Palladium catalyst liquid
Patent Information
- Application Number
- JP2024520264
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-24
- Filing Date
- 2023-02-24
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2043-02-24
AI Technical Summary
Existing palladium catalyst solutions using inorganic acids for electroless nickel plating on copper circuits suffer from copper corrosion, complex rinsing processes, insufficient nickel plating precipitation, and poor patternability due to nickel plating spread.
A palladium catalyst liquid comprising an organic acid, a chloride, and a palladium salt, specifically containing organic sulfonic acids, sodium chloride, and palladium sulfate, which suppresses copper corrosion and enhances nickel plating deposition and patternability.
The solution effectively prevents copper corrosion, improves nickel plating precipitation, and restricts nickel plating spread, resulting in excellent patternability on copper surfaces.
Abstract
Description
Palladium catalyst solution
[0001] The present invention relates to a palladium catalyst liquid.
[0002] In the electronics-related field, such as printed wiring boards, semiconductor packages, and electronic components, electroless nickel plating is performed on copper circuits.
[0003] When electroless nickel plating is performed on a copper circuit, an inorganic acid such as hydrochloric acid or sulfuric acid is used as a palladium catalyst solution.
[0004] However, the above-mentioned palladium catalyst solution using an acid has the problem of corroding copper.
[0005] It has been disclosed that a substrate containing a copper surface is brought into contact with a palladium ion-containing composition, and then contacted with a composition containing an organic acid such as an organic aminocarboxylic acid (see Patent Document 1).
[0006] However, with the composition disclosed in Patent Document 1, after the step of contacting with the palladium ion-containing composition, it is necessary to rinse with the composition in order to remove the palladium ions and their precipitates, which makes the process complicated.
[0007] Furthermore, the composition disclosed in Patent Document 1 has the problem that it does not sufficiently inhibit copper corrosion.
[0008] Furthermore, the composition disclosed in Patent Document 1 has problems in that the deposition properties of the nickel plating are insufficient in the subsequent step, and the nickel plating tends to spread, resulting in poor patterning.
[0009] Therefore, there is a need for the development of a palladium catalyst solution that can inhibit copper corrosion, impart excellent nickel plating deposition properties to the copper surface, and inhibit the spreading of nickel plating on copper to impart excellent patterning properties.
[0010] Patent No. 5570585
[0011] The present invention has been made in view of the above problems, and aims to provide a palladium catalyst solution that inhibits copper corrosion, can impart excellent nickel plating deposition properties to the copper surface, and can inhibit the spreading of nickel plating on the copper to impart excellent patterning properties.
[0012] As a result of extensive research into achieving the above object, the present inventors have found that the above object can be achieved by a palladium catalyst solution containing (A) an organic acid, (B) a chloride, and (C) a palladium salt, and have thus completed the present invention.
[0013] That is, the present invention relates to the following palladium catalyst solutions: 1. A palladium catalyst solution containing (A) an organic acid, (B) a chloride, and (C) a palladium salt. 2. The palladium catalyst solution according to Item 1, wherein the organic acid is at least one selected from the group consisting of organic sulfonic acids, organic carboxylic acids, and organic phosphonic acids. 3. The palladium catalyst solution according to Item 1 or 2, wherein the organic acid content is 10 to 250 g / L. 4. The palladium catalyst solution according to Item 1 or 2, wherein the chloride is at least one selected from the group consisting of sodium chloride, potassium chloride, ammonium chloride, and calcium chloride. 5. The palladium catalyst solution according to Item 1 or 2, wherein the chloride content is 3 to 50 g / L. 6. 6. The palladium catalyst solution according to Item 1 or 2, wherein the palladium salt is at least one selected from the group consisting of palladium sulfate, palladium chloride, palladium oxide, palladium iodide, palladium bromide, palladium nitrate, palladium acetate, tetraamminepalladium chloride, dinitrodiamminepalladium, and dichlorodiethylenediaminepalladium. 7. The palladium catalyst solution according to Item 1 or 2, wherein the content of the palladium salt is 1 to 100 mg / L.
[0014] The palladium catalyst solution of the present invention inhibits copper corrosion, can impart excellent nickel plating deposition properties to the copper surface, and can inhibit the spreading of nickel plating on the copper, thereby imparting excellent patternability.
