Polyimide resin composition and molded body
Patent Information
- Application Number
- JP2024504594
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-06
AI Technical Summary
Polyimide resins with thermoplasticity face challenges in achieving high flame retardancy and maintaining a good appearance, especially when the thickness of molded products is thin, such as in flexible printed circuit boards, where existing solutions like metal phosphinate flame retardants can lead to issues like precipitation and bleed-out.
A polyimide resin composition combining specific polyimide structural units with an aromatic condensed phosphate ester flame retardant, which maintains compatibility and prevents thermal decomposition, ensuring high flame retardancy and good appearance even in thin products.
The composition achieves high flame retardancy and low dielectric properties, suitable for applications like 5G communication components, while maintaining excellent moldability and appearance, even in thin products.
Smart Images

Figure 2023166971000001 
Figure 2023166971000002 
Figure 2023166971000003
Abstract
Description
Polyimide resin composition and molded article
[0001] The present invention relates to a polyimide resin composition and a molded article.
[0002] Polyimide resins are useful engineering plastics with high thermal stability, strength, and solvent resistance due to the rigidity of their molecular chains, resonance stabilization, and strong chemical bonds, and are used in a wide range of fields. While polyimide resins have high heat resistance, they lack thermoplasticity and have the drawback of poor moldability. However, in recent years, thermoplastic polyimide resins have been reported. Thermoplastic polyimide resins not only have the inherent heat resistance of polyimide resins, but also have excellent moldability. Therefore, thermoplastic polyimide resins can be used to mold products used in harsh environments where general-purpose thermoplastic resins such as nylon and polyester cannot.
[0003] One commonly known molecular design technique for imparting thermoplasticity to polyimide resins is to incorporate flexible structures, such as aliphatic structures, into the main chain. Aliphatic structures have the advantages of relatively easily imparting thermoplasticity to polyimides and of easily exhibiting low dielectric properties due to their bulkiness. However, they have the drawback of being inferior in oxidation resistance compared to aromatic structures, which ultimately reduces the inherently high flame retardancy of polyimides. To apply such thermoplastic polyimide resins to applications requiring high flame retardancy, efforts have been made to improve flame retardancy by adding flame retardants. For example, Patent Document 1 discloses that a polyimide resin composition containing a polyimide resin of a specific structure and a metal phosphinate flame retardant exhibits excellent moldability, high flame retardancy, and a good appearance.
[0004] International Publication No. 2019 / 220968
[0005] Among polyimide resins, semi-aromatic polyimide resins, fully aliphatic polyimide resins, and polyimide resins containing bulky substituents such as fluorine, in addition to the inherent high heat resistance and dimensional stability of polyimide resins, can achieve extremely low dielectric properties (low dielectric constant and low dielectric dissipation factor) as a resin material. Therefore, polyimide resins are also attracting attention for their application to fifth-generation mobile communication system (5G) related components (flexible printed circuit boards, antennas, etc.) and other electrical and electronic components, which require low dielectric properties. In addition to low dielectric properties, these applications require high flame retardancy, as with the technology disclosed in Patent Document 1, and a good appearance without bleed-out or other issues even when flame retardants are added. However, when the molded product is thin, such as in flexible printed circuit boards, it is extremely difficult to achieve high flame retardancy and a good appearance when the thickness of the molded product is 500 μm or less, 200 μm or less, or even less than 100 μm. The technology disclosed in Patent Document 1 leaves room for improvement in this regard. An object of the present invention is to provide a polyimide resin composition from which a molded article can be produced that has both high flame retardancy and good appearance even when the molded article has a small thickness (for example, 500 μm or less).
[0006] The present inventors have found that a polyimide resin composition containing a polyimide resin having a specific combination of different polyimide structural units in a specific ratio and an organic flame retardant having a specific structure can solve the above problems. Specifically, the present invention relates to the following: [1] A polyimide resin composition comprising: a polyimide resin (A) containing repeating structural units represented by the following formula (1) and repeating structural units represented by the following formula (2), wherein the content of the repeating structural units of formula (1) relative to the total of the repeating structural units of formula (1) and the repeating structural units of formula (2) is 20 to 70 mol %; and a compound (B) represented by the following formula (5). (R 1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. 2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. 1 and X 2 are each independently a tetravalent group containing at least one aromatic ring and having 6 to 22 carbon atoms. (R 51 is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. 52 ~R 53 , and R 61 ~R 66 are each independently an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 51 is an integer from 0 to 6, p 52 and p 53 are each independently an integer of 0 to 4, and p 63 and p 66 are each independently an integer of 0 to 3. 51 ~p 53 , p 63 , or p 66 When R is 2 or more, a plurality of R 51 ~R 53 , R 63 or R 66 may be the same or different, and n is an integer of 1 to 10.
[0007] The polyimide resin composition of the present invention can produce a molded article that has both high flame retardancy and good appearance even when the molded article has a thin thickness (for example, 500 μm or less). Furthermore, the polyimide resin composition and a molded article containing the same have high heat resistance (high glass transition temperature) and low dielectric properties. Therefore, the polyimide resin composition and molded article of the present invention can be used in applications requiring high flame retardancy, a low dielectric constant, and a low dielectric dissipation factor, such as 5G or sixth-generation mobile communication system (6G) related components using a frequency band of 70 GHz to 300 GHz, various antennas, various antenna substrates, wire coating materials, bonding sheets, insulating films, raw materials for carbon fiber reinforced plastics (CFRP), high-frequency circuit boards, printed wiring boards, chip-on-film (COF) flexible substrates, multilayer laminates, LED-mounted substrates, industrial robot substrates, communication substrates for household robots, semiconductor element materials, wafers for high-frequency devices, Wi-Fi chips, wireless communication devices, transmission lines, bearing coatings, heat-insulating shafts, trays, various belts, heat-resistant low-dielectric tapes, heat-resistant low-dielectric tubes, various sensors, various radars, radomes (radar domes), optical communication modules (TOSA / ROSA), 8k-TV cable mobile terminals or digital home appliances, base stations, drones, surveillance cameras, indoor or outdoor servers, artificial satellites, and communication equipment for space stations.
[0008] [Polyimide Resin Composition] The polyimide resin composition of the present invention contains a polyimide resin (A) that contains a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content of the repeating structural unit of formula (1) relative to the total of the repeating structural units of formula (1) and formula (2) is 20 to 70 mol %, and a compound (B) that is represented by the following formula (5). (R 1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. 2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. 1 and X 2 are each independently a tetravalent group containing at least one aromatic ring and having 6 to 22 carbon atoms. (R 51is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. 52 ~R 53 , and R 61 ~R 66 are each independently an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 51 is an integer from 0 to 6, p 52 and p 53 are each independently an integer of 0 to 4, and p 63 and p 66 are each independently an integer of 0 to 3. 51 ~p 53 , p 63 , or p 66 When R is 2 or more, a plurality of R 51 ~R 53 , R 63 or R 66 may be the same or different, and n is an integer of 1 to 10.
[0009] The polyimide resin composition of the present invention exhibits thermoplasticity by containing a polyimide resin (A) formed by combining specific different polyimide structural units in the above-mentioned specific ratio, resulting in a resin composition with excellent moldability. Furthermore, by combining the polyimide resin (A) with a specific compound (B), molded articles can be produced that exhibit both high flame retardancy and good appearance, even when the article is thin (e.g., 500 μm or less). The reason for the above effects of the present invention is unclear, but it is thought to be as follows: Compound (B) has high heat resistance among aromatic condensed phosphate ester-based flame retardants. On the other hand, since Compound (B) is an organic flame retardant with a melting point, it is believed to have relatively high compatibility with the polyimide resin (A) during thermoforming, unlike granular flame retardants without a melting point, such as metal phosphinate-based flame retardants. Therefore, the polyimide resin composition of the present invention can exhibit high flame retardancy even when a thin molded article is produced, and it is believed that precipitation, thermal decomposition, bleed-out, etc. of Compound (B) in the molded article are unlikely to occur, thereby maintaining a good appearance.
[0010] Polyimide resin (A) is a highly crystalline thermoplastic resin. When a granular flame retardant without a melting point, such as a metal phosphinate-based flame retardant, is added to the polyimide resin (A), the flame retardant tends to act as a crystal nucleating agent and promote crystallization. Generally, if the crystallization of a crystalline thermoplastic resin is too rapid, solidification progresses as the crystallization progresses, which can lead to a decrease in extrudability during melt mixing and cooling. However, compound (B) has the effect of delaying the crystallization of polyimide resin (A), i.e., slowing the solidification rate, and also has the effect of improving the extrudability of the resulting polyimide resin composition. Furthermore, polyimide resin compositions containing compound (B) can maintain or improve the low dielectric properties inherent in polyimide resin (A), thereby achieving extremely low dielectric constants and dielectric loss tangents as resin materials.
[0011] <Polyimide Resin (A)> The polyimide resin (A) used in the present invention contains a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), and the content ratio of the repeating structural unit of formula (1) to the total of the repeating structural units of formula (1) and formula (2) is 20 to 70 mol %. (R 1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. 2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. 1 and X 2 are each independently a tetravalent group containing at least one aromatic ring and having 6 to 22 carbon atoms.
[0012] The polyimide resin (A) used in the present invention is a thermoplastic resin, and is preferably in the form of powder or pellets. Thermoplastic polyimide resins are distinguished from polyimide resins that do not have a glass transition temperature (Tg) or that decompose at a temperature lower than the glass transition temperature, and are formed by molding a polyimide precursor such as polyamic acid and then closing the imide ring.
[0013] The repeating structural unit of formula (1) is described in detail below. 1is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. Here, the alicyclic hydrocarbon structure refers to a ring derived from an alicyclic hydrocarbon compound, and the alicyclic hydrocarbon compound may be saturated or unsaturated, and may be monocyclic or polycyclic. Examples of alicyclic hydrocarbon structures include, but are not limited to, cycloalkane rings such as a cyclohexane ring, cycloalkene rings such as cyclohexene, bicycloalkane rings such as norbornane, and bicycloalkene rings such as norbornene. Among these, a cycloalkane ring is preferred, a cycloalkane ring having 4 to 7 carbon atoms is more preferred, and a cyclohexane ring is even more preferred. R 1 has 6 to 22 carbon atoms, preferably 8 to 17. 1 contains at least one alicyclic hydrocarbon structure, preferably 1 to 3.
