Regenerated composite material using recycled polyamide composite material derived from scrapped automobiles and method for manufacturing the same

A recycled composite material with specific resin and additive ratios, manufactured through a multi-step process, addresses the challenge of maintaining mechanical properties under harsh conditions, achieving performance comparable to virgin materials while reducing carbon emissions.

KR103044891B1Active Publication Date: 2026-11-10BGF ECO MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
KR1020240114378
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2026-11-10
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing recycled polyamide composite materials from end-of-life vehicles face challenges in maintaining mechanical properties such as tensile strength, flexural strength, flexural modulus, impact strength, and heat distortion temperature, especially under harsh conditions like high temperatures, due to weakened structural bonds from prolonged exposure to high temperatures during recycling processes.

Method used

A recycled composite material comprising 30 to 55 weight percent of polyamide virgin resin, 20 to 40 weight percent of recycled polyamide composite material, 20 to 30 weight percent of virgin reinforcing agent, and 2.5 to 6 weight percent of additives, manufactured through a process involving crushing, washing, and regeneration steps, ensuring the material maintains mechanical properties under harsh environments.

Benefits of technology

The solution provides a recycled composite material with mechanical properties comparable to virgin materials, reducing carbon emissions and maintaining strength and durability even under high temperatures, making it environmentally friendly and cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024093100159-PAT00001
    Figure 112024093100159-PAT00001
  • Figure 112024093100159-PAT00002
    Figure 112024093100159-PAT00002
Patent Text Reader

Abstract

The present invention relates to a recycled composite material comprising a recycled polyamide composite material and a method for manufacturing the same, wherein waste polyamide is recycled in an environmentally friendly manner, while possessing excellent physical properties comparable to those of a composite material manufactured using only virgin polyamide resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a recycled composite material using a polyamide recycled composite material derived from end-of-life vehicles and a method for manufacturing the recycled composite material. It is possible to achieve physical properties comparable to those of a composite material using virgin polyamide resin while utilizing a polyamide recycled composite material derived from end-of-life vehicles. Using a recycled composite resin made of the polyamide recycled composite material of the present invention instead of virgin polyamide resin can reduce carbon emissions, making it environmentally friendly. Background Technology

[0002] Until now, research has focused on increasing the molecular weight of virgin polyamide to improve the strength of virgin polyamide (nylon) fibers and molded products.

[0003] However, with the recent emergence of issues such as environmental pollution, the development of recycling technologies for waste polyamide products is becoming increasingly important due to tightening regulations on resin usage in various countries, the growing awareness of reducing carbon emissions—a cause of climate change—and consumer demands emphasizing social responsibility. Recycling technology can provide a sustainable method to reduce the amount of waste released.

[0004] Mechanical recycling, thermal recycling, and chemical recycling have been proposed as methods for recycling waste polyamide composite materials, and currently, mechanical recycling is the most widely applied commercially.

[0005] When recycling waste polyamide derived from end-of-life vehicles, there is a problem in that the structural bonds of the polymer are weakened due to prolonged exposure to high temperatures. Therefore, there is a need to develop a method to ensure physical properties while utilizing composite materials made from recycled polyamide derived from end-of-life vehicles.

[0006] Recently, there have been studies on methods for producing pelletized recycled polyamide resins from waste automobiles through crushing, washing, mixing, and chain extension reactions, but there is still a need for continuous research on recycled composite materials that can improve mechanical properties such as tensile strength and impact strength and maintain their properties even under harsh conditions such as high temperatures. Prior art literature

[0008] Korean Registered Patent No. 10-1575372 (Publication Date: Dec. 07, 2015) The problem to be solved

[0009] Accordingly, the present invention provides a regenerative composite material and a method for manufacturing the same,

[0010] The purpose is to provide a recycled composite material that satisfies a certain level of mechanical properties (tensile strength, flexural strength, flexural modulus, impact strength, and heat distortion temperature) and maintains its mechanical properties, especially in harsh environments.

