Resin composition suitable for dentin layer and dental simulation material using the same

A resin composition for dental prosthetics optimizes mechanical strength and viscosity by balancing filler content, enabling 3D printing and preventing cutting issues, thus producing a tooth-mimicking material with enhanced mechanical properties.

KR103045084B1Active Publication Date: 2026-11-06OSSTEMIMPLANT CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
KR1020240138743
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2026-11-06
Estimated Expiration
2044-10-11

AI Technical Summary

Technical Problem

Conventional 3D printing resins used for dental prosthetics face a trade-off between mechanical strength and viscosity, with high inorganic filler content leading to high viscosity, making 3D printing impossible, while low filler content results in unsuitable mechanical properties for prosthetics like crowns.

Method used

A resin composition for a dentin layer comprising specific ratios of polymerizable monomers, crosslinkable monomers, nanofillers, pigments, and photoinitiators, optimized to achieve high mechanical strength and low viscosity, suitable for 3D printing, with a titanium-based coupling agent enhancing curing efficiency.

Benefits of technology

The resin composition provides a tooth-mimicking material with mechanical properties similar to natural dentin, maintaining low viscosity for 3D printing and preventing sticking during cutting, ensuring excellent cutting power and workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024110734512-PAT00007_ABST
    Figure 112024110734512-PAT00007_ABST
Patent Text Reader

Abstract

A resin composition for a dentin layer is disclosed, comprising 30 to 40 parts by weight of a first polymerizable monomer; 0 to 5 parts by weight of a second polymerizable monomer; 10 to 30 parts by weight of a crosslinkable monomer; 10 to 30 parts by weight of a nanofiller; 0.01 to 0.5 parts by weight of a pigment; and 0.1 to 3 parts by weight of a photoinitiator.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a photocurable resin composition for a dentin layer with cutting power and mechanical properties similar to those of a real tooth, and a tooth-mimicking material using the same. Background Technology

[0002] When teeth are lost due to damage or defects caused by caries or fractures, it impairs speech, chewing, and aesthetics. Furthermore, adjacent teeth shift into the empty space, disrupting the normal alignment of the teeth and making them susceptible to cavities or gum disease as food gets trapped between them. When tooth damage or loss occurs, treatment is provided through dental restorations or prosthetic procedures.

[0003] Prosthetic procedures are a treatment method that replaces the site where a tooth has been extracted with fixed prosthetics, such as crowns or bridges, or removable prosthetics, such as dentures, in order to minimize side effects caused by tooth loss. Fixed prosthetics are installed by removing a portion of the surface of the adjacent natural teeth in front of and behind the missing tooth and then placing the prosthesis over them. Because they resemble natural teeth, making pronunciation comfortable and providing excellent chewing efficiency, the method of restoration using fixed prosthetics is generally preferred over removable prosthetics such as dentures.

[0004] Dental prosthetics generally include restorative materials, fillers, full and partial crowns, bridges, inlays, onlays, veneers, implants, and posts. Materials commonly used for dental prosthetics include gold, ceramics, amalgam, porcelain, PFM, PFG, and composites. Until recently, amalgam was preferred for tooth restorations and prosthetics due to its low cost and long lifespan.

[0005] However, amalgam has problems such as reduced aesthetics due to the natural color of mercury, toxicity to the human body, and environmental pollution. Gold is used for large fillings or inlays, but like amalgam, it has the problem of reduced aesthetics due to its natural color. Accordingly, ceramic or resin-ceramic materials that match the color of the teeth have been proposed.

[0006] Before performing actual procedures with such dental prosthetics, tooth-mimicking materials used in dental practice to practice procedures are also being actively developed. However, conventional tooth-mimicking materials produced by injection / injection methods based on ceramic or resin-ceramic materials have limitations in perfectly reproducing the shape of the tooth, and it is difficult to accurately replicate the structure of the tooth, and there are problems in that they cannot express the differences in physical properties between the enamel layer and the dentin layer present in the tooth.