[0014] R 1 is preferably a divalent group represented by the following formula (R1-1) or (R1-2): (m 11 and m 12 are each independently an integer of 0 to 2, preferably 0 or 1. 13 ~m 15 are each independently an integer of 0 to 2, preferably 0 or 1.
[0015] R 1 is particularly preferably a divalent group represented by the following formula (R1-3): In the divalent group represented by the above formula (R1-3), the positional relationship of the two methylene groups with respect to the cyclohexane ring may be either cis or trans, and the ratio of cis to trans may be any value.
[0016] X 1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a single ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited to these. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred. X 1has 6 to 22 carbon atoms, preferably 6 to 18. 1 contains at least one aromatic ring, preferably 1 to 3.
[0017] X 1 is preferably a tetravalent group represented by any one of the following formulae (X-1) to (X-4). (R 11 ~R 18 are each independently an alkyl group having 1 to 4 carbon atoms. 11 ~p 13 are each independently an integer of 0 to 2, preferably 0. 14 , p 15 , p 16 and p 18 are each independently an integer of 0 to 3, preferably 0. 17 is an integer of 0 to 4, preferably 0. 11 ~L 13 are each independently a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms. 1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, and therefore, R 12 , R 13 , p 12 and p 13 is selected so that the number of carbon atoms in the tetravalent group represented by formula (X-2) is in the range of 10 to 22. Similarly, L in formula (X-3) 11 , R 14 , R 15 , p 14 and p 15 is selected so that the number of carbon atoms of the tetravalent group represented by formula (X-3) is in the range of 12 to 22, and L in formula (X-4) 12 , L 13 , R 16 , R 17 , R 18 , p 16 , p 17 and p 18 is selected so that the number of carbon atoms in the tetravalent group represented by formula (X-4) falls within the range of 18 to 22.
[0018] X 1is particularly preferably a tetravalent group represented by the following formula (X-5) or (X-6).
[0019] Next, the repeating structural unit of formula (2) will be described in detail below. 2 is a divalent chain aliphatic group having 5 to 16 carbon atoms, preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms. Here, the chain aliphatic group means a group derived from a chain aliphatic compound, and the chain aliphatic compound may be saturated or unsaturated, linear or branched, and may contain a heteroatom such as an oxygen atom. 2 is preferably an alkylene group having 5 to 16 carbon atoms, more preferably an alkylene group having 6 to 14 carbon atoms, even more preferably an alkylene group having 7 to 12 carbon atoms, and among these, an alkylene group having 8 to 10 carbon atoms is preferred. The alkylene group may be a linear alkylene group or a branched alkylene group, but is preferably a linear alkylene group. 2 is preferably at least one selected from the group consisting of an octamethylene group and a decamethylene group, and particularly preferably an octamethylene group.
[0020] Also, R 2 Another preferred embodiment of the group R2-1 is a divalent chain aliphatic group containing an ether group and having 5 to 16 carbon atoms. The number of carbon atoms is preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10. Among these, a divalent group represented by the following formula (R2-1) or (R2-2) is preferred. (m 21 and m 22 are each independently an integer of 1 to 15, preferably 1 to 13, more preferably 1 to 11, and even more preferably 1 to 9. 23 ~m 25 are each independently an integer of 1 to 14, preferably 1 to 12, more preferably 1 to 10, and even more preferably 1 to 8. 2is a divalent chain aliphatic group having 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms), and therefore, m in formula (R2-1) 21 and m 22 is selected so that the carbon number of the divalent group represented by formula (R2-1) is in the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). 21 +m 22 is 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10). 23 ~m 25 is selected so that the carbon number of the divalent group represented by formula (R2-2) is in the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). 23 +m 24 +m 25 has 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms).
[0021] X 2 is X in formula (1). 1 The definitions and preferred embodiments are the same as above.
[0022] The content ratio of the repeating structural unit of formula (1) relative to the total of the repeating structural units of formula (1) and formula (2) is 20 to 70 mol%. When the content ratio of the repeating structural unit of formula (1) is within the above range, the polyimide resin can be sufficiently crystallized even in a typical injection molding cycle. If the content ratio is less than 20 mol%, moldability decreases, and if it exceeds 70 mol%, crystallinity decreases, resulting in decreased heat resistance. From the viewpoint of achieving high crystallinity, the content ratio of the repeating structural unit of formula (1) relative to the total of the repeating structural units of formula (1) and formula (2) is preferably 65 mol% or less, more preferably 60 mol% or less, and even more preferably 50 mol% or less. In particular, the content ratio of the repeating structural unit of formula (1) relative to the total of the repeating structural units of formula (1) and formula (2) is preferably 20 mol% or more but less than 40 mol%. Within this range, the crystallinity of the polyimide resin (A) is increased, resulting in a resin composition with even better heat resistance. From the viewpoint of moldability, the content ratio is preferably 25 mol% or more, more preferably 30 mol% or more, and even more preferably 32 mol% or more, and from the viewpoint of expressing high crystallinity, it is even more preferably 35 mol% or less.
[0023] The total content of the repeating structural units of formula (1) and formula (2) relative to all repeating structural units constituting the polyimide resin (A) is preferably 50 to 100 mol %, more preferably 75 to 100 mol %, even more preferably 80 to 100 mol %, and still more preferably 85 to 100 mol %.
[0024] The polyimide resin (A) may further contain a repeating structural unit of the following formula (3). In this case, the content ratio of the repeating structural unit of formula (3) relative to the total of the repeating structural units of formula (1) and formula (2) is preferably 25 mol% or less. On the other hand, there is no particular lower limit, as long as it is greater than 0 mol%. From the viewpoint of improving heat resistance, the content ratio is preferably 5 mol% or more, more preferably 10 mol% or more, while from the viewpoint of maintaining crystallinity, the content ratio is preferably 20 mol% or less, more preferably 15 mol% or less. (R 3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. 3 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.
[0025] R 3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a single ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited to these. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred. R 3 has 6 to 22 carbon atoms, preferably 6 to 18. 3 contains at least one aromatic ring, preferably 1 to 3. The aromatic ring may have a monovalent or divalent electron-withdrawing group bonded thereto. Examples of the monovalent electron-withdrawing group include a nitro group, a cyano group, a p-toluenesulfonyl group, halogen, a halogenated alkyl group, a phenyl group, and an acyl group. Examples of the divalent electron-withdrawing group include a fluorinated alkylene group (e.g., -C(CF 3 ) 2 -, - (CF 2 ) p In addition to halogenated alkylene groups such as - (where p is an integer from 1 to 10), -CO-, -SO 2 -, -SO-, -CONH-, -COO- and the like.
[0026] R 3 is preferably a divalent group represented by the following formula (R3-1) or (R3-2). (m 31 and m 32 are each independently an integer of 0 to 2, preferably 0 or 1. 33 and m 34 are each independently an integer of 0 to 2, preferably 0 or 1. 21 , R 22 , and R 23 are each independently an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or an alkynyl group having 2 to 4 carbon atoms. 21 , p22 and p 23 is an integer of 0 to 4, preferably 0. 21 is a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms. 3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, and therefore, m 31 , m 32 , R 21 and p 21 is selected so that the number of carbon atoms of the divalent group represented by formula (R3-1) is in the range of 6 to 22. Similarly, L in formula (R3-2) 21 , m 33 , m 34 , R 22 , R 23 , p 22 and p 23 is selected so that the number of carbon atoms in the divalent group represented by formula (R3-2) falls within the range of 12 to 22.
[0027] X 3 is X in formula (1). 1 The definitions and preferred embodiments are the same as above.
[0028] The polyimide resin (A) may further contain a repeating structural unit represented by the following formula (4). (R 4 Ha-SO 2 - or -Si(R x ) (R y ) is a divalent group containing O—, and R x and R y each independently represents a chain aliphatic group having 1 to 3 carbon atoms or a phenyl group. 4 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. 4 is X in formula (1). 1 The definitions and preferred embodiments are the same as above.
[0029] The terminal structure of the polyimide resin (A) is not particularly limited, but it is preferable that the polyimide resin (A) has a chain aliphatic group having 5 to 14 carbon atoms at the terminal. The chain aliphatic group may be saturated or unsaturated, and may be linear or branched. When the polyimide resin (A) has the above-mentioned specific group at the terminal, a resin composition with excellent heat aging resistance can be obtained. Examples of saturated chain aliphatic groups having 5 to 14 carbon atoms include an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, a lauryl group, an n-tridecyl group, an n-tetradecyl group, an isopentyl group, a neopentyl group, a 2-methylpentyl group, a 2-methylhexyl group, a 2-ethylpentyl group, a 3-ethylpentyl group, an isooctyl group, a 2-ethylhexyl group, a 3-ethylhexyl group, an isononyl group, a 2-ethyloctyl group, an isodecyl group, an isododecyl group, an isotridecyl group, and an isotetradecyl group. Examples of unsaturated chain aliphatic groups having 5 to 14 carbon atoms include 1-pentenyl, 2-pentenyl, 1-hexenyl, 2-hexenyl, 1-heptenyl, 2-heptenyl, 1-octenyl, 2-octenyl, nonenyl, decenyl, dodecenyl, tridecenyl, and tetradecenyl groups. Among these, the chain aliphatic groups are preferably saturated chain aliphatic groups, and more preferably saturated linear chain aliphatic groups. Furthermore, from the viewpoint of obtaining heat aging resistance, the chain aliphatic groups preferably have 6 or more carbon atoms, more preferably 7 or more carbon atoms, and even more preferably 8 or more carbon atoms, and preferably have 12 or less carbon atoms, more preferably 10 or less carbon atoms, and even more preferably have 9 or less carbon atoms. The chain aliphatic groups may be of one type, or two or more types. The chain aliphatic group is particularly preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, a 2-ethylhexyl group, an n-nonyl group, an isononyl group, an n-decyl group, and an isodecyl group, further preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, a 2-ethylhexyl group, an n-nonyl group, and an isononyl group, and most preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, and a 2-ethylhexyl group.From the viewpoint of heat aging resistance, the polyimide resin (A) preferably has, at its terminals, only chain aliphatic groups having 5 to 14 carbon atoms in addition to terminal amino groups and terminal carboxy groups. When a group other than the above is present at its terminals, the content thereof is preferably 10 mol % or less, more preferably 5 mol % or less, based on the chain aliphatic groups having 5 to 14 carbon atoms.