[0011] However, the problems that the present invention aims to solve are not limited to those mentioned above, and other problems not mentioned but intended to be solved will be clearly understood by those skilled in the art to which the present invention belongs from the content to be described below. means of solving the problem

[0012] One aspect of the present invention is, based on 100% by weight of the total weight of the recycled composite material,

[0013] It comprises 30 to 55 weight percent of polyamide virgin resin, and

[0014] It comprises 20 to 40 weight percent of recycled polyamide composite material,

[0015] It contains 20 to 30 weight percent of a virgin reinforcing agent, and

[0016] Containing 2.5 to 6 weight percent of additives,

[0017] Provides recycled composite materials.

[0018] Another aspect of the present invention is a method for manufacturing the above-mentioned regenerative composite material,

[0019] First step of crushing waste polyamide composite material;

[0020] A second step of producing a recycled polyamide composite material by washing the waste polyamide composite material obtained from the first step above; and

[0021] A third step of regenerating the above-mentioned polyamide recycled composite material; comprising

[0022] A method for manufacturing a regenerative composite material is provided. Effects of the invention

[0023] When using the recycled composite material of the present invention, carbon emissions can be reduced, making it environmentally friendly. In particular, the mechanical properties of the recycled composite material of the present invention (tensile strength, flexural strength, flexural modulus, impact strength, heat distortion temperature, etc.) satisfy a certain level or higher, and excellent mechanical properties can be maintained even when exposed to harsh environments, such as high temperatures, for a long time. Specific details for implementing the invention

[0024] Hereinafter, the operation and effects of the invention will be described in more detail through specific embodiments and drawings. However, these embodiments are merely examples of the invention and do not define the scope of the invention.

[0025] Prior to this, terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0026] Therefore, it should be understood that the configuration of the embodiments described in this specification is merely one of the most preferred embodiments of the present invention and does not represent all of the technical ideas of the present invention, and that various equivalents and modifications that can replace them may exist at the time of filing this application.

[0027] In this specification, singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, terms such as “comprising,” “comprising,” or “having” are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0028] Where various parameters in this specification are given as an enumeration of ranges, preferred ranges, preferred upper limits, and preferred lower limits, it should be understood that any pair of any upper range limit or preferred value and any lower range limit or preferred value specifically discloses all ranges formed by any pair of any upper range limit or preferred value, regardless of whether the range is disclosed separately.

[0029] Where a range of numerical values ​​is mentioned in this specification, unless otherwise described, the range is intended to include its endpoint and all integers and fractions within the range.

[0030] The scope of the present invention is not intended to be limited to specific values ​​mentioned when defining the scope.

[0031] In the present specification, "a to b" and "a~b" indicating numerical ranges are defined as ≥a and ≤b.

[0032] In this specification, the waste polyamide composite material refers to a composite material containing polyamide that is subject to recycling, and may mean a polyamide composite material derived from parts of a scrapped vehicle.

[0033] In this specification, a recycled polyamide composite material may mean that the waste polyamide composite material has undergone steps such as crushing and washing for recycling.

[0034] In this specification, a recycled composite material may mean a material that has undergone a recycling step using the polyamide recycled composite material, and the recycling step may mean extruding the polyamide recycled composite material by adding a polyamide virgin resin, a virgin reinforcing agent, and / or additives.

[0035] In this specification, the virgin reinforcing agent may refer to a new reinforcing agent added during the regeneration step.

[0036] Embodiments of the present invention have been described in detail below, but the present invention is not limited thereto.

[0038] A recycled composite material according to one embodiment of the present invention may comprise 30 to 55 weight% of a polyamide virgin resin, 20 to 40 weight% of a polyamide recycled composite material, 20 to 45 weight% of a virgin reinforcing agent, and 2.5 to 6 weight% of an additive, based on 100 weight% of the total weight of the recycled composite material.

[0039] For example, based on 100 weight% of the total weight of the recycled composite material, the polyamide virgin resin may be 30 to 55 weight%, 33 to 50 weight%, 35 to 48 weight%, 37 to 46 weight%, or 38 to 44 weight%.

[0040] If the content of the above-mentioned polyamide virgin resin exceeds that of the present invention, the relative content of the virgin resin increases, which may lead to increased manufacturing costs and carbon emissions of the recycled composite material; if it falls below that, there may be a problem in that the physical properties of the recycled composite material are not sufficiently secured.

[0041] For example, based on 100% by weight of the total weight of the recycled composite material, the polyamide recycled composite material may be 20 to 40% by weight, 23 to 37% by weight, 25 to 35% by weight, or 27 to 33% by weight.