[0007] Furthermore, there is a disadvantage in that the material burns and sticks to the cutting bur during the cutting process in dental practice, making bur recycling difficult. In addition, the cutting force of the tooth-mimicking material used as a teaching aid must be maintained above a certain level to ensure stable use in practice and, furthermore, to achieve physical properties and shapes similar to teeth.

[0008] Meanwhile, attempts are continuing to combine these tooth-mimicking materials with 3D printing technology by manufacturing them in the form of 3D printing resins. The aforementioned 3D printing technology is being introduced into the dental field because it facilitates multi-variety, small-batch production and personalized manufacturing, and is being most actively applied in the fields of prosthetics and orthodontics. Temporary crowns, splints, surgical guides, etc., are being fabricated using these 3D printing resins.

[0009] However, 3D printing resins have low mechanical strength, which makes them unsuitable for prosthetics such as crowns. Generally, the mechanical strength of resins is improved by increasing the amount of inorganic filler, but conventional resin compositions with high inorganic filler content have high viscosity, which makes 3D printing impossible.

[0010] As such, there is a trade-off relationship between mechanical strength and viscosity depending on the inorganic filler content, so the inorganic filler content of conventional 3D printing resins is limited to less than 10 parts by weight per 100 parts by weight of the total composition.

[0011] Therefore, there is an increasing demand for resin compositions for 3D printing that are applicable to 3D printers and have excellent mechanical properties, such as cutting power and mechanical properties above a certain level. The problem to be solved

[0012] The objective of the present invention is to provide a resin composition for a dentin layer with improved cutting power and mechanical properties by controlling the content of inorganic fillers, and a tooth-mimicking material using the same. means of solving the problem

[0013] According to one aspect, a resin composition for a dentin layer is provided, comprising 30 to 40 parts by weight of a first polymerizable monomer, 0 to 5 parts by weight of a second polymerizable monomer, 10 to 30 parts by weight of a crosslinkable monomer, 10 to 30 parts by weight of a nanofiller, 0.01 to 0.5 parts by weight of a pigment, and 0.1 to 3 parts by weight of a photoinitiator.

[0014] In one embodiment, the first polymerizable monomer is urethane dimethacrylate (UDMA), and the second polymerizable monomer is one or more selected from the group consisting of ethoxylated bisphenol A dimethacrylate (Bis-EMA), propoxylated bisphenol A dimethacrylate, ethoxylated bisphenol A diacrylate, propoxylated bisphenol A diacrylate, polyethylene glycol dimethacrylate, and polyethylene glycol diacrylate; and the crosslinking monomer is trimethylolpropane trimethacrylate (TMPTMA), trimethylolpropane triacrylate (TMPTA), tris (2-hydroxyethyl) isocyanurate triacrylate, ethoxylated trimethylolpropane triacrylate, and pentaerythritol. It may be one or more selected from the group consisting of triacrylates (Pentaerythritol Triacrylate).

[0015] In one embodiment, the nanofiller may have an average particle size of 1 to 100 nm.

[0016] In one embodiment, the photoinitiator may be one or more selected from the group consisting of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, camphoquinone, and 2-(dimethylamino)methacrylate.

[0017] In one embodiment, the resin composition for the dentin layer further comprises a titanium-based coupling agent, and the titanium-based coupling agent may be titanium oxide.

[0018] In one embodiment, the content of the titanium-based coupling agent may be 0 to 0.2 parts by weight per 100 parts by weight of the resin composition for the entire dentin layer.

[0019] According to another aspect, a tooth-mimicking material is provided by 3D printing the resin composition for the dentin layer. Effects of the invention

[0020] According to one aspect, a resin composition for a dentin layer suitable for 3D printing having excellent mechanical strength and low viscosity, and a tooth-mimicking material using the same are provided.

