Method and System for Manufacturing Defect-Free Carbon Thin Films for Electrostatic Chucks

By employing two FCVA devices with angled carbon plasma beams and rotating the electrostatic chuck, a defect-free, hydrogen-free carbon thin film is formed, enhancing durability and heat resistance, overcoming the limitations of conventional DLC coatings.

KR103043745B1Active Publication Date: 2026-11-06박창하 +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
KR1020260026286
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-02-10
Publication Date
2026-11-06
Estimated Expiration
2046-02-10

AI Technical Summary

Technical Problem

Existing DLC thin films on electrostatic chucks used in semiconductor manufacturing face issues with adhesion, delamination, cracking, and non-uniform thickness, leading to reduced durability and heat resistance, especially in high-temperature and high-load environments.

Method used

A method using two FCVA devices with obliquely oriented carbon plasma beam exits to form a defect-free, hydrogen-free carbon thin film of uniform thickness on the electrostatic chuck by rotating the chuck during the coating process, ensuring the beams reach different regions at angled orientations.

Benefits of technology

The method results in an electrostatic chuck with enhanced durability and heat resistance, featuring ultra-high hardness (30 GPa or more) and uniform film thickness, addressing the limitations of conventional DLC coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112026017313568-PAT00002_ABST
    Figure 112026017313568-PAT00002_ABST
Patent Text Reader

Abstract

The objective of the present invention is to provide a new coating method and coating apparatus capable of stably forming a defect-free carbon thin film, thereby overcoming the limitations of existing DLC ​​coating technology to further improve the durability and heat resistance of an electrostatic chuck. In accordance with the above purpose, the present invention provides a method for forming a defect-free carbon thin film on the surface of an electrostatic chuck by configuring two or more FCVA devices and arranging the directions of the carbon plasma beam exits of the FCVA devices so as to be oblique to each other, thereby forming different angles of carbon plasma beams radiated onto the surface of the electrostatic chuck, and coating a defect-free hydrogen-free carbon thin film with a uniform thickness over the entire surface of the electrostatic chuck.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a coating technology for improving the durability and heat resistance of an electrostatic chuck, and more specifically, to a method and apparatus for enabling stable chucking and de-chucking even in high-temperature and high-load environments occurring in semiconductor manufacturing processes by coating a defect-less carbon thin film on an electrostatic chuck. Background Technology

[0002] Electrostatic chucks used in semiconductor manufacturing processes are critical components that secure wafers using electrostatic force; they require high durability and heat resistance in high-temperature plasma environments and during repetitive chucking and de-chucking operations. In particular, as multilayer thin films form on the wafer surface, process temperatures rise and wafer warpage intensifies, leading to frequent reports of surface damage and particle generation issues on the electrostatic chuck. To address these problems, a technology has conventionally been proposed to reduce friction and ensure heat resistance by coating the electrostatic chuck surface with a Diamond-Like Carbon (DLC) thin film. The commonly used DLC thin film is a hydrogen-containing (aC:H) film, which is an amorphous hydrogen-containing film with a hardness of approximately 15 to 20 GPa and exhibits insulating properties. Furthermore, DLC films have weak adhesion to metal bases, leading to issues such as delamination or cracking. The relatively high resistance of DLC films results in prolonged chucking and de-chucking times, posing a risk of wafer misalignment or breakage. For example, Registered Patent No. 10-2809182 (JESCO Co., Ltd.) proposed an electrostatic chuck with a low-resistance and adhesion-enhanced DLC thin film. This technology improves the adhesion of the DLC thin film by forming a multilayer structure of Ti and TiC intermediate layers, and reports the effect of reducing chucking / de-chucking time by lowering the resistance value of the DLC thin film to the level of 1 to 20 Ω. However, the coating film has a hardness of 5 to 10 GPa, which is almost equivalent to the deposition of carbon particles, and there is still a possibility of stress problems occurring during the DLC thin film deposition process and defects occurring within the thin film. In particular, there are limitations in that the stability of the thin film is not sufficiently ensured when used for a long time in a high-temperature and high-voltage environment. The problem to be solved

[0003] Therefore, the objective of the present invention is to overcome the limitations of existing DLC ​​coating technology to further improve the durability and heat resistance of an electrostatic chuck, and to provide a new coating method and coating apparatus capable of stably forming a defect-free carbon thin film.

