Water-based primer

By forming chemical bonds with substrates using chemical radiation and removing residual liquid without drying, the method addresses inefficiencies in UV-curing water-based primers, enhancing adhesion and reducing energy consumption and costs.

KR1020260162301APending Publication Date: 2026-11-10메르케네 코팅스 아베
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267030280
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-15
Filing Date
2025-03-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing UV-curing water-based primers for non-absorbent substrates require an energy-consuming drying step to evaporate water before UV exposure, which increases costs and is inefficient for applying small amounts per unit area.

Method used

A method involving applying an aqueous liquid that forms a chemical bond with the substrate through chemical radiation irradiation, allowing the liquid to remain on the substrate during irradiation, followed by removing any remaining liquid and applying a subsequent coating without drying.

Benefits of technology

Eliminates the need for a drying step, reduces energy consumption, and enables the application of very small amounts of material, while maintaining mechanical properties and adhesion, thus reducing costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A method for coating a non-absorbent substrate of poly(ethylene terephthalate), poly(1-methylethylene), poly(1-chloroethylene), or polyethylene is disclosed. A layer of an aqueous liquid in the form of a solution or emulsion of a compound having the ability to form a chemical bond to the substrate by chemical radiation irradiation is applied. Next, while the substrate is still wet, the substrate is irradiated to initiate a reaction that forms a covalent bond. Next, the remaining aqueous liquid is removed, and a subsequent coating is applied and cured.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for coating a substrate in which an aqueous liquid remains on the substrate when the substrate is irradiated with actinic radiation. Background Technology

[0002] WO 2019 / 185302 discloses a method for coating a substrate comprising at least one secondary amine by contacting the substrate surface with a compound comprising at least one carbon-carbon double bond, wherein an electron withdrawing group is located on at least one side of the carbon-carbon double bond, so that a complex is formed between the nitrogen in the secondary amine and the carbon-carbon double bond. Subsequently, a reaction is initiated to form a covalent bond by the reaction between the nitrogen in the secondary amine and the carbon-carbon double bond by irradiating at least a portion of the formed complex with chemical radiation, wherein the wavelength of the chemical radiation is adapted to be absorbed by the complex.

[0003] WO 2021 / 148588 discloses a method for coating a substrate comprising the step of applying a first mixture, wherein the first mixture reacts to form a covalent bond on the surface of the substrate, and the unreacted portion of the first mixture undergoes diffusion mixing with a second layer applied on top of the first mixture. This prevents the formation of a brittle layer that, otherwise, could reduce adhesion. Mechanical properties, including scratch resistance as well as adhesion, are improved.

[0004] For all UV-curing water-based primers in the prior art, particularly for non-absorbent substrates where water is not absorbed, it has been a common practice to evaporate the water before UV exposure. The main reason for evaporating water in UV-curing formulations is that a uniform liquid film is formed after the water evaporates, and this film subsequently cures to form a solid layer. The presence of water creates voids within the film, which significantly degrades mechanical properties. To address this, it is a practice to evaporate water from water-based formulations. This is described, for example, in Reinhold Schwalm’s UV Coatings: Basics, Recent Developments and New Applications, Elsevier, December 21, 2006, ISBN 978-0444529794, specifically on page 211.

[0005] Although the latest technology operates smoothly, there is still room for improvement regarding the application of small amounts per unit area, such as an amount corresponding to a coating layer of 1, 2, or 3 µm or similar at a typical concentration of primer solution. In addition, there is also room for improvement regarding the energy consumption of the coating process.

[0006] The object of the present invention is to provide a method for coating a substrate that mitigates at least some of the disadvantages of the prior art.

[0007] In a first embodiment, a method for coating a substrate is provided, and the method

[0008] a) a step of providing a substrate, wherein the substrate comprises at least one polymer selected from the group consisting of poly(ethylene terephthalate), poly(1-methylethylene), poly(1-chloroethylene) and polyethylene, and the substrate is non-absorbent to water.