[0021] The effects of one aspect of this specification are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configurations described in the detailed description or claims of this specification. Brief explanation of the drawing

[0022] FIG. 1 is a photograph of an inventive prototype realized through the resin composition for a dentin layer of the present specification. FIG. 2 is an SEM image of nanofiller particles according to one embodiment of the present specification. Figure 3 is a graph of physical properties (flexural strength, flexural Young's modulus) according to the nano-filler content in an embodiment of the present specification. FIG. 4 is a graph of the physical properties (indentation modulus) of the embodiments and reference examples of the present specification. FIG. 5 is a graph of the physical properties (indentation hardness) of the embodiments and reference examples of the present specification. FIG. 6 is a graph of the physical properties (Vickers hardness) of the embodiments and reference examples of the present specification. FIG. 7 is a cross-sectional microscope image of the invention prototype during cutting of the embodiments and reference examples of the present specification. Specific details for implementing the invention

[0023] Hereinafter, one aspect of the present specification will be described with reference to the attached drawings. However, the details described in the present specification may be implemented in various different forms and are therefore not limited to the embodiments described herein. Furthermore, in order to clearly explain one aspect of the present specification in the drawings, parts unrelated to the explanation have been omitted, and similar parts throughout the specification have been given similar reference numerals.

[0024] When a range of numerical values ​​is described in this specification, unless a specific range is otherwise described, the value has the precision of significant figures provided according to the standard rules in chemistry for significant figures. For example, 10 includes a range of 5.0 to 14.9, and the number 10.0 includes a range of 9.50 to 10.49.

[0025] Hereinafter, an embodiment of the present specification will be described in detail with reference to the attached drawings.

[0026] Resin composition for the dentin layer

[0027] A resin composition for a dentin layer according to one aspect of the present specification may comprise 30 to 40 parts by weight of a first polymerizable monomer, 0 to 5 parts by weight of a second polymerizable monomer, 10 to 30 parts by weight of a crosslinkable monomer, 10 to 30 parts by weight of a nanofiller, 0.01 to 0.5 parts by weight of a pigment, and 0.1 to 3 parts by weight of a photoinitiator.

[0028] Conventional resin compositions for dentin layers used in 3D printing consist of a polymer resin of 90% or more by weight based on 100% by weight of the total composition due to printing issues, while the content of inorganic fillers is less than 10% by weight. Artificial teeth, including crowns, are subjected to repetitive external forces during activities such as eating, so they must possess high mechanical strength. While the strength of such resin compositions can be improved by increasing the proportion of inorganic fillers, there is a limitation in that increasing the weight ratio of inorganic fillers increases the viscosity of the resin composition, making it difficult to apply to 3D printing.

[0029] A resin composition for a dentin layer according to one aspect of the present specification has the advantage of improving mechanical strength by increasing the amount of nano-filler added, and furthermore, having a strength similar to that of the dentin layer of an actual tooth, while at the same time, the resin composition does not burn due to high-temperature frictional heat during cutting and does not stick to the tooth cutting bur.

[0030] The first polymerizable monomer may be urethane dimethacrylate (UDMA), but is not limited thereto. The urethane dimethacrylate is a material that is highly elastic and has properties suitable for use in photocurable resins. The urethane dimethacrylate may be a urethane dimethacrylate oligomer prepared by synthesizing an isocyanate-terminated urethane by reacting a polyol and a diisocyanate by a known method, and then reacting it with a (meth)acrylate containing a hydroxyl group. At this time, mechanical properties such as strength, Young's modulus, hardness, elongation, and viscosity of the resin composition for the dentin layer can be controlled depending on the type of polyol, the type of isocyanate, and the type of (meth)acrylate containing a hydroxyl group. When using urethane dimethacrylate as the first polymerizable monomer, a material having a Tg (glass transition temperature) of 20°C or higher or a viscosity of 2,000 cps or higher at 25°C may be used, but is not limited thereto.

[0031] The content of the first polymerizable monomer may be 30 to 40 parts by weight per 100 parts by weight of the total resin composition for the dentin layer, most preferably 32 to 38 parts by weight, but is not limited thereto. For example, the content of the first polymerizable monomer may be 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, or a value between two of these values, per 100 parts by weight of the resin composition for the dentin layer. If the content of the first polymerizable monomer is below the above range, the viscosity of the resin composition for the dentin layer increases, making it difficult to use for 3D printing purposes, and if it exceeds the above range, the mechanical properties deteriorate, which may weaken the strength and cutting power of the tooth-mimicking material produced thereby.