[0042] If the content of the above-mentioned recycled polyamide composite material exceeds that of the present invention, there may be a problem in that the physical properties of the recycled composite material are not sufficiently secured, and if it falls below that, there may be a problem in that the cost of manufacturing the recycled composite material increases.

[0043] For example, based on 100 weight% of the total weight of the recycled composite material, the virgin reinforcing agent may be 20 to 30 weight%, 23 to 28 weight%, or 25 to 27 weight%.

[0044] For example, based on 100 weight% of the total weight of the recycled composite material, the additive may be 2.0 to 6 weight%, 2.3 to 5 weight%, 2.6 to 4.5 weight%, or 2.8 to 4.0 weight%.

[0045] If the content of the above virgin reinforcing agent exceeds that of the present invention, there may be problems such as increased manufacturing costs for the recycled composite material and increased specific gravity of the recycled composite material, and if it falls below that, there may be problems such as a lower load deformation temperature, which prevents the physical properties of the recycled composite material from being sufficiently secured.

[0046] Meanwhile, the above polyamide may be polyamide (or nylon) 6, polyamide (or nylon) 6,6 or a combination thereof.

[0047] A recycled composite material according to one embodiment of the present invention may include a polyamide virgin resin, and the relative viscosity of the polyamide virgin resin may be 1.5 or higher and 3.5 or lower.

[0048] At this time, relative viscosity may mean that it is expressed in comparison with the viscosity of a comparative substance. In the present invention, the comparative substance for the relative viscosity may refer to distilled water, and the viscosity of the polyamide virgin resin may be expressed by assuming the viscosity of distilled water to be 1.0.

[0049] For example, the relative viscosity of the above polyamide virgin resin may be 1.7 or more and 3.3 or less, 1.9 or more and 3.1 or less, 2.1 or more and 2.9 or less, 2.2 or more and 2.7 or less, or 2.3 or more and 2.5 or less.

[0050] A recycled composite material according to one embodiment of the present invention may include the polyamide recycled composite material, and the polyamide recycled composite material may be derived from scrapped vehicle parts.

[0051] For example, the scrap parts may include a cylinder head cover, an oil filter cover, a manifold, an engine cover, an engine cooling fan, a front end module, a radiator fan, an EV sensor housing, a motor housing, a battery cooling valve, or a combination thereof.

[0052] A recycled composite material according to one embodiment of the present invention may include a polyamide recycled composite material, and the polyamide recycled composite material may include a polyamide resin and a reinforcing agent, and the weight ratio of the polyamide resin to the reinforcing agent (weight of the polyamide resin: weight of the reinforcing agent) may be 6:4 to 8:2. In this case, the reinforcing agent may include glass fibers, carbon fibers, aramid fibers, or a combination thereof.

[0053] For example, the weight ratio of polyamide resin to glass fiber can be 6:4, 6.5:3.5, 7:3, 7.5:2.5, or 8:2.

[0054] The polyamide recycled composite material according to one embodiment of the present invention may have a specific gravity of 0.8 to 2 as measured in accordance with ISO 1183.

[0055] For example, the specific gravity of the above-mentioned polyamide recycled composite material may be 0.8 to 2, 0.9 to 1.8, 1.0 to 1.6, 1.1 to 1.5, or 1.2 to 1.4.

[0056] According to one embodiment of the present invention, a polyamide recycled composite material may have a tensile strength of 100 MPa or more when measured in accordance with ISO 527 at 23°C.

[0057] For example, the tensile strength of the above polyamide recycled composite material measured at 23°C in accordance with ISO 527 may be 100 to 140 MPa, 105 to 135 MPa, 110 to 130 MPa, or 115 MPa to 120 MPa.

[0058] According to one embodiment of the present invention, a recycled polyamide composite material may have a flexural strength of 170 MPa or more as measured in accordance with ISO 178 at 23°C.

[0059] For example, the tensile strength of the above polyamide recycled composite material measured at 23°C according to ISO 178 may be 170 to 230 MPa, 180 to 220 MPa, 190 to 210 MPa, or 195 MPa to 205 MPa.

[0060] According to one embodiment of the present invention, the flexural modulus of a recycled polyamide composite material measured in accordance with ISO 178 at 23°C may be 6,500 MPa or higher.

