superabsorbent resin with improved water absorption. In addition, one or more monomers selected from the group consisting of anionic monomers and salts of maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid, or 2-(meth)acrylamido-2-methylpropanesulfonic acid; nonionic hydrophilic monomers containing (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, or polyethylene glycol (meth)acrylate; and amino group-containing unsaturated monomers and quaternary derivatives of (N,N)-dimethylaminoethyl (meth)acrylate or (N,N)-dimethylaminopropyl (meth)acrylamide.
[0032] Here, the acrylic acid monomer has an acidic group, and at least a portion of the acidic group is partially neutralized using a neutralizing solution. In this case, basic substances such as sodium hydroxide, potassium hydroxide, and ammonium hydroxide, which can neutralize the acidic group, can be used as the neutralizing agent contained in the neutralizing solution.
[0033] In this case, the degree of neutralization of the monomer may be 40 to 95 mol%, 40 to 80 mol%, or 45 to 75 mol%. The range of the degree of neutralization may vary depending on the final physical properties, but if the degree of neutralization is excessively high, neutralized monomers may precipitate, making polymerization difficult. Conversely, if the degree of neutralization is excessively low, not only will the water absorption of the polymer decrease significantly, but it may also exhibit properties similar to an elastic rubber that is difficult to handle.
[0034] As used herein, the term "internal crosslinking agent" is used to distinguish it from "surface crosslinking agent" used to crosslink the surface of the base resin, and plays a role in crosslinking and polymerizing the unsaturated bonds of the aforementioned acrylic acid monomer. The crosslinking in the above step is carried out without distinction between the surface and the interior, but as a result of the surface crosslinking step of the base resin described later, the surface of the particles of the final superabsorbent polymer consists of a structure crosslinked by the surface crosslinking agent, and the interior consists of a structure crosslinked by the internal crosslinking agent.
[0035] The internal crosslinking agent can be a polyfunctional component, and for example, one or more selected from the group consisting of N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triarylamine, ethylene glycol diglycidyl ether, propylene glycol, glycerin, and ethylene carbonate can be used. Preferably, polyethylene glycol di(meth)acrylate or propylene glycol di(meth)acrylate can be used.
[0036] The internal crosslinking agent can be used in an amount of 100 ppmw to 10,000 ppmw relative to the weight of the acrylic acid monomer. When included within the above content range, sufficient crosslinking is possible, achieving a strength above an appropriate level, and sufficient water retention capacity can be achieved by introducing an appropriate crosslinking structure. Preferably, it can be included in an amount of 100 ppmw or more, 200 ppmw or more, 300 ppmw or more, or 600 ppmw or more, and also in amounts of 10,000 ppmw or less, 9,000 ppmw or less, 7,000 ppmw or 5,000 ppmw or less, 200 ppmw to 9,000 ppmw, 300 ppmw to 7,000 ppmw or 600 ppmw to 5,000 ppmw. If the content of the internal crosslinking agent is excessively low, crosslinking may not occur sufficiently, making it difficult to achieve a strength above an appropriate level. Conversely, if the content of the internal crosslinking agent is excessively high, the internal crosslinking density may become too high, making it difficult to achieve the desired water retention capacity.
[0037] As the polymerization initiator, a thermal polymerization initiator or a photopolymerization initiator can be used depending on the polymerization method. However, even with the photopolymerization method, a certain amount of heat is generated by ultraviolet irradiation, and a certain amount of heat is also generated by the progress of the polymerization reaction, which is an exothermic reaction, so a thermal polymerization initiator may also be included.
[0038] Here, as the photopolymerization initiator, for example, one or more compounds selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone can be used. Among these, as specific examples of acyl phosphine, commercially available lucirin TPO, i.e., 2,4,6-trimethyl-benzoyl-trimethyl phosphine oxide, or diphenyl(2,4,6-trimethylbenzoyl)-phosphine oxide can be used. A wider variety of photopolymerization initiators are disclosed on page 115 of Reinhold Schwalm's book, "UV Coatings: Basics, Recent Developments and New Applications (Elsevier, 2007)," which can be referenced.
[0039] Furthermore, one or more compounds selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid can be used as the thermal polymerization initiator. Specifically, examples of persulfate initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8). Furthermore, azo-based initiators include 2,2-azobis(2-amidinopropane)dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, 2-(carbamoylazo)isobutylonitrile, 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, and 4,4-azobis-(4-cyanovaleric acid). Examples include acids. A wider variety of thermal polymerization initiators are disclosed on page 203 of Odian's book "Principle of Polymerization" (Wiley, 1981), which can be consulted.
