Manufacturing method of multilayer glass substrate for semiconductors and multilayer glass substrate for semiconductors

By forming a bonding glass layer with a lower melting point and using brazing adhesive layers with conductive metals, the method addresses interlayer separation issues in multilayer glass substrates, ensuring strong and reliable bonding for semiconductor applications.

KR103043836B1Active Publication Date: 2026-11-06AMOSENSE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020240095780
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2026-11-06
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The challenge of interlayer separation due to the difference in thermal expansion coefficients between bonding materials and glass substrates during the manufacturing of multilayer glass substrates for semiconductors has not been adequately addressed, leading to bonding reliability issues.

Method used

A method involving the formation of a bonding glass layer with a lower melting point than the glass core, followed by pre-sintering and secondary sintering in a vacuum atmosphere, along with the use of a brazing adhesive layer and conductive metal to enhance bonding strength through fusion brazing interfaces.

Benefits of technology

This approach effectively matches the thermal expansion coefficients, resolving interlayer separation and enhancing the bonding reliability of multilayer glass substrates for semiconductors, thereby improving adhesion and electrical connections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024078816707-PAT00001_ABST
    Figure 112024078816707-PAT00001_ABST
Patent Text Reader

Abstract

A method for manufacturing a multilayer glass substrate for semiconductors and a multilayer glass substrate for semiconductors are disclosed. The disclosed method for manufacturing a multilayer glass substrate for semiconductors is characterized by comprising the steps of: applying glass frit paste to the surface of a glass core and then performing a first pre-sintering to form a bonding glass layer; placing another glass core on top of the glass core so as to face each other with the bonding glass layer in between; and performing a second main-sintering of the bonding glass layer in a vacuum atmosphere to seal and bond the two stacked glass cores.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a glass substrate, and in particular to a method for manufacturing a multilayer glass substrate for semiconductors in which two or more glass substrates are laminated and bonded, and to a multilayer glass substrate for semiconductors. Background Technology

[0002] In the manufacturing of electronic components, the process of implementing circuits on a semiconductor wafer is called the Front-End (FE) process. The process of assembling the wafer into a state suitable for use in actual products is called the Back-End (BE) process. This Back-End (BE) process includes the Multi-Chip Package (MQP) process, which involves assembling multiple semiconductors produced in wafer form into a bundle advantageous for device integration.

[0003] Semiconductor technology is evolving into various forms, such as micro- and nano-scale linewidths, more than ten million cells, high-speed operation, and high heat dissipation; however, the technology to perfectly package these technologies has not been adequately supported. Consequently, the electrical performance of semiconductors is sometimes determined by packaging technology and the resulting electrical connections rather than by the performance of the semiconductor technology itself.

[0004] Ceramic or resin is generally used as the material for packaging substrates. However, ceramic substrates are difficult to mount high-performance, high-frequency semiconductor devices due to their high resistance or dielectric constant. While resin substrates offer the advantage of being relatively easy to mount high-performance, high-frequency semiconductor devices, they have limitations in reducing wiring pitch and, in particular, are restricted for high-performance semiconductor packaging undergoing continuous miniaturization due to their uneven surfaces.

[0005] Although a method using smooth-surfaced silicon as an alternative packaging substrate has been developed, this approach has the disadvantages of high costs and difficulty in large-area manufacturing. In particular, silicon packaging substrates have the disadvantage of a high Coefficient of Thermal Expansion (CTE), making them unsuitable for use in die packaging where micro-sized bumps are formed at high density, such as in High Bandwidth Memory (HBM).

[0006] Glass substrates are a technology that has recently been gaining attention as a potential replacement for silicon substrates. Glass substrates are more cost-effective than silicon substrates and offer the advantage of enabling the production of a large number of chips due to the ability to design and manufacture them over larger areas. Furthermore, the inherent properties of glass result in a very smooth and flat surface that allows for detailed circuit design, making it advantageous for implementing high-performance, high-density circuits.

[0007] However, glass substrates have the disadvantage that interlayer bonding is difficult when manufactured in the form of multilayer glass substrates using stacked layers due to their material properties. Furthermore, when general bonding materials are used for interlayer bonding of glass substrates, bonding reliability issues arise, such as interlayer separation occurring due to the difference in the coefficient of thermal expansion between the bonding material and the glass. Prior art literature

[0008] Korean Registered Patent No. 10-1261468 (Publication Date: May 10, 2013) Korean Registered Patent No. 10-0523940 (Publication Date: October 26, 2005) The problem to be solved

[0009] The technical problem that the present invention aims to solve is to provide a method for manufacturing a multilayer glass substrate for semiconductors and a multilayer glass substrate for semiconductors that can resolve the problem of interlayer separation caused by the difference in thermal expansion coefficients between the bonding material and the glass during the manufacturing of a multilayer glass substrate. means of solving the problem

[0010] According to one aspect of the present invention as a means of solving the problem,

[0011] (a) A step of forming a bonding glass layer by applying glass frit paste to the surface of a glass core and then performing a first pre-sintering;

[0012] (b) a step of placing another glass core on top of the glass core so as to face each other with a bonding glass layer in between; and

[0013] (c) a step of sealing and bonding two stacked glass cores by secondary sintering (Main-sinter) of the bonding glass layer in a vacuum atmosphere; the present invention provides a method for manufacturing a multilayer glass substrate for semiconductors.