[0009] b) a step of applying a layer of an aqueous liquid onto a substrate, wherein the aqueous liquid comprises at least one compound having the ability to form a chemical bond to the substrate by chemical radiation irradiation,

[0010] c) a step of irradiating a substrate with chemical radiation to initiate a reaction that forms a chemical bond by a reaction between at least one compound and the substrate, wherein a layer of aqueous liquid is still on the substrate when the irradiation begins,

[0011] d) a step of removing any remaining aqueous liquid from the substrate,

[0012] e) Includes the step of applying and curing a subsequent coating.

[0013] In a second embodiment, a coated substrate is provided as described above.

[0014] One advantage is that the energy-consuming drying step in the process is eliminated.

[0015] In addition, since it is possible to apply a very small amount of material to the surface, costs are reduced.

[0016] The present invention also enables the use of water-based liquids while avoiding the use of harmful solvents. Specific details for implementing the invention

[0017] Before the present invention is disclosed and described in detail, it should be understood that the invention is not limited to the specific compounds, compositions, method steps, substrates, and materials disclosed herein, as such compounds, compositions, method steps, substrates, and materials may be modified to some extent. Furthermore, it should be understood that the terms used herein are used merely for the purpose of describing specific embodiments and are not intended to be limiting, as the scope of the invention is limited only by the appended claims.

[0018] It should be noted that, as used in this specification and the appended claims, the singular forms (“a,” “an,” and “the”) include plural objects unless the context clearly indicates otherwise.

[0019] Unless otherwise defined, any terms and scientific terms used herein are intended to have the meaning generally understood by a person skilled in the art to which the present invention pertains.

[0020] As used here, "(meth)acrylate" is a general term encompassing both acrylate and methacrylate.

[0021] As used herein, the term non-absorbent means that a non-absorbent substrate does not absorb water, or at least does not absorb water to any significant degree for the intended purpose. The amount of water absorbed after immersing the substrate in water at 23°C is measured according to ISO 62:2008. To be considered non-absorbent, the substrate must not absorb more than 2 wt% of water when measured according to ISO 62:2008. In the case of a solid substrate composed of PP (poly(1-methylethylene)), the amount of water absorbed is close to 0 wt%. By comparison, porous materials such as wood and MDF boards (medium-density fiberboard) absorb about 20 to 40 wt% of water.

[0022] In a first embodiment, a method for coating a substrate is provided, and the method

[0023] a) a step of providing a substrate, wherein the substrate comprises at least one polymer selected from the group consisting of poly(ethylene terephthalate), poly(1-methylethylene), poly(1-chloroethylene) and polyethylene, and the substrate is non-absorbent to water, a step of providing a substrate,

[0024] b) a step of applying a layer of an aqueous liquid onto a substrate, wherein the aqueous liquid comprises at least one compound having the ability to form a chemical bond to the substrate by chemical radiation irradiation,

[0025] c) a step of irradiating a substrate with chemical radiation to initiate a reaction that forms a chemical bond by a reaction between at least one compound and the substrate, wherein a layer of aqueous liquid is still on the substrate when the irradiation begins,

[0026] d) a step of removing any remaining aqueous liquid from the substrate,

[0027] e) Includes the step of applying and curing a subsequent coating.

[0028] The present invention relates to substrates comprising the following:

[0029] Poly(ethylene terephthalate) (also abbreviated as PET),

[0030] Poly(1-methylethylene) (also abbreviated as PP),

[0031] Poly(1-chloroethylene) (also abbreviated as PVC) and / or

[0032] Polyethylene (also abbreviated as PE).

[0033] Substrates comprising at least one of the polymers described above are typically non-absorbent if they are not porous. Substrates comprising at least one of the polymers described above are non-absorbent if they are made of a solid polymer. Substrates having pores are not suitable for use according to the present invention.

