Integrated Low-k Recovery and ALD Metal Deposition Process for Advanced Technology Nodes

By exposing damaged low-k films to recovery precursors and UV light, followed by atomic layer deposition, the method addresses the issue of undesirable surface properties, enhancing the films' suitability for subsequent processing and deposition.

KR1020260163508APending Publication Date: 2026-11-16APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267035241
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-07-16
Filing Date
2025-03-28
Publication Date
2026-11-16

AI Technical Summary

Technical Problem

Existing processes for recovering low-k dielectric films result in undesirable surface properties that are unfavorable for subsequent atomic layer deposition, leading to device performance degradation.

Method used

A method involving sequential exposure of damaged low-k films to recovery precursors and UV light sources, followed by atomic layer deposition of a liner layer, to restore the dielectric constant and hydrophobicity of the films.

Benefits of technology

The method effectively reduces the dielectric constant and increases hydrophobicity of low-k films, making them suitable for subsequent processing and deposition operations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00022_ABST
    Figure PCT00022_ABST
Patent Text Reader

Abstract

In some embodiments, the method includes the step of positioning a substrate within a processing chamber. The substrate comprises a first low-k film having a first water contact angle. The first low-k film is placed over an interconnect structure. The method further includes the step of cleaning the substrate within the processing chamber to form a cleaned substrate. The cleaned substrate comprises a damaged low-k film having a second water contact angle. The method further includes the step of exposing the cleaned substrate to a recovery precursor to form a recovered substrate. The recovered substrate comprises a recovered low-k film. The method further includes the step of exposing the recovered substrate to a UV light source to form a treated substrate. The treated substrate comprises a treated low-k film having a third water contact angle. The method further includes the step of depositing a liner layer on the treated substrate via atomic layer deposition (ALD).
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The embodiments described herein generally relate to processing low-k dielectric films. More specifically, the embodiments described herein relate to processes for recovering low-k dielectric films and depositing metal layers thereon. Background Technology

[0002] As device scaling continues, the dielectric constant (k) of dielectric films in semiconductor manufacturing is continuously decreasing. Minimizing integrated damage to low dielectric constant (low-k) films is beneficial for enabling the continued reduction of feature sizes. Unfortunately, damage to low-k films caused by various processes can lead to an increase in dielectric constant and an increase in surface hydrophilicity, both of which can result in device performance degradation (e.g., potential failure of integrated circuits).

[0003] Efforts have been directed toward developing processes designed to recover properties lost due to accumulated damage in low-k films. However, the resulting properties of low-k films produced through these processes may not allow for subsequent processing and deposition operations. In many cases, low-k films that have undergone dielectric constant recovery processes exhibit undesirable surface properties that are disadvantageous for subsequent atomic layer deposition processes.

[0004] Therefore, there is a need for improved processes for recovering the dielectric constant.

[0005] The embodiments described herein generally relate to processes for processing low-k dielectric films. More specifically, the embodiments described herein relate to processes for recovering low-k dielectric films and depositing metal layers thereon.

[0006] In some embodiments, the method includes the step of positioning a substrate within a processing chamber. The substrate comprises a first low-k film having a first water contact angle. The first low-k film is placed over an interconnect structure. The method further includes the step of cleaning the substrate within the processing chamber to form a cleaned substrate. The cleaned substrate comprises a damaged low-k film having a second water contact angle. The damaged low-k film is formed from the first low-k film. The method further includes the step of exposing the cleaned substrate to a recovery precursor to form a recovered substrate. The recovered substrate comprises a recovered low-k film. The recovered low-k film is formed from the damaged low-k film. The method further includes the step of exposing the recovered substrate to a UV light source to form a processed substrate. The processed substrate comprises a processed low-k film having a third water contact angle. The processed low-k film is formed from the recovered low-k film. The method further includes the step of depositing a liner layer on a treated substrate via atomic layer deposition (ALD).

[0007] In some embodiments, the method includes the step of positioning a substrate within a processing chamber. The substrate comprises a first low-k film having a first water contact angle. The first low-k film is placed over an interconnect structure. The method further includes the step of cleaning the substrate within the processing chamber to form a cleaned substrate. The cleaned substrate comprises a damaged low-k film having a second water contact angle. The damaged low-k film is formed from the first low-k film. The method further includes the step of exposing the cleaned substrate to a UV light source to form a treated substrate. The treated substrate comprises a treated low-k film having a third water contact angle. The treated low-k film is formed from the damaged low-k film. The method further includes the step of exposing the treated substrate to a recovery precursor to form a recovered substrate. The recovered substrate comprises a recovered low-k film. The recovered low-k film is formed from the treated low-k film. The method further includes the step of depositing a liner layer on the recovered substrate via atomic layer deposition (ALD).

[0008] In some embodiments, the method includes the step of positioning a substrate within a processing chamber. The substrate comprises a first low-k film having a first water contact angle. The first low-k film is placed over an interconnect structure. The method further includes the step of cleaning the substrate within the processing chamber to form a cleaned substrate. The cleaned substrate comprises a damaged low-k film having a second water contact angle. The damaged low-k film is formed from the first low-k film. The method further includes the step of exposing the cleaned substrate to a recovery precursor to form a recovered substrate. The recovered substrate comprises a recovered low-k film. The recovered low-k film is formed from the damaged low-k film. The method further includes the step of exposing the recovered substrate to a UV light source to form a treated substrate. The treated substrate comprises a treated low-k film having a third water contact angle. The treated low-k film is formed from the recovered low-k film. The method further includes the step of depositing a liner layer on the treated substrate via atomic layer deposition (ALD). The first water contact angle is greater than the second water contact angle, and the second water contact angle is smaller than the third water contact angle. Brief explanation of the drawing

[0009] In a manner that the features of the above disclosure can be understood in detail, a more specific description of the above disclosure, briefly summarized above, may be made with reference to embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the accompanying drawings merely illustrate typical embodiments of the present disclosure and are therefore not to be construed as limiting the scope of the present disclosure, and that other equally valid embodiments may be permitted.

[0010] FIG. 1 is a schematic cross-sectional view of a process chamber according to one or more embodiments.

[0011] FIG. 2 is a schematic block diagram of a substrate processing method according to one or more embodiments.

[0012] FIG. 3a is a partial schematic side cross-sectional view of an interconnect structure during the method according to one or more embodiments.

[0013] FIG. 3b is a partial schematic side cross-sectional view of an interconnect structure during the method according to one or more embodiments.

[0014] FIG. 3c are partial schematic side cross-sectional views of an interconnect structure during the method according to one or more embodiments.

[0015] FIG. 3d are partial schematic side cross-sectional views of an interconnect structure during the method according to one or more embodiments.

[0016] FIG. 4a is a molecular representation of a low-k film during the method according to one or more embodiments.

[0017] FIG. 4b is a molecular representation of a low-k film during the method according to one or more embodiments.

[0018] FIG. 4c is a molecular representation of a low-k film during the method according to one or more embodiments.