[0030] From the viewpoint of exhibiting excellent heat aging resistance, the content of the chain aliphatic groups having 5 to 14 carbon atoms in the polyimide resin (A) is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, and even more preferably 0.2 mol% or more, based on 100 mol% of the total of all repeating structural units constituting the polyimide resin (A). Furthermore, in order to ensure a sufficient molecular weight and obtain good mechanical properties, the content of the chain aliphatic groups having 5 to 14 carbon atoms in the polyimide resin (A) is preferably 10 mol% or less, more preferably 6 mol% or less, and even more preferably 3.5 mol% or less, based on 100 mol% of the total of all repeating structural units constituting the polyimide resin (A). The content of the chain aliphatic groups having 5 to 14 carbon atoms in the polyimide resin (A) can be determined by depolymerizing the polyimide resin (A).
[0031] The polyimide resin (A) preferably has a melting point of 360°C or lower and a glass transition temperature of 150°C or higher. From the viewpoint of heat resistance, the melting point of the polyimide resin is more preferably 280°C or higher, even more preferably 290°C or higher. From the viewpoint of exhibiting high moldability, it is preferably 345°C or lower, more preferably 340°C or lower, even more preferably 335°C or lower. From the viewpoint of exhibiting high moldability, the glass transition temperature of the polyimide resin (A) is more preferably 160°C or higher, more preferably 170°C or higher. From the viewpoint of exhibiting high moldability, it is preferably 250°C or lower, more preferably 230°C or lower, even more preferably 200°C or lower. The melting point and glass transition temperature of the polyimide resin (A) can both be measured by a differential scanning calorimeter. Furthermore, from the viewpoint of improving crystallinity, heat resistance, mechanical strength, and chemical resistance, the polyimide resin (A) preferably has a heat value of 5.0 mJ / mg or more, more preferably 10.0 mJ / mg or more, and even more preferably 17.0 mJ / mg or more, of the heat value of the crystallization exotherm peak observed when the polyimide resin is melted and then cooled at a temperature decreasing rate of 20°C / min, as measured by a differential scanning calorimeter. The upper limit of the heat value of crystallization is not particularly limited, but is usually 45.0 mJ / mg or less. The melting point, glass transition temperature, and heat value of crystallization of the polyimide resin (A) can be specifically measured by the method described in the Examples.
[0032] The logarithmic viscosity of a 0.5 mass % solution of polyimide resin (A) in concentrated sulfuric acid at 30°C is preferably in the range of 0.2 to 2.0 dL / g, more preferably 0.3 to 1.8 dL / g. If the logarithmic viscosity is 0.2 dL / g or higher, sufficient mechanical strength can be obtained when the resulting polyimide resin composition is molded into a molded article, and if it is 2.0 dL / g or lower, good moldability and handleability can be obtained. The logarithmic viscosity μ can be calculated by measuring the flow times of concentrated sulfuric acid and the polyimide resin solution at 30°C using a Cannon-Fenske viscometer, and then using the following formula: μ=ln(ts / t 0 ) / C t 0 : Time during which concentrated sulfuric acid flows ts: Time during which polyimide resin solution flows C: 0.5 (g / dL)
[0033] The weight-average molecular weight Mw of the polyimide resin (A) is preferably in the range of 10,000 to 150,000, more preferably 15,000 to 100,000, even more preferably 20,000 to 80,000, still more preferably 30,000 to 70,000, and even more preferably 35,000 to 65,000. If the weight-average molecular weight Mw of the polyimide resin (A) is 10,000 or more, the mechanical strength of the resulting molded article will be good; if it is 40,000 or more, the stability of the mechanical strength will be good; and if it is 150,000 or less, the moldability will be good. The weight-average molecular weight Mw of the polyimide resin (A) can be measured by gel permeation chromatography (GPC) using polymethyl methacrylate (PMMA) as a standard sample.
[0034] (Method for Producing Polyimide Resin (A)) The polyimide resin (A) can be produced by reacting a tetracarboxylic acid component with a diamine component. The tetracarboxylic acid component contains a tetracarboxylic acid and / or a derivative thereof having at least one aromatic ring, and the diamine component contains a diamine having at least one alicyclic hydrocarbon structure and a chain aliphatic diamine.
[0035] The tetracarboxylic acid containing at least one aromatic ring is preferably a compound in which four carboxy groups are directly bonded to the aromatic ring, and may contain an alkyl group in the structure. The tetracarboxylic acid preferably has 6 to 26 carbon atoms. Examples of the tetracarboxylic acid include pyromellitic acid, 2,3,5,6-toluenetetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, and 1,4,5,8-naphthalenetetracarboxylic acid. Among these, pyromellitic acid is more preferred.
[0036] Examples of the derivative of a tetracarboxylic acid containing at least one aromatic ring include anhydrides or alkyl esters of tetracarboxylic acids containing at least one aromatic ring. The tetracarboxylic acid derivative preferably has 6 to 38 carbon atoms. Examples of the anhydrides of tetracarboxylic acids include pyromellitic acid monoanhydride, pyromellitic acid dianhydride, 2,3,5,6-toluenetetracarboxylic acid dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic acid dianhydride, 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, and 1,4,5,8-naphthalenetetracarboxylic acid dianhydride. Examples of alkyl esters of tetracarboxylic acids include dimethyl pyromellitic acid, diethyl pyromellitic acid, dipropyl pyromellitic acid, diisopropyl pyromellitic acid, dimethyl 2,3,5,6-toluenetetracarboxylate, dimethyl 3,3',4,4'-diphenylsulfonetetracarboxylate, dimethyl 3,3',4,4'-benzophenonetetracarboxylate, dimethyl 3,3',4,4'-biphenyltetracarboxylate, dimethyl 1,4,5,8-naphthalenetetracarboxylate, etc. In the alkyl esters of tetracarboxylic acids, the alkyl group preferably has 1 to 3 carbon atoms.
[0037] The tetracarboxylic acid and / or derivative thereof containing at least one aromatic ring may be at least one compound selected from the above, and may be used alone or in combination of two or more compounds.
[0038] The diamine containing at least one alicyclic hydrocarbon structure preferably has 6 to 22 carbon atoms, and examples thereof include 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, 4,4'-methylenebis(2-methylcyclohexylamine), carvonediamine, limonenediamine, isophoronediamine, norbornanediamine, bis(aminomethyl)tricyclo[5.2.1.0] ... 2,6]decane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylpropane, etc. are preferred. These compounds may be used alone, or two or more compounds selected from these may be used in combination. Of these, 1,3-bis(aminomethyl)cyclohexane is preferably used. Note that diamines containing an alicyclic hydrocarbon structure generally have structural isomers, but the ratio of cis / trans isomers is not limited.
[0039] The chain aliphatic diamine may be linear or branched, and preferably has 5 to 16 carbon atoms, more preferably 6 to 14, and even more preferably 7 to 12. Furthermore, as long as the chain portion has 5 to 16 carbon atoms, it may contain an ether bond therebetween. Preferred examples of the chain aliphatic diamine include 1,5-pentamethylenediamine, 2-methylpentane-1,5-diamine, 3-methylpentane-1,5-diamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine, and 2,2'-(ethylenedioxy)bis(ethyleneamine). The chain aliphatic diamine may be used alone or in combination. Among these, chain aliphatic diamines having 8 to 10 carbon atoms are preferably used, and at least one selected from the group consisting of 1,8-octamethylenediamine and 1,10-decamethylenediamine is particularly preferably used.
[0040] In producing the polyimide resin (A), the molar ratio of the amount of the diamine containing at least one alicyclic hydrocarbon structure charged to the total amount of the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine is preferably 20 to 70 mol %. This molar ratio is preferably 25 mol % or more, more preferably 30 mol % or more, and even more preferably 32 mol % or more, and from the viewpoint of achieving high crystallinity, is preferably 60 mol % or less, more preferably 50 mol % or less, even more preferably less than 40 mol %, and even more preferably 35 mol % or less.
[0041] The diamine component may also contain a diamine containing at least one aromatic ring. The diamine containing at least one aromatic ring preferably has 6 to 22 carbon atoms, and examples thereof include ortho-xylylenediamine, meta-xylylenediamine, para-xylylenediamine, 1,2-diethynylbenzenediamine, 1,3-diethynylbenzenediamine, 1,4-diethynylbenzenediamine, 1,2-diaminobenzene, 1,3-diaminobenzene, 1,4-diaminobenzene, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, α,α'-bis(4-aminophenyl)1,4-diisopropylbenzene, α,α'-bis(3-aminophenyl)-1,4-diisopropylbenzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,6-diaminonaphthalene, and 1,5-diaminonaphthalene.
[0042] In the above, the molar ratio of the amount of the diamine containing at least one aromatic ring to the total amount of the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine is preferably 25 mol% or less. On the other hand, the lower limit is not particularly limited, as long as it is greater than 0 mol%. From the viewpoint of improving heat resistance, the molar ratio is preferably 5 mol% or more, more preferably 10 mol% or more, while from the viewpoint of maintaining crystallinity, the molar ratio is preferably 20 mol% or less, more preferably 15 mol% or less. Furthermore, from the viewpoint of reducing coloration of the polyimide resin (A), the molar ratio is preferably 12 mol% or less, more preferably 10 mol% or less, even more preferably 5 mol% or less, and even more preferably 0 mol%.
[0043] When producing the polyimide resin (A), the ratio of the amount of the tetracarboxylic acid component to the amount of the diamine component charged is preferably 0.9 to 1.1 moles of the diamine component per mole of the tetracarboxylic acid component.
[0044] Furthermore, when producing the polyimide resin (A), a terminal-capping agent may be mixed in addition to the tetracarboxylic acid component and the diamine component. The terminal-capping agent is preferably at least one selected from the group consisting of monoamines and dicarboxylic acids. The amount of terminal-capping agent used may be any amount sufficient to introduce the desired amount of terminal groups into the polyimide resin (A), and is preferably 0.0001 to 0.1 mol, more preferably 0.001 to 0.06 mol, and even more preferably 0.002 to 0.035 mol per mol of the tetracarboxylic acid and / or its derivative. Among these, monoamine terminal-capping agents are preferred. From the viewpoint of introducing the aforementioned linear aliphatic group having 5 to 14 carbon atoms to the terminal of the polyimide resin (A) to improve heat aging resistance, monoamines having a linear aliphatic group having 5 to 14 carbon atoms are more preferred, and monoamines having a saturated linear aliphatic group having 5 to 14 carbon atoms are even more preferred. The end-capping agent is particularly preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, isononylamine, n-decylamine, and isodecylamine, more preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, and isononylamine, and most preferably at least one selected from the group consisting of n-octylamine, isooctylamine, and 2-ethylhexylamine.