[0040] Such polymerization initiators can be used in amounts of 10 ppmw to 10,000 ppmw relative to the weight of the acrylic acid monomer. Preferably, they can be present in amounts of 10 ppmw or more, 30 ppmw or more, 50 ppmw or more, and 10,000 ppmw or less, 5,000 ppmw or less, or 3,000 ppmw or less, and may be present in amounts of 30 ppmw to 5,000 ppmw, 50 ppmw to 3,000 ppmw, or 80 ppmw to 2,500 ppmw. If the concentration of the polymerization initiator is excessively low, the polymerization rate may slow down, and a large amount of residual monomer may be extracted into the final product, which is undesirable. Conversely, if the concentration of the polymerization initiator is excessively high, the polymer chains forming the network may become shorter, increasing the content of water-soluble components, and potentially degrading the physical properties of the resin, such as reducing its pressure absorption capacity, which is undesirable. The content of the polymerization initiator refers to the mixed content when both a photopolymerization initiator and a thermal polymerization initiator are used.
[0041] In addition, the monomer composition may further contain additives such as foaming agents, surfactants, thickeners, plasticizers, preservatives, and antioxidants, as needed.
[0042] The foaming agent plays a role in increasing the surface area by causing foaming during polymerization and forming pores within the water-containing gel polymer. The foaming agent can be a carbonate, and as an example, sodium bicarbonate, sodium carbonate, potassium bicarbonate, potassium carbonate, calcium bicarbonate, calcium carbonate, magnesium bicarbonate, or magnesium carbonate can be used.
[0043] Furthermore, it is preferable to use the blowing agent in an amount of 1500 ppmw or less relative to the weight of the water-soluble ethylene-based unsaturated monomer. If the amount of blowing agent used exceeds 1500 ppmw, the number of pores will increase excessively, which may reduce the gel strength of the superabsorbent polymer, decrease its density, and cause problems in distribution and storage. Furthermore, it is preferable to use the blowing agent in an amount of 500 ppmw or more, or 1000 ppmw or more, relative to the weight of the water-soluble ethylene-based unsaturated monomer.
[0044] The surfactant is intended to induce a uniform dispersion of the foaming agent, enabling uniform foaming during foaming and preventing a decrease in gel strength or density. It is preferable to use an anionic surfactant as the surfactant. Specifically, the surfactant is SO3 - Compounds containing anions, represented by the following chemical formula 2, can be used.
[0045] [Chemical formula 2] R-SO3Na
[0046] In the aforementioned chemical formula 2, R is an alkyl group having 8 to 16 carbon atoms.
[0047] Furthermore, it is preferable to use the surfactant at an amount of 300 ppmw or less relative to the weight of the acrylic acid monomer. If the amount of surfactant used exceeds 300 ppmw, the surfactant content in the superabsorbent polymer becomes too high, which is undesirable. Furthermore, it is preferable to use the surfactant at an amount of 100 ppmw or more, or 150 ppmw or more, relative to the weight of the water-soluble ethylene-based unsaturated monomer.
[0048] Such monomer compositions may be prepared in the form of a solution in which the aforementioned monomers, internal crosslinking agents, foaming agents, initiators, and other raw materials are dissolved in a solvent.
[0049] In this case, any solvent that can dissolve the aforementioned raw materials can be used without being limited in its composition. For example, the solvent can be water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide, or mixtures thereof.
[0050] The step of forming a hydrated gel polymer by polymerization of the monomer composition may be carried out by a conventional polymerization method, and the process is not particularly limited. As an unrestrictive example, it may be carried out in a reactor equipped with a movable conveyor belt.
[0051] Specifically, when photopolymerization of the monomer composition is carried out in a reactor equipped with a movable conveyor belt, a sheet-like hydrated gel polymer can be obtained. In this case, the thickness of the sheet may vary depending on the concentration and injection rate of the monomer composition being injected, but it is preferable to adjust the thickness to 0.5 to 10 cm in order to ensure that the entire sheet is polymerized uniformly while also ensuring a sufficient production rate.
[0052] The typical water content of a water-containing gel polymer obtained by this method may be 40% to 80% by weight. On the other hand, throughout this specification, "water content" refers to the amount of water relative to the total weight of the water-containing gel polymer, and means the value obtained by subtracting the weight of the dry polymer from the weight of the water-containing gel polymer. Specifically, it is defined as the value calculated by measuring the weight loss due to water evaporation in the polymer during the drying process by raising the temperature of the polymer through infrared heating. In this case, the drying conditions are set to raise the temperature to 180°C at room temperature and then maintain it at 180°C, with a total drying time of 20 minutes, including a 5-minute temperature rise step, and the water content is measured.
[0053] (Drying, grinding, and classification steps) Next, a method for producing a superabsorbent resin according to one embodiment of the invention further includes the steps of drying, pulverizing, and classifying the produced water-containing gel polymer to form a base resin powder.