[0061] For example, the flexural modulus of the above polyamide recycled composite material measured according to ISO 178 at 23°C may be 6,500 to 8,500 MPa, 6,700 to 8,200 MPa, 6,900 to 8,000 MPa, or 7,100 to 7,800 MPa.

[0062] The IZOD impact strength of a recycled polyamide composite material according to one embodiment of the present invention, measured at 23°C in accordance with ISO 180, is 55 KJ / m 2 It could be more than that.

[0063] For example, the impact strength of the above recycled polyamide composite material measured at 23°C in accordance with ISO 180 is 55 to 100 KJ / m 2 , 57 to 95 KJ / m 2 , 60 to 90 KJ / m 2 or 62 to 85 KJ / m 2 It could be.

[0064] According to one embodiment of the present invention, a polyamide recycled composite material may have a hardness of 100 HRR or more when measured on an R-scale according to ISO 2039-2 at 23°C.

[0065] For example, the hardness of the above polyamide recycled composite material measured on an R-scale according to ISO 2039-2 at 23°C may be 100 to 160 HRR, 105 to 150 HRR, 110 to 140 HRR, or 115 to 135 HRR.

[0066] A recycled composite material according to one embodiment of the present invention comprises a virgin reinforcing agent, and said virgin reinforcing agent may be glass fiber, carbon fiber, aramid fiber, or a combination thereof.

[0067] In this case, the glass fiber may be a high-rigidity S-glass fiber. S-glass fiber has higher tensile strength and tensile modulus compared to other types of glass fiber, making it suitable for use as a reinforcing agent.

[0068] For example, the high-rigidity S-glass fiber can have a tensile strength of 4,500 MPa or more at 22°C and a tensile modulus of elasticity of 80 GPa or more.

[0069] In addition, the S-glass fiber may include silicon dioxide (SiO2), aluminum oxide (Al2O3), and magnesium oxide (MgO), and the content of each component may be 55 to 75 weight%, 20 to 30 weight%, and 5 to 15 weight%, and optionally may additionally include sodium oxide (Na2O).

[0070] A recycled composite material according to one embodiment of the present invention may include an additive, and said additive may include an acid inhibitor, a heat retardant, a lubricant, a pigment, or a combination thereof.

[0071] For example, the above acid inhibitor may be N,N'-(Hexane-1,6-diyl)bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide)(N,N'-(Hexane-1,6-diyl)bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide))(CAS No. 23128-74-7) and may be 0.1 to 0.6 weight% based on 100 weight% of the total weight of the recycled composite material.

[0072] For example, the above heat-resistant agent may be one or more of the above heat-resistant agents, and the first heat-resistant agent may be Tris(2-ethylhexyl) Trimellitate (CAS No. 3319-31-1), Magnesium stearate (CAS No. 557-04-0), Potassium iodide (CAS No. 7681-11-0), Cuprous iodide (CAS No. 7681-65-4), or a combination thereof, and may be 1.0 to 2 weight% based on 100 weight% of the total weight of the recycled composite material.

[0073] For example, the second heat-resistant agent may be a dipentaerythritol hexaacrylate-dipentaerythritol pentaacrylate copolymer (CAS No. 82277-45-0), and may be 0.3 to 1.0 weight% based on 100 weight% of the total weight of the recycled composite material.

[0074] For example, the above lubricant may be ethylene distearamide (Cas No. 68390-94-3) and may be 0.1 to 0.6 weight% based on 100 weight% of the total weight of the recycled composite material.

[0075] For example, the pigment may be Solvent Black 7 (Cas No. 8005-02-5) and may be 0.5 to 1.8 weight percent based on 100 weight percent of the total weight of the recycled composite material.

[0077] A recycled composite material according to one embodiment of the present invention may have a tensile strength of 190 MPa or more when measured at a test speed of 5 mm / min in accordance with ISO 527.

[0078] For example, the tensile strength of the above recycled composite material measured according to ISO 527 at 23°C may be 190 to 240 MPa, 195 to 230 MPa, or 200 to 220 MPa.

[0079] A recycled composite material according to one embodiment of the present invention may have a flexural strength of 275 MPa or more when measured at a test speed of 2 mm / min in accordance with ISO 178.

