Polarizing film and method of manufacturing the same
A polarizing film with specific boron-containing compound ratios and distributions addresses the challenges of high polarization performance and transmittance in LCDs by enhancing crosslinking and orientation, achieving improved optical properties and manufacturing efficiency.
Patent Information
- Application Number
- KR1020227030416
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-13
- Filing Date
- 2021-03-11
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2041-03-11
AI Technical Summary
Existing polarizing films face challenges in achieving high polarization performance and transmittance, particularly in high-resolution LCDs, due to issues with PVA stretchability and iodine-based pigment decomposition, and existing methods do not adequately address these needs.
A polarizing film comprising PVA with specific ratios and concentrations of boron-containing compounds, such as monoboronic acid and boric acid, is formulated to enhance crosslinking and orientation, ensuring high boron element content near the surface and controlled distribution throughout the film.
The film achieves high polarization performance and transmittance, with improved orientation and reduced iodine-based pigment relaxation, resulting in enhanced optical properties and manufacturing ease.
Smart Images

Figure 112022092255359-PCT00008_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a polarizing film and a method for manufacturing the same. Background Technology
[0002] Polarizers, which possess light transmission and shielding functions, are fundamental components of liquid crystal displays (LCDs) along with liquid crystals that change the polarization state of light. To prevent fading or shrinkage of the polarizing film, most polarizers have a structure in which a protective film, such as a tricellulose acetate (TAC) film, is laminated onto the surface of the polarizing film. As for the polarizing film constituting the polarizer, an iodine-based dye (I 3- I 5- The mainstream consists of adsorbed substances (etc.).
[0003] LCDs are widely used in small devices such as electronic desktop calculators and wristwatches, smartphones, laptop computers, liquid crystal monitors, liquid crystal color projectors, liquid crystal televisions, automotive navigation systems, and measuring instruments used indoors and outdoors. Recently, 4K and 8K LCDs have been commercialized and the resolution of LCDs is increasing, but the decrease in light extraction efficiency due to the decrease in aperture ratio is becoming a problem. In this regard, to compensate for the decrease in light extraction efficiency caused by the decrease in aperture ratio, a polarizing film with high polarization performance and high transmittance is required.
[0004] A method for obtaining a polarizing film with high polarization performance is known to use PVA with a high degree of polymerization (e.g., Patent Document 1). However, using PVA with a high degree of polymerization has a problem in that the yield of the polarizing film decreases because the stretchability of the PVA film is reduced.
[0005] In addition, a method of treating a polarizing film with a reducing agent to decompose unnecessary iodine-based pigments is also known (e.g., Patent Document 2). However, industrial implementation was difficult because if the concentration of the reducing agent is not strictly controlled, the iodine-based pigments are decomposed beyond what is necessary.
[0006] However, recently, a method using an aqueous solution of boronic acid has been developed to crosslink PVA molecular chains in a polarizing film. For example, Patent Document 3 describes that a polarizing film with excellent moisture and heat resistance is obtained by immersing a PVA film, after uniaxial stretching, in an aqueous solution (fixing treatment bath) containing boronic acids such as methylboronic acid and 1,4-butanediboronic acid and potassium iodide. In addition, Patent Documents 4 and 5 describe that a polarizing film with excellent moisture and heat resistance, high polarization performance, and small shrinkage at high temperatures is obtained by treating a PVA film with monoboronic acid to impart hydrophobicity.
[0007] However, in order to meet the demand for high precision in electronic devices, the polarizing films described in Patent Documents 3 to 5 still had insufficient polarization performance. Prior art literature
[0008] Japanese Published Patent Application No. Hei 01-084203 Japanese Published Patent Application No. 2013-156621WO 2018 / 021274KR 10-2015-0052777WO 2019 / 146677 The problem to be solved
[0009] The present invention is made to solve the above problem and aims to provide a polarizing film having high polarization performance and high transmittance, and a method for manufacturing the same. means of solving the problem
[0010] As a result of careful examination by the inventors, it was found that in order to obtain a polarizing film with high polarization performance and high transmittance, it is important to adjust the amount and ratio of boric acid (C) and boron-containing compound (B) used for crosslinking PVA molecular chains in the polarizing film to an appropriate range, and to have a relatively large amount of boron-containing compound (B) near the surface of the polarizing film.
[0011] The present invention is,
[0012] [1] A polarizing film comprising PVA (A), at least one boron-containing compound (B) selected from the group consisting of monoboronic acid represented by the following formula (I) and a compound that can be converted into the monoboronic acid in the presence of water, and boric acid (C), wherein the boron element content (b) derived from the boron-containing compound (B) t ) is 0.3 to 2.0 mass%, the total boron element content (T) is 3.0 to 7.0 mass%, and also (b for (T). t The ratio of ) (b t / T) is 0.10 to 0.30, and the boron element concentration (b) derived from the boron-containing compound (B) in the range of up to 7.5% of the total thickness from at least one surface inward (hereinafter, said range may be referred to as the surface portion). o Polarizing film having ) 2.2 to 10.0 atomic%;
[0013] [Chemical Formula 1]
[0014]
[0015] [In Equation (I), R 1 is a monovalent aliphatic group with 1 to 20 carbon atoms, and R 1 The boronic acid group is connected by a boron-carbon bond.