[0054] Specifically, the obtained water-containing gel polymer is dried. If necessary, a step of coarse grinding (chopping) the water-containing gel polymer before drying may be performed to increase the efficiency of the drying step.
[0055] In this case, the pulverizer used is not limited in its configuration, but may include any one selected from the group of pulverizing equipment consisting of a vertical pulverizer, turbo cutter, turbo grinder, rotary cutter mill, cutter mill, disc mill, shred crusher, crusher, chopper, and disc cutter, but is not limited to the examples mentioned above.
[0056] In this step, the coarse grinding step can be performed to grind the water-containing gel polymer to a particle size of 2 mm to 10 mm. Grinding to a particle size of less than 2 mm is technically difficult due to the high water content of the water-containing gel polymer, and a phenomenon of aggregation between the ground particles may occur. On the other hand, grinding to a particle size of more than 10 mm may have little effect on increasing the efficiency of the subsequent drying step.
[0057] As described above, the hydrated gel polymer is either coarsely ground or dried immediately after polymerization without undergoing the coarse grinding step. At this time, the drying temperature in the drying step may be 150 to 250°C. If the drying temperature is less than 150°C, the drying time may be excessively long, which may reduce the physical properties of the final superabsorbent resin. If the drying temperature exceeds 250°C, only the polymer surface may be excessively dried, which may generate fine powder in the subsequent grinding step, and may reduce the physical properties of the final superabsorbent resin. Therefore, preferably, the drying may be carried out at a temperature of 150 to 200°C, and more preferably at a temperature of 150 to 190°C.
[0058] In the case of drying time, it may be carried out for 20 to 90 minutes, taking into consideration process efficiency, but it is not limited to this.
[0059] On the other hand, the drying step may be carried out in a multi-stage process within the aforementioned temperature range.
[0060] The drying method for the drying step can be selected and used without limitation, as long as it is one that is commonly used in the drying process of water-containing gel polymers. Specifically, the drying step may be carried out by methods such as hot air supply, infrared irradiation, ultra-high frequency irradiation, or ultraviolet irradiation. In the case of hot air supply, this may be done by using an oven in which the direction of the airflow can be changed vertically.
[0061] The water content of the polymer after such a drying step may be about 0.1 to about 10% by weight.
[0062] Next, the dried polymer obtained through this drying step is pulverized.
[0063] The polymer powder obtained after the grinding step may have a particle size of 150 to 850 μm. The grinders used to grind to such a particle size may include, but are not limited to, pin mills, hammer mills, screw mills, roll mills, disc mills, or jog mills.
[0064] Furthermore, in order to control the physical properties of the superabsorbent polymer powder that is finalized after such a grinding step, the polymer powder obtained after grinding may undergo a separate process of classification by particle size. Preferably, polymers with a particle size of 150 μm to 850 μm are classified, and only polymer powders having such particle sizes can be processed into a product through a surface crosslinking reaction step. More specifically, the base resin powder that has undergone the classification may have a particle size of 150 μm to 850 μm, and may contain 50% by weight or more of particles with a particle size of 300 μm to 600 μm, and may contain less than 3% by weight of fine powder with a particle size of less than 150 μm.
[0065] On the other hand, fine powder with a particle size of less than 150 μm may be generated in the polymerization, drying, and grinding steps. This fine powder with a particle size of less than 150 μm, which is classified in the classification step described above, can be recycled into base resin powder by undergoing a reassembly process to produce normal particles of 150 μm or more.
[0066] The reassembly process of the fine powder can be carried out using methods commonly applied in this art, for example, by performing a process of agglomerating the fine powder in a wet state. Specifically, the classified fine powder can be mixed with water to agglomerate, and then the water can be dried through a re-drying process to produce normal particles. In the reassembly process, additives such as water-soluble polymers can be selectively used to improve the agglomeration strength of the particles. The surface crosslinking solution is included in an amount of 1 to 10 parts by weight per 100 parts by weight of the base resin powder.
[0067] (Surface crosslinking step) On the other hand, after producing the base resin powder through the classification process described above, the process may further include a step of surface crosslinking the base resin powder while heat-treating it in the presence of a surface crosslinking agent.
[0068] According to one embodiment of the invention, the surface crosslinking step is carried out using a surface crosslinking solution in which the surface tension is controlled within a specific range. Specifically, by ensuring that the surface tension of the surface crosslinking solution is 36 mN / m to 50 mN / m, a superabsorbent resin with excellent liquid permeability can be produced.