[0034] In one embodiment, the substrate comprises a polymer selected from the group consisting of poly(ethylene terephthalate), poly(1-methylethylene), poly(1-chloroethylene), and polyethylene. In one embodiment, the substrate comprises a polymer selected from the group consisting of poly(ethylene terephthalate) and poly(1-methylethylene).

[0035] In the above method, a layer of aqueous liquid is applied onto a substrate, wherein at least one compound is present in the aqueous liquid. At least one compound has the ability to form a chemical bond to the substrate by chemical radiation irradiation.

[0036] The formation of chemical bonds can be achieved by any mechanism known in the prior art. Chemical bonds are formed through reactive intermediates generated by a decomposition reaction on a substrate surface initiated by chemical radiation.

[0037] The chemical bond is a covalent bond in one embodiment.

[0038] For example, at least one compound having the ability to form a chemical bond to a substrate by chemical radiation irradiation may be a compound that can be exposed to UV radiation to initiate a reaction and form a covalent bond to the substrate in the presence of an initiator, for example, such as a UV initiator.

[0039] An advantage is that there is no need to dry the liquid before irradiation. As can be seen from the examples, the above method can often be performed even when drying the liquid before irradiation in step c), but there are other disadvantages, such as a time-consuming drying step that increases energy consumption and / or adds costs. When chemical bonds are formed by chemical radiation irradiation, such as UV radiation, the liquid remaining on the substrate surface is removed, and a subsequent coating is applied and cured as known in the prior art. In one embodiment, the subsequent coating is the final coating, where the subsequent coating is the top coating. Alternatively, additional coatings may be applied, and then additional coatings may be applied on top of the subsequent coating. In one embodiment, the top coating is applied on the subsequent coating.

[0040] Before a subsequent coating is applied and cured, any remaining aqueous liquid is removed from the substrate to ensure proper application and curing of the subsequent coating. Any remaining aqueous liquid is intended to mean any aqueous liquid that could have a negative effect on the subsequent coating. This refers to a substrate that is generally defined by those skilled in the art as a dry substrate, and does not exclude the presence of extremely small amounts of residue or aqueous liquid, but such residues do not have a substantial effect on the result. Therefore, removing any remaining aqueous liquid from the substrate means that the substrate is subsequently dried to the extent that it is recognized as dry by those skilled in the art, so that any trace amount of residual water does not have any negative effect on the subsequent coating applied thereafter.

[0041] In one embodiment, the substrate comprises at least one selected from the group consisting of poly(ethylene terephthalate) and poly(1-methylethylene).

[0042] In one embodiment, the dry material in the aqueous liquid applied in step b) is up to 25 wt%, preferably up to 10 wt%. An advantage of using this method is that a low concentration of material can be applied.

[0043] In one embodiment, at least one compound constitutes up to 25 wt%, preferably up to 10 wt%, of the aqueous liquid applied in step b).

[0044] In one embodiment, the aqueous liquid applied in step b) is one selected from the group consisting of: a) an aqueous solution, wherein at least one compound having the ability to form a chemical bond to a substrate by chemical radiation is dissolved in the aqueous solution; and b) an aqueous emulsion comprising at least one compound having the ability to form a chemical bond to a substrate by chemical radiation. Thus, the aqueous liquid may be an aqueous solution in which at least one compound is dissolved, or an aqueous emulsion in which at least one compound is present in any form within the emulsion. That the emulsion is aqueous means that the emulsion contains water in any phase. The aqueous emulsion may be of different types:

[0045] - An oil-in-water emulsion, wherein at least one compound is more hydrophobic and non-water-soluble, and exists in the form of droplets within a continuous aqueous phase.

[0046] - A water-in-water emulsion comprising droplets of molecules solvated with water within another continuous aqueous solution; comprising different molecules in which both the droplet phase and the continuous phase are completely water-soluble. In such an emulsion, at least one compound is water-soluble and is present in one of the phases.

[0047] - A water-in-oil emulsion, wherein at least one compound is more hydrophobic and not water-soluble, and water exists in the form of droplets within a continuous phase of a non-aqueous phase containing at least one compound.