[0032] The second polymerizable monomer is one or more selected from the group consisting of ethoxylated bisphenol A dimethacrylate (Bis-EMA), propoxylated bisphenol A dimethacrylate, ethoxylated bisphenol A diacrylate, propoxylated bisphenol A diacrylate, polyethylene glycol dimethacrylate, and polyethylene glycol diacrylate, and preferably may be ethoxylated bisphenol A dimethacrylate (Bis-EMA), but is not limited thereto. The second polymerizable monomer can perform the function of preventing excessive shrinkage of the resin composition due to the addition of the crosslinking monomer and controlling physical properties by controlling the ethoxylated length.

[0033] The content of the second polymerizable monomer may be 0 to 5 parts by weight per 100 parts by weight of the total resin composition for the dentin layer. For example, the content of the second polymerizable monomer may be 0 parts by weight, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, or a value between two of these values ​​per 100 parts by weight of the resin composition for the dentin layer. If the content of the second polymerizable monomer does not satisfy the above range, the viscosity of the resin composition for the dentin layer becomes excessively low, which may result in poor mechanical properties, and thereby weaken the strength and cutting power of the tooth-mimicking material produced.

[0034] The above-mentioned crosslinking monomer is one or more selected from the group consisting of trimethylolpropane trimethacrylate (TMPTMA), trimethylolpropane triacrylate (TMPTA), tris (2-Hydroxy Ethyl) Isocyanurate triacrylate, ethoxylated trimethylolpropane triacrylate, and pentaerythritol triacrylate, and preferably may be trimethylolpropane trimethacrylate (TMPTMA), but is not limited thereto. The above-mentioned crosslinking monomer has a trisubstitution reaction group and can serve as a crosslinker that strengthens the polymer network structure and controls the viscosity of the resin composition.

[0035] The content of the above-mentioned crosslinkable monomer may be 10 to 30 parts by weight per 100 parts by weight of the total resin composition for the dentin layer, but is not limited thereto. For example, the content of the above-mentioned crosslinkable monomer may be 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, or a value between two of these values, per 100 parts by weight of the resin composition for the dentin layer. If the content of the above-mentioned crosslinkable monomer falls outside the above range, the polymerization reaction may decrease or the viscosity may increase excessively.

[0036] The above nanofiller can be added to a resin composition to achieve high mechanical strength. The nanofiller is not limited in shape and may be silica having various forms such as needle-shaped, cylindrical, or amorphous.

[0037] The content of the nano-filler may be 10 to 30 parts by weight per 100 parts by weight of the resin composition for the dentin layer, but is not limited thereto. For example, the content of the nano-filler may be 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, or a value between two of these values, per 100 parts by weight of the resin composition for the dentin layer. If the content of the nano-filler exceeds the above range, the viscosity may increase excessively, which may degrade the output quality during 3D printing, and if it is below the above range, the mechanical properties may deteriorate, which may weaken the strength and cutting power of the tooth-mimicking material produced therefrom.

[0038] The above photoinitiator can form free radicals to induce a chain photopolymerization reaction of the oligomer or monomer. The above photoinitiator may be one selected from the group consisting of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, camphoquinone, 2-(dimethylamino)methacrylate, and a mixture of two or more of these, and preferably may be phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, but is not limited thereto.

[0039] The content of the above photoinitiator may be 0.1 to 3 parts by weight per 100 parts by weight of the total resin composition for the dentin layer. For example, it may be 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, or a range between two of these values, but is not limited thereto. If the content of the above photoinitiator falls outside the above range, sufficient polymerization and curing may not occur, and the physical properties of the resin composition may deteriorate.

[0040] As shown in Figure 1, the enamel layer corresponding to part a of the tooth-mimicking material is the part exposed to the outside of the tooth, and the dentin layer of part b is the inner part of the tooth and does not come into direct contact with the outside, so it must have a lower indentation modulus, indentation hardness, flexural modulus of Young, and a higher flexural strength compared to part a.