[0004] In addition, the objective of the present invention is to provide a manufacturing technology for a coating film that can impart conductivity to the deposited coating film while exhibiting high hardness characteristics of 20 to 45 GPa. means of solving the problem

[0005] In accordance with the above objective, the present invention provides a method for forming a defect-free carbon thin film on the surface of an electrostatic chuck by configuring two or more FCVA devices and arranging the directions of the carbon plasma beam exits of the FCVA devices obliquely to each other, thereby forming different angles of carbon plasma beams radiated onto the surface of the electrostatic chuck, and coating the entire surface of the electrostatic chuck with a defect-free hydrogen-free carbon thin film of uniform thickness. Since the exit positions of the carbon plasma beams and the angles of the carbon plasma beams are different and obliquely formed, the carbon plasma beams reaching the surface of the electrostatic chuck are concentrated in the center of the electrostatic chuck, thereby resolving the problem where the thickness of the defect-free carbon thin film is thick at the center and becomes thinner towards the periphery.

[0006] The carbon plasma beam outlet of the above FCVA device is oriented toward the surface of the electrostatic chuck, and the carbon plasma beam outlets of each of the two FCVA devices are arranged so that the carbon plasma beam is emitted at an oblique angle to each other and reaches different points on the electrostatic chuck.

[0007] That is, the present invention is,

[0008] As an electrostatic chuck surface coating system,

[0009] A chamber into which an electrostatic chuck is loaded;

[0010] A first FCVA device and a second FCVA device mounted in the chamber above; and

[0011] Includes a jig for an electrostatic chuck capable of rotating the electrostatic chuck; and

[0012] The above electrostatic chuck is positioned vertically within the chamber, and

[0013] The present invention provides an electrostatic chuck surface coating system characterized in that a first beam outlet, which is a beam outlet of a first FCVA device, and a second beam outlet, which is a beam outlet of a second FCVA device, are oriented toward an electrostatic chuck, and each emits a carbon plasma beam at a different angle so that the carbon plasma beams reach different regions of the electrostatic chuck at oblique angles to each other, and the electrostatic chuck is rotated during the process to uniformly form a hydrogen-free carbon coating film over the entire surface of the electrostatic chuck.

[0014] In the above, the first beam emitted from the first beam exit reaches an area corresponding to 2R / 3 from the center with respect to the radius R of the electrostatic chuck, and the second beam emitted from the second beam exit reaches an area extending from R / 2 to 4R / 3.

[0015] In the above, a linear ion source and a sputter source are further mounted in the chamber, and the linear ion source, the sputter source, the first FCVA device, and the second FCVA device are arranged to surround the electrostatic chuck, and the electrostatic chuck can be oriented to face each process source by means of a jig for the electrostatic chuck.

[0016] In addition, the present invention,

[0017] As a surface coating method for an electrostatic chuck,

[0018] The electrostatic chuck is loaded into the chamber and fixed to a rotatable jig, and

[0019] Vacuum the chamber,

[0020] Plasma etching of the electrostatic chuck surface using a linear ion source and

[0021] A buffer layer is formed using at least one material among Ti, Cr, and W, and

[0022] The present invention provides a method for forming a hydrogen-free carbon thin film using a first FCVA device and a second FCVA device, wherein a first beam emitted from the first FCVA device and a second beam emitted from the second FCVA device are emitted at oblique angles to each other so as to reach different regions of the electrostatic chuck, thereby forming a hydrogen-free carbon thin film of uniform thickness over the entire surface of the electrostatic chuck.

[0023] In the above, the electrostatic chuck is rotated during the coating process, and the first beam emitted from the first FCVA device reaches the 2R / 3 region from the center of the radius R of the electrostatic chuck, and the second beam emitted from the second FCVA device reaches the 4R / 3 region from R / 2 to form a uniform coating on the entire surface.