[0048] In one embodiment, the aqueous liquid applied in step b) is an aqueous solution, wherein at least one compound having the ability to form a chemical bond to a substrate by chemical radiation irradiation is dissolved in the aqueous solution.

[0049] In one embodiment, the layer of aqueous liquid applied in step b) has a thickness in the range of 5 to 30 µm. An advantage is that a layer that is not excessively thin can be applied while using only a very small amount of a compound at a low concentration compared to the prior art. The alternative of adding a very thin layer is more difficult and costly in large-scale manufacturing. For some substrates, it is also difficult to apply a thin and uniform layer.

[0050] In one embodiment, the layer of aqueous solution applied in step b) is applied using spray coating and has a thickness in the range of 30 to 200 μm.

[0051] In one embodiment, at least one compound having the ability to form a chemical bond to a substrate by chemical radiation irradiation has the ability to form a covalent bond to a substrate by chemical radiation irradiation. In the case of substrates poly(ethylene terephthalate), poly(1-methylethylene), and polyethylene, the chemical bond is a covalent bond. In the case of a substrate containing poly(1-chloroethylene), the inventors believe that the chemical bond is a covalent bond. The inventors believe that when poly(1-chloroethylene) is irradiated with chemical radiation to form radicals, a covalent bond can also be formed in a substrate containing poly(1-chloroethylene).

[0052] In one embodiment, at least one compound is a compound comprising at least one carbon-carbon double bond.

[0053] In one embodiment, an electron-withdrawing group adjacent to the carbon-carbon double bond is present. In one embodiment, the electron-withdrawing group is at least one selected from the group consisting of a trilyl group, a trihalide group, a cyano group, a sulfonate group, a nitro group, an ammonium group, an aldehyde group, a keto group, a carboxyl group, an acyl chloride group, an ester group, an amide group, an ether group, and a halide.

[0054] In one embodiment, at least one compound is selected from the group consisting of maleic anhydride and maleimide. In the case of maleic anhydride, it is soluble in water and reacts slowly with water to form maleic acid and heat.

[0055] In one embodiment, at least one compound is at least one compound selected from the group consisting of maleate and fumarate.

[0056] In one embodiment, at least one compound is at least one compound selected from the group consisting of acrylates and methacrylates.

[0057] In one embodiment, at least one compound is at least one compound selected from the group consisting of acrylates and divinyl ethers.

[0058] In one embodiment, the removal in step d) is performed by drying. In one embodiment, the removal in step d) is performed by passive evaporation, that is, without applying heat from a heat source other than the ambient heat and air of the room where the experiment is performed. In one embodiment, the latent heat generated from irradiation with chemical radiation, such as UV radiation, is at least partially utilized for evaporation.

[0059] In one embodiment, removal in step d) is performed by blowing unheated air toward the substrate. Using unheated air can save energy, but using heated air is also possible. Unheated air refers to ambient air blown toward the substrate, which has the same temperature as the room, typically room temperature.

[0060] In one embodiment, the subsequent coating comprises acrylate. In one embodiment, the subsequent coating is UV-curable.

[0061] In one embodiment, the coating after step e) has a Hamberger value of 20 N or more. This is measured according to the instructions provided to the measuring instrument. The force is increased until fracture occurs through the coating and reaches the substrate. This value is recorded.

[0062] In one embodiment, the coating after step e) has a cross cut of 0 when measured according to ISO 2409:2020. The cross cut is measured as a quality indicator of the coating. The cross cut is measured according to ISO 2409:2020. ISO 2409:2020 specifies a test method for evaluating the resistance of paint coatings and varnishes (including wood stains) to separation from the substrate when a right-angle grid pattern is cut through the coating to penetrate the substrate. The characteristics determined by this empirical test procedure depend, among other factors, on the adhesion of the coating to the previous coating or the substrate. However, this procedure is not a means for measuring adhesion.