[0069] More specifically, by using a combination of an epoxy-based surface crosslinking agent, a monohydric alcohol-based solvent, and a hydrophobic dispersant as the surface crosslinking solution, the surface tension of the solution is adjusted to the aforementioned range. This results in a relatively lower surface tension (36 mN / m to 50 mN / m) compared to the surface tension of commonly used surface crosslinking solutions, further slowing the diffusion rate of the surface crosslinking solution into the base resin. As a result, the surface crosslinking solution can be uniformly applied to the surface of the base resin particles, improving the absorbent properties of the final superabsorbent resin particles, and in particular, further improving the gel bed permeability (GBP).
[0070] If the surface tension of the surface crosslinking solution is less than 36 mN / m, the surface crosslinking solution containing the epoxy surface crosslinking agent will not penetrate easily into the base resin powder, making it difficult to achieve uniform surface crosslinking to the desired degree. If the surface tension exceeds 50 mN / m, the surface crosslinking solution may penetrate excessively into the base resin powder, leading to a high surface crosslink density and a decrease in water retention capacity. Preferably, the surface tension of the surface crosslinking solution may be 36 mN / m or more, 37 mN / m or more, 38 mN / m or more, or 49 mN / m or less, or 48.5 mN / m or less. Within this range, it is possible to produce a superabsorbent resin with excellent absorbent properties without the aforementioned problems, which is preferable. The surface tension of the surface crosslinking solution may be adjusted by the type and content of the epoxy crosslinking agent, monohydric alcohol solvent, and hydrophobic dispersant, which are specific components of the solution, but is not limited thereto.
[0071] On the other hand, the surface tension can be measured at room temperature of 23±2℃ using the Wilhelmy plate method. A specific method for measuring such surface tension will be explained in more detail in the experimental examples described later.
[0072] The surface crosslinking step involves inducing a crosslinking reaction on the surface of the base resin powder in the presence of a surface crosslinking agent. The unsaturated bonds of the acrylic acid monomers that remained on the surface without being crosslinked are crosslinked by the surface crosslinking agent, resulting in the formation of a superabsorbent resin with a high surface crosslink density.
[0073] Specifically, a surface crosslinked layer can be formed in the heat treatment process in the presence of a surface crosslinking agent. In this heat treatment process, the surface crosslink density, i.e., the external crosslink density, increases, but the internal crosslink density remains unchanged. Therefore, the superabsorbent polymer with the manufactured surface crosslinked layer has a structure in which the external crosslink density is higher than the internal crosslink density.
[0074] The surface crosslinking solution used in the aforementioned surface crosslinking step includes an epoxy-based surface crosslinking agent.
[0075] The epoxy crosslinking agent can readily crosslink with ester groups present on the surface of the base resin powder at relatively low temperatures (approximately 100°C to 140°C), thereby improving pressurized properties such as 0.9 AUL and GBP. Furthermore, it is used in combination with a monohydric alcohol solvent and a hydrophobic dispersant in the surface crosslinking solution to control the surface tension within a desired range.
[0076] The epoxy crosslinking agent is a compound containing at least one epoxy group, preferably two or more epoxy groups, within its molecule, and may also be a compound containing an ether structure within its molecule together with the epoxy groups. As the epoxy crosslinking agent, for example, one or more selected from the group consisting of ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, glycerol triglycidyl ether, polyethylene glycol diglycidyl ether, and propylene glycol diglycidyl ether can be used, and preferably ethylene glycol diglycidyl ether and polyethylene glycol diglycidyl ether can be used.
[0077] On the other hand, even if the crosslinking agent is a compound containing an epoxy group, in the case of compounds such as epoxyalkyl phosphates, the concentration of the phosphate may adversely affect the absorbent properties of the absorber when forming the crosslink density of the polymer. Compared to the epoxy-based crosslinking agent according to the present invention, under the same water retention property criteria, the surface tension will deviate from the desired level (36 mN / m to 50 mN / m).
[0078] Preferably, the epoxy crosslinking agent is not an epoxyalkyl phosphate compound.
[0079] The epoxy crosslinking agent can be used in an amount of 0.01 to 10 parts by weight per 100 parts by weight of the base resin powder. Preferably, it can be used in an amount of 0.05 parts by weight or more, 0.1 parts by weight or more, or 8 parts by weight or less, 5 parts by weight or less, or 1 part by weight or less. By adjusting the content range of the epoxy crosslinking agent within the above-mentioned range, a superabsorbent resin exhibiting excellent absorption performance and various physical properties such as liquid permeability can be produced.
[0080] The surface crosslinking solution used in the aforementioned surface crosslinking step contains a monohydric alcohol-based solvent as the solvent.
[0081] The monohydric alcohol-based solvent relatively lowers the surface tension of the surface crosslinking solution, slowing its diffusion and allowing the surface crosslinking solution to be applied more uniformly to the surface of the base resin powder. To this end, it can effectively improve the gel bed permeability (GBP) among the pressurized properties, and together with the epoxy crosslinking agent and hydrophobic dispersant in the surface crosslinking solution, it can control the surface tension within the desired range.