[0080] For example, the flexural strength of the above recycled composite material measured according to ISO 178 at 23°C may be 275 to 350 MPa, 277 to 340 MPa, or 280 to 330 MPa.

[0081] A recycled composite material according to one embodiment of the present invention may have a flexural modulus of 8,000 MPa or more when measured at a test speed of 2 mm / min in accordance with ISO 178.

[0082] For example, the flexural modulus of the above recycled composite material measured according to ISO 178 at 23°C may be 8,000 to 13,000 MPa, 8,200 to 12,000 MPa, or 8,400 to 11,000 MPa.

[0083] A recycled composite material according to one embodiment of the present invention has an IZOD impact strength of 110 KJ / m² as measured in accordance with ISO 180. 2 It could be more than that.

[0084] For example, the IZOD impact strength of the above recycled composite material measured at 23°C in accordance with ISO 180 is 110 to 140 KJ / m 2 , 112 to 138 KJ / m 2 , 114 to 136 KJ / m 2 or 115 to 134 KJ / m 2 It could be.

[0085] According to one embodiment of the present invention, the recycled composite material may have a heat deformation temperature of 240°C or higher under a load of 1.82 MPa measured in accordance with ISO 75.

[0086] For example, the heat deformation temperature of the above recycled composite material may be 240 to 280°C, 245 to 270°C, 247 to 265°C, or 250 to 260°C.

[0087] A recycled composite material according to one embodiment of the present invention may have a tensile strength of 85% or more based on the tensile strength measured before leaving the recycled composite material in a test solution at 160°C for 1,000 hours. In this case, the test solution may refer to a solution prepared by mixing antifreeze and distilled water in a weight ratio of 1:1.

[0088] For example, the tensile strength measurement value after leaving the recycled composite material in a test solution at 160°C for 1,000 hours may be 85% or more and 98% or less, 87% or more and 95% or less, and 88% or more and 93% or less of the tensile strength measurement value before leaving the recycled composite material in the test solution.

[0089] According to one embodiment of the present invention, the regenerated composite material may have an impact strength of 85% or more based on the impact strength measured before leaving the regenerated composite material in a test solution at 160°C for 1,000 hours. In this case, the test solution may refer to a solution prepared by mixing antifreeze and distilled water in a weight ratio of 1:1.

[0090] For example, the impact strength measurement value after leaving the recycled composite material in a test solution at 160°C for 1,000 hours may be 85% or more and 98% or less, 87% or more and 95% or less, and 88% or more and 93% or less of the impact strength measurement value before leaving the recycled composite material in the test solution.

[0091] A method for manufacturing a recycled composite material according to one embodiment of the present invention may include: a first step of crushing a waste polyamide composite material; a second step of washing the waste polyamide composite material that has undergone the first step to produce the polyamide recycled composite material; and a third step of regenerating the polyamide recycled composite material.

[0092] The above first and second steps may be repeated with the same process or with different degrees of crushing and / or washing methods, and the washing step may include a dehydration step.

[0093] In a method for manufacturing a recycled composite material according to one embodiment of the present invention, the washing solution used to wash the waste polyamide composite material in the second step may include tannic acid, sodium lignin sulfonate, Triton X-100, or a combination thereof.

[0094] For example, based on 100% by weight of the total weight of the washing solution, the washing solution may contain 2 to 5% by weight of the tannic acid, 5 to 10% by weight of the sodium lignin sulfonate, 2 to 6% by weight of the Triton X-100, and 80 to 90% by weight of distilled water.

[0095] The third step of the method for manufacturing a recycled composite material according to one embodiment of the present invention may include a process of adding the polyamide virgin resin, the virgin reinforcing agent, the additive, or a combination thereof to the recycled composite material and extruding it.

[0097] The operation and effects of the invention will be described in more detail below through specific embodiments. However, these embodiments are merely examples of the invention and do not define the scope of the invention.

[0099] Preparation Example

[0100] A recycled polyamide composite material was manufactured by crushing and washing polypolyamide composite materials derived from scrapped vehicle parts.

[0101] First, the waste polyamide composite material was crushed to an average size of 45 mm using a crusher (first crushing step).

[0102] Subsequently, the crushed waste polyamide composite material was washed. The crushed waste polyamide composite material was introduced into a washing tank filled with a first liquid (water) maintained at 90°C and equipped with a bubble generating device, and was washed with bubble circulating water for 4 minutes to generate microbubbles (bubble average diameter: 20μm) (first washing step), and dehydrated at a temperature of 70°C for 4 hours (first dehydration step).