[0014] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the bonding glass layer may include a glass frit with a melting point lower than that of a glass core.

[0015] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the glass core may be oxide-strengthened glass having a thickness of 20 to 30 μm and having high strength, corrosion resistance, transparency, and hardness at room temperature.

[0016] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the glass core may be borosilicate glass or aluminum silicate glass.

[0017] In step (a) of the method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the glass frit paste can be applied to the surface of the glass core with a uniform thickness using screen printing.

[0018] A method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention also,

[0019] (a') may further include the step of forming a trench electrode on the glass core prior to step (a).

[0020] Step (a') of the method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention may include: (a'-1) forming a trench in the glass core through etching; (a'-2) forming a brazing adhesive layer with a specific thickness on the inner wall surface of the trench using a brazing alloy having a melting point lower than that of the glass core; (a'-3) forming an electrode by filling the trench where the brazing adhesive layer is formed with a conductive metal having a melting point higher than that of the brazing alloy; and (a'-4) performing heat treatment under specific conditions so that the brazing adhesive layer mediates mutual bonding between the glass core and the electrode.

[0021] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, at (a'-4), heat treatment may be performed in a reducing atmosphere or a nitrogen atmosphere maintained at a first temperature range that is higher than the eutectic point of the brazing alloy and lower than the melting point of the glass core.

[0022] Here, the first temperature range may be 577℃ or higher and less than 600℃.

[0023] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the brazing alloy may be an aluminum-silicon (Al-Si) alloy having a silicon (Si) content of 12.5 to 12.6 weight% based on the total alloy and the remainder being aluminum.

[0024] According to another aspect of the present invention as a means of solving the problem,

[0025] Two or more glass cores arranged in a stacked array; and

[0026] A bonding glass layer mediating a sealing bond between glass cores between two adjacent glass cores; comprising,

[0027] The above bonding glass layer provides a multilayer glass substrate for semiconductors comprising a glass frit with a melting point lower than that of the glass core.

[0028] In a multilayer organic plate for semiconductors according to another aspect of the present invention, the glass core may include a trench electrode.

[0029] In a multilayer organic plate for semiconductors according to another aspect of the present invention, a brazing adhesive layer made of a brazing alloy is formed with a specific thickness between the inner wall surface of a trench constituting the trench electrode and a conductive metal, wherein the brazing adhesive layer can form a fused brazing interface that mediates mutual bonding between the inner wall surface of the trench and the conductive metal during heat treatment.

[0030] In a multilayer organic plate for semiconductors according to another aspect of the present invention, the brazing alloy is an aluminum-silicon (Al-Si) alloy having a silicon (Si) content of 12.5 to 12.6 weight% and the remainder being aluminum based on the total alloy, and the conductive metal may be copper (Cu).

[0031] Here, the fusion brazing interface may be formed by heat treatment performed in a reducing atmosphere or nitrogen atmosphere maintained at a first temperature range that is higher than the eutectic point of the brazing alloy and lower than the melting point of the glass core, wherein the first temperature range may be 577°C or higher and less than 600°C.

[0032] In a multilayer glass substrate for semiconductors according to another aspect of the present invention, the glass core may be oxide-strengthened glass having a thickness of 20 to 30 μm and having high strength, corrosion resistance, transparency, and hardness at room temperature.

[0033] In a multilayer glass substrate for semiconductors according to another aspect of the present invention, the glass core may be borosilicate glass or aluminosilicate glass.

[0034] In a multilayer glass substrate for semiconductors according to another aspect of the present invention, the bonding glass layer can be formed by pre-sintering performed after applying glass frit paste to the surface of a glass core. Effects of the invention

[0035] According to the present invention, when manufacturing a multilayer glass substrate, multilayer bonding is implemented using a glass material with a lower melting point than the glass core, which is the core substrate, thereby matching the coefficient of thermal expansion (CTE) of the glass core and the bonding layer. As a result, the problem of interlayer separation caused by the difference in the coefficient of thermal expansion can be clearly resolved, and a highly reliable multilayer glass substrate with improved bonding reliability between glass cores (glass substrates) can be provided.