[0024] In the above, the etching step is characterized by being performed under conditions of power of 1.0 to 1.5 kW, current of 0.1 to 0.3 A, a bias applied to the electrostatic chuck of a negative bias of 10 to 150 V with a high-frequency pulse of 20 to 250 kHz, and an inert gas flow rate of 20 to 50 sccm.

[0025] In the above, the buffer layer forming step is characterized by being performed under conditions of a current of 5 to 8 A, a voltage of 400 to 500 V, a bias applied to the electrostatic chuck of a negative bias of 10 to 150 V with a high-frequency pulse of 20 to 250 kHz, and an inert gas flow rate of 80 to 150 sccm.

[0026] In the above, the hydrogen-free carbon thin film formation step is characterized by being performed under conditions of a current of 50 to 70 A, a voltage of 20 to 40 V, and a negative bias of 10 to 150 V with a bias high-frequency pulse of 20 to 250 kHz applied to the electrostatic chuck.

[0027] In the above, the step of forming a hydrogen-free carbon thin film is performed by selectively injecting nitrogen (N₂) with an inert gas (Ar), and the nitrogen supply is characterized by being controlled in a range of 0 to 30% in terms of flow rate ratio relative to the inert gas. Effects of the invention

[0028] According to the present invention, a defect-free hydrogen-free carbon thin film can be formed on an electrostatic chuck by forming a carbon thin film using an FCVA device. Such a defect-free hydrogen-free carbon thin film provides an electrostatic chuck having strong durability and heat resistance with ultra-high hardness (30 GPa or more).

[0029] In addition, the present invention uses two or more FCVA devices and orients the angles of the carbon plasma beams emitted from them at an angle to each other, thereby preventing the carbon plasma beams of the FCVA devices from being concentrated in a part of the electrostatic chuck, particularly in the central part, so that the thickness of the thin film in the central part is thick and becomes thinner towards the edges.

[0030] That is, the present invention causes the first beam and the second beam of the first FCVA device and the second FCVA device to reach different regions of the electrostatic chuck, and the electrostatic chuck is rotated during the process to form a hydrogen-free carbon thin film of uniform thickness over the entire surface of the electrostatic chuck. Brief explanation of the drawing

[0031] Figure 1 is a schematic cross-sectional diagram illustrating the problem of non-uniformity in surface coating thickness of an electrostatic chuck according to the prior art. FIG. 2 is a cross-sectional view showing the configuration of the coating system of the present invention, the FCVA beam exit array, and the position of the electrostatic chuck, and a schematic diagram explaining the incident positions of the first beam and the second beam on the electrostatic chuck accordingly. FIG. 3 is a schematic planar diagram illustrating the positions where the first beam and the second beam reach the electrostatic chuck surface according to the FCVA beam exit arrangement of the coating system of the present invention. Figure 4 is a graph showing the uniformity of the surface etching rate of an electrostatic chuck according to the present invention. Figure 5 is a graph showing the uniformity of the deposition rate of the buffer layer for the surface position of the electrostatic chuck according to the present invention. Figure 6 is a graph showing the uniformity of the deposition rate of a hydrogen-free carbon coating layer for a surface location of an electrostatic chuck according to the present invention. Figure 7 is a photograph of the coating result showing the difference between non-uniform (no rotation) and uniform (rotation) coating thickness depending on whether the electrostatic chuck rotates during the coating process. Figure 8 is a graph showing the change in hardness of the coating film according to nitrogen supply. Specific details for implementing the invention

[0032] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings.

[0033] The present invention relates to a surface coating for an electrostatic chuck for metal etching, wherein the electrostatic chuck is applied in a vacuum atmosphere at a temperature of 100 to 400°C. The surface of the electrostatic chuck must possess heat resistance and durability to ensure an appropriate service life. Conventional Ti and TiN coating films have poor wear resistance and a short service life.