[0103] After crushing the waste polyamide composite material through the first washing step and the first dehydration step into an average size of 3 mm using a crusher (second crushing step), it is introduced into a washing tank filled with a second liquid (water containing a detergent) maintained at 50°C, washed for 4 minutes (second washing step), dehydrated at a temperature of 70°C for 4 hours (second dehydration step), and dried at a temperature of 70°C for 4 hours.

[0104] The second liquid of the second washing step contained 7 wt% sodium lignin sulfonate (Cas No. 8061-54-6), 3 wt% tannic acid (Cas No. 1401-55-4), and 4 wt% Triton X-100 (Cas No. 9036-19-5) based on 100 wt% of the total weight of the second liquid.

[0106] Examples

[0107] A recycled composite material was prepared by adding polyamide virgin resin (relative viscosity 2.4), a virgin reinforcing agent, and additives to the polyamide recycled composite material prepared according to the preparation example and extruding it. The content of each component is shown in Table 1 below.

[0108] At this time, the polyamide recycled composite material prepared according to the manufacturing example was subjected to ash content measurement in accordance with ISO 3451, and it was confirmed that the weight ratio of the polyamide resin and glass fiber constituting the polyamide was 7:3. Accordingly, the content of glass fiber contained in the polyamide recycled composite material was 9% by weight based on 100% by weight of the total weight of the recycled composite material.

[0109] The total glass fiber content of the recycled composite material of the example was 35% by weight, based on 100% by weight of the total weight of the recycled composite material, by adding the glass fibers included in the polyamide recycled composite material and the added virgin reinforcing agent.

[0111] ingredient Composition (weight %) recycled composite materials 30 Polyamide virgin resin 40.6 Virgin Reinforcement (S-Glass Fiber, HMG135TMS) 26 additives 1st heat-resistant agent 1.5 pigment 1 2nd heat-resistant agent 0.5 Sanbangjeje 0.2 lubricant 0.2 total 100

[0113] In Table 1 above, the first heat-resistant agent was a combination of Tris(2-ethylhexyl) Trimellitate (CAS No. 3319-31-1), Magnesium stearate (CAS No. 557-04-0), Potassium iodide (CAS No. 7681-11-0), and Cuprous iodide (CAS No. 7681-65-4).

[0114] In Table 1 above, the pigment was solvent black 7 (Cas No. 8005-02-5).

[0115] In Table 1 above, the second heat-resistant agent was dipentaerythritol hexaacrylate-dipentaerythritol pentaacrylate copolymer (CAS No. 82277-45-0).

[0116] In Table 1 above, the acid inhibitor was N,N'-(hexane-1,6-diyl)bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide)(N,N'-(Hexane-1,6-diyl)bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide))(CAS No. 23128-74-7).

[0117] In Table 1 above, the lubricant was ethylene distearamide (Cas No. 68390-94-3).

[0119] Comparative Example 1

[0120] A composite material was manufactured by mixing polyamide virgin resin, a virgin reinforcing agent, and additives, and then extruding the mixture, without using recycled composite materials. At this time, general glass fibers for NY were used as the virgin reinforcing agent. The content of each component is shown in Table 2 below.

[0121] The glass fiber content included in Comparative Example 1 was 35% by weight based on 100% by weight of the total weight of the composite material, which was the same as the total glass fiber content of the example.

[0123] ingredient Composition (weight %) Polyamide virgin resin 61.6 Virgin Reinforcement (Glass Fiber for NY, T-435) 35 additives 1st heat-resistant agent 1.5 pigment 1 2nd heat-resistant agent 0.5 Sanbangjeje 0.2 lubricant 0.2 total 100

[0125] In Table 2 above, the Cas No. of each component was the same as in the example.

[0127] Comparative Example 2

[0128] A composite material was prepared in the same manner as Comparative Example 1, except that high-rigidity S-glass fibers were used as the virgin reinforcing agent. The content of each component is shown in Table 3 below.

[0129] The glass fiber content included in Comparative Example 2 is 35% by weight based on 100% by weight of the total weight of the composite material, which is the same as the total glass fiber content of the Example and Comparative Example 1.