[0045] As a polymerization method for producing the polyimide resin (A), a known polymerization method can be applied, and the method described in WO 2016 / 147996 can be used.
[0046] <Compound (B)> The polyimide resin composition of the present invention contains a polyimide resin (A) and a compound (B) represented by the following formula (5). By using the compound (B) represented by formula (5) as a flame retardant for the polyimide resin (A) having the specific structure, the obtained molded article can have high flame retardancy and a good appearance even when it is thin. Furthermore, the use of compound (B) improves the extrudability of the polyimide resin composition, and furthermore, it is possible to achieve an extremely low dielectric constant and dielectric loss tangent for a resin material. (R 51 is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. 52 ~R 53 , and R 61 ~R 66 are each independently an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 51 is an integer from 0 to 6, p 52 and p 53 are each independently an integer of 0 to 4, and p 63 and p 66 are each independently an integer of 0 to 3. 51 ~p 53 , p 63 , or p 66 When R is 2 or more, a plurality of R 51 ~R 53 , R 63 or R 66 may be the same or different, and n is an integer of 1 to 10.
[0047] In formula (5), R 51 is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably an alkyl group having 1 to 4 carbon atoms.
[0048] The alkyl group having 1 to 10 carbon atoms may be either linear or branched, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a 2-methylbutyl group, a 1-methylbutyl group, a 1,2-dimethylpropyl group, a neopentyl group (2,2-dimethylpropyl group), a tert-pentyl group (1,1-dimethylpropyl group), an n-hexyl group, an isopropyl ... hexyl group, 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 1-ethylbutyl group, 2-ethylbutyl group, 1,1-dimethylbutyl group, 1,2-dimethylbutyl group, 1,3-dimethylbutyl group, 2,2-dimethylbutyl group, 2,3-dimethylbutyl group, 1-ethyl-1-methylpropyl group, 1-ethyl-2-methylpropyl group, n-heptyl group, isoheptyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methyl propylhexyl group, 4-methylhexyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1-propylbutyl group, 1,1-dimethylpentyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 1,4-dimethylpentyl group, 1-ethyl-1-methylbutyl group, 1-ethyl-2-methylbutyl group, 1-ethyl-3-methylbutyl group, 2-ethyl-1-methylbutyl group, 2-ethyl-1-methylbutyl group, 2- Examples of alkyl groups include ethyl-2-methylbutyl, 2-ethyl-3-methylbutyl, 1,1-diethylpropyl, n-octyl, isooctyl, 1-methylheptyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 5-methylheptyl, 1-ethylhexyl, 2-ethylhexyl, 3-ethylhexyl, 4-ethylhexyl, 1-propylheptyl, 2-propylheptyl, nonyl, and decyl.
[0049] Among the above alkyl groups, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a 2-methylbutyl group, a 1-methylbutyl group, a 1,2-dimethylpropyl group, a neopentyl group (2,2-dimethylpropyl group), a tert-pentyl group (1,1-dimethylpropyl group), an n-hexyl group, an isohexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1-ethylpentyl group, a 2-ethylpentyl group, a 3-ethylpentyl group, a 2 ...
[0044] Preferred are a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, or a tert-butyl group, and more preferred are a methyl group or an ethyl group, and still more preferred is a methyl group.
[0050] The alkoxy group having 1 to 10 carbon atoms may be either linear or branched, and examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentyloxy group, an isopentyloxy group, a 2-methylbutoxy group, a 1-methylbutoxy group, a 1,2-dimethylpropoxy group, a neopentyloxy group (2,2-dimethylpropoxy group), a tert-pentyloxy group (1,1-dimethylpropoxy group), an n-hexyloxy group, an isohexyloxy group, and the like. groups, 1-methylpentyloxy group, 2-methylpentyloxy group, 3-methylpentyloxy group, 1-ethylbutoxy group, 2-ethylbutoxy group, 1,1-dimethylbutoxy group, 1,2-dimethylbutoxy group, 1,3-dimethylbutoxy group, 2,2-dimethylbutoxy group, 2,3-dimethylbutoxy group, 1-ethyl-1-methylpropoxy group, 1-ethyl-2-methylpropoxy group, n-heptyloxy group, isoheptyloxy group, 1-methylhexyloxy group, 2-methylhexyloxy group, 3-methylhexyloxy group, 4-methylhexyloxy group, 1-ethylpentyloxy group, 2-ethylpentyloxy group, 3-ethylpentyloxy group, 1-propylbutoxy group, 1,1-dimethylpentyloxy group, 1,2-dimethylpentyloxy group, 1,3-dimethylpentyloxy group, 1,4-dimethylpentyloxy group, 1-ethyl-1-methylbutoxy group, 1-ethyl-2-methylbutoxy group, 1-ethyl-3-methylbutoxy group, 2-ethyl-1-methylbutoxy group, 2-ethyl-1-methylbutoxy group, 2-ethyl-2-methylbutoxy Examples thereof include a silyl group, a 2-ethyl-3-methylbutoxy group, a 1,1-diethylpropoxy group, an n-octyloxy group, an isooctyloxy group, a 1-methylheptyloxy group, a 2-methylheptyloxy group, a 3-methylheptyloxy group, a 4-methylheptyloxy group, a 5-methylheptyloxy group, a 1-ethylhexyloxy group, a 2-ethylhexyloxy group, a 3-ethylhexyloxy group, a 4-ethylhexyloxy group, a 1-propylheptyloxy group, a 2-propylheptyloxy group, a nonyloxy group, and a decyloxy group.
[0051] Among the above alkoxy groups, a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentyloxy group, an isopentyloxy group, a 2-methylbutoxy group, a 1-methylbutoxy group, a 1,2-dimethylpropoxy group, a neopentyloxy group (2,2-dimethylpropoxy group), a tert-pentyloxy group (1,1-dimethylpropoxy group), an n-hexyloxy group, an isohexyloxy group, a 1-methylpentyloxy group, a 2- Methylpentyloxy group, 3-methylpentyloxy group, 1-ethylbutoxy group, 2-ethylbutoxy group, 1,1-dimethylbutoxy group, 1,2-dimethylbutoxy group, 1,3-dimethylbutoxy group, 2,2-dimethylbutoxy group, 2,3-dimethylbutoxy group, 1-ethyl-1-methylpropoxy group, or 1-ethyl-2-methylpropoxy group is preferred, and methoxy group, ethoxy group, n-propoxy group, isopropoxy group, n-butoxy group, isobutoxy group, or tert-butoxy group is more preferred.
[0052] R 52 ~R 53 , and R 61 ~R 66 are each independently an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and even more preferably an alkyl group having 1 or 2 carbon atoms. The alkyl group having 1 to 4 carbon atoms may be either linear or branched, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group. Of the above alkyl groups, a methyl group, an ethyl group, an n-propyl group, or an isopropyl group is preferred, a methyl group or an ethyl group is more preferred, and a methyl group is even more preferred.
[0053] The alkoxy group having 1 to 4 carbon atoms may be either linear or branched, and examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, and a tert-butoxy group. Among the above alkoxy groups, a methoxy group, an ethoxy group, an n-propoxy group, and an isopropoxy group are preferred, and a methoxy group or an ethoxy group is more preferred.
[0054] In formula (5), p 51 is an integer of 0 to 6, preferably 0 to 5, more preferably 0 to 3. 52 and p 53 are each independently an integer of 0 to 4, preferably 0 to 2, and more preferably 0. 63 and p 66 are each independently an integer of 0 to 3, preferably 0 or 1, and more preferably 0. n is an integer of 1 to 10, preferably 1 to 5, more preferably 1 to 3, and even more preferably 1.
[0055] From the viewpoint of achieving both high flame retardancy and good appearance even in a thin molded article having a thickness of, for example, 500 μm or less, compound (B) is preferably at least one selected from the group consisting of compounds represented by the following structural formulas (B1) to (B3). More preferably, compound (B) is a compound represented by the following structural formula (B3).
[0056] As the compound (B), commercially available products such as "SR-3000" manufactured by Daihachi Chemical Industry Co., Ltd. can also be used.
[0057] The content of compound (B) in the polyimide resin composition is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 30 parts by mass, even more preferably 1 to 30 parts by mass, still more preferably 2 to 30 parts by mass, still more preferably 4 to 25 parts by mass, still more preferably 5 to 25 parts by mass, still more preferably 5 to 20 parts by mass, and still more preferably 5 to 15 parts by mass, relative to 100 parts by mass of polyimide resin (A). When the content of compound (B) is 0.1 part by mass or more relative to 100 parts by mass of polyimide resin (A), it is easy to impart improved flame retardancy and low dielectric properties, and when it is 30 parts by mass or less, good appearance and heat resistance can be maintained.
[0058] <Component (C): At Least One Member Selected from the Group Consisting of Metal Phosphinate (C1) and Fluororesin (C2)> The polyimide resin composition of the present invention may contain at least one member (C) selected from the group consisting of metal phosphinate (C1) and fluororesin (C2) for the purposes of improving the drip prevention effect and further enhancing flame retardancy.
[0059] (Metal Phosphinate (C1)) From the viewpoint of improving the drip prevention effect, the metal phosphinate (C1) is preferably a salt of at least one metal selected from the group consisting of Mg, Ca, Al, Zn, Ti, Sn, Zr, and Fe. The metal is more preferably at least one selected from the group consisting of Mg, Ca, and Al, and even more preferably Al.
[0060] From the viewpoint of improving the drip prevention effect and obtaining a good appearance, the metal phosphinate (C1) is preferably a compound represented by the following formula (i): (R' and R" each independently represent a hydrocarbon group having 1 to 12 carbon atoms, M represents a metal atom, and p represents the valence of the metal atom represented by M.)