[0016] [2] The boron element concentration (b) derived from the boron-containing compound (B) in the range from the center to the outside of the above polarizing film, up to 7.5% of the total thickness (hereinafter, the range may be referred to as the center). i ) is 0.5 to 2.0 atomic %, and also the boron element concentration derived from boric acid (C) (c i A polarizing film of [1] having 3.5 to 8.0 atomic%;
[0017] [3] The concentration of boron element derived from boric acid (C) in the range of up to 7.5% of the total thickness from the center to the outside of the polarizing film (c i ) for which elemental boron concentration derived from boron-containing compound (B) (b i The ratio of ) (b i / c i A polarizing film of [1] or [2] with a polarization value of 0.01 to 0.25;
[0018] [4] A boron element concentration (c) derived from boric acid (C) in the range of up to 7.5% of the total thickness, inward from at least one surface of the polarizing film. o A polarizing film of any of [1] to [3] having 3.3 to 7.8 atomic%;
[0019] [5] A boron element concentration (b) derived from a boron-containing compound (B) in the range of up to 7.5% of the total thickness, inward from at least one surface of the polarizing film. o ) a boron element concentration (b) derived from a boron-containing compound (B) in a range of up to 7.5% of the total thickness from the center to the outside of the polarizing film. i Polarizing film of any of [1] to [4] higher than ) ;
[0020] [6] A boron element concentration (c) derived from boric acid (C) in the range of up to 7.5% of the total thickness, inward from at least one surface of the polarizing film. o ) a boron element concentration (c) derived from boric acid (C) in a range of up to 7.5% of the total thickness from the center to the outside of the polarizing film. i Polarizing film of any of [1] to [5] lower than ) ;
[0021] [7] R 1 Polarizing film of any of [1] to [6] which is a saturated aliphatic group;
[0022] [8] R 1 A polarizing film of any of [1] to [7] which is a straight-chain aliphatic hydrocarbon;
[0023] [9] R 1 Polarizing film of any of [1] to [8] having 2 to 5 carbon atoms;
[0024]
[10] A polarizing film of any of [1] to [9] having a transmittance of 42% or more when the degree of polarization is 99.9% or more;
[0025]
[11] A method for manufacturing a polarizing film comprising a dyeing treatment of a polyvinyl alcohol film with a dichroic dye and a stretching treatment of the film uniaxially stretching the film, wherein the film is immersed in an aqueous solution containing a boric acid crosslinking agent, and then immersed in an aqueous solution of 35 to 80°C containing 1.5 to 5.0 mass% of a boron-containing compound (B). [1] A method for manufacturing a polarizing film of any one of [1] to
[10] . Effects of the invention
[0026] The polarizing film of the present invention has high polarization performance and high transmittance. According to the manufacturing method of the present invention, such a polarizing film can be easily manufactured. Brief explanation of the drawing
[0027] Figure 1 is a schematic diagram showing a cross-section in the thickness direction of a polarizing film of the present invention. FIG. 2 is of the polarizing film obtained in Example 1. 1 This is an H-NMR chart. Specific details for implementing the invention
[0028] Polarizing Film
[0029] The polarizing film of the present invention is a polarizing film comprising PVA (A), at least one boron-containing compound (B) selected from the group consisting of monoboronic acid represented by the following formula (I) and a compound that can be converted into the monoboronic acid in the presence of water, and boric acid (C), wherein the boron element content (b) derived from the boron-containing compound (B) t ) is 0.3 to 2.0 mass%, the total boron element content (T) is 3.0 to 7.0 mass%, and also (b for (T). t The ratio of ) (b t / T) is 0.10 to 0.30, and the boron element concentration (b) derived from the boron-containing compound (B) is in the range of up to 7.5% of the total thickness from at least one surface inward. o ) is 2.2 to 10.0 atomic %.
[0030] [Chemical Formula 2]
[0031]
[0032] [In Equation (I), R 1 is a monovalent aliphatic group with 1 to 20 carbon atoms, and R 1 The boronic acid group is connected by a boron-carbon bond.
[0033] Thus, the total boron element content (T) in the polarizing film, and the boron element content (b) of the boron-containing compound (B) t ) and their ratios are set to a specific range, and also, the boron element concentration (b) derived from the boron-containing compound (B) on the surface of the polarizing film oBy setting the range to a specific range, high polarization performance and high transmittance are obtained. The reason for this is that the leaching of boric acid (C) from the inside is suppressed because a relatively large amount of boron-containing compound (B) is present on the surface of the polarizing film. This is thought to be due to the suppression of the relaxation of the orientation of PVA in the center of the polarizing film, as well as the removal of unnecessary iodine-based pigments on the surface of the polarizing film by the boron-containing compound (B).