[0034] DLC thin films formed by PECVD or sputtering are aC:H containing hydrogen and lack heat resistance. Fine pinholes or porosity may form within the coating, leading to problems such as reduced electrical insulation properties and decreased mechanical strength.

[0035] Accordingly, the present invention forms a defect-free hydrogen-free carbon thin film on an electrostatic chuck. The hydrogen-free carbon thin film ta-C (tetrahedral amorphous carbon) contains a high proportion of sp³ bonds (diamond structure) and thus possesses properties similar to diamond. It exhibits excellent durability even in ultra-high hardness and high-load environments at levels of 30 to 80 GPa or 3,000 to 8,000 HV, displays a low coefficient of friction of less than 0.1 under dry conditions, and possesses high-temperature stability with a maximum operating temperature of approximately 400 ℃. It is preferable that such a hydrogen-free carbon coating be performed using an FCVA device.

[0036] Since the FCVA device extracts and filters only carbon ions from the arc plasma, hydrogen is not involved. Accordingly, high-density hydrogen-free carbon thin films such as ta-C can be deposited. Meanwhile, although the FCVA process has the advantage of being able to form hydrogen-free carbon thin films, there is a problem in that it is difficult to form a uniform thin film on a large-area substrate because the deposition area is relatively narrow.

[0037] Figure 1 illustrates the problem of non-uniformity in film thickness when electrostatic chuck surface coating is performed using an FCVA device. When the beam outlets are arranged so that the radiation direction of the carbon plasma beam is perpendicular to the surface of the electrostatic chuck, the carbon plasma beam is concentrated in the central part of the electrostatic chuck, showing a problem where the film thickness is formed thickly in the central part and becomes thinner towards the outer edge.

[0038] To solve this problem, the present invention arranges two FCVA devices as shown in FIG. 2 and arranges the orientations of carbon plasma beams emitted from each beam exit at an angle to each other to make the coating thickness on the electrostatic chuck uniform overall.

[0039] That is, the electrostatic chuck (10) is rotated during the coating process, and the first beam (100), which is a carbon plasma beam emitted from the first FCVA device, and the second beam (110), which is emitted from the second FCVA device, are incident on the electrostatic chuck (10) at different positions to form a coating layer of uniform thickness over the entire surface of the electrostatic chuck. That is, the first beam (100) and the second beam (110) reach the surface of the electrostatic chuck in oblique directions relative to each other to form a coating layer of uniform thickness over the entire surface of the electrostatic chuck.

[0040] FIG. 2 shows a cross-sectional configuration of a coating system equipped with a first FCVA device, a second FCVA device, a sputter source, and a linear ion source. The first beam outlet (200) and the second beam outlet (210) of the first FCVA device and the second FCVA device are positioned to emit carbon plasma beams at different angles toward the electrostatic chuck (10), a sputter source is positioned between the first beam outlet (200) and the second beam outlet (210), and a linear ion source is positioned next to the second beam outlet. The electrostatic chuck (10) is positioned at the center of the chamber wall, and the beam outlets of the first FCVA device, the sputter source, the second FCVA device, and the linear ion source are all oriented toward the electrostatic chuck.

[0041] In particular, the first beam outlet (200) and the second beam outlet (210) of the first and second FVCA devices are arranged to emit carbon plasma beams at different angles toward the electrostatic chuck (10), so that the first beam (100) and the second beam (110) form different regions at the positions where they reach the electrostatic chuck (10) (bottom right of FIG. 2). That is, when the two beams are irradiated onto the round electrostatic chuck (10), they reach different locations (yellow marked areas; 100, 110) as shown.

[0042] This is illustrated in detail in FIG. 3. FIG. 3 shows that the first beam (100) radiates a beam to an area corresponding to 2R / 3 from the center with respect to the radius R of the electrostatic chuck (10) (the center of the first beam of the first FCVA is located at 2R / 3 from the center of the electrostatic chuck to perform coating), and the second beam (110) radiates a beam to an area from R / 2 to 4R / 3, schematically showing that a uniform coating occurs on all surfaces of the electrostatic chuck as the electrostatic chuck rotates.