[0061] In the formula (i), R' and R" each independently represent a hydrocarbon group having 1 to 12 carbon atoms. Examples of the hydrocarbon group include an alkyl group, a cycloalkyl group, an alkenyl group, an aryl group, and an aralkyl group. Examples of the alkyl group include an alkyl group having 1 to 12 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, a lauryl group, an isopropyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an isopentyl group, a neopentyl group, a 2-methylpentyl group, a 2-methylhexyl group, a 2-ethylpentyl group, a 3-ethylpentyl group, an isooctyl group, a 2-ethylhexyl group, a 3-ethylhexyl group, an isononyl group, a 2-ethyloctyl group, an isodecyl group, and an isododecyl group. Examples of the cycloalkyl group include cycloalkyl groups having 5 to 12 carbon atoms, such as cyclopentyl, cyclohexyl, cyclooctyl, and cyclodecanyl. Examples of the alkenyl group include alkenyl groups having 2 to 12 carbon atoms, such as vinyl, allyl, butenyl, 1-pentenyl, 2-pentenyl, 1-hexenyl, 2-hexenyl, 1-heptenyl, 2-heptenyl, 1-octenyl, 2-octenyl, nonenyl, decenyl, and dodecenyl. Examples of the aryl group include aryl groups having 6 to 12 carbon atoms, such as phenyl, toluyl, biphenyl, and naphthyl. Examples of the aralkyl group include aralkyl groups having 7 to 12 carbon atoms, such as benzyl, phenylethyl, and phenylpropyl. Among the above, R' and R" are preferably alkyl groups. The number of carbon atoms in the alkyl group is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 3. R' and R" may be the same or different, but are preferably the same.
[0062] In the formula (i), M is a metal atom and is preferably at least one selected from the group consisting of Mg, Ca, Al, Zn, Ti, Sn, Zr, and Fe. M is more preferably at least one selected from the group consisting of Mg, Ca, and Al, and even more preferably Al.
[0063] The metal phosphinate (C1) is preferably a compound (aluminum dialkylphosphinate) in which R' and R" are alkyl groups having 1 to 12 carbon atoms and M is Al in the formula (i). In this case, p in the formula (i) is 3. More preferred embodiments of R' and R" are the same as those described above. More preferably, the metal phosphinate (C1) is a compound (aluminum diethylphosphinate) in which R' and R" are ethyl groups and M is Al in the formula (i). Aluminum diethylphosphinate is a compound represented by the following structural formula (ii):
[0064] Since the metal phosphinate (C1) is a metal phosphinate, it is usually a solid compound, and from the viewpoint of dispersibility in the polyimide resin (A), it is preferably in powder form. Furthermore, from the viewpoint of improving the drip prevention effect and maintaining a good appearance, it is preferable that the particle size of the metal phosphinate (C1) is small. From the above viewpoints, the particle size (D50) of the metal phosphinate (C1) is preferably 40 μm or less, more preferably 30 μm or less, even more preferably 20 μm or less, still more preferably 10 μm or less, and even more preferably 5 μm or less. When the particle size (D50) of the metal phosphinate (C1) is 40 μm or less, particularly 10 μm or less, the resulting polyimide resin composition and molded article can have higher flame retardancy and good appearance. The particle size (D50) of the metal phosphinate (C1) is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more, from the viewpoints of handleability (flying-up tendency) and suppression of aggregation. The particle size (D50) of the metal phosphinate (C1) can be measured by a laser diffraction particle size distribution analyzer.
[0065] The phosphorus content of the metal phosphinate (C1) is preferably 0.5% by mass or more, more preferably 1% by mass or more, from the viewpoint of improving the drip prevention effect, and is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, from the viewpoint of exhibiting higher flame retardancy in addition to the drip prevention effect. Furthermore, from the viewpoint of improving dispersibility in the polyimide resin (A) and maintaining a good appearance, the phosphorus content of the metal phosphinate (C1) is preferably 40% by mass or less.
[0066] The metal phosphinate (C1) can be produced by a known method. Alternatively, a commercially available metal phosphinate flame retardant can be used as the metal phosphinate (C1). Examples of commercially available metal phosphinate flame retardants include "EXOLIT OP1230," "EXOLIT OP1240," "EXOLIT OP1400," "EXOLIT OP930," "EXOLIT OP935," "EXOLIT OP945," and "EXOLIT OP945TP," all manufactured by Clariant Chemicals K.K.
[0067] (Fluororesin (C2)) As fluororesin (C2), for example, polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), copolymer of tetrafluoroethylene and hexafluoropropylene (FEP), copolymer of tetrafluoroethylene and perfluoroalkyl vinyl ether (PFA), copolymer of tetrafluoroethylene and ethylene (ETFE), copolymer of tetrafluoroethylene and perfluoroalkoxyethylene etc. can be enumerated, and one or more of these can be used.Among them, from the viewpoint of improving drip prevention effect, maintaining good appearance and heat resistance, polytetrafluoroethylene is preferred.
[0068] The fluororesin (C2) used in the present invention is preferably in a powder form from the viewpoints of dispersibility in the polyimide resin (A) and ease of handling. When the fluororesin (C2) is in a powder form, its average particle size (D50) is not particularly limited, but from the viewpoints of dispersibility in the polyimide resin (A) and ease of handling, it is preferably 1 to 50 μm, more preferably 2 to 40 μm, even more preferably 3 to 30 μm, and still more preferably 5 to 20 μm. The average particle size (D50) can be measured using a laser diffraction light scattering particle size distribution analyzer.
[0069] Commercially available products can also be used as the fluororesin (C2). Among the commercially available fluororesins, examples of polytetrafluoroethylene include "KT-300M", "KT-400M", "KT-600M", "KTL-450A", "KTL-450", "KTL-610", "KTL-610A", "KTL-620", "KTL-20N", "KTL-10N", "KTL-10S", "KTL-9N", "KTL-9S", "KTL-8N", "KTL-4N", "KTL-2N", "KTL-1N", "KTL-8F", "KTL-8FH", and "KTL-500F" manufactured by Kitamura Co., Ltd.; Examples of such powders include 3M Dyneon PTFE micropowder "TF9201Z," "TF9205," and "TF9207" manufactured by Japan Co., Ltd., and "Polyflon MPA" series such as FA-500H and FA-5601 manufactured by Daikin Industries, Ltd., "Polyflon PTFE-M" series, "Polyflon PTFE-F" series, and "Polyflon PTFE Lubron" series.
[0070] One or more types of component (C) may be used, and a metal phosphinate (C1) and a fluororesin (C2) may be used in combination. From the viewpoints of improving the drip prevention effect, maintaining good appearance and heat resistance, and adhesion to metals such as copper and steel sheets, a metal phosphinate (C1) is preferred as component (C).
[0071] When component (C) is used, the content of component (C) in the polyimide resin composition is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, even more preferably 0.1 to 2 parts by mass, and even more preferably 0.2 to 2 parts by mass, per 100 parts by mass of polyimide resin (A). When the content of component (C) in the polyimide resin composition is 0.01 parts by mass or more per 100 parts by mass of polyimide resin (A), a drip prevention effect is easily imparted, and when it is 5 parts by mass or less, good appearance and heat resistance can be maintained. Furthermore, when component (C) is used, the mass ratio of component (B) to component (C) in the polyimide resin composition [(B) / (C)] is preferably 1.0 to 40, more preferably 5.0 to 30, and even more preferably 10 to 20, from the viewpoint of obtaining drip prevention effect, flame retardancy, good appearance, and heat resistance.
[0072] However, from the viewpoint of obtaining high flame retardancy, good appearance, and heat resistance even in a thin molded article having a thickness of 500 μm or less, and particularly from the viewpoint of reducing the burning time of the resulting polyimide resin composition and molded article, the content of component (C) in the polyimide resin composition is preferably low. From the viewpoint of prioritizing the reduction in the burning time of the polyimide resin composition and molded article, the content of component (C) in the polyimide resin composition can be more preferably 1.5 parts by mass or less, even more preferably 1 part by mass or less, even more preferably 0.5 parts by mass or less, and even more preferably 0.1 parts by mass or less, per 100 parts by mass of polyimide resin (A).
[0073] <Additives> The polyimide resin composition of the present invention can optionally contain additives other than component (C), such as fillers, reinforcing fibers, delustering agents, plasticizers, antistatic agents, coloring inhibitors, antigelling agents, colorants, sliding property improvers, antioxidants, conductive agents, and resin modifiers. Regarding the effects of various additives, for example, the addition of inorganic fillers such as mica or talc, particularly micro- to submicron-sized or nano-sized powders (solid particles), is preferred because it can impart the filler's low CTE (coefficient of linear expansion) effect while maintaining the appearance of the resulting molded product (particularly a film). Furthermore, the addition of hollow materials such as hollow silica, particularly micro- to submicron-sized or nano-sized hollow materials, is preferred because it can impart the filler's low dielectric property improvement effect while maintaining the appearance of the film. From the viewpoint of imparting a low CTE effect or a low dielectric property improvement effect while ensuring a good appearance, the particle diameter (D50) of the solid particles and hollow materials is preferably 40 μm or less, more preferably 30 μm or less, even more preferably 20 μm or less, even more preferably 10 μm or less, and even more preferably 5 μm or less. Furthermore, from the viewpoint of improving handleability (suppressing flying up) and suppressing aggregation, it is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. D50 can be measured using a laser diffraction particle size distribution analyzer. When the above additives are used, there are no particular restrictions on their amount. However, from the viewpoint of exhibiting the effects of the additives while maintaining the physical properties inherent in the polyimide resin (A), their amount in the polyimide resin composition is typically 50% by mass or less, preferably 0.0001 to 30% by mass, more preferably 0.001 to 15% by mass, and even more preferably 0.01 to 10% by mass.
[0074] The polyimide resin composition of the present invention may contain resins other than the polyimide resin (A) to the extent that their properties are not impaired. Such resins are preferably highly heat-resistant thermoplastic resins, such as polyamide resins, polyester resins, polyimide resins other than the polyimide resin (A), polycarbonate resins, polyetherimide resins, polyamideimide resins, polyphenylene etherimide resins, polyphenylene sulfide resins, polysulfone resins, polyethersulfone resins, polyarylate resins, liquid crystal polymers, polyetheretherketone resins, polyetherketone resins, polyetherketoneketone resins, polyetheretherketoneketone resins, polybenzimidazole resins, and the like. Among these, from the viewpoints of heat resistance, moldability, strength, and solvent resistance, one or more resins selected from the group consisting of polyetherimide resins, polyphenylene sulfide resins, and polyetheretherketone resins are preferred. Liquid crystal polymers are preferred from the viewpoint of low water absorption, and polyphenylene sulfide resins are preferred from the viewpoint of achieving high flame retardancy. When the polyimide resin (A) is used in combination with other resins, there are no particular limitations on the blending ratio, as long as the properties of the polyimide resin composition are not impaired.