[0019] FIG. 5 is a schematic block diagram of a substrate processing method according to one or more embodiments.

[0020] FIG. 6 is a schematic block diagram of a substrate processing method according to one or more embodiments.

[0021] FIG. 7 is a schematic block diagram of a substrate processing method according to one or more embodiments.

[0022] FIG. 8 is a schematic block diagram of a substrate processing method according to one or more embodiments.

[0023] FIG. 9 is a series of surface images of an interconnect structure after a method according to one or more embodiments. Specific details for implementing the invention

[0024] The present disclosure provides methods for recovering the properties of damaged low-k films during substrate processing procedures. The recovery processes disclosed herein generally comprise a series of sequential property recovery operations, including exposing a substrate to one or more recovery precursors and exposing the substrate to a UV light source. The recovery processes disclosed herein can reduce the elevated k values ​​of damaged low-k films and can also increase the surface hydrophobicity of these films. Additionally, the sequential recovery processes of the present disclosure provide a balance between the recovery of low-k values ​​and the recovery of hydrophilic / hydrophobic properties so that the surface of the resulting films is favorable for subsequent ALD metal film deposition.

[0025] FIG. 1 is a schematic cross-sectional view of a process chamber (100) according to one or more embodiments. The process chamber (100) may be a vapor deposition chamber containing UV radiation to assist a silylation reaction. In one or more embodiments, the process chamber (100) may be an ONYX® or SILENA® process chamber available from Applied Materials, Inc., Santa Clara, California. The process chamber (100) comprises a chamber body (102) and a chamber lid (104) disposed over the chamber body (102). The chamber body (102) and the chamber lid (104) form an internal volume (106). A substrate support assembly (108) is disposed in the internal volume (106). The substrate support assembly (108) may receive and support a substrate (110) thereon for processing.

[0026] A first UV transparent gas distribution showerhead (116) can be suspended in the internal volume (106) through the central opening (112) of the chamber lid (104) by means of an upper clamping member (118) and a lower clamping member (120). The UV transparent gas distribution showerhead (116) can be positioned toward the substrate support assembly (108) to distribute one or more processing gases across the distribution volume (122) located below the first UV transparent gas distribution showerhead (116). A second UV transparent gas showerhead (124) can be suspended in the internal volume (106) through the central opening (112) of the chamber lid (104) located below the first UV transparent gas distribution showerhead (116). Each of the UV transparent gas distribution showerheads (116, 124) can be placed in a recess formed in the chamber lid (104). The first recess (126) may be an annular recess around the inner surface of the chamber lid (104), and the first UV clear gas distribution showerhead (116) is fitted into the first recess (126). Likewise, the second recess (128) may accommodate the second UV clear gas distribution showerhead (124).

[0027] A UV transparent window (114) may be positioned over a first UV transparent gas distribution showerhead (116). The UV transparent window (114) may be positioned over the first UV transparent gas distribution showerhead (116) to form a gas volume (130) between the UV transparent window (114) and the first UV transparent gas distribution showerhead (116). The UV transparent window (114) may be secured to the chamber lid (104) by any means such as clamps, screws, bolts, etc.

[0028] The UV transparent window (114) and the first and second UV transparent gas distribution showerheads (116, 124) may be at least partially transparent to thermal energy or radiant energy within UV wavelengths. The UV transparent window (114) may be quartz or another UV transparent material, such as sapphire, CaF2, MgF2, AlON, silicon oxide material, silicon oxynitride material, or another transparent material.

[0029] A UV source (150) may be placed over a UV transparent window (114). The UV source (150) may be configured to generate UV energy and project UV energy toward a substrate support assembly (108) through the UV transparent window (114), a first UV transparent gas distribution showerhead (116), and a second UV transparent gas distribution showerhead (124), thereby exposing a substrate (110) on the substrate support assembly (108) to UV light. A cover (not shown) may be placed over the UV source (150). In one or more embodiments, the cover may be shaped to assist in the projection of UV energy from the UV source (150) toward the substrate support.

[0030] In one or more embodiments, the UV source (150) may include one or more UV lights (152) for generating UV radiation. The UV lights (152) may be lamps, LED emitters, or other UV emitters. In one or more embodiments, the UV lights (152) may be rare earth near-ultraviolet lamps, such as argon lamps emitting radiation at 126 nm, krypton lamps emitting at 146 nm, xenon lamps emitting at 172 nm, krypton chloride lamps emitting at 222 nm, xenon chloride lamps emitting at 308 nm, mercury lamps emitting at 254 nm or 365 nm, metal vapor lamps such as zinc emitting at 214 nm, and europium-doped strontium borate or fluoroborate lamps emitting at 368-371 nm, among other examples.

[0031] The process chamber (100) may include flow channels (132, 134, 136) configured to supply one or more processing gases across the substrate support assembly (108) to process a substrate (110) placed on the substrate support assembly (108). The first flow channel (132) provides a flow path for gas to enter the gas volume (130) and be exposed to UV radiation from the UV source (150). Gas from the gas volume (130) may flow into the distribution volume (122) through the first UV transparent gas distribution showerhead (116). The second flow channel (134) may provide a flow path for precursor compounds and gases to enter directly into the distribution volume (122) without passing through the first UV transparent gas distribution showerhead (116) and be mixed with the gas previously exposed to UV radiation within the gas volume (130). The mixed gases within the distribution volume (122) may be further exposed to UV radiation through the first UV transparent gas distribution showerhead (116) before flowing into the space near the substrate support assembly (108) through the second UV transparent gas distribution showerhead (124). The gas near the substrate support assembly (108) and the substrate placed on the substrate support assembly (108) are further exposed to UV radiation through the second UV transparent gas distribution showerhead (124). Purge gases may be provided through the opening (138) at the bottom of the process chamber (100), so that the purge gas flows around the substrate support assembly (108) to prevent processing gases from entering the space below the substrate support assembly (108). One or more gases may be exhausted through the opening (138).

[0032] The first UV transparent gas distribution showerhead (116) may include a plurality of holes (140) that allow processing gas to flow from a gas volume (130) to a distribution volume (122). The second UV transparent gas distribution showerhead (124) may also include a plurality of holes (142) that allow processing gas to flow from the distribution volume (122) into a processing space near a substrate support assembly (108). The holes (140, 142) of the first and second UV transparent gas distribution showerheads (116, 124) may be uniformly distributed or irregularly spaced.

[0033] A purge gas or carrier gas source (154) may be coupled to the first flow channel (132) through the conduit (156). The purge gas from the purge gas source (154) may be provided through the first flow channel (132) during substrate processing to prevent process gases from entering the gas volume (130). A cleaning gas source (174) may also be coupled to the first flow channel (132) through the conduit (156) to provide cleaning of the conduit (156), the first flow channel (132), the gas volume (130), and the rest of the chamber body (102) when substrates are not being processed.

[0034] A process gas or precursor compound source (158) may be coupled to a second flow channel (134) via a conduit (160) to provide a mixture to the chamber body (102) as described above. The process gas source (158) may also be coupled to a third flow channel (136). Suitable valves may allow for the selection of one or both of the flow channels (134, 136) to flow the process gas mixture into the chamber body (102).