[0043] As described above, the positional arrangement of the first beam exit (200) and the second beam exit (210) is determined such that the beam areas reaching the electrostatic chuck are different from each other, thereby forming a coating layer of uniform thickness over the entire surface of the electrostatic chuck. The beam exit positions spaced apart from each other have the effect of avoiding interference problems on the equipment, sufficiently securing the beam width expansion area, and preventing localized overheating of the electrostatic chuck.

[0044] An FCVA device of this type is configured in a chamber to form a hydrogen-free carbon thin film on an electrostatic chuck.

[0045] The above embodiment can be modified to increase the number of beam exits to three, with one beam each located at the center and on the left and right sides; however, increasing the number of expensive FCVA devices may be disadvantageous in terms of production costs. Additionally, there may be issues with device interference and difficulties in precise installation.

[0046] The electrostatic chuck is positioned vertically inside the chamber. That is, to prevent particle contamination, a vertical positioning of the electrostatic chuck is more advantageous than a horizontal positioning relative to the direction of gravity. The linear ion source, sputter source, and FCVA device are positioned to surround the electrostatic chuck, and the orientation of the electrostatic chuck can be switched so that it faces each process source. Additionally, the electrostatic chuck rotates (rotates) around the central axis of the electrostatic chuck during the process by each source. The FCVA is equipped with a carbon target and includes a filtration section (formed as a branch section relative to the beam transport section) that filters macroparticles and a beam exit that injects carbon plasma into the chamber, and the beam path is controlled by a magnetic field.

[0047] To form a defect-free carbon thin film on the surface of an electrostatic chuck and to capture macroparticles (such as 40 μm droplets) generated from an arc plasma, the duct is designed to be 45° to 90°, a mesh or grid filter is added to the middle section of the duct, and a bias electrode is added to the duct wall or inside to configure an FCVA device for removing macroparticles.

[0048] An electrostatic chuck surface treatment process according to one embodiment of the present invention includes the following steps.

[0049] Pumping step (Pumping); vacuum state inside the chamber (10 -5 to 10 -6 It is formed into torr to ensure that subsequent processes can be performed stably.

[0050] Etching step (using an LIS ion source); plasma etching is performed on the surface of the electrostatic chuck using a linear ion source. This is carried out for 40 to 80 minutes, preferably about 60 minutes, and a thickness of 200 to 400 nm, preferably about 300 nm, is etched. The conditions at this time are a power of 1.0 to 1.5 kW, a current of 0.1 to 0.3 A, a substrate bias of a high-frequency pulse of 20 to 250 kHz, a negative bias of 10 to 150 V, and an inert gas (such as Ar) gas flow rate of 20 to 50 sccm.

[0051] Buffer layer formation step (UBM sputtering); a buffer layer with a thickness of 1 to 3 μm is formed using materials such as Ti, Cr, and W. The conditions at this time include a current of 5 to 8 A, a voltage of 400 to 500 V, a substrate bias of 20 to 250 kHz with a negative bias of 10 to 150 V, and an inert gas (Ar) gas flow rate of 80 to 150 sccm.

[0052] A hydrogen-free carbon film deposition step (ta-C coating); a ta-C coating with a thickness of 0.5 to 2 μm is formed. This coating can control hardness and resistance, and the conditions include a current of 50 to 70 A, a voltage of 20 to 40 V, and a substrate bias of a high-frequency pulse of 20 to 250 kHz and a negative bias of 10 to 150 V.

[0053] In addition, hardness can be controlled by selectively injecting nitrogen (N₂) with an inert gas (Ar). The nitrogen supply can be set to a flow rate ratio of 0 to 30% relative to the inert gas. Although nitrogen doping lowers the ultra-hard properties, it lowers electrical resistance, making discharge control easier, and is advantageous in terms of stress relief, improved adhesion, reduction of particles due to low friction, thermal stability, and improved wear characteristics.