[0034] Typically, when a boric acid-crosslinked PVA film is immersed in an aqueous solution of a boron-containing compound (B), the reaction in which boric acid (C) is substituted with the boron-containing compound (B) proceeds from the surface of the PVA film. Here, in order to have a relatively large amount of the boron-containing compound (B) present on the surface of the PVA film, it is important to accelerate the substitution reaction between boric acid (C) and the boron-containing compound (B) on the surface of the PVA film by immersing the PVA film in an aqueous solution of the boron-containing compound (B) at a relatively high concentration and high temperature, as described below. When the concentration of the boron-containing compound (B) is low, the elution of boric acid (C) proceeds preferentially over the adsorption of the boron-containing compound (B). In this case, the boric acid (C) in the center of the PVA film is also eluted, and the orientation of the PVA is relaxed, making it difficult to obtain a polarizing film with high polarization performance and high transmittance. In addition, there is a risk that the rigidity of the polarizing film may decrease, causing wrinkles to form. When the aqueous solution of the boron-containing compound (B) is at a low temperature, boric acid (C) is difficult to leach out, so the boron-containing compound (B) is not adsorbed. In this case, the effect of improving polarization performance by adding the boron-containing compound (B) is insufficient, so a polarizing film with high polarization performance and high transmittance cannot be obtained. On the other hand, when a boric acid-crosslinked PVA film is immersed in an aqueous solution of the boron-containing compound (B) at a relatively high concentration and high temperature, the above substitution reaction proceeds rapidly on the surface of the PVA film. As a result, the relaxation of the orientation of PVA in the central part of the PVA film is suppressed, and unnecessary iodine-based pigments on the surface of the PVA film are removed by the boron-containing compound (B), so it is thought that a polarizing film with high polarization performance and high transmittance is obtained.
[0035] The boron-containing compound (B) in the polarizing film of the present invention is at least one selected from the group consisting of a monoboronic acid represented by formula (I) and a compound capable of being converted into the monoboronic acid in the presence of water. Here, in formula (I), R 1 is a monovalent aliphatic group with 1 to 20 carbon atoms, and R 1 The boronic acid group is connected by a boron-carbon bond.
[0036] Monoboronic acid is a compound represented by the above formula (I) and has one boronic acid group [-B(OH)2] in one molecule. The said boronic acid group has a structure in which a boron atom bonded to two hydroxyl groups is bonded to a carbon atom, and in the compound represented by formula (I), R 1 The boron group is connected by a boron-carbon bond. In boric acid [B(OH)3], the boron atom is bonded to three hydroxyl groups, whereas the boron group is different in that it has a boron-carbon bond. Representative boron-containing groups that can be converted into boron groups in the presence of water include the boron ester group described below, but are not limited to this.
[0037] The hydroxyl group in the boronic acid group contained in monoboronic acid can form alcohols and esters, just like the hydroxyl group in boric acid. Formula (II) below represents 1 molecule of alcohol (R) relative to boronic acid. 2 -OH) is the reacted monoboronic acid monoester. Here, when the boronic acid group is bonded to the hydroxyl group of PVA (A), R in formula (II) 2 It is a PVA chain, and a carbon-containing group is bonded to the PVA chain by interposing a boron atom.
[0038] [Chemical Formula 3]
[0039]
[0040] Formula (III) below contains 2 molecules of alcohol (R) relative to monoboronic acid2 -OH) is an example of a monoboronic acid diester that has reacted. Here, when the boronic acid group is bonded to the hydroxyl group of PVA, the two Rs in formula (III) 2 They are all PVA chains.
[0041] [Chemical Formula 4]
[0042]
[0043] Monoboronic acid has two hydroxyl groups capable of reacting with the hydroxyl groups of PVA to form an ester, and the PVA chain becomes appropriately cross-linked. Although the reason is not clear, it is thought that the polarization performance of the polarizing film is improved by increasing the orientation of PVA through this cross-linking, or by destabilizing and reducing unnecessary iodine-based pigments, thereby resulting in a polarizing film with high transmittance and high polarization performance.
[0044] In Equation (I), R 1 R is a monovalent aliphatic group with 1 to 20 carbon atoms. 1 By having an appropriate length, the solubility of the boron-containing compound (B) in water or the reactivity with the hydroxyl groups of PVA can be controlled. In terms of obtaining a polarizing film with good adsorption to the polarizing film and excellent optical performance, R 1 The number of carbon atoms is preferably 10 or less, more preferably 6 or less, and even more preferably 5 or less. Meanwhile, in terms of the particularly excellent balance between the optical performance and shrinkage force of the polarizing film, R 1 The number of carbon atoms is preferably 2 or more, and more preferably 3 or more.