[0075] However, from the viewpoint of obtaining the effects of the present invention, the total content of the polyimide resin (A) and the compound (B) in the polyimide resin composition of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, still more preferably 70% by mass or more, still more preferably 80% by mass or more, still more preferably 90% by mass or more, and still more preferably 95% by mass or more, but is 100% by mass or less.
[0076] The polyimide resin composition of the present invention can take any form, but is preferably in the form of pellets. Because the polyimide resin composition of the present invention and the polyimide resin (A) used therein are thermoplastic, for example, polyimide resin (A), compound (B), and various optional components, if necessary, can be dry-blended, or compound (B) and optional components can be separately fed into the extruder from a location separate from the feed of polyimide resin (A), followed by melt-kneading in the extruder to extrude strands, which can then be cut and pelletized. Furthermore, molded articles having desired shapes can be easily produced by introducing the pellets into various molding machines and thermoforming them using the methods described below. While bleed-out or thermal decomposition of the flame retardant, discoloration, whitening, and the like are typically prone to occur during the pellet production and thermoforming processes, the polyimide resin composition of the present invention is less susceptible to these problems and maintains a good appearance. From the perspective of pelletization, the polyimide resin composition of the present invention preferably does not contain a solvent. Specifically, the solvent content in the polyimide resin composition is preferably 5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.1% by mass or less.
[0077] [Molded Article] The present invention provides a molded article containing the polyimide resin composition. The shape of the molded article is not particularly limited. However, from the viewpoint of effectively demonstrating the effect of the present invention, namely, high flame retardancy and good appearance even in a thin molded article, a film-like shape having a thickness of 500 μm or less, preferably 200 μm or less, more preferably less than 100 μm, even more preferably 80 μm or less, and even more preferably 60 μm or less is preferred. The lower limit of the thickness is usually 5 μm or more, preferably 10 μm or more. In this specification, the "thickness of the film-like molded article" refers to the average thickness of the film-like molded article. Furthermore, film-like molded articles include resin film forms, resin layer forms constituting multilayer laminates, coating layer forms, and the like. However, the shape of the molded article of the present invention is not limited to a film-like shape having a thickness of 500 μm or less. For example, the effect of the present invention can be obtained even with a flat plate-like molded article having a thickness of more than 500 μm.
[0078] Because the polyimide resin composition of the present invention is thermoplastic, the molded article of the present invention can be easily produced by thermoforming. Examples of thermoforming methods include injection molding, extrusion molding, inflation molding, blow molding, hot press molding, vacuum molding, pressure molding, laser molding, welding, and adhesion. Any molding method involving a thermal melting step can be used. When producing a film-shaped molded article having a thickness of 500 μm or less, extrusion molding is preferred. Furthermore, when producing a plate-shaped molded article having a thickness of more than 500 μm, injection molding can be used. Thermoforming is preferred because it allows molding without setting the molding temperature to a high temperature, for example, exceeding 400°C. In particular, injection molding is preferred because it allows molding without setting the molding temperature and mold temperature during molding to a high temperature. For example, injection molding can be performed at a molding temperature of preferably 400°C or less, more preferably 360°C or less, and a mold temperature of preferably 260°C or less, more preferably 220°C or less. The polyimide resin (A) used in the present invention has a crystallization rate that is extremely fast compared with that of general crystalline resins, and therefore, crystallization can proceed even at a mold temperature that is significantly lower than the glass transition temperature (for example, Tg-50°C).
[0079] The method for producing a molded article preferably includes a step of thermoforming a polyimide resin composition at 290 to 360°C. While thermoforming at temperatures above 360°C up to 390°C is also possible, thermoforming at temperatures of 360°C or less is preferred from the viewpoint of suppressing deterioration of the polyimide resin (A) and other resin components. Specific procedures include, for example, the following method. First, the compound (B) and various optional components, if necessary, are added to the polyimide resin (A) and dry-blended the mixture. The mixture is then introduced into an extruder, melted preferably at 290 to 360°C, and melt-kneaded and extruded to produce pellets. Alternatively, the polyimide resin (A) may be introduced into an extruder, melted preferably at 290 to 360°C, and the compound (B) and various optional components, if necessary, are introduced thereto. The mixture is then melt-kneaded with the polyimide resin (A) and extruded to produce the pellets. The pellets may then be dried and then introduced into various molding machines, where they are thermoformed, preferably at 290 to 360°C, to produce a molded article having a desired shape. The polyimide resin composition of the present invention can be subjected to thermoforming such as extrusion molding at a relatively low temperature of 290 to 360°C, and therefore has excellent moldability, making it possible to easily produce molded articles having desired shapes. The temperature during thermoforming is preferably 310 to 360°C.
[0080] The polyimide resin composition and molded article of the present invention exhibit high flame retardancy even when formed into a thin molded article having a thickness of 500 μm or less. The flame retardancy can be evaluated by a method conforming to the UL94VTM test (thin material vertical combustion test; ASTM D4804), specifically, by the method described in the examples.
[0081] <Low Dielectric Properties> The polyimide resin composition and molded article of the present invention have low dielectric properties, and can achieve, for example, a dielectric constant of 3.0 or less and a dielectric loss tangent of 0.005 or less at a measurement frequency of 10 GHz. The dielectric constant is preferably 2.90 or less, more preferably 2.85 or less, and the dielectric loss tangent is preferably 0.004 or less, more preferably 0.003 or less. The dielectric constant and dielectric loss tangent can be measured specifically by the methods described in the examples.
[0082] <Uses> The polyimide resin composition of the present invention makes it possible to produce a molded article that has both high flame retardancy and good appearance even when the thickness is thin (for example, 500 μm or less). Furthermore, since the polyimide resin composition and a molded article containing the same have high heat resistance (high glass transition temperature) and low dielectric properties, they are suitable for applications requiring high flame retardancy, low dielectric constant, and low dielectric dissipation factor, such as 5G or sixth-generation mobile communication system (6G) related parts using frequency bands of 70 GHz to 300 GHz (smartphones, flexible printed circuit boards, metal foil laminates such as copper-clad laminates, antennas, antenna substrates, etc.), various antennas other than those mentioned above (microwave antennas, millimeter-wave antennas, waveguide slot antennas, horn antennas, lens antennas, printed antennas, triplate antennas, microstrip antennas, patch antennas, etc.), various antenna substrates (antenna substrates for 77 GHz automotive millimeter-wave radar, antenna substrates for terahertz wave radar, antenna substrates for aircraft radar, antenna substrates for caterpillar-type special vehicles, antenna substrates for WiGig, etc.), wire coating materials (low-dielectric wire coating materials, etc.), bonding sheets, insulating films, raw materials for carbon fiber reinforced plastics (CFRP), high-frequency circuit boards, and printed wiring Substrates, chip-on-film (COF) flexible substrates, multilayer laminates, LED-mounted substrates, industrial robot substrates, communication substrates for household robots, semiconductor element materials, wafers for high-frequency devices, Wi-Fi chips, wireless communication devices, transmission lines (coaxial lines, strip lines, microstrip lines, coplanar lines, parallel lines, etc.), bearing coatings, heat-insulating shafts, trays, various belts (seamless belts, etc.), heat-resistant low-dielectric tapes, heat-resistant low-dielectric tubes, various sensors (touch sensors, etc.), various radars (automotive radar, aerospace radar, etc.), radomes (radar domes), optical communication modules (TOSA / ROSA), 8k-TV cables, mobile terminals or digital home appliances (tablet terminals, notebook PCs, flat-screen TVs, retractable TVs, digital cameras, smart glasses, smart watches, etc.), base stations (macrocell base stations, small cell base stations, C-RAN base stations, etc.), drones (commercial drones, long-distance drones, etc.), surveillance cameras, indoor or outdoor servers, artificial satellites, space station communications equipment, etc.Among the above, the polyimide resin composition and molded article of the present invention are more preferably used for metal foil laminates, mainly copper-clad laminates. Metal foil laminates will be described below.
[0083] [Metal Foil Laminate] The present invention provides a metal foil laminate having a layer made of a molded article containing the polyimide resin composition and a layer made of metal foil. Examples of metal foil laminates include copper-clad laminates, which may include a layer made of a film-shaped molded article containing the polyimide resin composition (hereinafter simply referred to as a "resin film layer") and at least one copper foil layer. Examples include laminates in which copper foil is laminated on at least one side, preferably both sides, of a resin film containing the polyimide resin composition.
[0084] The resin film used in producing the copper-clad laminate can be produced by the same method as the method for producing the molded article. The thickness of the resin film and the resin film layer in the copper-clad laminate is preferably 5 to 500 μm, more preferably 10 to 300 μm, and even more preferably 12.5 to 200 μm, from the viewpoint of ensuring the strength of the copper-clad laminate and improving the adhesion between the resin film layer and the copper foil layer.
[0085] The copper foil used in the manufacture of copper-clad laminates is not particularly limited; commercially available rolled copper foils, electrolytic copper foils, etc. can be used, but rolled copper foils are preferred from the standpoint of flexibility. The thickness of the copper foil layer and the copper foil used to form it is preferably 2 to 50 μm, more preferably 3 to 30 μm, and even more preferably 5 to 20 μm, from the standpoint of ensuring sufficient conductivity and improving adhesion to the resin film layer. This thickness refers to the thickness per copper foil layer or per copper foil. The surface roughness of the copper foil used in the manufacture of copper-clad laminates is not particularly limited, but the surface roughness of the copper foil is directly related to the electrical properties of the laminate itself obtained after lamination with the resin film. Generally, a lower roughness results in a laminate with better dielectric properties. Therefore, the maximum height Rz of the copper foil surface is preferably in the range of 0.1 to 1 μm, more preferably 0.2 to 0.8 μm. The maximum height Rz of the copper foil surface can be measured, for example, using a surface roughness meter.
[0086] From the viewpoint of improving the strength and conductivity of the copper-clad laminate, the thickness of the copper-clad laminate is preferably 15 to 600 μm, more preferably 25 to 500 μm, and even more preferably 50 to 300 μm. The copper-clad laminate may have any layer other than the resin film layer and the copper foil layer, as long as the effects of the present invention are not impaired.