[0063] In one embodiment, the substrate comprises poly(1-methylethylene) and / or polyethylene, wherein the substrate is treated prior to step b) with at least one selected from the group consisting of corona, plasma, and flame. The treatment time and treatment conditions are appropriately set to increase the hydrophilicity of the substrate. Corona and / or flame treatment has the effect of increasing the hydrophilicity of the substrate to improve wettability to aqueous liquids. Additionally, corona treatment has the advantage of creating chemical groups on the surface, and these chemical groups are typically more suitable for participating in additional chemical reactions and / or forming chemical bonds.

[0064] The coating after step e) shows that the cross-cut value measured according to ISO 2409:2020 is superior (i.e., has a lower value) to the cross-cut value of the same subsequent coating(s) on the same substrate without a primer, compared, for example, when steps b) to d) in claim 1 are omitted.

[0065] In one embodiment, the aqueous liquid applied in step b) comprises at least one selected from the group consisting of surfactants, starches, and disinfectants.

[0066] In a second embodiment, a coated substrate is provided as described above.

[0067] In an additional version, a method for coating a substrate is provided, and said method

[0068] a) a step of providing a substrate, wherein the substrate comprises poly(1-methylethylene) and the substrate is non-absorbent to water, a step of providing a substrate,

[0069] b) a step of applying a layer of an aqueous liquid onto a substrate, wherein the aqueous liquid comprises at least one compound containing an acrylate group, and at least one compound has the ability to form a chemical bond to the substrate by chemical radiation irradiation, and the aqueous liquid comprises a Norrish type II photoinitiator, a step of applying,

[0070] c) a step of irradiating a substrate with chemical radiation to initiate a reaction that forms a chemical bond by a reaction between at least one compound and the substrate, wherein, when the irradiation begins, a layer of aqueous liquid is at least partially dried or still on the substrate, irradiating step,

[0071] d) a step of removing any remaining aqueous liquid from the substrate,

[0072] e) Includes the step of applying and curing a subsequent coating.

[0073] In this version, the aqueous liquid contains a nolish type II photoinitiator. In this case, the nolish type II initiator absorbs energy and uses it to transfer it to a peroxide, which is then cleaved into two radical fragments. The radical fragments bonded to the substrate react with the double bond to form a covalent bond.

[0074] In this version, when the investigation begins, the aqueous liquid may be completely dried, partially dried, or remain completely on the substrate.

[0075] In another version, a method for coating a substrate is provided, and the method

[0076] a) a step of providing a substrate, wherein the substrate comprises poly(1-chloroethylene) and the substrate is non-absorbent to water, a step of providing a substrate,

[0077] b) a step of applying a layer of an aqueous liquid onto a substrate, wherein the aqueous liquid comprises at least one compound containing an acrylate group, and at least one compound has the ability to form a chemical bond to the substrate by chemical radiation irradiation, a step of applying,

[0078] c) a step of irradiating a substrate with chemical radiation to initiate a reaction that forms a chemical bond by a reaction between at least one compound and the substrate, wherein, when the irradiation begins, a layer of aqueous liquid is at least partially dried or still on the substrate, irradiating step,

[0079] d) a step of removing any remaining aqueous liquid from the substrate,

[0080] e) Includes the step of applying and curing a subsequent coating.

[0081] Also, in this version, when the investigation begins, the aqueous liquid may be completely dried, partially dried, or remain completely on the substrate.

[0082] In all versions and embodiments, for example, if there is no aqueous liquid remaining after step c) due to heating and evaporation during investigation, the liquid is not removed in step d).

[0083] Other features, uses, and associated advantages of the present invention will be apparent to those skilled in the art from reading the description and examples in this specification.

[0084] It should be understood that the present invention is not limited to the specific embodiments presented herein. The embodiments are provided for illustrative purposes only and are not intended to limit the scope of the invention, as the scope of the invention is defined by the appended claims.

[0085] Throughout the description and claims of this specification, all percentages are calculated based on weight.

[0086] Examples

[0087] Example 1

[0088] It was investigated whether curing a wet aqueous primer on PET could have equivalent performance compared to curing in a dry state.