[0131] ingredient Composition (weight %) Polyamide virgin resin 61.6 Virgin Reinforcement (S-Glass Fiber, HMG135TMS) 35 additives 1st heat-resistant agent 1.5 pigment 1 2nd heat-resistant agent 0.5 Sanbangjeje 0.2 lubricant 0.2 total 100

[0133] In Table 3 above, the Cas No. of each component was the same as Comparative Example 1.

[0135] Evaluation Example 1

[0136] In addition, the physical properties of the above-mentioned recycled polyamide composite material, including specific gravity, tensile strength, flexural strength, flexural modulus, IZOD impact strength, and hardness, were measured. The measurement method, measurement conditions, and measurement values ​​for each physical property are shown in Table 4 below.

[0138] Physical properties Evaluation method Measured temperature Test speed Measured value specific gravity ISO 1183 - - 1.367 tensile strength ISO 527 23℃ 5 mm / min 116 MPa Flexural strength ISO 178 23℃ 2 mm / min 197 MPa Flexural modulus ISO 178 23℃ 2 mm / min 7,228 MPa IZOD Impact Strength ISO 180 23℃ - 71 KJ / m 2 hardness ISO 2039-2 - 120 R-Scale

[0140] The specific gravity of the above recycled polyamide composite material was 1.367, which was not significantly different from the examples and comparative examples, but it was confirmed that the tensile strength, flexural strength, flexural modulus, and impact strength were significantly lower.

[0141] In other words, it was confirmed that the desired physical properties cannot be sufficiently secured using recycled composite materials alone.

[0143] Evaluation Example 2

[0144] The tensile strength, flexural strength, flexural modulus, IZOD impact strength, and heat distortion temperature of the composite materials prepared according to the above examples and comparative examples were measured. The measurement methods, measurement conditions, and results for each property are shown in Table 5 below.

[0146] Physical properties Evaluation method Measured temperature Test speed (mm / min) unit Examples Comparative Example 1 Comparative Example 2 specific gravity ISO 1183 - - - 1.409 1.419 1.409 tensile strength ISO 527 23℃ 5 MPa 213.2 206.2 222.7 Flexural strength ISO 178 23℃ 2 MPa 308 277.7 312.2 Flexural modulus ISO 178 23℃ 2 MPa 10,671 10,229 10,596 IZOD Impact Strength ISO 180 23℃ - KJ / m 2 121 112 138 Heat distortion temperature ISO 75 - - ℃ 254 253 254

[0148] The tensile strength of the example was 213.2 MPa, which was superior to that of Comparative Example 1 and close to that of Comparative Example 2. This was also confirmed in the flexural strength and impact strength tests, and the flexural modulus was found to be superior to that of Comparative Example 2.

[0149] The heat distortion temperature of the example, comparative example 1, and comparative example 2 all showed similar values.

[0150] That is, according to Evaluation Example 2, it was confirmed that the embodiment of the present invention can exhibit excellent physical properties comparable to Comparative Examples 1 and 2 through recycling.

[0151] Therefore, it was confirmed that by using the embodiments of the present invention, a composite material having excellent physical properties can be manufactured at a low cost while reducing carbon emissions through recycling.

[0153] Evaluation Example 3

[0154] The tensile strength of the recycled composite material prepared according to the above example was measured after leaving it in a test solution at 160°C for 1,000 hours.

[0155] At this time, the above test solution was prepared by mixing an antifreeze containing ethylene glycol (Hyundai Mobis, 07100-00321) and distilled water in a weight ratio of 1:1.

[0156] The tensile strength after being left in the test solution was expressed as a percentage based on the tensile strength before being left, according to Formula 1 below.

[0158] [Equation 1]

[0159]

[0161] The tensile strength of the recycled composite material left in the test solution for 1,000 hours was 191.4 MPa.

[0162] According to the above Equation 1, the tensile strength retention rate of the example was found to be 89%.

[0164] In other words, it was confirmed that the recycled composite material manufactured according to the embodiment of the present invention maintains sufficient tensile strength even when exposed to high heat for a long time, and is a recycled composite material that can be used in high-temperature environments.

[0166] Evaluation Example 4

[0167] The regenerated composite material prepared according to the above example was left in a test solution at 160°C for 1,000 hours, and then its impact strength was measured.