[0035] The substrate temperature can be controlled by providing heating and cooling features to the substrate support assembly (108). A coolant conduit (164) may be coupled to a coolant source (170) to provide coolant within a cooling plenum (162) placed in the substrate support assembly (108). An example of a coolant that can be used is a mixture of 50% ethylene glycol in water by volume. The coolant flow is controlled to maintain the temperature of the substrate below a desired level to facilitate the deposition of UV-activated oligomers or fragments on the substrate. A heating element (166) may also be provided to the substrate support assembly (108). The heating element (166) may be a resistive heater and may be coupled to a heating source (172), such as a power supply, by a conduit (168). The heating element (166) may be used to heat the substrate during the curing process described above.

[0036] FIG. 2 is a schematic block diagram of a substrate processing method (200) according to one or more embodiments. FIG. 3a through 3d are partial schematic side cross-sectional views of interconnect structures (300A–300D) during the method (200) according to one or more embodiments. FIG. 4a through 4c are molecular diagrams of low-k films (302a, 302b, and 302c) during the method (200) according to one or more embodiments.

[0037] In operation (210), a substrate that may include the interconnect structure (300A) illustrated in FIG. 3a is transferred into a process chamber. The process chamber may be a deposition process chamber such as the process chamber (100) illustrated in FIG. 1. In operation (210), the interconnect structure (300A) is a post-deposition interconnect structure. In other words, the interconnect structure (300A) includes a low-k film deposited thereon prior to operation (210). The interconnect structure (300A) illustrated in FIG. 3a may include a low-k film (302a) on an etching stop layer (304), a metal barrier (306) between the etching stop layer (304) and the copper layer (310), a metal barrier (306) between the copper layer (310) and the substrate (308), a residue (314) on the copper layer (310), and a residue (314) on the low-k film (302a). The interconnect structure (300A) may also include an intermediate layer (312) between the substrate (308) and the etching stop layer (304). In some embodiments, an interconnect structure having a configuration different from that illustrated in FIG. 3a may be utilized in the method (200).

[0038] FIG. 4a is a molecular diagram of the low-k film (302a) in operation (210). In FIG. 4a, the low-k film (302a) has Si-O bonds, Si-CH3 bonds, and Si-H bonds. In some embodiments, the metal barrier (306) is tantalum nitride (TaN), hafnium oxide (HfO2), or aluminum oxide (AlO2). x It may include zirconium oxide (ZrO2), titanium nitride (TiN), nickel oxide (NiO), nickel nitride (NiN), and combinations thereof.

[0039] In operation (220), the interconnect structure (300A) is cleaned in a process chamber such as the process chamber (100). As a result of operation (220), the low-k film (302a) of the interconnect structure (300A) may be damaged. As illustrated in FIGS. 4a and 4b, the total number of Si-CH3 bonds initially present in the low-k film (302a) may be reduced and Si-OH bonds may be formed, thereby creating a low-k film (302b). Due to the increase in Si-OH bonds, the low-k film (302b) becomes more hydrophilic compared to the low-k film (302a), which is undesirable. The reduction in Si-CH3 bonds in the low-k film (302b) results in an increase in the k value of the low-k film (302b) compared to the initial k value of the low-k film (302a). In some embodiments, the cleaning operations of the operation (220) may include etching, ashing, wet cleaning operations, or a combination thereof.

[0040] In at least one embodiment, the cleaning operations of the operation (220) may include a plasma etching process. In one exemplary embodiment, the process pressure within the processing chamber (100) is controlled to about 10 mTorr to about 5000 mTorr, e.g., about 10 mTorr to about 400 mTorr, e.g., about 200 mTorr. RF bias power at a frequency of about 13 MHz may be applied to maintain plasma within the processing gas mixture (e.g., a hydrogen-containing gas such as diatomic hydrogen). For example, RF bias power of less than 100 watts, e.g., about 5 watts to about 50 watts, may be applied to maintain plasma inside the processing chamber (100). The processing gas mixture may be flowed into the chamber at a rate of about 100 sccm to about 800 sccm. The interconnect structure (300A) is maintained at a temperature of about 25°C to about 300°C, for example, about 50°C to about 140°C, for example, about 50°C to about 130°C, for example, about 110°C to about 125°C. The interconnect structure (300A) may undergo cleaning operations of operation (220) for about 5 seconds to about 300 seconds, for example, about 30 seconds to about 90 seconds.

[0041] In operation (230), the interconnect structure (300B) undergoes a post-processing process, and in the post-processing process, the low-k film (302b) of the interconnect structure (300B) is restored. In this way, the k value of the low-k film (302c) of the interconnect structure (300C) is reduced compared to the k value of the low-k film (302b). Additionally, as a result of the restored chemical structure of the low-k film (302c), the hydrophobicity of the low-k film (302c) is increased compared to the hydrophobicity of the low-k film (302b). Operation (230) may be performed in the same chamber as operation (220) or in a different chamber. As illustrated in FIG. 4c, the low-k film (302c) has fewer or no Si-OH bonds and a larger proportion of Si-CH3 bonds than the low-k film (302a) and / or low-k film (302b) illustrated in FIG. 3a and 3b, respectively. In conventional recovery processes, low-k films that have undergone a dielectric constant recovery process exhibit hydrophobic surface properties that are unfavorable to subsequent atomic layer deposition processes. However, aspects of the present disclosure result in more favorable (e.g., less hydrophobic) surface properties.

[0042] In some embodiments, the operation (230) may include exposing the low-k film (302b) of the interconnect structure (300B) to a recovery precursor, an ultraviolet (UV) light source, or a combination thereof. In some embodiments, the operation (230) includes the removal of Si-OH bonds of the low-k film (302b) and the formation of Si-O-Si bonds of the low-k film (302c). Without being bound by theory, these chemical reactions may be carried out via reaction schemes (1) and (2) illustrated below. The chemical reactions of reaction schemes (1) and (2) exemplify the removal of Si-OH bonds and the formation of Si-CH3 bonds when the low-k film (302b) is exposed to a recovery precursor.

[0043] In some embodiments, the operation (230) may also be performed using UV light, for example, the interconnect structure (300B) may be exposed to UV light during the operation (230).

[0044] In operation (240), and as illustrated in FIG. 3c and FIG. 3d, the interconnect structure (300C) undergoes a liner deposition process, and in the liner deposition process, a liner layer (316) is placed on the surface of the interconnect structure (300C), which includes at least the surface of the low-k film (302c) and / or the copper layer (310), to form the interconnect structure (300D). The liner layer (316) of the interconnect structure (300D) may be deposited by any suitable deposition method, such as atomic layer deposition (ALD), chemical vapor deposition (CVD), high pressure CVD (HPCVD), high density plasma CVD, remote plasma CVD, microwave assisted CVD, NBECVD, or plasma enhanced atomic layer deposition (PEALD) — wherein the terms ALD, CVD, HPCVD, NBECVD, and PEALD refer to the sequential introduction of reactants or precursors to deposit a layer on a substrate structure — or by any other suitable deposition process. In at least one embodiment, the liner layer (316) of the interconnect structure (300D) is a metal liner, such as TaN and / or HfO2, deposited by an ALD process.