[0041] To this end, by optimizing the composition ratio of the resin composition for the dentin layer to satisfy the above content ratio, the mechanical properties are controlled to be excellent, and when manufacturing a tooth-mimicking material, particularly a dentin layer of a tooth, with the resin composition, a tooth-mimicking material with excellent mechanical properties and cutting power and excellent workability can be obtained.

[0042] The average particle size of the nanofiller may be 10 to 100 nm, preferably 10 to 50 nm, but is not limited thereto. For example, it may be 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, or a value between two of these values, but is not limited thereto. If the average particle size of the nanofiller satisfies the above range, the mechanical strength of the resin composition and the degradation of physical properties due to moisture can be effectively improved. On the other hand, if the average particle size of the nanofiller deviates from the above range, the mixability with other components may decrease, or excessive bubbles may be generated, which may degrade the physical properties of the resin composition.

[0043] The average particle size of the silica used as the nanofiller can be measured using software after field emission scanning electron microscopy (FE-SEM) imaging as shown in Fig. 2, but is not limited thereto and may also be measured using a particle size analyzer, light scattering method, electrophoretic scattering method, centrifugation method, electrical resistance method, etc.

[0044] The above nanofiller may be functionalized with 0.5 to 3 parts by weight of a silane compound. The above silane compound may be at least one selected from the group consisting of chlorosilane, alkoxysilane, aminosilane, and silazane. Examples include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, gamma-methacryloxypropyltrimethoxysilane, dimethyl dichlorosilane, hexamethylene disilazane, and dimethyl polysiloxane, but are not limited thereto. Silane-functionalized silica may have improved dispersibility due to changes in surface properties. Silane-functionalized silica can form a network structure through chemical bonding, and the mechanical properties of the final product may be improved. Using such silica, it is possible to prepare a resin composition for a dentin layer that has low viscosity while containing 10 parts by weight or more of nanofiller per 100 parts by weight of the total composition.

[0045] The resin composition for the dentin layer may include a pigment to distinguish it from other compositions. There are no restrictions on the color of the pigment, but iron oxide (III) may be used, and is not limited thereto.

[0046] The content of the above pigment may be 0.01 to 0.5 parts by weight per 100 parts by weight of the resin composition for the dentin layer. For example, the content of the above pigment may be 0.01 parts by weight, 0.02 parts by weight, 0.03 parts by weight, 0.04 parts by weight, 0.05 parts by weight, 0.06 parts by weight, 0.07 parts by weight, 0.08 parts by weight, 0.09 parts by weight, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, or 0.5 parts by weight per 100 parts by weight of the resin composition for the dentin layer. If the content of the above pigment exceeds the above range, the mechanical properties of the resin composition may deteriorate or the viscosity may become excessively high.

[0047] The resin composition for the dentin layer above may further include a titanium-based coupling agent. Here, it is preferable to use a titanium-based coupling agent that improves the curing efficiency by the active energy line during photopolymerization, and it can be appropriately selected depending on the wavelength of the active energy line used during curing.

[0048] The above titanium-based coupling agent may be titanium oxide or titanium yellow, preferably titanium oxide, but is not limited thereto.

[0049] The content of the titanium-based coupling agent may be 0 to 0.2 parts by weight per 100 parts by weight of the resin composition for the dentin layer. For example, the content of the titanium-based coupling agent may be 0 parts by weight, 0.01 parts by weight, 0.02 parts by weight, 0.03 parts by weight, 0.04 parts by weight, 0.05 parts by weight, 0.06 parts by weight, 0.07 parts by weight, 0.08 parts by weight, 0.09 parts by weight, 0.1 parts by weight, 0.11 parts by weight, 0.12 parts by weight, 0.13 parts by weight, 0.14 parts by weight, 0.15 parts by weight, 0.16 parts by weight, 0.17 parts by weight, 0.18 parts by weight, 0.19 parts by weight, 0.2 parts by weight, or a value between two of these values, per 100 parts by weight of the resin composition for the dentin layer. If the content of the titanium-based coupling agent exceeds the above range, curing proceeds excessively quickly, which may reduce the workability of the resin composition.