[0015] The present invention will be described in detail below.
[0016] 1. Palladium Catalyst Solution The palladium catalyst solution of the present invention is characterized by containing (A) an organic acid, (B) a chloride, and (C) a palladium salt. Hereinafter, these components will also be referred to as "component (A)," "component (B)," and "component (C)," respectively. By containing the components (A) and (C), the palladium catalyst solution of the present invention can impart excellent nickel plating deposition properties to the copper surface while suppressing corrosion of the copper surface. Furthermore, by containing the component (B), the palladium catalyst solution of the present invention can impart excellent patternability by suppressing the spreading of nickel plating on the copper while suppressing corrosion of the copper surface. While the mechanism by which the inclusion of component (C) exerts the above-mentioned effects is unclear, it is believed that the inclusion of component (C) in the palladium catalyst solution of the present invention improves the selective deposition of palladium on the copper surface and suppresses localized corrosion of the copper surface. That is, the palladium catalyst solution of the present invention, which contains the above-mentioned components (A) to (C), inhibits copper corrosion, can impart excellent nickel plating deposition properties to the copper surface, and can also inhibit the spreading of the nickel plating on the copper, thereby imparting excellent patternability.
[0017] Component (A) The component (A) is an organic acid. By including the component (A) in the palladium catalyst solution of the present invention, it is possible to impart excellent nickel plating deposition properties to the copper surface while inhibiting corrosion of the copper surface.
[0018] The organic acid is not particularly limited, and examples thereof include organic sulfonic acids, organic carboxylic acids, organic phosphonic acids, etc. Among these, organic sulfonic acids are preferred because they are more effective in inhibiting corrosion of copper surfaces and further improve the deposition properties of nickel plating on copper surfaces.
[0019] Examples of organic sulfonic acids include aliphatic sulfonic acids having 1 to 5 carbon atoms, such as methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, and pentanesulfonic acid, and aromatic sulfonic acids, such as toluenesulfonic acid, pyridinesulfonic acid, and phenolsulfonic acid. Among these, methanesulfonic acid is preferred because it is more effective in inhibiting corrosion of copper surfaces and further improves the deposition properties of nickel plating on copper surfaces.
[0020] Examples of organic carboxylic acids include aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, sebacic acid, maleic acid, and fumaric acid, and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid. Among these, succinic acid is preferred because it is more effective in inhibiting corrosion of copper surfaces and further improves the deposition properties of nickel plating on copper surfaces.
[0021] Examples of organic phosphonic acids include methyldiphosphonic acid, aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP), nitrilotrismethylenephosphonic acid (NTMP), ethylenediaminetetra(methylenephosphonic acid), etc. Among these, 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP) is preferred in that it is more effective in inhibiting corrosion of copper surfaces and further improves the deposition properties of nickel plating on copper surfaces.
[0022] The organic acids may be used alone or in combination of two or more.
[0023] The concentration of the organic acid in the palladium catalyst solution is not particularly limited, and is preferably 10 to 250 g / L, more preferably 50 to 200 g / L, and even more preferably 80 to 150 g / L. Note that, for example, when 70% methanesulfonic acid is used, the concentration of the organic acid is the amount of methanesulfonic acid in the 70% methanesulfonic acid; for example, when 70% methanesulfonic acid is used at a concentration of 150 g / L, the concentration of methanesulfonic acid is 105 g / L.
[0024] Component (B) The component (B) is a chloride. By including the component (B) in the palladium catalyst solution of the present invention, corrosion of the copper surface can be suppressed, while the spreading of nickel plating on the copper can be suppressed, thereby providing better patternability.
[0025] The chloride is not particularly limited, and examples thereof include sodium chloride, potassium chloride, ammonium chloride, calcium chloride, etc. Among these, sodium chloride is preferred in that it can inhibit the corrosion of the copper surface while suppressing the spread of nickel plating on the copper, thereby imparting better patternability. Furthermore, as the chloride, it is preferable to use a chloride other than hydrochloric acid in that it further inhibits copper corrosion, and it is preferable that the palladium catalyst solution of the present invention does not contain hydrochloric acid.