[0045] In some embodiments, the operation (240) includes depositing a liner layer (316) on an interconnect structure (300C) via an ALD process. The ALD process may be performed in a process chamber such as the process chamber (100) shown in FIG. 1. In at least one embodiment, the ALD process includes exposing the interconnect structure (300C) to a metal precursor and a reactant (e.g., alcohol and / or ammonia gas) to form a metal layer on the interconnect structure (300C). The metal precursor may include one or more of aluminum, hafnium, zirconium, nickel, zinc, tantalum, or titanium. The metal precursor may also include a carboligand, an aminoligand, a halide ligand, or a combination thereof.

[0046] During the ALD process, the temperature of the interconnect structure (300C) may be any suitable temperature depending on, for example, the precursor(s) used. During processing, the interconnect structure (300C) may be heated or cooled. Such heating or cooling may be achieved by any suitable means. In some embodiments, the interconnect structure (300C) is maintained at a temperature of about 25°C or higher, or about 50°C or higher, or about 100°C or higher, or about 150°C or higher, or about 200°C or higher, or about 250°C or higher, or about 300°C or higher, or about 350°C or higher, or about 400°C or higher, or about 450°C or higher, or about 500°C or higher. In some embodiments, the temperature of the interconnect structure (300C) is maintained at about 600°C or less, or about 550°C or less, or about 500°C or less, or about 450°C or less, or about 400°C or less, or about 350°C or less, or about 300°C or less, or about 250°C or less, or about 200°C or less, or about 150°C or less, or about 100°C or less, or about 50°C or less, or about 25°C or less. In some embodiments, the temperature of the interconnect structure (300C) is maintained at about 350°C.

[0047] A metal precursor and a reactant may be provided to a processing chamber. The flow rate of the metal precursor and the reactant may be any suitable flow rate, such as about 1 sccm to about 5000 sccm, such as about 200 sccm to about 4000 sccm, such as about 300 sccm to about 3000 sccm, and such as about 500 sccm to about 2000 sccm. The metal precursor and the reactant may be provided at any suitable pressure, such as about 5 mTorr to about 25 Torr, such as about 100 mTorr to about 20 Torr, such as about 5 Torr to about 20 Torr, such as about 50 mTorr to about 2000 mTorr, such as about 100 mTorr to about 1000 mTorr, and such as about 200 mTorr to about 500 mTorr.

[0048] The time period during which the interconnect structure (300C) is exposed to the metal precursor and reactant may be any suitable amount of time required to allow a suitable nucleation layer to form on the surface of the interconnect structure (300C). The interconnect structure (300C) may be exposed to the metal precursor and reactant for about 0.1 seconds to about 90 seconds, e.g., about 0.5 seconds to about 60 seconds, e.g., about 1 second to about 30 seconds, e.g., about 2 seconds to about 25 seconds, e.g., about 3 seconds to about 20 seconds, e.g., about 4 seconds to about 15 seconds, e.g., about 5 seconds to about 10 seconds.

[0049] In some embodiments, an inert gas may be additionally supplied to the process chamber simultaneously with the metal precursor and the reactant. The inert gas may be flowed into the process chamber at a constant flow rate of about 1 sccm to about 10,000 sccm. The inert gas may be any inert gas, such as argon, helium, neon, combinations thereof, or similar.

[0050] In some embodiments, the process chamber is maintained at a pressure of about 0.2 Torr to about 100 Torr throughout the ALD process, e.g., about 0.3 Torr to about 90 Torr, e.g., about 0.5 Torr to about 80 Torr, e.g., about 1 Torr to about 50 Torr. During deposition, the processing chamber pressure may be about 50 mTorr to 750 Torr, e.g., about 100 mTorr to about 400 Torr, e.g., about 1 Torr to about 100 Torr, e.g., about 2 Torr to about 10 Torr.

[0051] In some embodiments, the resulting liner layer (316) of the interconnect structure (300D) has a thickness of about 1200 Å to about 1300 Å, e.g., about 1225 Å to about 1275 Å, e.g., about 1240 Å to about 1260 Å, alternatively about 1200 Å to about 1225 Å, alternatively about 1225 Å to about 1240 Å, alternatively about 1260 Å to about 1275 Å, alternatively about 1275 Å to about 1300 Å.

[0052] FIG. 5 is a schematic block diagram of a substrate processing method (500) according to one or more embodiments. Similar to method (200), in operation (210), a substrate, such as a wafer having an interconnect structure (300A) shown in FIG. 3a, is transferred into a process chamber. The process chamber may be a deposition process chamber, such as the process chamber (100) shown in FIG. 1. In operation (210), the interconnect structure (300A) is a post-deposition interconnect structure. That is, the interconnect structure (300A) includes a low-k film deposited thereon prior to operation (210). In operation (220), the interconnect structure (300A) is cleaned in the process chamber (100). As previously discussed, the cleaning operations of operation (220) can damage the chemical composition of the low-k film (302a) of the interconnect structure (300A), thereby causing an increase in hydrophilicity and k values ​​of the low-k film (302b) of the interconnect structure (300B).

[0053] In operation (510), the interconnect structure (300B) undergoes a post-processing process, in which the raw-k film (302b) of the interconnect structure (300B) is restored through exposure to a recovery precursor, and as a result, a raw-k film (302c) of the interconnect structure (300C) is produced. The recovery precursor may be an aminosilane. For example, the recovery precursor may include a molecule selected from Group 1. In Group 1, each R may be independently selected from methyl, ethyl, isopropyl, tert-butyl, and H. Each R' may be independently selected from alkanes, alkenes, and alkynes. Each R' may independently include 1 to 20 carbon atoms, e.g., 2 to 10 carbon atoms, e.g., 3 to 5 carbon atoms.

[0054] In one or more embodiments, the recovery precursor may be one or more of the molecules shown in the examples of Group 1 below.

[0055] In some embodiments, the recovery precursor may comprise an oxysilane, such as an oxysilane selected from Group 2. In Group 2, each R may be independently selected from methyl, ethyl, isopropyl, and tert-butyl. Each R' may be independently selected from alkyl, cycloalkyl, alkynyl, and aryl. Each R' may independently comprise 1 to 20 carbon atoms, such as 2 to 10 carbon atoms, and such as 3 to 5 carbon atoms.

[0056] In certain embodiments, the recovery precursor may comprise a halosilane, such as a halosilane selected from Group 3. In Group 3, each X may independently be Cl, Br, or I. Each R' may independently be selected from alkyl, cycloalkyl, alkynyl, and aryl. Each R' may independently comprise 1 to 20 carbon atoms, such as 2 to 10 carbon atoms, such as 3 to 5 carbon atoms.