[0036] In addition, by forming a brazing adhesive layer in the trench of the glass core and filling it with a conductive metal to form an electrode, and then performing heat treatment under specific conditions, the fusion brazing interface resulting from the phase change (solid to liquid) of the brazing adhesive layer occurring during the heat treatment process can mediate a strong bond between the glass core and the electrode, thereby significantly improving or enhancing the adhesion (bonding strength) and adhesion characteristics of the electrode. Brief explanation of the drawing

[0037] FIG. 1 is a flowchart illustrating a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention. FIG. 2 is a schematic diagram illustrating the overall manufacturing process of a multilayer glass substrate for semiconductors according to an embodiment of the present invention. Figure 3 is a flowchart illustrating the process of forming trench electrodes on a glass core in sequence. Figure 4 is a schematic process diagram illustrating the trench electrode formation process of Figure 3. FIG. 5 is a cross-sectional view of a multilayer glass substrate for semiconductors manufactured by a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention. FIG. 6 is an enlarged view of the main part of a multilayer glass substrate for semiconductors shown in FIG. 5, and is an enlarged view of the main part of the present invention showing the enlarged view of part 'A' of FIG. 5. FIG. 7 is a cross-sectional view showing another preferred embodiment of a multilayer glass substrate for semiconductors. FIG. 8 is a cross-sectional view showing another preferred embodiment of a multilayer glass substrate for semiconductors. Specific details for implementing the invention

[0038] Hereinafter, preferred embodiments of the present invention will be described in detail.

[0039] In describing the embodiments of the present invention, identical or similar components are assigned the same reference numerals, and redundant descriptions thereof are omitted. Furthermore, detailed descriptions of related prior art are omitted if it is determined that such detailed descriptions could obscure the essence of the embodiments disclosed in this specification.

[0040] In addition, the attached drawings are intended only to facilitate understanding of the embodiments disclosed in this specification, and the technical concept disclosed in this specification is not limited by the attached drawings, and it should be noted that they include all modifications, equivalents, and substitutions that fall within the concept and technical scope of the present invention.

[0041] Additionally, terms including ordinal numbers, such as first, second, etc., may be used to describe various components, but said components are not limited by said terms. These terms are used solely for the purpose of distinguishing one component from another.

[0042] Furthermore, when it is mentioned that a component is "connected" or "joined" to another component, it should be understood that while it may be directly connected or joined to that other component, there may also be other components in between.

[0043] On the other hand, when it is stated that one component is "directly connected" or "directly coupled" to another component, it should be understood that there are no other components in between.

[0044] Furthermore, terms such as "comprising," "having," and "having" used in describing embodiments of the present invention are intended to specify the existence of features, numbers, steps, actions, components, parts, or combinations thereof of the invention, and should be understood as not excluding in advance the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof.

[0045] And the fact that one component is in the "front," "rear," "upper," or "lower" of another component includes, unless there are special circumstances, not only being placed in the "front," "rear," "upper," or "lower" of the other component in direct contact with it, but also having another component placed in between.

[0046] The drawings are intended solely to facilitate an understanding of the concept of the present invention and should not be interpreted as limiting the scope of the invention. Furthermore, it is noted that relative thicknesses, lengths, or sizes in the drawings may be exaggerated for convenience and clarity of explanation.

[0047] FIG. 1 is a flowchart for explaining a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention, and FIG. 2 is a schematic diagram of the overall manufacturing process of a multilayer glass substrate for semiconductors according to an embodiment of the present invention.

[0048] Referring to FIGS. 1 and 2, a manufacturing method according to an embodiment is a method for manufacturing a multilayer glass substrate for semiconductors that can significantly improve interlayer bonding when manufacturing a multilayer glass substrate, comprising the steps of forming a bonding glass layer on the surface of a glass core (S200), stacking another glass core on the glass core on which the bonding glass layer is formed (S300), and sealing bonding the two stacked glass cores (S300).

[0049] In the step (S100) of forming a bonding glass layer on the surface of a glass core, glass frit paste is applied to the surface (upper or lower surface, or upper and lower surfaces) of the glass core (10). Subsequently, a bonding glass layer (20) can be formed by performing a first pre-sintering. In the step (S100) of forming a bonding glass layer on the surface of a glass core, the bonding glass layer (20) includes glass frit with a melting point approximately 100°C lower than that of the glass core (10).

[0050] In the step (S100) of forming a bonding glass layer on the surface of the glass core, the glass frit paste can be formed with a uniform film thickness on the surface of the glass core (10). If the film thickness of the glass frit paste applied to the surface of the glass core (10) is not uniform, when a pair of glass cores (10a, 10b) are overlapped, the uniformity of contact between the bonding glass layer (20) and the glass cores (10a, 10b) decreases, and the bonding quality between the glass cores (10a, 10b) may be significantly degraded.