[0089] Formulation 2: DVE3 2.4% UCECoat 7156 2.4% Starch c* productl S2 0.12% SDBS 0.09% BYK 025 0.036% H2O 95%

[0090] All percentages are based on weight.

[0091] Here, DVE3 is triethylene glycol divinyl ether from BASF®, Germany, BYK 025 is a surfactant from BYK Chemie®, Germany, UCECoat is an acrylate dispersion from Allnex®, Germany, and SDBS is sodium dodecylbenzenesulfonate.

[0092] method:

[0093] * "Toray Lumimirror 40.01", a 150㎛ thick PET foil from Toray® of France, was used.

[0094] A PET foil was cut to a size of 10 × 20 cm and attached to a support with tape across the entire top and bottom edges.

[0095] The above formulation 2 was applied onto PET using a 22 µm rod applicator.

[0096] - When testing wet curing, the samples were immediately placed in a quartz glass box where humidity was maintained.

[0097] - When testing dry curing, the samples were dried with an unheated airflow and then placed in a quartz glass box where humidity was maintained.

[0098] The samples were cured at the set UV intensity and line speed.

[0099] * Wet samples were dried with an unheated airflow at room temperature.

[0100] * UT 7710, a 1K acrylate UV top coating, was applied using a 15㎛ smoothing applicator and cured at 2 × 100% UV at 4 m / min to impart a dose of 800 mJ / cm² (UVA).

[0101] result Coating thickness (㎛) Dry content (wt%) UV Oven Passage Count (#) UV Intensity (%) UVA dose (mJ / cm²) Wet / Dry Cross cut 22 5 2 100 800 moist 0 22 5 2 100 800 dry 0 22 5 1 100 400 moist 0 22 5 1 100 200 moist 0 22 5 1 50 100 moist 0 0 (Control group without primer) - - - - - 5 12 1 1 40 80 moist 0 12 1 1 40 80 dry 0

[0102] All samples cured in a wet state were removed from the UV oven in a wet state inside a quartz glass box and then dried with an unheated airflow before subsequent coating application.

[0103] conclusion

[0104] Primer performance is excellent regardless of whether it is cured in wet or dry conditions.

[0105] A primer is required on the PET to ensure adhesion of the top coating.

[0106] Primers with low drying content can be applied even at high line speeds due to their low UV capacity.

[0107] Example 2

[0108] We investigated whether curing a wet aqueous primer on PP (poly(1-methylethylene)) could have equivalent performance compared to curing it in a dry state.

[0109] Formulation 3: Speedcure BMS 0.31 HDDA 3.89 Ucec 7156 2.01 H2O 93.68 SDBS 0.05 BYK 028 0.06 Tot 100

[0110] The percentages in the above chart are based on weight.

[0111] Here, BMS is 4-benzoyl-4'-methyldiphenylsulfide from Lambson® of the UK, and HDDA is hexanediol diacrylate from Arkema® of France.

[0112] method:

[0113] PP is an untreated, 2 mm thick extruded dark gray sheet manufactured for use as an edge band for furniture.

[0114] * PP was cut into pieces measuring 5 × 10 cm, and fixed to a support with double-sided tape so that the glossy side of the PP faced upward.

[0115] PP was corona treated using the Multidyne 1000, a compact corona processor from 3DT®, USA. The substrate was fixed on a non-conductive rubber sheet, and a corona tip was positioned 10 mm away from the substrate. After starting the corona discharge, the corona tip moved back and forth 4 times over the substrate at a speed of 10 cm / s for 5 seconds, performing a total of 8 passes.

[0116] The above formulation 3 was diluted to a dry content of 5 wt% and applied onto PP using a 22 μm rod applicator.

[0117] - When testing wet curing, the samples were immediately placed in a quartz glass box where humidity was maintained.

[0118] - When testing dry curing, the samples were dried with an unheated airflow and then placed in a quartz glass box where humidity was maintained.