[0026] The chlorides may be used alone or in combination of two or more.
[0027] The chloride concentration in the palladium catalyst solution is not particularly limited, but is preferably 3 to 50 g / L, more preferably 5 to 30 g / L, and even more preferably 7 to 20 g / L.
[0028] Component (C) The component (C) is a palladium salt. By including the component (C) in the palladium catalyst solution of the present invention, it is possible to impart excellent nickel plating deposition properties to the copper surface while inhibiting corrosion of the copper surface.
[0029] The palladium salt is not particularly limited, and examples thereof include palladium sulfate, palladium chloride, palladium oxide, palladium iodide, palladium bromide, palladium nitrate, palladium acetate, tetraamminepalladium chloride, dinitrodiamminepalladium, dichlorodiethylenediaminepalladium, etc. Among these, palladium sulfate is preferred in that it is more effective in inhibiting corrosion of copper surfaces and further improves the deposition properties of nickel plating on copper surfaces.
[0030] The palladium salts may be used alone or in combination of two or more.
[0031] The concentration of the palladium salt in the palladium catalyst solution is not particularly limited, and is preferably 1 to 100 mg / L, more preferably 20 to 80 mg / L, even more preferably 30 to 70 mg / L, and particularly preferably 40 to 60 mg / L.
[0032] Other Components The palladium catalyst solution of the present invention may contain other components in addition to the above-mentioned components (A), (B), and (C). Examples of other components include a stabilizer.
[0033] The palladium catalyst solution of the present invention preferably contains the above-mentioned components (A), (B), and (C), as well as other components that may be included as needed, in the solvent in the amounts described above. As such a solvent, water is preferred in terms of its environmental friendliness and safety.
[0034] The content of the solvent in the palladium catalyst solution is not particularly limited, and may be the remainder after adding the above-mentioned components (A), (B), and (C), as well as other components that may be included as necessary.
[0035] The pH of the palladium catalyst solution of the present invention is not particularly limited, and is preferably not more than 5, more preferably not more than 3, even more preferably not more than 1, and particularly preferably not more than 0.5. When the upper limit of the pH is within the above range, it is possible to impart superior nickel plating deposition properties to the copper surface, and also to suppress the spreading of the nickel plating on the copper, thereby imparting superior patternability.
[0036] 2. Method for Producing Palladium Catalyst Solution The method for producing the palladium catalyst solution of the present invention is not particularly limited, and the solution can be produced by a production method including a step of adding the above-described components (A), (B), and (C), as well as other components that may be included as needed, to a solvent.
[0037] In the above step, the palladium catalyst solution can be prepared by sequentially adding the components (A), (B), and (C), as well as other components that may be included as needed, to a solvent, and the order in which the components are added is not particularly limited.
[0038] In the above step, the conditions for preparing the palladium catalyst solution are not particularly limited, and the palladium catalyst solution may be prepared by stirring and mixing in a mixing vessel or the like at 10 to 40° C. for about 1 to 10 minutes.
[0039] 3. Palladium Catalyst Application Method The method for applying a palladium catalyst to a copper surface using the palladium catalyst solution of the present invention is not particularly limited, and examples thereof include a palladium catalyst application method comprising a step of immersing a copper plate in the palladium catalyst solution.
[0040] The temperature of the palladium catalyst solution in the above step is not particularly limited, but is preferably 20 to 40°C, more preferably 25 to 35°C. When the lower limit of the temperature of the palladium catalyst solution is within the above range, the deposition properties of nickel plating on the copper surface are further improved, and spreading of the nickel plating is suppressed, resulting in better patterning. When the upper limit of the temperature of the palladium catalyst solution is within the above range, corrosion of copper is further suppressed.
[0041] The immersion time in the above step is not particularly limited, but is preferably 0.5 to 5 minutes, more preferably 1 to 3 minutes. When the lower limit of the immersion time is within the above range, the deposition of nickel plating on the copper surface is further improved, and the spreading of the nickel plating is suppressed, resulting in better patternability. When the upper limit of the immersion time is within the above range, copper corrosion is further suppressed.