[0057] In certain embodiments, the recovery precursor may comprise an acetylsilane, such as an acetylsilane of Group 4. In Group 4, each R' may be independently selected from alkyl, cycloalkyl, alkynyl, and aryl. Each R may be an alkyl. Each R' may comprise 1 to 20 carbon atoms, such as 2 to 10 carbon atoms, such as 3 to 5 carbon atoms.

[0058] In certain embodiments, the recovery precursor may comprise an ester, e.g., an ester selected from Group 5. In Group 5, each R and R' may be independently selected from hydrogen, alkyl, cycloalkyl, alkynyl, and aryl. In embodiments where R and / or R' contain carbon atoms, each R and R' may independently comprise 1 to 20 carbon atoms, e.g., 2 to 10 carbon atoms, e.g., 3 to 5 carbon atoms.

[0059] In certain embodiments, the recovery precursor may comprise a molecule selected from Group 6. In Group 6, each R, R', and R'' may be independently selected from hydrogen, alkanes, alkenes, alkynes, and aryls. In embodiments where R, R', and / or R'' contain carbon, R, R', and R'' may comprise 1 to 20 carbon atoms, e.g., 2 to 10 carbon atoms, e.g., 3 to 5 carbon atoms.

[0060] In some embodiments, the operation (510) may be performed in a processing chamber such as the process chamber (100) shown in FIG. 1. In some embodiments, the recovery precursor may be introduced into the processing chamber using a precursor gas flow rate of about 100 mg / min (mgm) to about 2000 mgm, e.g., about 250 mgm to about 1500 mgm, e.g., about 500 mgm to about 1000 mgm, alternatively about 100 mgm to about 250 mgm, alternatively about 250 mgm to about 500 mgm, alternatively about 1000 mgm to about 1500 mgm, alternatively about 1500 mgm to about 2000 mgm. In some embodiments, the recovery precursor may be introduced into the processing chamber with a carrier gas, e.g., He, Ar, N2, and combinations thereof. The carrier gas can be introduced into the processing chamber using a gas flow rate of about 1,000 standard cubic centimeters / min (sccm) to about 5,000 sccm, for example, about 2,000 sccm to about 4,000 sccm, for example, about 2,500 sccm to about 3,500 sccm, alternatively about 1,000 sccm to about 2,000 sccm, alternatively about 2,000 sccm to about 2,500 sccm, alternatively about 3,500 sccm to about 4,000 sccm, alternatively about 4,000 to about 5,000 sccm.

[0061] In one or more embodiments, the pressure in the process chamber during operation (510) may be about 3 Torr to about 100 Torr, e.g., about 10 Torr to about 50 Torr, e.g., about 25 Torr to about 35 Torr, alternatively about 3 Torr to about 10 Torr, alternatively about 10 Torr to about 25 Torr, alternatively about 35 Torr to about 50 Torr, alternatively about 50 Torr to about 100 Torr. In one or more embodiments, the temperature inside the processing chamber during operation (510) may be about 75°C to about 500°C, e.g., about 150°C to about 400°C, e.g., about 250°C to about 350°C, alternatively about 75°C to about 150°C, alternatively about 150°C to about 250°C, alternatively about 350°C to about 400°C, alternatively about 400°C to about 500°C. In one or more embodiments, the substrate may be exposed to the recovery precursor for about 1 minute to about 10 minutes, e.g., about 2.5 minutes to about 7.5 minutes, e.g., about 4 minutes to about 6 minutes, alternatively about 1 minute to about 2.5 minutes, alternatively about 2.5 minutes to about 4 minutes, alternatively about 6 minutes to about 7.5 minutes, alternatively about 7.5 minutes to about 10 minutes.

[0062] When the low-k film (302b) is recovered through exposure to a recovery precursor, the method (500) further comprises an operation (240), in which the interconnect structure (300C) undergoes a liner deposition process, and in the liner deposition process, a liner layer (316) is disposed on the surface of the interconnect structure (300C), which includes at least the surface of the low-k film (302c) and / or the copper layer (310), to form an interconnect structure (300D). In at least one embodiment, the liner layer (316) of the interconnect structure (300D) is a metal liner deposited by an ALD process.

[0063] FIG. 6 is a schematic block diagram of a substrate processing method (600) according to one or more embodiments. Similar to method (200), in operation (210), a substrate such as the interconnect structure (300A) shown in FIG. 3a is transferred into a process chamber. The process chamber may be a deposition process chamber such as the process chamber (100) shown in FIG. 1. In operation (210), the interconnect structure (300A) is a post-deposited interconnect structure. That is, the interconnect structure (300A) includes a low-k film deposited thereon prior to operation (210). In operation (220), the interconnect structure (300A) is cleaned in the process chamber (100). As previously discussed, the cleaning operations of operation (220) can damage the low-k film (302a) of the interconnect structure (300A), resulting in increased hydrophilicity and an increased k value of the low-k film (302b) of the interconnect structure (300B). In operation (610), the interconnect structure (300B) undergoes a post-processing process, in which the low-k film (302b) of the interconnect structure (300B) is restored through simultaneous exposure to a recovery precursor and a UV light source (e.g., UV-assisted silylation reaction).

[0064] In some embodiments, the operation (610) may be performed in a processing chamber such as the process chamber (100) shown in FIG. 1. In some embodiments, the recovery precursor may be introduced into the processing chamber using a precursor gas flow rate of about 100 mgm to about 2000 mgm, e.g., about 250 mgm to about 1500 mgm, e.g., about 500 mgm to about 1000 mgm, alternatively about 100 mgm to about 250 mgm, alternatively about 250 mgm to about 500 mgm, alternatively about 1000 mgm to about 1500 mgm, alternatively about 1500 mgm to about 2000 mgm. In some embodiments, the recovery precursor may be introduced into the processing chamber with a carrier gas, e.g., He, Ar, N2, and combinations thereof. The carrier gas can be introduced into the processing chamber using a gas flow rate of about 1000 sccm to about 5000 sccm, for example, about 2000 sccm to about 4000 sccm, for example, about 2500 sccm to about 3500 sccm, alternatively about 1000 sccm to about 2000 sccm, alternatively about 2000 sccm to about 2500 sccm, alternatively about 3500 sccm to about 4000 sccm, or alternatively about 4000 to about 5000 sccm.

[0065] In one or more embodiments, the pressure in the process chamber during operation (610) may be about 3 Torr to about 100 Torr, e.g., about 10 Torr to about 50 Torr, e.g., about 25 Torr to about 35 Torr, alternatively about 3 Torr to about 10 Torr, alternatively about 10 Torr to about 25 Torr, alternatively about 35 Torr to about 50 Torr, alternatively about 50 Torr to about 100 Torr. In one or more embodiments, the temperature inside the processing chamber during operation (610) may be about 75°C to about 500°C, e.g., about 150°C to about 400°C, e.g., about 250°C to about 350°C, alternatively about 75°C to about 150°C, alternatively about 150°C to about 250°C, alternatively about 350°C to about 400°C, alternatively about 400°C to about 500°C. In one or more embodiments, the substrate may be exposed to the recovery precursor for about 1 minute to about 10 minutes, e.g., about 2.5 minutes to about 7.5 minutes, e.g., about 4 minutes to about 6 minutes, alternatively about 1 minute to about 2.5 minutes, alternatively about 2.5 minutes to about 4 minutes, alternatively about 6 minutes to about 7.5 minutes, alternatively about 7.5 minutes to about 10 minutes.