[0082] Examples of the monohydric alcohol solvent include one or more selected from the group consisting of methanol, ethanol, n-propanol, isopropanol, and butanol, and preferably ethanol and isopropanol can be used.
[0083] The surface crosslinking solution may further contain additional solvents in addition to the monohydric alcohol solvent, for example, water and / or a hydrophilic organic solvent, and preferably, water may be used together with the monohydric alcohol solvent.
[0084] The monohydric alcohol solvent may be included in an amount of 1 to 5 parts by weight relative to the total content of the surface crosslinking solution. Preferably, it can be used in an amount of 1.5 parts by weight or more, 2 parts by weight or more, or 4.5 parts by weight or less, 4 parts by weight or less, or 3 parts by weight or less. By adjusting the content range of the monohydric alcohol solvent to the range described above, the surface tension of the surface crosslinking solution can be adjusted to the desired range, and a superabsorbent resin exhibiting excellent absorption performance and liquid permeability and other physical properties can be produced.
[0085] The surface crosslinking solution used in the aforementioned surface crosslinking step contains a hydrophobic dispersant.
[0086] The hydrophobic dispersant relatively lowers the surface tension of the surface crosslinking solution, slowing its diffusion and allowing the surface crosslinking solution to be applied more uniformly to the surface of the base resin powder. To this end, it can effectively improve the gel bed permeability (GBP) among the pressurized properties, and together with the epoxy crosslinking agent and monohydric alcohol solvent in the surface crosslinking solution, it can control the surface tension within the desired range.
[0087] Examples of the hydrophobic dispersants mentioned above include sodium dodecyl sulfate, poly(dimethyldiallylammonium chloride), aqueous-dispersible silica, calcium stearate, and di(C 12-20 One or more selected from the group consisting of alkyldimethylammonium salts and polyethylene glycol can be used, preferably sodium dodecyl sulfate and aqueous dispersion silica.
[0088] The hydrophobic dispersant may be included in an amount of 0.0001 to 1 part by weight relative to the total content of the surface crosslinking solution. Preferably, it can be used in an amount of 0.0002 parts by weight or more, 0.003 parts by weight or less, or 0.5 parts by weight or less, 0.45 parts by weight or less. By adjusting the content range of the hydrophobic dispersant within the range described above, the surface tension of the surface crosslinking solution can be adjusted to the desired range, and a superabsorbent resin exhibiting excellent absorption performance and liquid permeability and other physical properties can be produced. For reference, when water-dispersible silica is used as the hydrophobic dispersant, the content refers to the amount of solid silica.
[0089] The surface crosslinking solution may further contain additional additives in addition to the components described above. Specifically, the additional additives contained in the surface crosslinking solution can increase the mixing efficiency of the base resin particles and the surface crosslinking solution, allow for more uniform application of the surface crosslinking solution, and improve the GBP properties among the pressurized properties.
[0090] Specific examples of the aforementioned additional additives include one or more selected from the group consisting of methylene glycol, ethylene glycol, propylene glycol, and butene glycol, with propylene glycol being more preferable.
[0091] The aforementioned additional additive may be included in an amount of 0.1 to 5 parts by weight relative to the total content of the surface crosslinking solution, preferably in an amount of 0.5 to 3 parts by weight, 1 to 3 parts by weight, or 1.5 to 2.5 parts by weight, and can be included within the aforementioned content range to improve the applicability of the surface crosslinking solution and further improve the GBP properties among the pressurized physical properties.
[0092] On the other hand, the surface crosslinking agent is added to the base resin powder in the form of a surface crosslinking agent composition containing it, but there are no special limitations on the composition of such a surface crosslinking agent composition. For example, one can mix the surface crosslinking agent composition and the base resin powder in a reaction vessel, spray the surface crosslinking agent composition water onto the base resin powder, or continuously supply the base resin powder and the surface crosslinking agent composition to a continuously operating mixer and mix them.
[0093] The surface crosslinking step can be carried out by heat treatment at a temperature of 110°C to 200°C, or 110°C to 150°C for 30 minutes or more. More specifically, the surface crosslinking reaction can be carried out by heat treatment at the aforementioned temperature as the maximum reaction temperature for 30 to 80 minutes, or 40 to 70 minutes.
[0094] By satisfying these surface crosslinking process conditions (particularly the heating conditions and the reaction conditions at the maximum reaction temperature), it is possible to manufacture superabsorbent polymers that appropriately satisfy superior physical properties such as pressurized liquid permeability.