[0168] At this time, the above test solution was prepared by mixing antifreeze and distilled water in a weight ratio of 1:1.

[0169] The tensile strength after being left in the test solution was expressed as a percentage based on the tensile strength before being left, according to Formula 2 below.

[0171] [Equation 2]

[0172]

[0174] The impact strength of the recycled composite material left in the test solution for 1,000 hours was 134 KJ / m 2 was.

[0175] According to the above Equation 2, the impact strength retention rate of the example was found to be 90%.

[0177] In other words, it was confirmed that the recycled composite material manufactured according to the embodiment of the present invention maintains sufficient impact strength even when exposed to high heat for a long time, making it a recycled composite material that can be used in high-temperature environments.

[0179] The recycled composite material of the present invention can be manufactured in an eco-friendly manner at a low cost, possesses excellent mechanical properties comparable to those of non-recycled composite materials, and maintains its physical properties even at high temperatures. Therefore, it is a recycled composite material that can be used in various conditions and fields, including diverse harsh conditions such as high temperatures.

[0181] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will understand that other specific forms can be easily modified without altering the technical spirit or essential features of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.

[0182] The scope of the present invention is defined by the claims set forth below rather than by the detailed description above, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of the present invention.

Claims

Claim 1 A recycled composite material comprising, based on 100 weight% of the total weight of the recycled composite material, 30 to 55 weight% of a polyamide virgin resin, 20 to 40 weight% of a polyamide recycled composite material, 20 to 45 weight% of a virgin reinforcing agent, and 2.5 to 6 weight% of an additive, wherein the virgin reinforcing agent comprises glass fibers, carbon fibers, aramid fibers, or a combination thereof, and wherein the tensile strength of the recycled composite material measured at a test speed of 5 mm / min in accordance with ISO 527 is 190 MPa or higher. Claim 2 In paragraph 1, the polyamide recycled composite material is a recycled composite material derived from scrapped vehicle parts. Claim 3 In claim 1, the polyamide recycled composite material comprises a polyamide resin and a reinforcing agent, wherein the weight ratio of the polyamide resin to the reinforcing agent is 6:4 to 8:2, and the reinforcing agent comprises glass fiber, carbon fiber, aramid fiber, or a combination thereof. Claim 4 delete Claim 5 A recycled composite material according to claim 1, wherein the flexural strength of the recycled composite material measured at a test speed of 2 mm / min in accordance with ISO 178 is 275 MPa or higher. Claim 6 In claim 1, the IZOD impact strength of the recycled composite material measured in accordance with ISO 180 is 110 KJ / m 2 Lee Sang-in, recycled composite material. Claim 7 A recycled composite material according to claim 1, wherein the heat distortion temperature of the recycled composite material under a load of 1.82 MPa measured in accordance with ISO 75 is 240℃ or higher. Claim 8 In claim 1, the tensile strength measured after leaving the recycled composite material in a test solution at 160°C for 1,000 hours is 85% or more of the tensile strength measured before leaving the recycled composite material in the test solution, and the test solution is prepared by mixing antifreeze and distilled water in a weight ratio of 1:

1. Claim 9 In claim 1, the impact strength measured after leaving the recycled composite material in a test solution at 160°C for 1,000 hours is 85% or more of the impact strength measured before leaving the recycled composite material in the test solution, and the test solution is prepared by mixing antifreeze and distilled water in a weight ratio of 1:

1. Claim 10 A method for manufacturing a recycled composite material according to any one of claims 1 to 3 and claims 5 to 9, comprising: a first step of crushing a waste polyamide composite material; a second step of washing the waste polyamide composite material that has undergone the first step to produce a polyamide recycled composite material; and a third step of regenerating the polyamide recycled composite material.

Citation Information

Patent Citations

  • Composite material for recycling waste vehicle nylon products and preparation method thereof

    CN101792596A

  • Cross-linked structure long glass fiber reinforced multi-copolymerized bio-based high-temperature polyamide composition as well as preparation method and application thereof

    CN114350145A

  • The resin composition from used nylon resin, andpreparing method thereof

    KR100666794B1

  • Amorphous high performance polyamide

    KR1020170007766A

  • Black-colored polyamide composition with high laser transmittance for laser welding applications

    KR1020220008320A