[0066] In one or more embodiments, the interconnect structure (300B) may be simultaneously exposed to a UV light source for a portion of the time during which the substrate is exposed to the recovery precursor in operation (610). In at least one embodiment, the interconnect structure (300B) may be simultaneously exposed to a UV light source for the entire time during which the substrate is exposed to the recovery precursor. In one or more embodiments, the interconnect structure (300B) may be exposed to a UV light source of about 600 W / in during operation (610), such as about 400 W / in to about 800 W / in, such as about 500 W / in to about 700 W / in, alternatively about 400 W / in to about 500 W / in, alternatively about 500 W / in to about 600 W / in, alternatively about 600 W / in to about 700 W / in, alternatively about 700 W / in to about 800 W / in.

[0067] When the low-k film (302b) of the interconnect structure (300B) is recovered through simultaneous exposure to a recovery precursor and a UV light source to form the low-k film (302c) of the interconnect structure (300C), the method (600) further comprises an operation (240), in which the interconnect structure (300C) undergoes a liner deposition process, wherein in the liner deposition process, a liner layer (316) is disposed on the surface of the interconnect structure (300C), which includes at least the surface of the low-k film (302c) and / or the copper layer (310), to form the interconnect structure (300D). In at least one embodiment, the liner layer (316) of the interconnect structure (300D) is a metal liner deposited by an ALD process.

[0068] FIG. 7 is a schematic block diagram of a substrate processing method (700) according to one or more embodiments. Similar to the method (200) of FIG. 2, in operation (210) of FIG. 7, a substrate such as the interconnect structure (300A) shown in FIG. 3a is transferred into a process chamber. The process chamber may be a deposition process chamber such as the process chamber (100) shown in FIG. 1. In operation (210), the interconnect structure (300A) is a post-deposited interconnect structure. That is, the interconnect structure (300A) includes a low-k film deposited thereon prior to operation (210). In operation (220), the interconnect structure (300A) is cleaned in the process chamber (100). As previously discussed, the cleaning operations of operation (220) can damage the low-k film (302a) of the interconnect structure (300A), resulting in increased hydrophilicity and k values ​​of the low-k film (302b) of the interconnect structure (300B). In operation (510), the low-k film (302b) of the interconnect structure (300B) is restored through exposure to a recovery precursor.

[0069] In operation (710), the interconnect structure (300B) subsequently undergoes additional UV treatment through exposure to a UV light source. In some embodiments, operation (710) may be performed in a processing chamber such as the process chamber (100) shown in FIG. 1. In one or more embodiments, the interconnect structure (300B) may be exposed during operation (710) to a UV light source of about 600 W / in, e.g., about 400 W / in to about 800 W / in, e.g., about 500 W / in to about 700 W / in, alternatively about 400 W / in to about 500 W / in, alternatively about 500 W / in to about 600 W / in, alternatively about 600 W / in to about 700 W / in, alternatively about 700 W / in to about 800 W / in. In one or more embodiments, the interconnect structure (300B) may be exposed to a UV light source for about 1 second (s) to about 60 minutes (min) during operation (710), such as about 1 s to about 30 minutes, such as about 1 s to about 10 minutes.

[0070] In one or more embodiments, the pressure in the process chamber during operation (710) may be about 3 Torr to about 100 Torr, e.g., about 10 Torr to about 50 Torr, e.g., about 25 Torr to about 35 Torr, alternatively about 3 Torr to about 10 Torr, alternatively about 10 Torr to about 25 Torr, alternatively about 35 Torr to about 50 Torr, alternatively about 50 Torr to about 100 Torr. In one or more embodiments, the temperature inside the processing chamber during operation (710) may be about 75°C to about 500°C, e.g., about 150°C to about 400°C, e.g., about 250°C to about 350°C, alternatively about 75°C to about 150°C, alternatively about 150°C to about 250°C, alternatively about 350°C to about 400°C, alternatively about 400°C to about 500°C. In one or more embodiments, the substrate may be exposed to the recovery precursor for about 1 minute to about 10 minutes, e.g., about 2.5 minutes to about 7.5 minutes, e.g., about 4 minutes to about 6 minutes, alternatively about 1 minute to about 2.5 minutes, alternatively about 2.5 minutes to about 4 minutes, alternatively about 6 minutes to about 7.5 minutes, alternatively about 7.5 minutes to about 10 minutes.

[0071] In operation (240), the interconnect structure (300C) undergoes a liner deposition process, and in the liner deposition process, a liner layer (316) is disposed on the surface of the interconnect structure (300C), which includes at least the surface of the low-k film (302c) and / or the copper layer (310), to form the interconnect structure (300D). In at least one embodiment, the liner layer (316) of the interconnect structure (300D) is a metal liner deposited by an ALD process.

[0072] FIG. 8 is a schematic block diagram of a substrate processing method (800) according to one or more embodiments. Similar to the method (200) of FIG. 2, in operation (210) of FIG. 8, a substrate such as the interconnect structure (300A) shown in FIG. 3a is transferred into a process chamber. The process chamber may be a deposition process chamber such as the process chamber (100) shown in FIG. 1. In operation (210), the interconnect structure (300A) is a post-deposition interconnect structure. That is, the interconnect structure (300A) includes a low-k film deposited thereon prior to operation (210). In operation (220), the interconnect structure (300A) is cleaned in the process chamber (100). As previously discussed, the cleaning operations of operation (220) can damage the low-k film (302a) of the interconnect structure (300A), resulting in increased hydrophilicity and k values ​​of the low-k film (302b) of the interconnect structure (300B). In operation (710), the low-k film (302b) undergoes UV treatment through exposure to a UV light source. In operation (510), the low-k film (302b) of the interconnect structure (300B) is restored through exposure to a recovery precursor to form the low-k film (302c) of the interconnect structure (300C). In operation (240), the interconnect structure (300C) undergoes a liner deposition process, and in the liner deposition process, a liner layer (316) is disposed on the surface of the interconnect structure (300C), which includes at least the surface of the low-k film (302c) and / or the copper layer (310), to form the interconnect structure (300D). In at least one embodiment, the liner layer (316) of the interconnect structure (300D) is a metal liner deposited by an ALD process on the low-k film (302d).