[0119] The samples were cured at the set UV intensity and line speed.

[0120] * Wet samples were dried with an unheated airflow at room temperature.

[0121] UT 7710, a 1K acrylate UV top coating, was applied using a 22㎛ rod applicator and cured at 2 × 100% UV at 4 m / min to impart a capacity of 1 J / cm².

[0122] result Coating thickness (㎛) Dry content (wt%) COVID Pass (#) UV Oven Passage Count (#) UV Intensity (%) UVA dose (mJ / cm²) Wet / Dry Cross cut note 22 7.5 8 1 100 200 dry 0 22 7.5 8 1 100 200 moist 0 Humid condition outside the oven

[0123] conclusion

[0124] In PP, curing in a wet state is effective.

[0125] Example 3

[0126] A variation of Formulation 2 with a higher dry content was prepared by reducing the amount of water used in the formulation while maintaining the mutual ratios of all other components. The final dry content of this variation of Formulation 2 was 20%, and it was used in this example.

[0127] method:

[0128] PVC foil marked "PVC XT grey," a 1 mm thick PVC film from Norbergs Tekniska of Sweden, was used.

[0129] A PVC foil measuring 10 × 3 cm was attached to the support using double-sided tape.

[0130] A variation of Formulation 2 with 20% dry content was applied onto PVC using a rod applicator.

[0131] - When testing wet curing, the samples were immediately placed in a quartz glass box where humidity was maintained.

[0132] - When testing dry curing, the samples were dried with an unheated airflow and then placed in a quartz glass box where humidity was maintained.

[0133] * The samples were cured with 1 × 100% UV at 9.9 m / min to impart a dose of 200 mJ / cm² (UVA).

[0134] * Wet samples were dried with an unheated airflow at room temperature.

[0135] UT 7710, a 1K acrylate UV top coating, was applied using a 22㎛ rod applicator and cured at 2 × 100% UV at 4 m / min to impart a dose of 800 mJ / cm² (UVA).

[0136] result Wet coating thickness (㎛) Dry coverage (g / sqm) Dry content (%) UV Oven Passage Count (#) UV capacity (%) Line speed (m / min) Wet / Dry Cross cut note 12 2.4 20 1 0 0 dry 5 Uncured primer, top coating applied directly over it 12 2.4 20 1 100 9.9 dry 0 12 2.4 20 1 100 9.9 moist 1

[0137] The PVC sample cured with primer in a wet state remained wet even after being removed from the UV oven.

[0138] conclusion

[0139] The dry-cured primer provides excellent adhesion of the top coating to PVC.