[0045] In Equation (I), R 1 R is a monovalent aliphatic group, and it is sufficient that R1 and the boronic acid group are connected by a boron-carbon bond. 1 It may be a saturated aliphatic contribution or an unsaturated aliphatic contribution, but the former is preferred. R 1By being a saturated aliphatic group, the discoloration of the resulting polarizing film is suppressed, and durability is improved. Also, R 1 As this is a saturated aliphatic group, the orientation of dichroic pigments is enhanced, thereby further improving optical performance. Furthermore, an unsaturated aliphatic group refers to an aliphatic group having a structure containing multiple bonds of bond order 2 or higher, such as carbon-carbon double bonds, carbon-carbon triple bonds, carbon-oxygen double bonds, carbon-nitrogen double bonds, nitrogen-nitrogen double bonds, and carbon-sulfur double bonds, while a saturated aliphatic group refers to an aliphatic group having a structure consisting only of single bonds. R 1The monoboronic acids with this saturated aliphatic group include methylboronic acid, ethylboronic acid, propylboronic acid, butylboronic acid, pentyboronic acid, hexylboronic acid, heptylboronic acid, octylboronic acid, nonylboronic acid, decanylboronic acid, undecanyboronic acid, dodecanyboronic acid, tridecanyboronic acid, tetradecanylboronic acid, pentadecanylboronic acid, hexadecanylboronic acid, heptadecanylboronic acid, octadecanylboronic acid, nonadecanylboronic acid, icosanylboronic acid and their isomers, cyclopropylboronic acid, cyclobutylboronic acid, cyclopentylboronic acid, cyclohexylboronic acid, cycloheptylboronic acid, cyclooctyboronic acid, cyclononylboronic acid, cyclodecanylboronic acid, cycloundecanyboronic acid, Cyclododecanylboronic acid, cyclotridecanylboronic acid, cyclotetradecanylboronic acid, cyclopentadecanylboronic acid, cyclohexadecanylboronic acid, cycloheptadecanylboronic acid, cyclooctadecanylboronic acid, cyclononadecanylboronic acid, cycloicosanylboronic acid and their isomers, 2-oxa-propylboronic acid, 2-oxa-butylboronic acid, 2-oxa-hexylboronic acid, 2-oxa-heptylboronic acid, 2-oxa-octyboronic acid, 2-oxa-nonylboronic acid, 2-oxa-decanylboronic acid, 2-oxa-undecanylboronic acid, 2-oxa-dodecanylboronic acid, 2-oxa-tridecanylboronic acid, 2-oxa-tridecanylboronic acid, 2-oxa-tetradecanylboronic acid, 2-oxa-pentadecanylboronic acid, 2-oxa-hexadecanylboronic acid, 2-oxa-heptadecanylboronic acid, 2-oxa-octadecanylboronic acid, 2-oxa-nonadecanylboronic acid, 2-oxa-icosanylboronic acid and their isomers, 2-aza-propylboronic acid, 2-aza-butylboronic acid, 2-aza-hexylboronic acid, 2-aza-heptylboronic acid, 2-aza-octyboronic acid, 2-aza-nonylboronic acid, 2-aza-decanylboronic acid, 2-aza-undecanylboronic acid, 2-aza-dodecanylboronic acid, 2-aza-tridecanylboronic acid, 2-aza-tridecanylboronic acid, 2-Aza-pentadecanylboronic acid, 2-Aza-hexadecanylboronic acid, 2-Aza-heptadecanylboronic acid, 2-Aza-octadecanylboronic acid, 2-Aza-nonadecanylboronic acid, 2-Aza-icosanylboronic acid and their isomers, 2-phospha-propylboronic acid, 2-phospha-butylboronic acid, 2-phospha-hexylboronic acid, 2-phospha-heptylboronic acid, 2-phospha-octyboronic acid, 2-phospha-nonylboronic acid, 2-phospha-decanylboronic acid,2-phospha-undecanylboronic acid, 2-phospha-dodecanylboronic acid, 2-phospha-tridecanylboronic acid, 2-phospha-tetradecanylboronic acid, 2-phospha-pentadecanylboronic acid, 2-phospha-hexadecanylboronic acid, 2-phospha-heptadecanylboronic acid, 2-phospha-octadecanylboronic acid, 2-phospha-nonadecanylboronic acid, 2-phospha-icosanylboronic acid and their isomers, 2-thi-propylboronic acid, 2-thi-butylboronic acid, 2-thi-hexylboronic acid, 2-thi-heptylboronic acid, 2-thi-octyboronic acid, 2-thi-nonylboronic acid, 2-thi-decanylboronic acid, 2-thi-undecanylboronic acid, Examples include 2-thia-dodecanylboronic acid, 2-thia-tridecanylboronic acid, 2-thia-tredatecanylboronic acid, 2-thia-pentadecanylboronic acid, 2-thia-hexadecanylboronic acid, 2-thia-heptadecanylboronic acid, 2-thia-octadecanylboronic acid, 2-thia-nonadecanylboronic acid, 2-thia-icosanylboronic acid, and their isomers. Additionally, salts of said monoboronic acid may be cited as compounds that can be converted into the exemplified monoboronic acid in the presence of water.
[0046] R 1 It may be an aliphatic hydrocarbon, and it does not matter if it contains heteroatoms such as oxygen, nitrogen, sulfur, or halogens. Considering ease of availability, R 1 It is preferable that this be an aliphatic hydrocarbon group that does not contain heteroatoms. As for the aliphatic hydrocarbon group, it is preferable that it be a straight-chain aliphatic hydrocarbon group that does not have branches. This improves the adsorption to the polarizing film and enhances the effect of improving optical performance. In addition, R 1Examples of boronic acids that are straight-chain aliphatic hydrocarbon groups include, specifically, methylboronic acid, ethylboronic acid, n-propylboronic acid, n-butylboronic acid, n-pentylboronic acid, n-hexylboronic acid, n-heptylboronic acid, n-octyboronic acid, n-nonylboronic acid, n-decanylboronic acid, n-undecanylboronic acid, n-dodecanylboronic acid, n-tridecanylboronic acid, n-tetradecanylboronic acid, n-pentadecanylboronic acid, n-hexadecanylboronic acid, n-heptadecanylboronic acid, n-octadecanylboronic acid, n-nonadecanylboronic acid, n-icosanylboronic acid, etc. In addition, salts of said boronic acid may be examples of compounds that can be converted into the boronic acids exemplified in the presence of water.
[0047] Specifically, as the monoboronic acid represented by the above formula (I), ethylboronic acid, n-propylboronic acid, n-butylboronic acid, and n-pentylboronic acid are preferred, and n-propylboronic acid and n-butylboronic acid are more preferred. In addition, salts of said boronic acid may be cited as compounds that can be converted into the boronic acids exemplified above in the presence of water.