[0051] Therefore, in the step (S100) of forming a bonding glass layer on the surface of the glass core, when applying the glass frit paste to the surface of the glass core (10), it is important and required that the glass frit paste be applied to have a uniform film thickness on the glass core (10). Applying the glass frit paste with a uniform film thickness can be achieved, for example, by screen printing.

[0052] In the step (S100) of forming a bonding glass layer on the surface of the glass core, the glass frit paste applied to the glass core (10) may have a glass frit as its main base material having a melting point approximately 100°C lower than the melting point of the glass core (10), and may be composed of an organic solvent and a binder, etc., and the bonding glass layer (20) may be formed by removing the organic solvent or binder, etc. contained in the glass frit paste during the first pre-sintering process.

[0053] Glass frit may be, for example, a mixture of silica sand, aluminum oxide (Al2O3), and calcium carbonate (CaCO3) in specific proportions, melted at a high temperature, rapidly cooled, and then ground into a fine powder. The organic solvent may consist of, for example, butyl acetate or terpineol, or a combination thereof, and an acrylic binder or a nitrocellulose binder may be used as the binder.

[0054] If the glass frit paste is not heated sufficiently during the first pre-sintering process, the binder remains in the bonding glass layer (20), which can reduce bonding performance or cause it to crack easily. Therefore, during the first pre-sintering process, it is desirable to perform pre-sintering under temperature and pressure conditions that can sufficiently heat the glass frit paste while preventing deterioration of the glass core (10).

[0055] A drying step (not shown) for drying the glass frit paste may be added after the first preliminary sintering. If additional drying treatment is performed after the first preliminary sintering, the organic solvent remaining in the glass frit paste can be removed more effectively. In the drying step, it is preferable to perform the drying treatment at a temperature and time that allows the organic solvent to be removed by vaporization while also allowing the high-temperature glass frit paste to be cooled slowly.

[0056] In the step (S200) of stacking glass cores, two glass cores (10a, 10b) of the same material are arranged in a stacked structure so that they face each other with a bonding glass layer (20) in between. Considering that the alignment state of the stacking direction of the glass cores (10a, 10b) during the stacking process has a significant impact on the bonding quality in the subsequent sealing bonding step, it is desirable to use a dedicated stacking device including a sensor, an alignment unit, and a jig to enable accurate and precise stacking.

[0057] In the step (S300) of sealing the stacked glass cores, a process to achieve stacking bonding can be performed through secondary sintering (Main-sinter) of the bonding glass layer (20). In the step (S300) of sealing the stacked glass cores, preferably, the sealing bonding of the glass cores (10a, 10b) can be achieved by heating and pressing the bonding glass layer (20) while exhausting the gas between the two stacked glass cores (10a, 10b) in a vacuum atmosphere.

[0058] In the secondary sintering (Main-sinter) in which the bonding glass layer (20) is heated and pressed, the sintering may be performed at a temperature lower than the melting point and higher than the softening point of the glass frit, which is the main substrate of the bonding glass layer (20). In the embodiment, the secondary sintering temperature for achieving a sealed bond of the glass core (10a, 10b) may vary depending on the composition of the glass frit, but may be between approximately 500°C and 700°C.

[0059] In the method for manufacturing a semiconductor multilayer glass substrate according to the embodiment, the glass core (10) that serves as the main substrate may be oxide-strengthened glass. In the method for manufacturing a semiconductor multilayer glass substrate according to the embodiment, the glass core (10) that serves as the main substrate may be a strengthened glass having a thickness of 20 to 30 μm, high strength and corrosion resistance at room temperature, and a main component that is oxide.

[0060] As a preferred example, the glass core (10) that serves as the main substrate in the method for manufacturing a semiconductor multilayer glass substrate according to the embodiment may be a borosilicate glass that is a glass with boric acid as the main component instead of silicic acid, contains at least 5% or more of boric acid, has chemical acid resistance and weather resistance with a low coefficient of expansion, and has excellent thermal shock resistance.

[0061] As another preferred example, the glass core (10) that serves as the main substrate in the semiconductor multilayer glass substrate manufacturing method according to the embodiment may be aluminum silicate glass composed of alumina and boron oxide, which has characteristics similar to borosilicate glass, but has superior heat resistance and high chemical resistance compared to borosilicate glass.

[0062] The method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment may further include a step (S100) of forming a trench electrode on a glass core (10) prior to the aforementioned step S200. In the step (S100) of forming a trench electrode on a glass core, the trench electrode (30) may be formed by etching the glass core (10) to form a trench (32) in a desired pattern and filling it with a conductive metal, such as copper (Cu).

[0063] Referring to Figures 3 and 4, we will examine the process of forming electrodes on a glass core in more detail.

[0064] FIG. 3 is a flowchart illustrating the process of forming a trench electrode on a glass core in sequence, and FIG. 4 is a schematic process diagram illustrating the trench electrode formation process of FIG. 3.