Claims

Claim 1 A method for coating a substrate, the method comprising: a) providing a substrate, wherein the substrate comprises at least one polymer selected from the group consisting of poly(ethylene terephthalate), poly(1-methylethylene), poly(1-chloroethylene) and polyethylene, and wherein the substrate is non-absorbent to water; b) applying a layer of an aqueous liquid on the substrate, wherein the aqueous liquid comprises at least one compound having the ability to form a chemical bond to the substrate by chemical radiation irradiation; c) irradiating the substrate with chemical radiation to initiate a reaction forming a chemical bond by a reaction between the at least one compound and the substrate, wherein the layer of the aqueous liquid is still on the substrate when the irradiation begins; d) removing any remaining aqueous liquid from the substrate; and e) applying and curing a subsequent coating. Claim 2 A method according to claim 1, wherein the dry material in the aqueous liquid applied in step b) is at most 25 wt%, preferably at most 10 wt%. Claim 3 A method according to claim 1, wherein the at least one compound constitutes up to 25 wt%, preferably up to 10 wt%, of the aqueous liquid applied in step b). Claim 4 A method according to any one of claims 1 to 3, wherein the aqueous liquid applied in step b) is one selected from the group consisting of: a) an aqueous solution, wherein the at least one compound having the ability to form a chemical bond to the substrate by chemical radiation irradiation is dissolved in the aqueous solution; and b) an aqueous emulsion comprising the at least one compound having the ability to form a chemical bond to the substrate by chemical radiation irradiation. Claim 5 A method according to any one of claims 1 to 4, wherein the layer of the aqueous liquid applied in step b) has a thickness in the range of 5 to 30 μm. Claim 6 A method according to any one of claims 1 to 4, wherein the layer of the aqueous solution applied in step b) is applied using spray coating and has a thickness in the range of 30 to 200 μm. Claim 7 A method according to any one of claims 1 to 6, wherein the at least one compound having the ability to form a chemical bond to the substrate by chemical radiation irradiation has the ability to form a chemical bond to the substrate by chemical radiation irradiation, and the chemical bond formed in step c) is a covalent bond. Claim 8 A method according to any one of claims 1 to 7, wherein the at least one compound is a compound comprising at least one carbon-carbon double bond. Claim 9 In claim 8, a method in which an electron-attracting group adjacent to the carbon-carbon double bond exists. Claim 10 A method according to any one of claims 1 to 9, wherein the at least one compound is at least one compound selected from the group consisting of maleic anhydride and maleimide. Claim 11 A method according to any one of claims 1 to 10, wherein the at least one compound is at least one compound selected from the group consisting of maleates and fumarates. Claim 12 A method according to any one of claims 1 to 11, wherein the at least one compound is at least one compound selected from the group consisting of acrylates and methacrylates. Claim 13 A method according to any one of claims 1 to 12, wherein the at least one compound is at least one compound selected from the group consisting of acrylates and divinyl ethers. Claim 14 A method in which, in any one of claims 1 to 13, the removal step in step d) is performed by drying. Claim 15 A method in which, in any one of claims 1 to 14, the removal step in step d) is performed by blowing unheated air toward the substrate. Claim 16 A method according to any one of claims 1 to 15, wherein the coating after step e) has a Hamberger value of 20 N or more. Claim 17 A method according to any one of claims 1 to 16, wherein the coating after step e) has a cross cut of 0 when measured according to ISO 2409:2020. Claim 18 A method according to any one of claims 1 to 17, wherein the substrate comprises poly(1-methylethylene) and / or polyethylene, wherein the substrate is treated with at least one selected from the group consisting of corona, plasma and flame prior to step b). Claim 19 A method according to any one of claims 1 to 18, wherein the aqueous liquid applied in step b) comprises at least one selected from the group consisting of surfactants, starches, and disinfectants. Claim 20 A substrate coated according to any one of claims 1 to 19. Claim 21 A method for coating a substrate, the method comprising: a) providing a substrate, wherein the substrate comprises poly(1-methylethylene) and the substrate is non-absorbent to water; b) applying a layer of an aqueous liquid on the substrate, wherein the aqueous liquid comprises at least one compound comprising an acrylate group, wherein the at least one compound has the ability to form a chemical bond to the substrate by chemical radiation irradiation, and the aqueous liquid comprises a Norisi type II photoinitiator; c) irradiating the substrate with chemical radiation to initiate a reaction that forms a chemical bond by a reaction between the at least one compound and the substrate, wherein the layer of the aqueous liquid is at least partially dried or still on the substrate when the irradiation begins; d) removing any remaining aqueous liquid from the substrate; and e) applying and curing a subsequent coating. Claim 22 A method for coating a substrate, the method comprising: a) providing a substrate, wherein the substrate comprises poly(1-chloroethylene) and the substrate is non-absorbent to water; b) applying a layer of an aqueous liquid onto the substrate, wherein the aqueous liquid comprises at least one compound comprising an acrylate group and the at least one compound having the ability to form a chemical bond to the substrate by chemical radiation irradiation; c) irradiating the substrate with chemical radiation to initiate a reaction forming a chemical bond by a reaction between the at least one compound and the substrate, wherein the layer of the aqueous liquid is at least partially dried or still on the substrate when the irradiation begins; d) removing any remaining aqueous liquid from the substrate; and e) applying and curing a subsequent coating.