[0048] Boron element content (b) derived from the boron-containing compound (B) in the polarizing film of the present invention t ) needs to be 0.3 to 2.0 mass%. (b t If ) is less than 0.3 mass%, crosslinking by the boron-containing compound (B) becomes insufficient, so a polarizing film with high transmittance and high polarization performance cannot be obtained. For this reason, (b t ) is preferably 0.5 mass% or more. Meanwhile, (b t If ) exceeds 2.0 mass%, the reaction between the boron-containing compound (B) and PVA proceeds excessively, inhibiting the formation of iodine-based pigments, and thus it is not possible to obtain a polarizing film with high transmittance and high polarization performance. For this reason, (b t) is preferably 1.8 mass% or less, more preferably 1.6 mass% or less, even more preferably 1.4 mass% or less, particularly preferably 1.3 mass% or less, and most preferably 1.2 mass% or less. The boron element content (b) derived from the boron-containing compound (B) in the polarizing film. t ) silver, 1 It can be obtained by a method combining H-NMR measurement and ICP emission analysis, specifically by the method described in the examples. Boron element content (b t A polarizing film conditioned at 23°C and 50% RH for 16 hours is used as a sample for measuring the total boron element content (T) described below.
[0049] The total boron element content (T) of the polarizing film needs to be 3.0 to 7.0 mass%. If the total boron element content (T) in the polarizing film is less than 3.0 mass%, the number of crosslinking points becomes insufficient, the orientation of PVA becomes disordered, and a polarizing film with high transmittance and high polarization performance cannot be obtained. (T) is preferably 3.5 mass% or more, more preferably 4.1 mass% or more, and even more preferably 4.2 mass% or more. On the other hand, if the total boron element content (T) in the polarizing film exceeds 7.0 mass%, the polarization performance is degraded because an iodine-based dye is excessively adsorbed in the polarizing film. In addition, the PVA film is prone to breakage during the drying or stretching process described later, which reduces the productivity of the polarizing film. The total boron element content (T) in the polarizing film is preferably 6.5 mass% or less, more preferably 5.5 mass% or less, even more preferably 5.0 mass% or less, and particularly preferably 4.8 mass% or less. The total boron element content (T) in the polarizing film can be determined by ICP emission analysis, etc. Specifically, it can be obtained by the method described in the examples.
[0050] The boron element content (b) derived from the boron-containing compound (B) relative to the total boron element content (T) (mass%) in the polarizing film above. t Ratio of ) (mass%) (b t / T) needs to be 0.10 to 0.30. R (b t If / T) is less than 0.10, the ratio of crosslinking points derived from the boron-containing compound (B) among the total crosslinking points of PVA in the polarizing film is excessively low, so the effect of improving polarization performance by the boron-containing compound (B) becomes insufficient. Ratio (b t / T) is preferably 0.12 or higher, and more preferably 0.15 or higher. Meanwhile, the ratio (b t If / T) exceeds 0.30, the proportion of crosslinking points derived from the boron-containing compound (B) among the total crosslinking points of PVA in the polarizing film is excessively high, which inhibits the formation of iodine-based pigments and may result in a polarizing film with high transmittance and high polarization performance that cannot be obtained. Ratio (b t / T) is preferably 0.27 or less, more preferably 0.25 or less, even more preferably 0.23 or less, and particularly preferably 0.18 or less.
[0051] FIG. 1 is a schematic diagram showing a cross-section in the thickness direction of a polarizing film of the present invention. The polarizing film is further described using FIG. 1. Inwardly from at least one surface (1) of the polarizing film, the total thickness t t Range up to 7.5% for (surface part (2), thickness t of surface part (2) o and the total thickness t of the polarizing film t ne「t o = t t The boron element concentration derived from the boron-containing compound (B) in satisfying "× 0.075" (b o ) needs to be 2.2 to 10.0 atomic %. (b oIf ) is less than 2.2 atomic%, the effect of suppressing the leaching of boric acid by the boron-containing compound (B) on the surface of the polarizing film becomes insufficient, and since the effect of improving polarization performance is reduced, a polarizing film with high transmittance and high polarization performance is not obtained. (b o It is preferable that ) be 2.4 atomic% or more, and more preferable that it be 2.8 atomic% or more. Meanwhile, (b o If ) exceeds 10.0 atomic%, there is no problem with polarization performance, but the productivity of the polarization film is reduced due to the formation of precipitates of the boron-containing compound (B) on the surface of the polarization film. (b o ) is preferably 8 atomic% or less, more preferably 6 atomic% or less, even more preferably 5 atomic% or less, and particularly preferably 4 atomic% or less. The boron element concentration (b) derived from the boron-containing compound (B) on the surface portions (2) on both sides of the polarizing film. o It is desirable that ) be within the above range.
[0052] Boron element concentration (b o ) can be obtained using a gas cluster ion beam gun-attached X-ray photoelectron spectrometer (GCIB XPS). By repeating etching and measurement using GCIB XPS, the concentration of boron elements derived from the boron-containing compound (B) is measured at regular intervals from the surface of the polarizing film inward. Then, the average value of the concentration of boron elements derived from the boron-containing compound (B) in the above range (surface portion (2)) is the boron element concentration (b o ) is used. Specifically, it can be obtained by the method described in the examples below. The boron element concentration (b) described below i ), (c o ), and (c i ) also (b o It is obtained by the same method as ).