[0050] The viscosity of the resin composition for the dentin layer may be 3,000 cps or less at 25°C, but is not limited thereto. For example, the viscosity of the resin composition for the dentin layer may be 3,000 cps, 2,750 cps, 2,500 cps, 2,250 cps, 2,000 cps, 1,750 cps, 1,500 cps, 1,250 cps, 1,000 cps, 750 cps, 500 cps, 250 cps, or a value between two of these values ​​at 25°C, but is not limited thereto.

[0051] The viscosity of the resin composition for the dentin layer at 25°C may exceed 3,000 cps depending on the specifications of the output 3D printer or the presence or absence of additional devices, and output may be possible even in such cases. The additional devices may include a resin bath heating device, a surface level homogenization device (recoater), etc.

[0052] The 25°C viscosity of the resin composition for the dentin layer of the present invention is optimized for a photocurable 3D printer without the above-mentioned additional device, and is optimized to 3,000 cps or less, but is not limited thereto.

[0053] Here, if the remaining components excluding the nano-filler in the resin composition for the dentin layer are mixed such that the viscosity at 25°C is 1,000 cps or less, the viscosity at 25°C of the resin composition for the dentin layer can be easily adjusted to 3,000 cps or less.

[0054] tooth-mimicking material

[0055] A tooth-mimicking material according to another aspect of the present specification is manufactured by curing the resin composition for the dentin layer using a 3D printer or the like, and since it has excellent mechanical properties, it can have properties similar to the dentin layer of an actual tooth when used as a teaching aid for dental practice.

[0056] The flexural strength of the tooth-mimicking material cured from the resin composition for the dentin layer may be 100 to 150 MPa, but is not limited thereto. For example, the flexural strength of the tooth-mimicking material cured from the resin composition for the dentin layer may be 150 MPa, 145 MPa, 140 MPa, 135 MPa, 130 MPa, 125 MPa, 120 MPa, 115 MPa, 110 MPa, 105 MPa, 100 MPa, or a value between two of these values, but is not limited thereto. If the flexural strength of the tooth-mimicking material cured from the resin composition for the dentin layer falls outside the above range, the viscosity may become excessively high or the mechanical properties may deteriorate, making it impossible to secure the cutting power of the tooth-mimicking material, and the powder generated as the cured resin is ground during cutting may stick to the cutting bur due to high-temperature frictional heat.

[0057] The flexural modulus of the tooth-mimicking material cured from the resin composition for the dentin layer may be 3500 MPa or higher, but is not limited thereto. If the flexural modulus of the tooth-mimicking material cured from the resin composition for the dentin layer is below the above range, the mechanical properties may deteriorate, and the cutting power of the tooth-mimicking material may not be secured, and the powder generated as the cured resin is ground during cutting may stick to the cutting bur due to high-temperature frictional heat.

[0058] The indentation modulus of the tooth-mimicking material cured from the resin composition for the dentin layer may be 5 GPa or higher, but is not limited thereto. If the indentation modulus of the tooth-mimicking material cured from the resin composition for the dentin layer is below the above range, the mechanical properties may be weakened, and the cutting power of the tooth-mimicking material may not be secured, and the powder generated as the cured resin is ground during cutting may stick to the cutting bur due to high-temperature frictional heat.

[0059] The indentation hardness of the tooth-mimicking material cured from the resin composition for the dentin layer may be 0.3 GPa or higher, but is not limited thereto. If the indentation hardness of the tooth-mimicking material cured from the resin composition for the dentin layer is below the above range, the mechanical properties may be weakened, and the cutting power of the tooth-mimicking material may not be secured, and powder generated as the resin cured material is ground during cutting may stick to the cutting bur due to high-temperature frictional heat.

[0060] The Vickers hardness of the tooth-mimicking material cured from the resin composition for the dentin layer may be 30 HV or higher, but is not limited thereto. If the Vickers hardness of the tooth-mimicking material cured from the resin composition for the dentin layer is below the above range, the mechanical properties may be weakened, and the cutting power of the tooth-mimicking material may not be secured, and the powder generated as the cured resin is ground during cutting may stick to the cutting bur due to high-temperature frictional heat.