[0095] The means of raising the temperature for the surface crosslinking reaction are not particularly limited. Heating can be performed by supplying a heat transfer medium or by directly supplying a heat source. In this case, the type of heat transfer medium that can be used is not limited to steam, hot air, or heated fluids such as hot oil, and the temperature of the supplied heat transfer medium can be appropriately selected considering the type of heat transfer medium, the heating rate, and the target temperature. On the other hand, examples of directly supplied heat sources include heating by electricity and heating by gas, but are not limited to the examples mentioned above.
[0096] On the other hand, in the method for producing a superabsorbent resin according to one embodiment of the invention, aluminum salts such as aluminum sulfate and various other polyvalent metal salts may be further used during surface crosslinking to further improve properties such as liquid permeability. Such polyvalent metal salts may be included on the surface crosslinked layer of the final produced superabsorbent resin.
[0097] (Super absorbent resin) According to one embodiment of the invention, a superabsorbent resin produced by the method for producing the superabsorbent resin described above is provided. The superabsorbent resin produced by the method for producing the superabsorbent resin of the above embodiment can achieve excellent absorption performance, liquid permeability, and in particular, excellent gel bed permeability (GBP) at an appropriate crosslinking density.
[0098] The superabsorbent polymer may have a gel bed permeability (GBP) of 50 darcy or more, more preferably 53 darcy or more, 55 darcy or more, or 110 darcy or less, or 105 darcy or less. The specific method for measuring such gel bed permeability is the same as the method described in Korean Patent Application No. 10-2014-7018005, and will be explained in more detail in the experimental examples described later.
[0099] The operation and effects of the invention will be described in more detail below through specific embodiments of the invention. However, these embodiments are presented merely as examples of the invention and do not determine the scope of the invention's rights.
[0100] [Examples] (Example 1) As the manufacturing apparatus for the superabsorbent polymer, a continuous manufacturing apparatus consisting of a polymerization process, a water-containing gel pulverization process, a drying process, a pulverization process, a classification process, a surface crosslinking process, a cooling process, a classification process, and a transport process that connects each of these processes was used.
[0101] A monomer solution was prepared by mixing 100 parts by weight of acrylic acid with 0.43 parts by weight of polyethylene glycol diacrylate (weight-average molecular weight: ~500 g / mol) as an internal crosslinking agent and 0.01 parts by weight of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide as a photoinitiator. Next, while continuously supplying the monomer solution to a metering pump, 175 parts by weight of a 31.5% by weight sodium hydroxide aqueous solution was continuously mixed in the line to prepare a monomer aqueous solution. Furthermore, a monomer mixture was prepared by continuously mixing in the line 1.5 parts by weight of a 0.3% by weight sodium persulfate aqueous solution, 0.5 parts by weight of an aqueous solution containing 0.1% by weight of sodium bicarbonate as a foaming agent, and 0.25 parts by weight of an aqueous solution containing 0.05% by weight of calcium stearate as a surfactant.
[0102] Through this transfer process, a monomer aqueous solution is introduced into a polymerization reactor consisting of a moving conveyor belt, and ultraviolet light is irradiated through a UV irradiation device (irradiation dose: 2 mW / cm²). 2 UV polymerization was carried out for 2 minutes to produce a hydrated gel polymer.
[0103] The aforementioned water-containing gel was cut into pieces with an average size of approximately 300 mm or less, and then put into a pulverizer (equipped with a perforated plate containing multiple holes with a diameter of 10 mm) and pulverized.
[0104] Next, the pulverized water-containing gel was dried in a dryer with an adjustable airflow direction. The water-containing gel was uniformly dried by flowing 180°C hot air through it so that the water content of the dried powder was approximately 2% or less.
[0105] The dried resin was crushed in a pulverizer and then classified to obtain a base resin with a size of 150 to 850 μm.
[0106] Subsequently, 10.28 g of surface crosslinking solution (containing 6 g of water, 2 g of isopropanol, 0.15 g of ethylene glycol diglycidyl ether as a surface crosslinking agent, 0.07 g of water-dispersed silica (STO) as a hydrophobic dispersant, and 2 g of propyl glycol and 0.06 g of silicon dioxide (Aerosil 200) as other additives) was sprayed onto 100 parts by weight of the manufactured base resin powder and stirred at room temperature to mix the solution so that it was evenly distributed on the base resin powder.
[0107] Next, the base resin powder mixed with the surface crosslinking solution was placed in a surface crosslinking reactor to carry out the surface crosslinking reaction.
[0108] In this surface crosslinking reactor, the base resin powder was further reacted at a temperature of 140°C for 40 minutes. After surface crosslinking, 0.08 parts by weight of silicon dioxide (Aerosil 200) was added to 40 parts by weight of the resin powder and dried, and then a sample of the final produced superabsorbent resin was taken. After the surface crosslinking step, the sample was classified using an ASTM standard sieve to produce the superabsorbent resin of Example 1 having a particle size of 150 μm to 850 μm.