[0065] For reference, the term 'trench' used in the following description of the electrode formation process refers to a fine hole (via) or groove formed in the glass core through an etching process to form the electrode.

[0066] Referring to FIGS. 3 and 4, the trench electrode formation step (100) includes the step of forming a trench (32) in a glass core (10) through an etching process (S102), the step of forming a brazing adhesive layer (34) with a specific thickness on the inner wall surface of the trench (32) using a brazing alloy having a melting point lower than that of the glass core (10) (S104), the step of forming an electrode by filling the trench (32) where the brazing adhesive layer (34) is formed with a conductive metal (36) (S106), and the step of performing a heat treatment for brazing (S108).

[0067] In the step (S102) of forming a trench in the glass core, a pattern is formed on the glass core (10) using a photosensitive material through a known photolithography process of drawing a semiconductor circuit on a wafer, and a trench (32) can be formed by performing an etching process using the photosensitive material with the formed pattern as a mask. For the etching process to form the trench, dry etching using plasma or a laser or wet etching using an etching solution may be applied.

[0068] The step (S104) of forming the brazing adhesive layer (34) is a step of forming the brazing adhesive layer (34) on the inner wall surface of the trench (32) using a brazing alloy. In the step (S104) of forming the brazing adhesive layer (34), the brazing adhesive layer (34) serves as a part that mediates a strong bond between the glass core (10) and the conductive metal (36), and can be formed by depositing a brazing alloy to a specific thickness on the trench (32) formed in the glass core (10).

[0069] In the step (S104) of forming the brazing adhesive layer (34), the brazing alloy constituting the brazing adhesive layer (34) may be an alloy with a melting point lower than that of the glass core (10). The brazing alloy constituting the brazing adhesive layer (34) may preferably be an aluminum-silicon (Al-Si) alloy in which, based on the whole alloy, the silicon (Si) content is 12.5 to 12.6 weight% and the remainder is aluminum.

[0070] Aluminum-silicon (Al-Si) alloys are characterized by being lightweight and having high ductility and malleability. Aluminum-silicon (Al-Si) alloys also have low melting points and shrinkage rates, strong corrosion resistance, and good fluidity in the molten state. Because of this, they can easily melt at relatively low temperatures and form a fusion brazing interface that mediates a strong bond between glass and metal.

[0071] In the step (S104) of forming the brazing adhesive layer (34), the brazing adhesive layer (34) can be formed with a specific thickness in the trench of the glass core (10) through vacuum deposition. In the step (S104) of forming the brazing adhesive layer (34), the brazing adhesive layer (34) can be formed with a specific thickness (t1) in the trench of the glass core (10) through a sputtering process, which is a type of vacuum deposition method.

[0072] In the step (S104) of forming the brazing adhesive layer (34), the brazing adhesive layer (34) can be formed on the inner wall surface of the trench with a thickness of 25 to 100 nm. If the thickness of the brazing adhesive layer (34) is too thin, less than 25 nm, it cannot properly perform its function as an adhesive. Also, if the thickness of the brazing adhesive layer (34) exceeds 100 nm, it may result in increased costs due to the input of more material than necessary, and the electrode formation space will be reduced.

[0073] In the step of forming the electrode (S106), the electrode may be composed of a conductive metal (36) with a higher melting point than the brazing alloy constituting the brazing adhesive layer (34). In the step of forming the electrode (S106), the electrode may be formed by filling the trench (32) on which the brazing adhesive layer (34) is formed on the inner wall surface with the conductive metal (36) through an electroplating or a sputtering process, which is a type of vacuum deposition.

[0074] In the step of forming the electrode (S106), the conductive metal (36) constituting the electrode may be, for example, copper (Cu). In the step of forming the electrode (S106), the conductive metal (36) constituting the electrode may be a conductive material other than copper. In the step of forming the electrode (S106), the conductive metal constituting the electrode (36) may be, for example, one of aluminum (Al), titanium (Ti), or tungsten (W).

[0075] The heat treatment step (S108) is the final step of the trench electrode formation process, and is a step of brazing the electrode by heat treating the glass core (10) on which the electrode is formed under predetermined conditions. In the heat treatment step (S108), heat treatment is performed at a temperature condition that is higher than the melting point of the aforementioned brazing alloy and lower than the melting point of the glass core (10), thereby allowing the brazing adhesive layer (34) to mediate a strong bond between the glass core (10) and the electrode composed of the conductive metal (36).

[0076] In the heat treatment step (S108) for brazing, heat treatment can be performed in a reducing atmosphere or a nitrogen atmosphere maintained at a first temperature range that is higher than the eutectic point of the brazing alloy and lower than the melting point of the glass core (10). In the embodiment, the first temperature range is preferably 577°C or higher and less than 600°C, considering that the eutectic temperature of an aluminum-silicon alloy with a silicon (Si) content of 12.5% ​​is 577°C.