[0054] Figure 8 shows that the hardness changes depending on the ratio of selectively injecting nitrogen (N₂) based on an inert gas (Ar). As shown in Figure 8, as the N₂ / Ar flow rate ratio increases, the hardness of the coating layer tends to gradually decrease from about 70 GPa to 25 GPa. Although this decrease in hardness may be disadvantageous if only ultra-hard properties are considered, it imparts conductivity to the coating film, and by adjusting the nitrogen supply ratio, there is no problem at all in achieving the hardness characteristics of the coating film of 30 GPa or more pursued by the present invention. That is, high hardness and conductivity can be achieved by setting the nitrogen supply ratio to 5 to 20% as a flow rate ratio relative to the inert gas.

[0055] The ta-C coating formed according to the above process improves heat resistance and wear resistance compared to conventional coatings and provides the effect of extending the lifespan of the electrostatic chuck.

[0056] Figure 4 is a graph showing the uniformity of the surface etching rate of an electrostatic chuck according to the present invention. It shows the change in etching rate (nm / min) according to the substrate position (mm). As a result measured under LIS ion source conditions, a relatively constant etching rate is shown for each electrostatic chuck position, confirming uniform etching characteristics. This suggests that substrate rotation and source placement optimization contribute to securing etching uniformity.

[0057] Figure 5 is a graph illustrating the thickness uniformity of the buffer layer formed on the surface of the electrostatic chuck according to the present invention. It shows that the buffer layer deposition rate (nm / min) according to the electrostatic chuck position is nearly uniform. That is, as a result measured in the UBM sputtering process, it demonstrates that coating thickness uniformity is ensured when the deposition rate for each position is maintained at a constant level.

[0058] Figure 6 is a graph illustrating the thickness uniformity of a hydrogen-free carbon coating layer formed on the surface of an electrostatic chuck according to the present invention. It shows the deposition rate (nm / min) of the ta-C coating with respect to the electrostatic chuck position in the FCVA process. The graph shows the rate of change in thickness according to the electrostatic chuck position, and when a uniform deposition rate is secured, the color of the coating film appears uniform (yellow). When the thickness increases, black appears, and when it decreases, various colors such as blue and purple appear (see Figure 7).

[0059] Figure 7 is a photograph of the coating result showing the difference between non-uniform (no rotation) and uniform (rotation) coating thickness depending on whether the electrostatic chuck rotates during the coating process.

[0060] When a uniform deposition rate is secured, the color of the coating film appears uniform (yellow). When the electrostatic chuck is rotated during coating, the entire surface appears yellow, indicating that it is coated with a uniform thickness (right photo of Fig. 7).

[0061] When the thickness increases, black appears, and when it decreases, various colors such as blue and purple appear. When coated without rotation of the electrostatic chuck (left photo of Fig. 7), various colors can be seen.

[0062] Unless otherwise defined in the foregoing, all technical and scientific terms used herein have the same meaning as commonly understood by a skilled expert in the art to which the present invention pertains. Furthermore, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless explicitly and specifically defined otherwise. Throughout the specification, when a part is described as "comprising" or "having" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0063] In addition, the singular form may include the plural form depending on the context.

[0064] In addition, in this specification, "on or above" means being located above or below the target part, and does not necessarily mean being located on the upper side with respect to the direction of gravity.

[0065] Additionally, in this specification, terms such as "first," "second," etc., may be used to describe various components, but said components shall not be limited by said terms. These terms are used solely for the purpose of distinguishing one component from another.