[0053] From the center (3) of the above polarizing film outward, the total thickness t t Range up to 7.5% for (central part (4), thickness t of central part (4) i and the total thickness t of the polarizing film t ne「t i = t t The boron element concentration derived from the boron-containing compound (B) in satisfying × 0.15) (b i It is preferable that ) is 0.5 to 2.0 atomic%. Also, in the above range (central part (4)), the boron element concentration (c) derived from boric acid (C) is i It is also preferable that ) is 3.5 to 8.0 atomic%. In addition, in the above range (central part (4)), (b i ) is 0.5 to 2.0 atomic %, and also (c i It is more preferable that ) is 3.5 to 8.0 atomic%.
[0054] The boron element concentration (b) derived from the boron-containing compound (B) in the above range (central part (4)). i If ) exceeds 2.0 atomic%, the boron-containing compound (B) present inside the polarizing film becomes excessive, which may inhibit the formation of iodine-based pigments and is therefore undesirable. (b i ) is more preferably 1.8 atomic% or less, more preferably 1.5 atomic% or less, and particularly preferably 1.3 atomic% or less. Meanwhile, (b i If ) is less than 0.5 atomic%, the boron-containing compound (B) inside the polarizing film is insufficient, and the effect of improving polarization performance may become insufficient. (b i ) is more preferably 0.8 atomic% or more, and 0.9 atomic% or more is even more preferable.
[0055] The concentration of boron element derived from boric acid (C) in the above range (central part (4)) (c iIf ) exceeds 8.0 atomic%, it is undesirable because the adsorption of the boron-containing compound (B) into the polarizing film is inhibited. (c i ) is more preferably 7.0 atomic% or less, and even more preferably 6.0 atomic% or less. Meanwhile, (c i If ) is less than 3.5 atomic%, the number of crosslinking points becomes insufficient, and there is a concern that the PVA will not be maintained in an oriented state and a polarizing film with high polarization performance will not be obtained. (c i ) is more preferably 4.0 atomic% or more, more preferably 4.5 atomic% or more, and particularly preferably 5.0 atomic% or more.
[0056] The concentration of boron element derived from boric acid (C) in the above range (central part (4)) (c i ) for which elemental boron concentration derived from boron-containing compound (B) (b i The ratio of ) (b i / c i It is desirable that ) is 0.01 to 0.25. Ratio (b i / c i If ) is less than 0.01, there is a concern that the effect of improving polarization performance by adding the boron-containing compound (B) may be insufficient because the ratio of the boron-containing compound (B) to the boric acid (C) inside the polarizing film is low. Ratio (b i / c i ) is more preferably 0.08 or higher, even more preferably 0.10 or higher, particularly preferably 0.12 or higher, and most preferably 0.15 or higher. Meanwhile, ratio (b i / c i If ) exceeds 0.25, it is undesirable because the formation of iodine-based pigments is inhibited. R (b i / c i ) is more preferably 0.20 or less.
[0057] From at least one surface (1) of the polarizing film inwardly, the total thickness tt The boron element concentration (c) derived from boric acid (C) in the range of up to 7.5% (surface portion (2)) for o It is preferable that ) is 3.3 to 7.8 atomic%. (c o If ) is less than 3.3 atomic%, boric acid is often leached in excess from the polarizing film. If boric acid is leached in excess, a polarizing film with high polarization performance may not be obtained. (c o ) is more preferably 4.0 atomic% or more, and 4.5 atomic% or more is even more preferable. Meanwhile, (c o If ) exceeds 7.8 atomic%, there is a risk that scratches may easily form on the surface (1) of the polarizing film, or that the adsorption of the boron-containing compound (B) onto the PVA film may be inhibited. (c o ) is more preferably 7.0 atomic% or less, more preferably 6.5 atomic% or less, particularly preferably 5.5 atomic% or less, and most preferably 4.8 atomic% or less. The boron element concentration (c) derived from boric acid (C) in the surface portions (2) on both sides of the polarizing film. o It is more preferable that ) is within the above range.
[0058] From at least one surface (1) of the polarizing film inwardly, the total thickness t t The boron element concentration (b) derived from the boron-containing compound (B) in the range of up to 7.5% (surface portion (2)) for o ) extending from the center (3) of the polarizing film outward, with a total thickness t t The boron element concentration (b) derived from the boron-containing compound (B) in the range of up to 7.5% (central part (4)) for i It is desirable that it be higher than ) (b i (b) regarding ) o The ratio of ) (b o / b iIf ) is 1 or less, the effect of inhibiting the leaching of boric acid by the boron-containing compound (B) on the surface of the polarizing film becomes insufficient, and the effect of improving polarization performance becomes small, so there is a concern that a polarizing film with high transmittance and high polarization performance may not be obtained, or that the formation of iodine-based pigments may be inhibited because the boron-containing compound (B) present inside the polarizing film becomes excessive. (b i (b) regarding ) o The ratio of ) (b o / b i ) is more preferably 1.1 or higher, even more preferably 1.5 or higher, particularly preferably 2.0 or higher, and most preferably 2.5 or higher. Meanwhile, ratio (b o / b i ) is preferably 8.0 or less, and more preferably 7.0 or less. In terms of obtaining a polarizing film with very high polarization performance and transmittance, and further improving the productivity of the polarizing film, the ratio (b o / b i ) is preferably 6.0 or less, more preferably 5.0 or less, even more preferably 4.5 or less, and particularly preferably 4.0 or less. The boron element concentration (b) derived from the boron-containing compound (B) on the surface portions (2) on both sides of the polarizing film. o ) a, the concentration of boron element derived from the boron-containing compound (B) in the central part (4) (b i It is more desirable to have something higher than ).