[0073] In some embodiments, at least one of the low-k films (302a - 302d) of one of the interconnect structures (300A - 300D) manufactured through any of the processes disclosed herein may have a k value of about 2.65 to about 3.0, e.g., about 2.67 to about 2.8, e.g., about 2.68 to about 2.76, alternatively about 2.65 to about 2.67, alternatively about 2.67 to about 2.68, alternatively about 2.76 to about 2.8, alternatively about 2.8 to about 3.0. In some embodiments, at least one of the low-k films (302a - 302d) of one of the interconnect structures (300A - 300D) manufactured through any of the processes disclosed herein may have a thickness of about 1200 Å to about 1300 Å, e.g., about 1225 Å to about 1275 Å, e.g., about 1240 Å to about 1260 Å, alternatively about 1200 Å to about 1225 Å, alternatively about 1225 Å to about 1240 Å, alternatively about 1260 Å to about 1275 Å, alternatively about 1275 Å to about 1300 Å. In some embodiments, at least one of the low-k films (302a - 302c) of one of the interconnect structures (300A - 300C) manufactured through any of the processes disclosed herein may have a water contact angle of about 65° to about 85°, e.g., about 70° to about 80°, e.g., about 75° to about 80°, e.g., about 77.5° to about 79.5°, alternatively about 65° to about 70°, alternatively about 70° to about 75°, alternatively about 75° to about 77.5°, alternatively about 79.5° to about 80°, alternatively about 80° to about 85°.

[0074] The substrate preparation processes and conditions disclosed herein allow for the recovery of low-k values ​​and hydrophobic properties, which may have resulted from various processing procedures and / or variables. Additionally, these processes provide the capability for the deposition of additional liner layers, such as ALD metal film deposition. Interestingly, it has been confirmed that the order in which these recovery processes are performed is related to the degree of recovery of these properties and the enablement of ALD metal film deposition.

[0075] Additionally, it has been found that the recovery of hydrophobic properties must be complexly balanced with the recovery of low-k values. While complete recovery of low-k values ​​may be desirable, such recovery must be balanced so that the surface hydrophobicity of the recovered substrate is sufficient to allow for the capability for ALD metal film deposition. The processes disclosed herein incorporate sequential recovery operations that allow for operation control and provide a balanced recovery of low-k values ​​and hydrophilic / hydrophobic properties that is advantageous for subsequent ALD metal film deposition. Examples Example 1

[0076] Samples were prepared according to the methods described herein, wherein the samples comprise a low-k film on an etching stop layer, a metal barrier between the etching stop layer and the copper layer, and a metal barrier between the copper layer and the substrate. Each of the initial samples exhibited a k value of approximately 2.61 and a water contact angle of approximately 105.3° prior to processing. The samples subsequently underwent processing operations including etching, ashing, wet cleaning operations, or combinations thereof. The samples subsequently underwent various recovery processes, such as (1) no recovery, (2) exposure to a recovery precursor, (3) exposure to a UV light source, (4) simultaneous exposure to a recovery precursor and a UV light source, (5) exposure to a UV light source following exposure to a recovery precursor, and (6) exposure to a recovery precursor following exposure to a UV light source. The samples discussed herein are numbered according to the aforementioned recovery processes the samples undergo. The resulting k values ​​were measured according to ASTM F1392. The thickness of the samples was measured according to ASTM F576 both before and after treatment. The resulting water contact angles were also measured according to ASTM D5946. The results are summarized in Table 1. Each k value and water contact angle of each sample was compared with the corresponding values ​​prior to processing to verify characteristic recovery as a function of the implemented recovery process. Table 1: Summary of water contact angle and k recovery values ​​as a function of the recovery process Table 2: Summary of Low-k Film Thickness as a Function of Recovery Process

[0077] As can be confirmed from the analysis in Table 1, recovery treatments in which the sample undergoes some form of exposure to a recovery precursor (e.g., treatments 2 and 4-6) result in an increase in k-value recovery. Additionally, recovery treatments involving exposure to both a recovery precursor and a UV light source (e.g., treatments 4-6) show an increase in both water contact angle and k-value recovery. Without being bound by theory, these recovery phenomena can be understood by the molecular structures in Figures 4a through 4c. For example, the sample before processing can be exemplified by Figure 4a, in which the raw-k film includes Si-O bonds, Si-CH3 bonds, and Si-H bonds. Sample 1 (e.g., the processed sample that has not undergone the recovery process) can be exemplified by Figure 4b, in which the raw-k film includes the formation of a reduced number of Si-CH3 bonds and Si-OH bonds. The formation of Si-OH bonds can increase the hydrophilicity and k value of the low-k film, as indicated by the increased Δk and Δwater contact angle values ​​compared to samples 2-6. Samples 2-6 (e.g., processed samples that have undergone a recovery process) can be exemplified by Fig. 4c, in which the low-k film has a reduced number of Si-OH bonds and an increased number of Si-CH3 bonds compared to sample 1. Thus, the difference in the recovery values ​​of samples 2-6 can be attributed to the relative number of Si-OH and Si-CH3 bonds compared to the sample before processing.

[0078] Additionally, it can be confirmed from Table 2 that recovery treatments involving exposure to a UV light source result in a reduction in film thickness. Without being bound by theory, exposing low-k films to UV light can cause film shrinkage as a result of the intensity of the light source and / or the exposure time to the light source. Example 2

[0079] Figure 9 shows images of samples that have undergone ALD of tantalum nitride (TaN) following processing and various recovery processes. As can be observed, samples 1-2 and samples 5-6 each exhibit moderate to good continuity across the surface of each sample. Without being bound by theory, this finding suggests that the surface hydrophobic / hydrophilic properties of these samples are suitable for ALD of metal films. In contrast, the unprocessed sample and sample 4 do not exhibit the same uniformity as samples 1-2 and samples 5-6. As previously discussed, the hydrophilic / hydrophobic properties of the sample surface must be sufficient to facilitate favorable subsequent ALD metal film deposition. Additionally, surface homogeneity in hydrophilic / hydrophobic properties is desired to enable smooth ALD nucleation.

[0080] The recovery process of Sample 4 promotes a significant recovery of low-k values, while also greatly promoting the recovery of surface hydrophobicity to the extent that subsequent ALD metal film deposition is inhibited. As previously discussed, the recovery of hydrophobic properties can be balanced with the recovery of low-k values ​​to enable subsequent ALD metal film deposition. Interestingly, Samples 5–6 exhibit good continuity across the surface of each sample when undergoing ALD of TaN, suggesting that the surface hydrophobic / hydrophilic properties of these samples are suitable for ALD of metal films. Furthermore, Samples 5–6 exhibit a significant recovery of surface hydrophobic properties and k values, as demonstrated in Table 1. Accordingly, sequential recovery processes of samples 5-6 (e.g., (5) exposure to a recovery precursor followed by exposure to a UV light source and (6) exposure to a UV light source followed by exposure to a recovery precursor) were found to appropriately balance the recovery of low-k values ​​and hydrophilic / hydrophobic properties, so that the surface of the resulting films is favorable for subsequent ALD metal film deposition.