[0109] (Examples 2 to 9 and Comparative Examples 1 to 4) A superabsorbent polymer was produced in the same manner as in Example 1, except that the components and their contents used in the surface crosslinking step were as shown in Table 1 below.
[0110] [Table 1]
[0111] [Experimental Example 1. Evaluation of the physical properties of surface crosslinking solutions] The physical properties of the surface crosslinking solutions used in the above examples and comparative examples were evaluated using the following method, and the results are shown in Table 2.
[0112] Unless otherwise stated, all evaluations of the physical properties below were performed at room temperature (25±1℃).
[0113] (1)Surface tension (mN / m) The surface tension of the surface crosslinking solutions used in the examples and comparative examples was measured using the "plate method (the wilhelmy plate method)," which is a method for measuring static surface tension. Specifically, this refers to the maximum tension value up to the point where the solution being measured touches the surface of the plate tip. This was measured using a process tensiometer (KRUSS), and the results are shown in Table 1.
[0114] (2) Evaluation of water absorption of surface crosslinking solution (absorption rate, min) In the examples and comparative examples, the degree of absorption of the surface crosslinking solution by the base resin powder before surface crosslinking was measured during the manufacturing step.
[0115] Specifically, 2 g of base resin powder was added to a beaker containing 50 g of surface crosslinking solution, and the time it took for the resin to become completely saturated was measured. The results are shown in Table 1.
[0116] For reference, the aforementioned physical properties refer to the degree to which the base resin surface crosslinking solution is applied. Since the slower the absorption, the greater the applicability to the base resin surface, this indirectly demonstrates excellent properties under pressure.
[0117] [Experimental Example 2. Evaluation of the physical properties of superabsorbent polymers] The physical properties of the superabsorbent polymers produced in the above examples and comparative examples were evaluated using the following methods, and the results are shown in Table 2.
[0118] The following physical property evaluations were all performed at room temperature (23±1℃) and relative humidity (45±1%), in addition to the absorption rate (Vortex) evaluation. Physiological saline or salt water refers to a 0.9 wt% sodium chloride (NaCl) aqueous solution.
[0119] (1) Centrifuge Retention Capacity (CRC, Centrifuge Retention Capacity, g / g) Samples of superabsorbent polymer powders produced according to the examples and comparative examples, with particle sizes ranging from 150 to 850 μm, were taken, and their centrifugal water retention capacity (CRC) was measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP 241.2 based on absorption ratio under no load.
[0120] Specifically, the sample W0 (g) (approximately 0.2g) was uniformly placed in a nonwoven fabric envelope and sealed. The envelope was then immersed in physiological saline (0.9 wt%) at room temperature. After 30 minutes, the envelope was drained for 3 minutes under conditions of 250g using a centrifuge, and the mass of the envelope W2 (g) was measured. The same procedure was then performed without the sample, and the mass W1 (g) was measured. Using the obtained masses, the CRC (g / g) was calculated using the following formula 1.
[0121] [Formula 1] CRC(g / g)={[W2(g)-W1(g)] / W0(g)}-1
[0122] (2) Absorbency under pressure (AUP, g / g) In the examples and comparative examples, the 0.9 psi pressure absorption capacity of each superabsorbent polymer produced was measured using the EDANA method NWSP 242.0.R2. The resin classification used for the CRC measurement was employed for the pressure absorption capacity measurement.
[0123] Specifically, a 400-mesh stainless steel mesh was attached to the bottom of a 25mm inner diameter plastic cylinder. Under normal temperature (23±1℃) and relative humidity (45±1%) conditions, a water-absorbing resin W0 (g) (0.16g) was uniformly spread on the mesh, and a piston capable of uniformly applying a load of 0.9 psi was placed on top. The piston was slightly smaller than the 25mm outer diameter, with no gap between it and the inner wall of the cylinder, so that its vertical movement was not hindered. At this time, the weight W3 (g) of the device was measured.
[0124] A glass filter with a diameter of 90 mm and a thickness of 5 mm was placed inside a 150 mm diameter petroleum dish, and physiological saline solution composed of 0.9 wt% sodium chloride was poured in until it was level with the top surface of the glass filter. A sheet of filter paper with a diameter of 90 mm was placed on top of that. The measuring device was placed on top of the filter paper and allowed to absorb the liquid under load for 1 hour. After 1 hour, the measuring device was lifted and its weight W4 (g) was measured.
[0125] Using the obtained masses, the pressurized absorption capacity (g / g) was calculated using the following equation 2.
[0126] [Formula 2] AUP(g / g) = [W4(g) - W3(g)] / W0(g)
[0127] (3) Gel bed permeability (GBP, darcy) In the examples and comparative examples, the permeability of the manufactured superabsorbent polymer to a free-swell gel bed in physiological saline was measured, and the results are shown in Table 2 below.