[0059] From at least one surface (1) of the polarizing film inwardly, the total thickness t t The boron element concentration (c) derived from boric acid (C) in the range of up to 7.5% (surface portion (2)) for o ) a, from the center to the outside of the polarizing film, the total thickness t t The boron element concentration (c) derived from boric acid (C) in the range of up to 7.5% (central part (4)) fori It is desirable that it be lower than ). (c i (c) regarding ) o The ratio of ) (c o / c i If ) is 1 or more, there is a concern that scratches may easily form on the surface (1) of the polarizing film, the adsorption of the boron-containing compound (B) onto the PVA film may be inhibited, or the number of crosslinking points may become insufficient so that the PVA is not maintained in an oriented state and a polarizing film with high polarization performance cannot be obtained. (c i (c) regarding ) o The ratio of ) (c o / c i ) is more preferably 0.99 or less, even more preferably 0.95 or less, particularly preferably 0.90 or less, and most preferably 0.85 or less. Meanwhile, in terms of obtaining a polarizing film with higher polarization performance and facilitating the adsorption of the boron-containing compound (B) into the polarizing film, the ratio (c o / c i ) is preferably 0.5 or higher. The boron element concentration (c) derived from boric acid (C) in the surface portions (2) on both sides of the polarizing film. o ) is the concentration of boron element derived from boric acid (C) in the central part (4) (c i It is more desirable to have something lower than ).
[0060] The thickness of the above polarizing film is preferably 5 to 60 μm. If the thickness is less than 5 μm, stretching breakage is prone to occur during manufacturing, which may lead to a decrease in productivity. The thickness is more preferably 10 μm or more. On the other hand, if the thickness exceeds 60 μm, there is a risk that the performance required for the polarizing plate, such as thinning or weight reduction, may not be satisfied. Therefore, the thickness is more preferably 45 μm or less, even more preferably 30 μm or less, and particularly preferably 25 μm or less.
[0061] <PVA (A)>
[0062] PVA (A) in the present invention is a polymer having vinyl alcohol units (-CH2-CH(OH)-) as the main structural units.
[0063] The degree of polymerization of the PVA (A) included in the polarizing film of the present invention is preferably within the range of 1,500 to 6,000, more preferably within the range of 1,800 to 5,000, and even more preferably within the range of 2,000 to 4,000. By having a degree of polymerization of 1,500 or higher, the durability of the polarizing film obtained by uniaxial stretching of the film can be improved. On the other hand, by having a degree of polymerization of 6,000 or lower, an increase in manufacturing costs or poor process passability during film formation can be suppressed. Furthermore, the degree of polymerization of the PVA (A) in this specification refers to the average degree of polymerization measured in accordance with the description in JIS K 6726-1994.
[0064] The degree of saponification of PVA (A) included in the polarizing film of the present invention is preferably 95 mol% or more, more preferably 96 mol% or more, and even more preferably 98 mol% or more in terms of the water resistance of the polarizing film obtained by uniaxial stretching of the film. In addition, the degree of saponification of PVA in this specification refers to the ratio (mol%) of the number of moles of said vinyl alcohol units to the total number of moles of said vinyl alcohol units and said vinyl alcohol units, which are structural units (typically vinyl ester units) that can be converted into vinyl alcohol units (-CH2-CH(OH)-) by saponification, that said vinyl alcohol units have of PVA. The said degree of saponification can be measured in accordance with the description in JIS K 6726-1994.
[0065] The method for manufacturing PVA (A) used in the present invention is not particularly limited. For example, a method of converting vinyl ester units of polyvinyl ester obtained by polymerizing vinyl ester monomers into vinyl alcohol units may be cited. The vinyl ester monomers used in the manufacture of PVA (A) are not particularly limited, but examples include vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl versatate, vinyl caproate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl palmitate, vinyl stearate, vinyl oleate, vinyl benzoate, etc. From an economic perspective, vinyl acetate is preferred.
[0066] In addition, the PVA (A) used in the present invention may be obtained by converting the vinyl ester unit of a vinyl ester copolymer, obtained by copolymerizing a vinyl ester monomer with another monomer copolymerizable thereto, into a vinyl alcohol unit. Other monomers copolymerizable with the vinyl ester monomer include, for example, α-olefins having 2 to 30 carbon atoms, such as ethylene, propylene, 1-butene, and isobutene; (meth)acrylic acid or its salt; (Met)acrylic acid esters such as (meth)acrylate methyl, (meth)acrylate ethyl, (meth)acrylate n-propyl, (meth)acrylate i-propyl, (meth)acrylate n-butyl, (meth)acrylate i-butyl, (meth)acrylate t-butyl, (meth)acrylate 2-ethylhexyl, (meth)acrylate dodecyl, (meth)acrylate octadecyl, etc.; (meth)acrylate derivatives such as (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, diacetone(meth)acrylamide, (meth)acrylamidepropanesulfonic acid or its salt, (meth)acrylamidepropyldimethylamine or its salt, N-methylol(meth)acrylamide or its derivative; Examples include N-vinylamides such as N-vinylformamide, N-vinylacetamide, and N-vinylpyrrolidone; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether, n-butyl vinyl ether, i-butyl vinyl ether, t-butyl vinyl ether, dodecyl vinyl ether, and stearyl vinyl ether; vinyl cyanide such as (meth)acrylonitrile; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; maleic acid or its salt, ester, or acid anhydride; itaconic acid or its salt, ester, or acid anhydride; vinylsilyl compounds such as vinyltrimethoxysilane; and unsaturated sulfonic acids. The vinyl ester copolymer may have structural units derived from one or more of the other monomers mentioned above.The other monomer in question may be used by being present in the reaction vessel in advance when providing the vinyl ester monomer to the polymerization reaction, or by adding it to the reaction vessel during the progress of the polymerization reaction. From the perspective of optical performance, the content of units derived from the other monomer is preferably 10 mol% or less with respect to the total number of moles of structural units constituting PVA (A), more preferably 5 mol% or less, and even more preferably 2 mol% or less.