[0081] Overall, the present disclosure provides methods for recovering the properties of damaged low-k films. The processes disclosed herein generally include processing operations that can damage the molecular structure of the low-k film to cause an increase in k-values ​​and hydrophilicity. As discussed herein, the sequential recovery processes implemented herein (e.g., exposure to a recovery precursor followed by exposure to a UV light source, or exposure to a UV light source followed by exposure to a recovery precursor) enable a high degree of property recovery. Additionally, the sequential recovery processes disclosed herein provide a balance between the recovery of low-k values ​​and the recovery of hydrophilic / hydrophobic properties so that the surface of the resulting films is favorable for subsequent ALD metal film deposition.

[0082] For the purposes of this disclosure, and unless otherwise specified, the terms “alkyl” or “alkyl group” refer interchangeably to a hydrocarbyl group composed of carbon and hydrogen atoms. The alkyl group may be substituted or unsubstituted and may be linear, branched, or cyclic.

[0083] For the purposes of this disclosure, and unless otherwise specified, the terms “cycloalkyl” or “cycloalkyl group” refer interchangeably to hydrocarbyl groups in which carbon atoms form one or more ring structures.

[0084] For the purposes of this disclosure, and unless otherwise specified, the terms “alkenyl” or “alkenyl group” refer interchangeably to a linear unsaturated hydrocarbyl group containing a C=C bond therein.

[0085] For the purposes of this disclosure, and unless otherwise specified, the terms “aryl” or “aryl group” refer interchangeably to a hydrocarbyl group containing an aromatic ring structure.

[0086] Although the foregoing relates to embodiments of the present disclosure, other and additional embodiments of the disclosure may be devised without departing from the basic scope of the present disclosure, and the scope of the present disclosure is determined by the following claims.

Claims

Claim 1 As a method, the step of positioning a substrate within a processing chamber ― said substrate comprises a first low-k film having a first water contact angle, said first low-k film is disposed on an interconnect structure ―; the step of cleaning the substrate within the processing chamber to form a cleaned substrate ― said cleaned substrate comprises a damaged low-k film having a second water contact angle, said damaged low-k film is generated from said first low-k film ―; the step of exposing the cleaned substrate to a recovery precursor to form a recovered substrate ― said recovered substrate comprises a recovered low-k film, said recovered low-k film is generated from said damaged low-k film ―; the step of exposing the recovered substrate to a UV light source to form a processed substrate ― said processed substrate comprises a processed low-k film having a third water contact angle, said processed low-k film is generated from said recovered low-k film ―; A method comprising the step of depositing a liner layer on the processed substrate through atomic layer deposition (ALD). Claim 2 In claim 1, the first low-k film and the damaged low-k film each independently have a k value, and the k value of the first low-k film is smaller than the k value of the damaged low-k film. Claim 3 A method according to claim 1, wherein each of the damaged low-k film and the treated low-k film independently includes a k value, and the k value of the damaged low-k film is greater than the k value of the treated low-k film. Claim 4 A method according to claim 1, wherein each of the first low-k film and the processed low-k film independently includes a k value, and the k value of the first low-k film is smaller than the k value of the processed low-k film. Claim 5 In claim 1, the method wherein the first water contact angle is greater than the second water contact angle. Claim 6 In claim 1, the method wherein the second water contact angle is smaller than the third water contact angle. Claim 7 In claim 1, the first water contact angle is greater than the second water contact angle, and the second water contact angle is smaller than the third water contact angle. Claim 8 In claim 1, each of the first low-k film, the damaged low-k film, and the treated low-k film independently includes a k value, wherein The k value of the first low-k film is smaller than the k value of the damaged low-k film; A method in which the k value of the damaged raw-k film is greater than the k value of the processed raw-k film. Claim 9 The method of claim 1, wherein the step of exposing the cleaned substrate to a recovery precursor to form a recovered substrate comprises: introducing the recovery precursor into the processing chamber using a precursor gas flow rate of about 100 milligrams / min (mgm) to about 2000 mgm; introducing a carrier gas into the processing chamber using a gas flow rate of about 1000 standard cubic centimeters / min (sccm) to about 5000 sccm; and maintaining a pressure of about 3 Torr to about 100 Torr and a temperature of about 75°C to about 500°C within the processing chamber. Claim 10 A method according to claim 1, wherein the UV light source comprises an intensity of about 400 W / in to about 800 W / in. Claim 11 As a method, the step of positioning a substrate within a processing chamber ― said substrate comprises a first low-k film having a first water contact angle, said first low-k film is disposed on an interconnect structure ―; the step of cleaning the substrate within the processing chamber to form a cleaned substrate ― said cleaned substrate comprises a damaged low-k film having a second water contact angle, said damaged low-k film is generated from said first low-k film ―; the step of exposing the cleaned substrate to a UV light source to form a processed substrate ― said processed substrate comprises a processed low-k film having a third water contact angle, said processed low-k film is generated from said damaged low-k film ―; the step of exposing the processed substrate to a recovery precursor to form a recovered substrate ― said recovered substrate comprises a recovered low-k film, said recovered low-k film is generated from said processed low-k film ―; A method comprising the step of depositing a liner layer on the recovered substrate via atomic layer deposition (ALD). Claim 12 In claim 11, the first low-k film and the damaged low-k film each independently have a k value, and the k value of the first low-k film is smaller than the k value of the damaged film, method. Claim 13 In claim 11, the damaged low-k film and the recovered low-k film each independently have a k value, and the k value of the damaged low-k film is greater than the k value of the recovered low-k film, method. Claim 14 In claim 11, the first low-k film and the recovered low-k film each independently include a k value, and the k value of the first low-k film is smaller than the k value of the recovered low-k film. Claim 15 In paragraph 11, the method wherein the first water contact angle is greater than the second water contact angle. Claim 16 In paragraph 11, the method wherein the second water contact angle is smaller than the third water contact angle. Claim 17 In claim 11, the first water contact angle is greater than the second water contact angle, and the second water contact angle is smaller than the third water contact angle. Claim 18 In claim 11, the first low-k film, the damaged low-k film, and the recovered low-k film each independently include a k value, wherein The k value of the first low-k film is smaller than the k value of the damaged low-k film; A method in which the k value of the damaged low-k film is greater than the k value of the recovered low-k film. Claim 19 In claim 11, the method wherein the UV light source comprises an intensity of about 400 W / in to about 800 W / in. Claim 20 As a method, the step of positioning a substrate within a processing chamber ― said substrate comprises a first low-k film having a first water contact angle, said first low-k film is disposed on an interconnect structure ―; the step of cleaning the substrate within the processing chamber to form a cleaned substrate ― said cleaned substrate comprises a damaged low-k film having a second water contact angle, said damaged low-k film is generated from said first low-k film ―; the step of exposing the cleaned substrate to a recovery precursor to form a recovered substrate ― said recovered substrate comprises a recovered low-k film, said recovered low-k film is generated from said damaged low-k film ―; the step of exposing the recovered substrate to a UV light source to form a processed substrate ― said processed substrate comprises a processed low-k film having a third water contact angle, said processed low-k film is generated from said recovered low-k film ―; A method comprising the step of depositing a liner layer on the processed substrate by atomic layer deposition (ALD), wherein the first water contact angle is greater than the second water contact angle and the second water contact angle is smaller than the third water contact angle.