[0128] The gel bed permeability is the same as the method described in Korean Patent Application No. 10-2014-7018005 (using the same apparatus), and was measured according to Equation 3 below.
[0129] [Equation 3] K=[Q×H×Mu] / [A×Rho×P]
[0130] In Equation 3 above, K is the permeability (cm 2 ), Q is the flow rate (g / unit time), H is the height of the sample (cm), Mu is the liquid viscosity (poise) (approximately 1 cps for the test solution used in the test), A is the cross-sectional area for liquid flow (cm 2 ), Rho is the liquid density (g / cm 3 ) (relative to the test solution used in the corresponding test), and P is the hydrostatic pressure (dynes / cm 2 ) (typically about 3,923 dynes / cm 2 ).
[0131] The hydrostatic pressure is calculated by the following Equation 3-1.
[0132] [Equation 3-1] P=Rho×g×h
[0133] In Equation 3-1 above, Rho is the liquid density (g / cm 3 ), g is the gravitational acceleration, typically 981 cm / sec 2 , h is the fluid height (for example, 7.8 cm in the case of the permeability test described in the present application).
[0134] (4) Absorption rate (Vortex time, sec) In the examples and comparative examples, 2 ± 0.0001 g of the superabsorbent polymer (based on unclassified polymer) was added to 50 mL of physiological saline (24.4 ± 0.2 °C) and stirred at 600 rpm. The time until the vortex disappeared was measured in seconds.
[0135] [Table 2]
[0136] As can be seen from the data in Table 2 above, it was confirmed that the superabsorbent resin that underwent the surface crosslinking step using the surface crosslinking solution of the present invention exhibits excellent absorption properties. In particular, the above example showed an excellent absorption rate and a significant improvement in gel bed permeability.
Claims
1. A step of forming a hydrated gel polymer containing a crosslinked polymer obtained by crosslinking an acrylic acid monomer having at least a portion of its acidic groups neutralized in the presence of an internal crosslinking agent, The steps include drying, grinding, and classifying the aforementioned water-containing gel polymer to form a base resin powder, The step of crosslinking the surface of a base resin powder in the presence of a surface crosslinking solution comprising an epoxy-based surface crosslinking agent, a monohydric alcohol-based solvent, and a dispersant, and having a surface tension of 36 mN / m to 50 mN / m, A method for producing superabsorbent resins, The dispersant is one or more selected from the group consisting of sodium dodecyl sulfate, poly(dimethyldiallylammonium chloride), aqueous-dispersible silica, calcium stearate, and di(C12-20)alkyldimethylammonium salts. The superabsorbent resin has a gel bed permeability (GBP) of 50 darcy or more. A method for producing superabsorbent polymers.
2. The monohydric alcohol solvent is one or more selected from the group consisting of methanol, ethanol, n-propanol, isopropanol, and butanol. A method for producing a superabsorbent resin according to claim 1.
3. The monohydric alcohol solvent is included in an amount of 1 to 5 parts by weight relative to the total content of the base resin powder. A method for producing a superabsorbent resin according to claim 1.
4. The dispersant is included in an amount of 0.0001 to 1 part by weight relative to the total content of the base resin powder. A method for producing a superabsorbent resin according to claim 1.
5. The epoxy-based surface crosslinking agent is one or more selected from the group consisting of ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, glycerol triglycidyl ether, polyethylene glycol diglycidyl ether, and propylene glycol diglycidyl ether. A method for producing a superabsorbent resin according to claim 1.
6. The epoxy crosslinking agent is included in an amount of 0.01 to 10 parts by weight relative to the total content of the base resin powder. A method for producing a superabsorbent resin according to claim 1.
7. The surface crosslinking solution further comprises one or more additional additives selected from the group consisting of methylene glycol, ethylene glycol, propylene glycol, and butylene glycol. A method for producing a superabsorbent resin according to claim 1.
8. The aforementioned additional additive is included in an amount of 0.1 to 5 parts by weight relative to the total content of the base resin powder. A method for producing a superabsorbent resin according to claim 7.
9. The surface crosslinking solution is included in an amount of 1 to 10 parts by weight per 100 parts by weight of the base resin powder. A method for producing a superabsorbent resin according to claim 1.
Citation Information
Patent Citations
Manufacture of water-absorbing resin
JP1998119042A
Manufacturing method of superabsorbent resin
JP2019537633A
Highly water-absorbent resin and method for producing the same
JP2021505704A
Manufacturing method of superabsorbent resin
JP2023534848A
A method for preparing superabsorbent polymer and superabsorbent polymer prepared thereby
US20180147557A1