[0077] By performing the above heat treatment above the eutectic point of the brazing alloy, a phase change (solid to liquid) of the brazing adhesive layer (34) occurs, and a fusion brazing interface is formed between the glass core (10) and the electrode according to the phase change of the brazing adhesive layer (34) to mediate a strong bond between them, so that the electrode made of conductive metal (36) and the trench (32) formed in the glass core (10) can form a strong bond with each other.

[0078] Meanwhile, in the case of a glass core (10) having a trench electrode (30), when forming a bonding glass layer (20) on the surface of the glass core (10) (e.g., the upper or lower surface or both sides of the glass core (10)) in the aforementioned S200 step, it is preferable to form the bonding glass layer (20) only in the area excluding the trench electrode (30a) where the fine hole is formed, so that the trench electrode (through electrode, 30a) formed in the fine hole among the trench electrodes (30) mediates interlayer electrical connection when bonding the glass core (10).

[0079] According to the manufacturing method described above, when manufacturing a multilayer glass substrate, multilayer bonding is achieved by using a glass material with a lower melting point than the glass core, which is the core substrate, thereby matching the coefficient of thermal expansion (CTE) of the glass core and the bonding layer. Accordingly, the conventional problem of interlayer separation due to the difference in the coefficient of thermal expansion can be clearly resolved, and a highly reliable multilayer glass substrate with improved interlayer bonding characteristics between glass cores (glass substrates) can be provided.

[0080] In addition, by forming a brazing adhesive layer in the trench of the glass core and filling it with a conductive metal to form an electrode, and then performing heat treatment under specific conditions, the fusion brazing interface resulting from the phase change (solid to liquid) of the brazing adhesive layer occurring during the heat treatment process can mediate a strong bond between the glass core and the electrode, thereby significantly improving or enhancing the adhesion (bonding strength) and adhesion characteristics of the electrode.

[0081] FIG. 5 is a cross-sectional view of a semiconductor multilayer glass substrate manufactured by the method for manufacturing a semiconductor multilayer glass substrate described above, and FIG. 6 is an enlarged view of the main part of the semiconductor multilayer glass substrate shown in FIG. 5, and is an enlarged view of the main part of the present invention showing part 'A' of FIG. 5.

[0082] Referring to FIGS. 5 and 6, a multilayer glass substrate (1) for semiconductors comprises two or more glass cores (10a, 10b) arranged in a stacked configuration and a bonding glass layer (20) that mediates a sealing bond between the glass cores (10a, 10b) between two adjacent glass cores (10a, 10b). A trench electrode (30) may be formed on the glass cores (10a, 10b), and the bonding glass layer (20) may be formed on at least one of the upper and lower surfaces of the glass cores (10a, 10b) for a sealing bond between the glass cores (10a, 10b).

[0083] The glass core (10) may be tempered glass with a thickness of 20 to 30 μm. In the embodiment, the glass core (10) may be tempered glass having high strength, corrosion resistance, transparency, and hardness at room temperature, with the main component being an oxide. As a preferred example, the glass core (10) may be borosilicate glass. Depending on the embodiment, it may be aluminum silicate glass.

[0084] Borosilicate reinforced glass is a glass based on boric acid instead of silica, containing at least 5% boric acid. It has a low coefficient of expansion, possesses chemical acid resistance and weather resistance, and has excellent thermal shock resistance, making it suitable as a semiconductor glass substrate. Aluminum silicate reinforced glass is composed of alumina and boron oxide and has similar properties to borosilicate glass, but possesses superior heat resistance and high chemical resistance compared to borosilicate glass, making it suitable as a semiconductor glass substrate.

[0085] The trench electrode (30) can be formed by filling a trench (32), which is formed in the form of a groove or hole in the glass core (10) through an etching process, with a conductive metal (36). To ensure a strong bond between the trench (32) and the conductive metal (36), a brazing adhesive layer (34) made of a brazing alloy can be formed with a specific thickness (t1) between the inner wall surface of the trench (32) and the conductive metal (36). The brazing adhesive layer (34) can preferably be formed with a thickness of 25 to 100 nm.

[0086] The brazing adhesive layer (34) can form a fused brazing interface that mediates a strong mutual bond between the inner wall surface of the trench (32) formed in the glass core (10) during heat treatment for brazing bonding and the conductive metal (36) filled in the trench (32). The brazing adhesive layer (34) can be formed on the inner wall surface of the trench, for example, through a sputtering process, which is a type of vacuum deposition method.