[0087] The method for producing a copper-clad laminate is not particularly limited, and known methods can be used. For example, a lamination method can be used in which the resin film and copper foil are superimposed and then laminated under heat and pressure. Since the resin film contains a thermoplastic polyimide resin (A), the surface can be heat-melted and pressed to laminate the copper foil. The apparatus used for producing a copper-clad laminate can be any apparatus capable of laminating a resin film and a copper foil under heat and pressure, such as a roll laminator, a flat laminator, a vacuum press, or a double belt press. Among these, from the viewpoint of productivity of the copper-clad laminate and obtaining a copper-clad laminate with good appearance, a vacuum press or a double belt press is preferably used. A double belt press is an apparatus equipped with a pair of endless belts arranged above and below, in which film-shaped materials (resin film and copper foil) forming each layer are continuously fed between the belts, and the materials are heated and pressurized through the endless belt by a heating and pressurizing mechanism to produce a laminate. Examples of double belt press devices include the device described in JP 2010-221694 A and a double belt press device manufactured by Dymco Corporation.
[0088] The heating temperature when producing a copper-clad laminate by the above method is not particularly limited as long as it is a temperature that can soften or melt the resin film, but from the viewpoint of reducing the burden on the equipment and production, it is preferably in the range of 250 to 400°C, more preferably 280 to 350°C. Furthermore, the pressure conditions when producing a copper-clad laminate are preferably 0.1 to 20 MPa, more preferably 0.15 to 15 MPa, and even more preferably 0.2 to 12 MPa, from the viewpoint of improving the adhesion between the resin film and the copper foil and reducing the burden on the equipment and production. Furthermore, from the viewpoint of improving production efficiency, the pressure application time is preferably in the range of 1 to 600 seconds, more preferably 5 to 400 seconds, and even more preferably 10 to 300 seconds.
[0089] Although the resin film is characterized by its ability to be heat-sealed, it is also possible to use an adhesive to bond the resin film and copper foil together in the production of copper-clad laminates. The adhesive can be selected from a variety of adhesives, including varnish-type adhesives, sheet-type adhesives, and powder-type adhesives. From the perspective of ensuring low dielectric properties, adhesives with low dielectric properties are also preferred. Examples of adhesives with low dielectric properties include the polyimide adhesive "PIAD" series manufactured by Arakawa Chemical Industries, Ltd.
[0090] The present invention will now be described in more detail with reference to examples, but the present invention is not limited thereto. In addition, various measurements and evaluations in each production example and example were carried out as follows.
[0091] <Infrared Spectroscopic Analysis (IR Measurement)> IR measurement of the polyimide resin was carried out using a JIR-WINSPEC50 manufactured by JEOL Ltd.
[0092] <Logarithmic Viscosity μ> After drying a polyimide resin at 190 to 200°C for 2 hours, 0.100 g of the polyimide resin was dissolved in 20 mL of concentrated sulfuric acid (96%, manufactured by Kanto Chemical Co., Inc.) to prepare a polyimide resin solution as a measurement sample, and measurement was carried out at 30°C using a Cannon-Fenske viscometer. Logarithmic viscosity μ was calculated using the following formula: μ = ln(ts / t 0 ) / C t 0 : Time during which concentrated sulfuric acid flows ts: Time during which polyimide resin solution flows C: 0.5 g / dL
[0093] <Melting Point, Glass Transition Temperature, Crystallization Temperature, and Crystallization Heat Amount> The melting point Tm, glass transition temperature Tg, crystallization temperature Tc, and crystallization heat amount ΔHm of the polyimide resin or polyimide resin composition were measured using a differential scanning calorimeter (DSC-6220 manufactured by SII Nanotechnology Inc.). Under a nitrogen atmosphere, the polyimide resin or polyimide resin composition was subjected to the following thermal history. The thermal history conditions were a first heating (heating rate of 10°C / min), followed by cooling (heating rate of 20°C / min), followed by a second heating (heating rate of 10°C / min). The melting point Tm was determined by reading the peak top value of the endothermic peak observed during the second heating. The glass transition temperature Tg was determined by reading the value observed during the second heating. The crystallization temperature Tc was determined by reading the peak top value of the exothermic peak observed during cooling. The crystallization heat value ΔHm (mJ / mg) was calculated from the area of the exothermic peak observed during cooling.
[0094] <Crystallization Half Time> The crystallization half time of a polyimide resin was measured using a differential scanning calorimeter (DSC-6220 manufactured by SII Nanotechnology, Inc.). The measurement conditions for a polyimide resin with a crystallization half time of 20 seconds or less were as follows: the polyimide resin was held at 420°C for 10 minutes in a nitrogen atmosphere until it was completely melted, and then rapidly cooled at a cooling rate of 70°C / minute. The crystallization half time was determined by calculating the time required from the appearance of the observed crystallization peak until it reached its peak top.
[0095] <Weight-average molecular weight> The weight-average molecular weight (Mw) of the polyimide resin was measured using a gel permeation chromatography (GPC) measuring device "Shodex GPC-101" manufactured by Showa Denko K.K. under the following conditions: Column: Shodex HFIP-806M Mobile phase solvent: HFIP containing 2 mM sodium trifluoroacetate Column temperature: 40°C Mobile phase flow rate: 1.0 mL / min Sample concentration: approximately 0.1% by mass Detector: IR detector Injection volume: 100 μm Calibration curve: standard PMMA
[0096] <Flame Retardancy> For Examples 1 to 8 and Comparative Examples 1 to 3, a molded article (film) measuring 200 mm x 50 mm x 0.05±0.01 mm thick was prepared using the polyimide resin or the polyimide resin composition obtained in each example by the method described below. The film was conditioned for 48 hours at 23±2°C and 50±5% RH, and then subjected to the UL94VTM test (thin material vertical flame test; ASTM D4804) under the following test environment: 25±10°C and 75% RH. Specifically, the film was rolled into a cylindrical shape, attached vertically to a clamp, and subjected to two 3-second indirect flame tests using a 20 mm flame using methane gas. Flame retardancy was evaluated based on the resulting combustion behavior. For Example 9, a molded article in the shape of a flat plate measuring 80 mm x 10 mm x 4 mm thick was prepared by the method described below, and the flat plate was then conditioned at 23±2°C and 50±5% RH. After conditioning for 48 hours at 25±10°C and 75% RH, the specimens were used in a UL94V test (20 mm vertical flame test; ASTM D3801). Specifically, the flat plates were attached vertically to a clamp and subjected to two 10-second indirect flame tests using a 20 mm flame of methane gas, and the flame retardancy was evaluated based on the combustion behavior.
[0097] (Maximum flaming combustion time after first and second flame contact) The maximum flaming combustion time (seconds) after the flame contact was performed twice is shown in Tables 2 and 5 (n=5). A shorter burning time indicates better flame retardancy.
[0098] (Total Flaming Burning Time) The total flaming burning time (seconds) (n=5) is shown in Tables 2 and 5. A shorter total time means better flame retardancy.
[0099] (Total Flame and Flameless Combustion Time After Second Flame Contact) The total flame and flameless combustion time after the second flame contact is shown in Tables 2 and 5 (n=5). A shorter total time indicates better flame retardancy.
[0100] (Whether or not flame reached the 125 mm mark) In Examples 1 to 8 and Comparative Examples 1 to 3, the presence or absence of flame reaching the 125 mm mark from the bottom end of the film was observed, and the number of times that flame reached the 125 mm mark out of five tests is shown in Table 3. A smaller number of times indicates better flame retardancy.
[0101] (Whether or not cotton caught fire) In the above combustion test, whether or not the cotton placed 300 mm below the film or plate caught fire due to the dropped matter was observed. The number of times that the cotton caught fire out of five tests is shown in Tables 3 and 5. When there was no ignition, it was recorded as "0 / 5". A lower number of ignitions means a higher drip prevention effect.
[0102] (Determination of Flame Retardancy) In Table 3, the rank of flame retardancy was determined based on the UL94VTM criteria. Flame retardancy equivalent to VTM-0 according to the UL94VTM criteria was indicated as "VTM-0," flame retardancy equivalent to VTM-1 was indicated as "VTM-1," and flame retardancy equivalent to VTM-2 was indicated as "VTM-2." Flame retardancy increases in the order of VTM-0 > 1 > 2, and if flame retardancy equivalent to VTM-2 was not achieved, it was designated "VTM non-compliant." In Table 5, the rank of flame retardancy was determined based on the UL94V criteria. Flame retardancy equivalent to V-0 according to the UL94V criteria was designated as "V-0," flame retardancy equivalent to V-1 was designated as "V-1," and flame retardancy equivalent to V-2 was designated as "V-2." Flame retardancy is ranked in order of V-0>1>2, and if the flame retardancy does not reach the level of V-2, it is rated as "V not compliant."
[0103] <Dielectric Constant and Dielectric Loss Tangent> The polyimide resin or the polyimide resin composition obtained in each example was extrusion-molded by the method described below to produce a film-like molded article, which was then cut to obtain an evaluation film measuring 62 mm x 75 mm x 0.05±0.01 mm thick. The film was dried in a hot air dryer at 100°C for 24 hours and then conditioned at 23±2°C and 50±5% RH for 48 hours. It was then immediately used for measurement. The dielectric constant and dielectric loss tangent were measured using a Keysight Technologies, Inc. "P5008A Keysight Streamline USB Vector Network Analyzer, 53 GHz" in accordance with IEC 62631-2-1 at 23°C, 50% RH, and a measurement frequency of 10 GHz. The results are shown in Table 4. The measured values were averaged over three measurements.
[0104] <Appearance> Using the polyimide resin or the polyimide resin composition obtained in each example, a molded article measuring 200 mm x 50 mm x 0.05±0.01 mm thick was prepared by the method described below, and the appearance was visually observed and evaluated according to the following criteria, as shown in Table 4. A: The film surface was smooth and had a good appearance. B: Fine irregularities or wrinkles were observed on the film surface. C: The film was curved or had uneven thickness.