[0066] The rights of the present invention are not limited to the embodiments described above but are defined by what is stated in the claims, and it is obvious that a person skilled in the art may make various modifications and adaptations within the scope of the rights described in the claims. Explanation of the symbols

[0067] electrostatic chuck (10), first beam (100), second beam (110), first beam exit (200), second beam exit (210)

Claims

Claim 1 An electrostatic chuck surface coating system comprising: a chamber into which an electrostatic chuck is loaded; a first FCVA device and a second FCVA device mounted in the chamber; and a jig for an electrostatic chuck capable of rotating the electrostatic chuck; wherein the electrostatic chuck is arranged vertically within the chamber, and a first beam outlet, which is a beam outlet of the first FCVA device, and a second beam outlet, which is a beam outlet of the second FCVA device, are oriented toward the electrostatic chuck, and each emits a carbon plasma beam at a different angle so that the carbon plasma beams reach different regions of the electrostatic chuck at oblique angles to each other, and the electrostatic chuck is rotated during the process to uniformly form a hydrogen-free carbon coating film over the entire surface of the electrostatic chuck, wherein the first beam emitted from the first beam outlet reaches a region corresponding to 2R / 3 from the center with respect to the radius R of the electrostatic chuck, and the second beam emitted from the second beam outlet reaches a region ranging from R / 2 to 4R / 3. Claim 2 delete Claim 3 An electrostatic chuck surface coating system according to claim 1, characterized in that a linear ion source and a sputter source are further mounted in the chamber, such that the linear ion source, the sputter source, the first FCVA device, and the second FCVA device are arranged to surround the electrostatic chuck, and the electrostatic chuck can be oriented to face each process source by means of a jig for the electrostatic chuck. Claim 4 A method for surface coating of an electrostatic chuck, wherein the electrostatic chuck is placed in a chamber and fixed to a rotatable jig and positioned vertically within the chamber, the chamber is vacuumed, the surface of the electrostatic chuck is plasma etched using a linear ion source, a buffer layer is formed using at least one material among Ti, Cr, and W, and a hydrogen-free carbon thin film is formed using a first FCVA device and a second FCVA device, wherein a first beam emitted from the first FCVA device and a second beam emitted from the second FCVA device are emitted at oblique angles to each other so as to reach different regions of the electrostatic chuck, the electrostatic chuck is rotated during the coating process, the first beam emitted from the first FCVA device reaches the 2R / 3 region from the center of the radius R of the electrostatic chuck, and the second beam emitted from the second FCVA device reaches the R / 2 to 4R / 3 region, thereby forming a hydrogen-free carbon thin film of uniform thickness over the entire surface of the electrostatic chuck. Claim 5 delete Claim 6 A method for coating the surface of an electrostatic chuck according to claim 4, wherein the etching step is performed under conditions of power 1.0 to 1.5 kW, current 0.1 to 0.3 A, a high-frequency pulse of 20 to 250 kHz as a bias applied to the electrostatic chuck, a negative bias of 10 to 150 V, and an inert gas flow rate of 20 to 50 sccm. Claim 7 A method for coating the surface of an electrostatic chuck according to claim 4, wherein the buffer layer formation step is performed under conditions of a current of 5 to 8 A, a voltage of 400 to 500 V, a high-frequency pulse of 20 to 250 kHz as a bias applied to the electrostatic chuck, a negative bias of 10 to 150 V, and an inert gas flow rate of 80 to 150 sccm. Claim 8 A method for coating the surface of an electrostatic chuck according to claim 4, characterized in that the step of forming a hydrogen-free carbon thin film is performed under conditions of a current of 50 to 70 A, a voltage of 20 to 40 V, and a negative bias of 10 to 150 V with a high-frequency pulse of 20 to 250 kHz as a bias applied to the electrostatic chuck. Claim 9 A method for coating the surface of an electrostatic chuck according to claim 8, wherein the step of forming a hydrogen-free carbon thin film is performed by selectively injecting nitrogen (N₂) centered on an inert gas (Ar), and the nitrogen supply is controlled in a range of 0 to 30% in terms of the flow rate ratio relative to the inert gas.

Citation Information

Patent Citations

  • Filtered cathodic vacuum arc deposition apparatus and method

    EP2602354A1

  • Filtered cathodic arc deposition method and apparatus

    US20080116058A1

  • Electrostatic chuck and method of fabricating the same

    WO2002001611A2

  • Electrostatic chuck with embossments that comprise diamond-like carbon and deposited silicon-based material, and related methods

    US11612972B2

  • Filtered cathode arc source deposition apparatus

    US20030085123A1