[0087] The brazing alloy constituting the brazing adhesive layer (34) may be an alloy with a lower melting point than the glass core (10). The brazing alloy constituting the brazing adhesive layer (34) may preferably be an aluminum-silicon (Al-Si) alloy in which, based on the whole alloy, the silicon (Si) content is 12.5 to 12.6 weight% and the remainder is aluminum (Al), but is not limited thereto.

[0088] Aluminum-silicon (Al-Si) alloys are characterized by being lightweight and having high ductility and malleability. Aluminum-silicon (Al-Si) alloys also have low melting points and shrinkage rates, strong corrosion resistance, and good fluidity in the molten state. Because of this, they can easily melt at relatively low temperatures and form a fusion brazing interface that mediates a strong bond between glass and metal.

[0089] A fusion brazing interface can be formed by performing heat treatment in a reducing atmosphere or a nitrogen atmosphere maintained at a first temperature range that is higher than the eutectic point of the brazing alloy and lower than the melting point of the glass core (10). In the embodiment, the first temperature range may be 577°C or higher and less than 600°C, considering that the eutectic temperature of an aluminum-silicon alloy with a silicon (Si) content of 12.5% ​​is 577°C.

[0090] The conductive metal (36) constituting the trench electrode (30) may be a conductive material with a melting point higher than that of the glass core (10). The conductive metal (36) constituting the trench electrode (30) may preferably be copper (Cu). The conductive metal (36) constituting the trench electrode (30) may be a conductive material other than copper. For example, aluminum (Al), titanium (Ti), tungsten (W), etc. may be used as the conductive metal constituting the trench electrode (30).

[0091] A bonding glass layer (20) can be formed on the surface of a glass core (10) (upper or lower surface, or upper and lower surfaces) by applying glass frit paste and then pre-sintering. The bonding glass layer (20) includes glass frit with a melting point approximately 100°C lower than that of the glass core (10) and can be formed on the surface of the glass core (10) with a uniform film thickness. For example, it can be formed on the surface of the glass core (10) with a uniform film thickness through screen printing.

[0092] The glass frit paste applied to the glass core (10) to form the bonding glass layer (20) may be composed of the glass frit having a melting point approximately 100°C lower than the melting point of the glass core (10), and may include an organic solvent and a binder, etc., and the bonding glass layer (20) may be formed by removing the organic solvent or binder, etc. included in the glass frit paste during the pre-sintering process.

[0093] Glass frit may be, for example, a mixture of silica sand, aluminum oxide (Al2O3), and calcium carbonate (CaCO3) in specific proportions, melted at a high temperature, rapidly cooled, and then ground into a fine powder. The organic solvent may consist of, for example, butyl acetate or terpineol, or a combination thereof, and an acrylic binder or a nitrocellulose binder may be used as the binder.

[0094] Meanwhile, the electrode may be formed in a raised shape on one or both sides of the glass core, in addition to the trench electrode shape described above. For example, as in another embodiment shown in FIG. 7, it may be formed in a raised shape on the upper surface of the glass core (10'). The raised protruding electrode (30') may be formed by a method such as brazing a metal foil onto the upper surface of the glass core (10') and then removing the unnecessary portion of the metal foil through an etching process.

[0095] When a protruding electrode (30') is formed on the upper surface of a glass core (10'), the bonding glass layer (20') can be formed on the upper surface of the glass core (10') with a predetermined thickness in a manner that covers both the upper surface of the glass core (10') and the protruding electrode (30'), as shown in FIG. 7.

[0096] However, in this case, for electrical connection between the two glass cores (10a', 10b') when bonding the glass cores, the bonding glass layer (20) may be formed with a predetermined thickness only in the area excluding the electrode (through electrode, 30a') formed in the fine hole.

[0097] In some cases, as in another embodiment of FIG. 8, a bonding glass layer (20) may be formed first on the upper surface of a glass core (10), and an electrode may be formed in the form of a raised protruding electrode (30) on the bonding glass layer (20). In this case, the raised protruding electrode (30) may be formed, for example, by brazing a metal foil onto the upper surface of the bonding glass layer (20), and then removing the unnecessary portion of the metal foil through an etching process.

[0098] According to the multilayer glass substrate for semiconductors according to the above embodiment, a glass-based bonding layer having a lower melting point than the glass core, which is the core substrate, mediates the bonding between two glass cores to be bonded, thereby matching the coefficient of thermal expansion (CTE) of the glass core and the bonding layer. Accordingly, the problem of interlayer separation due to the difference in the coefficient of thermal expansion can be clearly resolved, and the bonding reliability between glass cores (glass substrates) can be further improved.

[0099] The above description is merely an illustrative explanation of the technical concept of the present invention, and those skilled in the art to which the present invention pertains will be able to make various modifications and variations within the scope of the essential characteristics of the present invention.