[0061] The embodiments of this specification will be described in more detail below. However, the following experimental results represent only representative results among the above embodiments, and the scope and content of this specification should not be interpreted as being narrowed or limited by the embodiments. The specific effects of each of the various embodiments of this specification that are not explicitly presented below will be described in detail in the relevant section. Unless otherwise stated, each experiment was performed at room temperature (20°C) and atmospheric pressure (1 bar).

[0062] Examples

[0063] A resin composition was prepared by adding 32.96 parts by weight of urethane dimethacrylate (UDMA), 4.99 parts by weight of ethoxylated bisphenol A dimethacrylate (Bis-EMA), 29.96 parts by weight of trimethylolpropane trimethacrylate (TMPTMA), 29.96 parts by weight of silica filler having an average particle size of 20 nm and an aspect ratio of 1:1, 2 parts by weight of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 0.08 parts by weight of titanium oxide, 0.04 parts by weight of yellow pigment (iron(III) oxide), and zirconia balls to a mixing container and performing ball milling for 12 hours at 100 rpm.

[0064] The prepared resin composition was degassed by rotating and revolving with a paste mixer PDM-300V (Daehwa Tech Co.) for 5 minutes at 1,000 rpm.

[0065] Comparative example

[0066] A resin composition was prepared in the same manner as in Example 1, except that 49.96 parts by weight of urethane dimethacrylate and 3 parts by weight of silica filler were used.

[0067] Reference Example

[0068] A 2-layer A20A-200 was used as a Nissin product used as a model for simulating teeth.

[0069] Experimental Example 1: Evaluation of Physical Properties of Resin Composition 1 (Flexural Strength and Flexural Young's Modulus)

[0070] To confirm the difference in physical properties according to the resin composition ratio of the examples and comparative examples, the resin compositions of the examples and comparative examples were printed using a 3D printer and processed into beam-shaped specimens with dimensions of 2*2*25 mm, and the flexural strength and flexural Young's modulus of each cured resin composition were measured in accordance with ISO 4049:2009, and the results are shown in Fig. 3.

[0071] Figure 3(a) shows the flexural strength measurements. It can be seen that the comparative example exhibits relatively high flexural strength as the viscosity increases due to the addition of less filler compared to the example. Additionally, Figure 3(b) records the flexural modulus measurements. Based on the fact that the flexural modulus of the example is higher than that of the comparative example, it can be confirmed that the viscosity of the example is maintained at an appropriate level, resulting in excellent moldability and workability for the desired shape, and thus making it easy to utilize as a tooth-mimicking material.

[0072] Experimental Example 2: Evaluation of Physical Properties of Resin Composition 2 (Indentation Modulus, Indentation Hardness, and Vickers Hardness)

[0073] In order to examine the differences in physical properties according to the resin composition ratios of the examples and reference examples, the resin compositions of the examples and reference examples were printed using a 3D printer, and the indentation modulus and indentation hardness were measured using an Ultra Nanoindentation Tester. Additionally, the Vickers hardness was measured according to ISO 9693 standards using a durometer, and the results are shown in Figures 4 to 6.

[0074] Referring to FIGS. 4 to 6, when checking the indentation hardness and Vickers hardness, which are important physical properties of tooth-mimicking materials, the embodiment satisfying the nano-filler content ratio of the present invention showed relatively low indentation hardness and Vickers hardness, and accordingly, it can be confirmed that mechanical properties similar to the dentin layer of actual natural teeth can be achieved. Therefore, it was confirmed that when a tooth-mimicking material is manufactured using the resin composition for the dentin layer of the present invention, it possesses excellent mechanical properties as an enamel layer for dental practice teaching aids.

[0075] In contrast, the reference example, which is a conventional resin composition, was found to have a higher indentation modulus compared to the example, but its indentation hardness and Vickers hardness were also higher than those of the example, so it is deemed unsuitable for use as an enamel layer and not suitable for use as a dentin layer.