[0042] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0043] The raw materials used in the examples and comparative examples are as follows:
[0044] (A) Organic acid: 70% methanesulfonic acid (B) Chloride: sodium chloride (C) Palladium salt: palladium sulfate
[0045] Examples and Comparative Examples The above-mentioned raw materials were added to water as a solvent in the amounts shown in Table 1, and the mixture was stirred in a mixing vessel to produce palladium catalyst solutions of Examples and Comparative Examples.
[0046] The resulting palladium catalyst solution was subjected to the following tests to evaluate its properties.
[0047] (Electroless Nickel Plating Solution) As the electroless nickel plating solution, ICP Nicoron FPF (trade name) manufactured by Okuno Chemical Industries Co., Ltd. was prepared.
[0048] (Plating Deposition Properties) A BGA (Ball Grid Array) resin substrate having overresist-type micro copper pads (φ60-130 μm, 30 pads) on a resin base material was used as the material for electroless plating. The material for electroless plating was subjected to acid degreasing and soft etching. Next, a catalyst application treatment was carried out using the palladium catalyst solution of the Examples and Comparative Examples. Next, electroless nickel plating was carried out at 84°C for 20 minutes using the electroless nickel plating solution prepared as described above, and the result was evaluated according to the following evaluation criteria. Note that a rating of ◯ indicates that the product can be used in actual use without any problems. ◯: No undeposited material was observed. △: A slight amount of undeposited material was observed. ×: A large amount of undeposited material was observed.
[0049] (Patternability) A BGA resin substrate with fine wiring (L / S = 50 / 50 μm) on a resin base material was prepared as the material to be electroless plated. The material to be electroless plated was subjected to acid degreasing and soft etching. A catalyst application treatment was then performed using the palladium catalyst solution of the Examples and Comparative Examples. Next, electroless nickel plating was performed on a wiring pattern with L / S = 50 / 50 μm at 84°C for 20 minutes using the electroless nickel plating solution prepared as described above. After nickel plating, the L / S = 50 / 50 μm wiring pattern was observed under a microscope (1000x magnification) to check for the presence or absence of electroless nickel plating spreading outside the wiring pattern, and evaluated according to the following evaluation criteria. A rating of ◯ indicates that the product can be used without any problems in actual use. ◯: No plating spreading was observed. △: Slight plating spreading was observed. ×: Extensive plating spreading occurred.
[0050] (Localized Copper Corrosion) A BGA resin substrate having an overresist-type copper pad on a resin base material was prepared as the material to be electroless plated. The material to be electroless plated was subjected to acid degreasing and soft etching. Next, a catalyst application treatment was performed using the palladium catalyst solution of the example and comparative example. Next, electroless nickel plating was performed at 84°C for 20 minutes using the electroless nickel plating solution prepared as described above. The cross section of the Cu-Ni interface of the film after nickel plating was observed (10,000x magnification) using an FIB device to observe the presence or absence of localized corrosion in the Cu layer, and evaluated according to the following evaluation criteria. Note that a rating of ◯ indicates that the product can be used without any problems in actual use. ◯: No localized corrosion at all △: Slight localized corrosion was observed ×: Numerous localized corrosion occurred
[0051] The results are shown in Table 1.
[0052]
Claims
1. (A) an organic acid, (B) a chloride, and (C) a palladium salt; The content of the organic acid is 80 to 250 g / L. A palladium catalyst solution comprising:
2. 2. The palladium catalyst solution according to claim 1, wherein the organic acid is at least one selected from the group consisting of an organic sulfonic acid, an organic carboxylic acid, and an organic phosphonic acid.
3. 3. The palladium catalyst solution according to claim 1, wherein the chloride is at least one selected from the group consisting of sodium chloride, potassium chloride, ammonium chloride, and calcium chloride.
4. 3. The palladium catalyst solution according to claim 1, wherein the chloride content is 3 to 50 g / L.
5. 3. The palladium catalyst solution according to claim 1, wherein the palladium salt is at least one selected from the group consisting of palladium sulfate, palladium chloride, palladium oxide, palladium iodide, palladium bromide, palladium nitrate, palladium acetate, tetraamminepalladium chloride, dinitrodiamminepalladium, and dichlorodiethylenediaminepalladium.
6. 3. The palladium catalyst solution according to claim 1, wherein the content of the palladium salt is 1 to 100 mg / L.