[0100] Accordingly, the embodiments disclosed in this invention are intended to illustrate, not limit, the technical concept of the invention, and the scope of the technical concept of the invention is not limited by these embodiments. The scope of protection of this invention shall be interpreted by the claims below, and all technical concepts within an equivalent scope shall be interpreted as being included within the scope of rights of this invention. Explanation of the symbols

[0101] 1: Glass substrate for semiconductors 10, 10', 10": Glass core 20, 20', 20": Bonding glass layer 30: Trench electrode 30', 30": Protruding electrode 32: Trench 34: Brazing adhesive layer t1: Thickness of the brazing adhesive layer

Claims

Claim 1 (a') a step of forming a trench electrode on a glass core; (a) a step of forming a bonding glass layer by applying glass frit paste to the surface of the glass core and then performing a first pre-sintering; (b) a step of placing another glass core on top of the glass core so as to face each other with the bonding glass layer in between; and (c) a step of sealing and bonding two stacked glass cores by secondary sintering (Main-sinter) of the bonding glass layer in a vacuum atmosphere; wherein step (a') comprises forming a trench in the glass core through etching, forming a brazing adhesive layer of a specific thickness on the inner wall surface of the trench using a brazing alloy having a melting point lower than that of the glass core, and forming an electrode by filling the trench in which the brazing adhesive layer is formed with a conductive metal having a melting point higher than that of the brazing alloy, wherein the brazing alloy is an aluminum-silicon (Al-Si) alloy having a silicon (Si) content of 12.5 to 12.6 weight% and the remainder being aluminum, based on the entire alloy. Claim 2 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 1, wherein the bonding glass layer comprises a glass frit with a melting point lower than that of a glass core. Claim 3 A method for manufacturing a multilayer glass substrate for semiconductors, wherein, in claim 1, the glass core is formed with a thickness of 20 to 30 μm. Claim 4 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 3, wherein the glass core is borosilicate glass or aluminum silicate glass. Claim 5 A method for manufacturing a multilayer glass substrate for semiconductors, wherein in step (a), the glass frit paste is applied to the surface of the glass core with a uniform thickness by screen printing. Claim 6 delete Claim 7 A method for manufacturing a multilayer glass substrate for semiconductors, wherein the step (a') further comprises the step of performing heat treatment under specific conditions so that the brazing adhesive layer mediates mutual bonding between the glass core and the electrode. Claim 8 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 7, wherein heat treatment is performed in a reducing atmosphere or a nitrogen atmosphere maintained at a first temperature range that is higher than the eutectic point of the brazing alloy and lower than the melting point of the glass core. Claim 9 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 8, wherein the first temperature range is 577°C or higher and less than 600°C. Claim 10 delete Claim 11 A multilayer glass substrate for semiconductors comprising: two or more glass cores arranged in a stacked array and including trench electrodes; and a bonding glass layer mediating a sealing bond between two adjacent glass cores, wherein the bonding glass layer includes a glass frit with a melting point lower than that of the glass cores, wherein the trench electrodes are formed by filling the trenches of each glass core with a conductive metal, wherein a brazing adhesive layer made of a brazing alloy is formed with a specific thickness between the inner wall surface of the trench and the conductive metal, and wherein the brazing alloy is an aluminum-silicon (Al-Si) alloy having a silicon (Si) content of 12.5 to 12.6 weight% and the remainder being aluminum, based on the entire alloy. Claim 12 delete Claim 13 A multilayer glass substrate for semiconductors according to claim 11, wherein the brazing adhesive layer forms a fusion brazing interface that mediates mutual bonding between the inner wall surface of the trench and the conductive metal during heat treatment. Claim 14 delete Claim 15 A multilayer glass substrate for semiconductors according to claim 13, wherein the fusion brazing interface is formed by heat treatment performed in a reducing atmosphere or nitrogen atmosphere maintained at a first temperature range higher than the eutectic point of the brazing alloy and lower than the melting point of the glass core. Claim 16 A multilayer glass substrate for semiconductors according to claim 15, wherein the first temperature range is 577°C or higher and less than 600°C. Claim 17 In claim 11, the glass core is a multilayer glass substrate for semiconductors formed with a thickness of 20 to 30 μm. Claim 18 In claim 17, the glass core is a multilayer glass substrate for semiconductors, wherein the glass core is borosilicate glass or aluminosilicate glass. Claim 19 In claim 11, the bonding glass layer is a multilayer glass substrate for semiconductors formed by applying glass frit paste to the surface of a glass core and then pre-sintering.

Citation Information

Patent Citations

  • Faceplate provided with electrodes made of conductivematerial

    KR1020030015396A

  • Ceramic circuit board, method for manufacture thereof and electric device for the same

    KR1020090071010A

  • Passive device packaging structure embedded in glass medium and method for manufacturing the same

    KR1020220021864A

  • Method of metallizing glass articles

    KR1020220125250A