[0105] <Strand extrudability> The strand extrudability of the polyimide resin or polyimide resin composition was evaluated according to the following criteria, and is shown in Table 4. AA: Continuous extrusion was possible while maintaining a constant strand diameter and without tearing. In addition, it took 3 seconds or more for the strand to become opaque after extrusion. A: Continuous extrusion was possible while maintaining a constant strand diameter and without tearing. In addition, the strand became opaque within 3 seconds after extrusion. B: Pulsation of the strand was observed and the diameter became unstable, or weak smoke was observed, but continuous extrusion was possible without tearing. C: Strand tearing, strong smoke, or vent-up occurred, making continuous extrusion difficult.
[0106] Production Example 1 (Production of Polyimide Resin 1) 500 g of 2-(2-methoxyethoxy)ethanol (manufactured by Nippon Nyukazai Co., Ltd.) and 218.12 g (1.00 mol) of pyromellitic dianhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were introduced into a 2 L separable flask equipped with a Dean-Stark apparatus, a Liebig condenser, a thermocouple, and four paddle blades. After nitrogen flow, the mixture was stirred at 150 rpm to obtain a uniform suspension. Meanwhile, using a 500 mL beaker, 49.79 g (0.35 mol) of 1,3-bis(aminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd., cis / trans ratio = 7 / 3) and 93.77 g (0.65 mol) of 1,8-octamethylenediamine (manufactured by Kanto Chemical Co., Ltd.) were dissolved in 250 g of 2-(2-methoxyethoxy)ethanol to prepare a mixed diamine solution. This mixed diamine solution was gradually added using a plunger pump. Although heat was generated during the dropwise addition, the internal temperature was adjusted to remain within the range of 40 to 80°C. During the dropwise addition of the mixed diamine solution, nitrogen flow was maintained throughout, and the stirring impeller rotation speed was set to 250 rpm. After the dropwise addition was completed, 130 g of 2-(2-methoxyethoxy)ethanol and 1.284 g (0.0100 mol) of n-octylamine (Kanto Chemical Co., Inc.), an end-capping agent, were added and further stirred. At this stage, a pale yellow polyamic acid solution was obtained. Next, the stirring speed was increased to 200 rpm, and the polyamic acid solution in the 2-L separable flask was heated to 190°C. During the temperature increase, precipitation of polyimide resin powder and dehydration associated with imidization were observed between 120 and 140°C. After holding at 190°C for 30 minutes, the solution was allowed to cool to room temperature and then filtered. The obtained polyimide resin powder was washed with 300 g of 2-(2-methoxyethoxy)ethanol and 300 g of methanol, filtered, and then dried in a dryer at 180°C for 10 hours to obtain 317 g of powder of polyimide resin 1. When the IR spectrum of polyimide resin 1 was measured, it was found that ν(C═O) -1 The inherent viscosity was 1.30 dL / g, Tm was 323°C, Tg was 184°C, Tc was 266°C, the exotherm of crystallization was 21.0 mJ / mg, the half-crystallization time was 20 seconds or less, and Mw was 55,000.
[0107] The composition and evaluation results of the polyimide resin in Production Example 1 are shown in Table 1. The mole percentages of the tetracarboxylic acid component and the diamine component in Table 1 are values calculated from the amounts of each component charged when the polyimide resin was produced.
[0108]
[0109] The abbreviations in Table 1 are as follows: PMDA: pyromellitic dianhydride 1,3-BAC: 1,3-bis(aminomethyl)cyclohexane OMDA: 1,8-octamethylenediamine
[0110] Examples 1 to 8 and Comparative Examples 1 to 3 (Production and Evaluation of Polyimide Resin Compositions and Molded Articles (Resin Films)) Polyimide resin 1 obtained in Production Example 1, the compounds shown in Tables 2 to 4, and other components were thoroughly mixed by dry blending. The resulting mixed powder was extruded into strands with a diameter of 2 to 3 mm using a co-rotating twin-screw kneading extruder ("HK-25D-41D" manufactured by Parker Corporation) at a barrel temperature of 350°C and a screw rotation speed of 120 rpm. The strand extrudability was evaluated according to the above criteria. The strands extruded from the extruder were air-cooled and then pelletized using a pelletizer ("Fan Cutter FC-Mini-4 / N" manufactured by Hoshi Plastics Co., Ltd.). The resulting pellets (polyimide resin composition) were dried at 190°C for 10 hours and then used for extrusion molding. The pellets were placed in a Φ20 mm single-screw extruder equipped with a 150 mm wide T-die, melt-kneaded at a resin temperature of 340 to 360°C, and continuously extruded from the T-die of the single-screw extruder. The mixture was then cooled with a metal cooling roll at 140°C to obtain a resin film with a thickness of 0.05±0.01 mm. The temperature of the Φ20 mm single-screw extruder was adjusted to 340 to 355°C, and the temperature of the T-die was adjusted to 350°C. The resulting pellets (polyimide resin composition) or the prepared resin film were evaluated using the methods described above. The results are shown in Tables 2 to 4.
[0111]
[0112]
[0113]
[0114] Details of each component shown in Tables 2 to 4 are as follows: <Polyimide Resin (A)> (A) Polyimide Resin 1 obtained in Production Example 1, Mw: 55,000 <Compound (B)> (B) SR-3000: Compound represented by the following structural formula (B3), manufactured by Daihachi Chemical Industry Co., Ltd. <Component (C)> (C1) EXOLIT OP945: a phosphinic acid metal salt-based flame retardant (aluminum diethylphosphinate) represented by the following structural formula (ii), manufactured by Clariant Chemicals K.K., particle size (D50): 1.3 μm, phosphorus content: 23 mass% (C2) KTL-450: Polytetrafluoroethylene (PTFE), manufactured by Kitamura Co., Ltd.
[0115] Tables 2 and 3 show the evaluation results of flame retardancy. Table 2 shows that the molded articles containing the polyimide resin composition of the present invention have a shorter burning time and better flame retardancy than the molded articles of the comparative examples. Table 3 also shows that, particularly in Examples 2 to 8, the molded articles were very thin, with a thickness of 0.05 mm ± 0.01 mm, but achieved flame retardancy equivalent to VTM-0 according to the UL94VTM criteria.
[0116] Table 4 shows the evaluation results of the thermal properties, dielectric properties, appearance, and strand extrudability. As can be seen from Table 4, all of the molded articles containing the polyimide resin composition of the present invention have good appearance. With regard to strand extrudability, the polyimide resin compositions of Examples 1 to 5, which contained only compound (B) as the flame retardant, showed particularly good results. This is thought to be because, unlike other flame retardants (component (C1)), compound (B) does not act as a crystal nucleating agent and has the effect of delaying the crystallization of the polyimide resin (A). Furthermore, the molded articles containing the polyimide resin composition of the present invention had a dielectric constant of 3 or less and a dielectric dissipation factor of 0.005 or less, which are extremely low for resin molded articles.
[0117] Example 9 (Production and Evaluation of Polyimide Resin Composition and Molded Article (4 mm Thick Plate)) Pellets of a polyimide resin composition were prepared in the same manner as in Example 2. The pellets were dried at 190°C for 10 hours and then used for injection molding. Using an injection molding machine ("ROBOSHOT α-S30iA" manufactured by Fanuc Corporation), injection molding was performed at a barrel temperature of 350°C, a mold temperature of 200°C, and a molding cycle of 50 seconds to prepare a 1A type test piece as specified in JIS K7161-2:2014. The obtained 1A type test piece was processed into a plate measuring 80 mm x 10 mm x 4 mm thick, and then flame retardancy was evaluated using the method described above. The results are shown in Table 5. The evaluation results other than flame retardancy were the same as in Example 2.
[0118]
[0119] As can be seen from Table 5, the molded article containing the polyimide resin composition of the present invention exhibited good flame retardancy even when the thickness exceeded 500 μm.
[0120] The polyimide resin composition of the present invention can produce a molded article that has both high flame retardancy and good appearance even when the molded article has a thin thickness (for example, 500 μm or less). Furthermore, the polyimide resin composition and a molded article containing the same have high heat resistance (high glass transition temperature) and low dielectric properties. Therefore, the polyimide resin composition and molded article of the present invention can be used in applications requiring high flame retardancy, a low dielectric constant, and a low dielectric dissipation factor, such as 5G or sixth-generation mobile communication system (6G) related components using a frequency band of 70 GHz to 300 GHz, various antennas, various antenna substrates, wire coating materials, bonding sheets, insulating films, raw materials for carbon fiber reinforced plastics (CFRP), high-frequency circuit boards, printed wiring boards, chip-on-film (COF) flexible substrates, multilayer laminates, LED-mounted substrates, industrial robot substrates, communication substrates for household robots, semiconductor element materials, wafers for high-frequency devices, Wi-Fi chips, wireless communication devices, transmission lines, bearing coatings, heat-insulating shafts, trays, various belts, heat-resistant low-dielectric tapes, heat-resistant low-dielectric tubes, various sensors, various radars, radomes (radar domes), optical communication modules (TOSA / ROSA), 8k-TV cable mobile terminals or digital home appliances, base stations, drones, surveillance cameras, indoor or outdoor servers, artificial satellites, and communication equipment for space stations.
Claims
1. The polyimide resin composition comprises: polyimide resin (A) containing a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), in which the content of the repeating structural unit of the formula (1) relative to the total of the repeating structural units of the formula (1) and the repeating structural units of the formula (2) is 20 to 70 mol %; and compound (B) represented by the following formula (5). 【Chemistry 1】 (R 1 R is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. 2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. 1 and X 2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. 【Chemistry 2】 (R 51 is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. 52 ~R 53 , and R 61 ~R 66 are each independently an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 51 is an integer from 0 to 6; p 52 and p 53 are each independently an integer of 0 to 4; 63 and p 66 Each independently represents an integer of 0 to 3. 51 ~p 53 , p 63 , or p 66 When R is 2 or more, multiple R 51 ~R 53 , R 63 Or R 66 may be the same or different, and n is an integer from 1 to 10.
2. 2. The polyimide resin composition according to claim 1, wherein the content of the compound (B) in the polyimide resin composition is 0.1 to 30 parts by mass per 100 parts by mass of the polyimide resin (A).
3. 2. The polyimide resin composition according to claim 1, wherein the compound (B) is at least one selected from the group consisting of compounds represented by the following structural formulas (B1) to (B3): 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】
4. A molded article comprising the polyimide resin composition according to any one of claims 1 to 3.
5. The molded article according to claim 4, which has a film shape with a thickness of 500 μm or less.
6. A metal foil laminate comprising a layer made of the molded article according to claim 4 and a layer made of metal foil.