[0076] Experimental Example 3: Evaluation of cutting-related properties of resin composition

[0077] In order to evaluate the cutting force and cutting efficiency when manufacturing tooth-mimicking materials using cured resin compositions, the resin compositions of the examples and reference examples were printed using a 3D printer, and cutting was performed by rotating a cutting bur at high speed. Subsequently, microscopic observations were performed regarding powder scattering during processing and the surface shape after processing, and the resulting photographs are shown in Fig. 7. In addition, a survey evaluation (10-point scale) by an operator regarding whether material adhered to the cutting bur and the cutting force was also conducted, assigning 10 points for the best results and 0 points for the worst results, which are recorded in Table 1 below.

[0078] natural teeth Examples Reference Example Whether cutting tools are stuck X X O cutting power 10 points 7.5 points 6.5 points

[0080] Referring to FIG. 7, it can be seen that in the example, powder is generated at a level similar to natural teeth during processing, and the shape of the surface after cutting is very similar to natural teeth. Therefore, it can be seen that the example satisfying the composition ratio of the present invention has excellent cutting power and possesses mechanical properties similar to actual teeth. In contrast, in the reference example, the cutting surface is excessively smooth during processing, and the shape of the generated fine powder is different from that of natural teeth.

[0081] In Table 1 above, it was confirmed that in the reference example, the powder of the resin cured product melted and stuck to the high-temperature cutting instrument, resulting in reduced workability. In addition, it was confirmed that the evaluation of the operator's cutting force was worse compared to natural teeth and the examples. Therefore, it was confirmed that the examples satisfying the composition ratio of the present invention have excellent cutting force and excellent workability, as mechanical properties similar to the dentin layer of actual teeth are secured.

[0082] The foregoing description of this specification is for illustrative purposes only, and those skilled in the art to which one aspect of this specification pertains will understand that other specific forms can be easily modified without altering the technical concept or essential features described in this specification. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.

[0083] The scope of this specification is defined by the claims set forth below, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of this specification.

Claims

Claim 1 30 to 40 parts by weight of urethane dimethacrylate (UDMA); 0 to 5 parts by weight of a second polymerizable monomer selected from the group consisting of ethoxylated bisphenol A dimethacrylate (Bis-EMA), propoxylated bisphenol A dimethacrylate, ethoxylated bisphenol A diacrylate, propoxylated bisphenol A diacrylate, polyethylene glycol dimethacrylate, and polyethylene glycol diacrylate; trimethylolpropane trimethacrylate (TMPTMA), trimethylolpropane triacrylate (TMPTA), tris (2-Hydroxy Ethyl) isocyanurate triacrylate, ethoxylated trimethylolpropane triacrylate, and pentaerythritol triacrylate. A resin composition for a dentin layer comprising: 10 to 30 parts by weight of a crosslinkable monomer selected from the group consisting of triacrylates; 10 to 30 parts by weight of a silica filler having an average particle size of 1 to 100 nm; 0.01 to 0.5 parts by weight of a pigment; and 0.1 to 3 parts by weight of a photoinitiator. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 A resin composition for a dentin layer according to claim 1, wherein the photoinitiator is one or more selected from the group consisting of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, camphoquinone, and 2-(dimethylamino)methacrylate. Claim 7 A resin composition for a dentin layer according to claim 1, wherein the resin composition for a dentin layer further comprises a titanium-based coupling agent, and the titanium-based coupling agent is titanium oxide. Claim 8 A resin composition for a dentin layer according to claim 7, wherein the content of the titanium-based coupling agent is 0 to 0.2 parts by weight per 100 parts by weight of the total resin composition for the dentin layer. Claim 9 A tooth-mimicking material manufactured by 3D printing a resin composition for a dentin layer according to any one of claims 1, 6 to 8.

Citation Information

Patent Citations

  • Photo-curable resin compositions and method of using the same in three-dimensional printing for manufacturing artificial teeth and denture base

    KR1020160055727A

  • Photo-curable resin compositions and article using the same

    KR1020190001784A

  • Photo-curable resin compositions and article using the same

    KR1020190001794A

  • Castable resin composition with quality of complete combustion and volumetric stability for dental 3D printer

    KR1020220049343A

  • Polymerizable monomer composition for dental restoration, method for producing the same, and method for using the same

    KR1020230015317A