[0067] Ethylene is preferred as a monomer copolymerizable with the vinyl ester monomer in that, along with improved stretchability, it can be stretched at higher temperatures, and the occurrence of troubles such as stretching breakage is reduced, thereby further improving the productivity of the polarizing film. When PVA (A) contains ethylene units, the content of ethylene units is preferably 1 to 10 mol% and more preferably 2 to 6 mol% with respect to the total number of structural units constituting PVA (A), in terms of stretchability and stretchable temperature as described above.
[0068] The PVA film used in the manufacture of the polarizing film of the present invention may include a plasticizer in addition to the PVA (A). Preferred plasticizers include polyhydric alcohols, and specific examples include ethylene glycol, glycerin, propylene glycol, diethylene glycol, diglycerin, triethylene glycol, tetraethylene glycol, trimethylolpropane, etc. In addition, one or more of these plasticizers may be included. Among these, glycerin is preferred in terms of the effect of improving stretchability.
[0069] The content of a plasticizer in the PVA film used to manufacture the polarizing film of the present invention is preferably in the range of 1 to 20 parts by mass per 100 parts by mass of PVA (A), more preferably in the range of 3 to 17 parts by mass, and even more preferably in the range of 5 to 15 parts by mass. When the said content is 1 part by mass or more, the stretchability of the film is improved. On the other hand, when the said content is 20 parts by mass or less, the film can be prevented from becoming excessively flexible and its handling properties from deteriorating.
[0070] In the PVA film used to manufacture the polarizing film of the present invention, other additives other than PVA (A) and plasticizers, such as fillers, processing stabilizers including copper compounds, weathering stabilizers, colorants, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, flame retardants, other thermoplastic resins, lubricants, fragrances, defoaming agents, deodorizing agents, fillers, release agents, mold release agents, reinforcing agents, crosslinking agents, antifungal agents, preservatives, and crystallization rate retardants, may be appropriately blended as needed. The content of other additives in the PVA film is typically 10 mass% or less, and preferably 5 mass% or less.
[0071] The degree of swelling of the PVA film used in the manufacture of the polarizing film of the present invention is preferably within the range of 160 to 240%, more preferably within the range of 170 to 230%, and particularly preferably within the range of 180 to 220%. By having a degree of swelling of 160% or more, extreme crystallization can be suppressed, and the film can be stretched stably up to a high magnification. On the other hand, by having a degree of swelling of 240% or less, dissolution during stretching is suppressed, making it possible to stretch even under higher temperature conditions.
[0072] <Method for Manufacturing Polarizing Film>
[0073] The thickness of the PVA film used to manufacture the polarizing film of the present invention is not particularly limited, but is generally 1 to 100 μm, preferably 5 to 60 μm, and particularly preferably 10 to 45 μm. If the PVA film is excessively thin, there is a tendency for stretching breakage to occur during the uniaxial stretching process for manufacturing the polarizing film. Also, if the PVA film is excessively thick, there is a tendency for stretching non-uniformity to occur during the uniaxial stretching process for manufacturing the polarizing film, and because the resulting polarizing film becomes thick, it tends to be difficult to use in thin and small devices such as smartphones and laptop computers.
[0074] The width of the PVA film used in the manufacture of the polarizing film of the present invention is not particularly limited and can be determined according to the application of the polarizing film being manufactured. Given that the screen size of liquid crystal televisions and liquid crystal monitors has recently been increasing, it is desirable for these applications if the width of the PVA film used in the manufacture of the polarizing film is 3 m or more. On the other hand, if the width of the PVA film used in the manufacture of the polarizing film is excessively large, it is easy to make it difficult to uniformly perform uniaxial stretching when manufacturing the polarizing film with a device that is in practical use; therefore, it is desirable that the width of the PVA film used in the manufacture of the polarizing film be 10 m or less.
[0075] The method of manufacturing the PVA film used in the manufacture of the polarizing film of the present invention is not particularly limited, and a manufacturing method in which the thickness and width of the film after film formation are uniform is preferably employed. For example, it may be manufactured using a film-forming stock solution in which PVA (A) and, if necessary, additionally one or more of the plasticizer, the other additive, and the surfactant described below are dissolved in a liquid medium, or a film-forming stock solution in which PVA (A) is molten and includes PVA (A) and, if necessary, additionally one or more of the plasticizer, other additive, surfactant, and liquid medium. When the film-forming stock solution contains at least one of the plasticizer, other additive, and surfactant, it is preferable that the components are uniformly mixed.
[0076] Examples of the liquid media used in the preparation of the film-forming stock solution include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, glycerin, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, trimethylolpropane, ethylenediamine, diethylenetriamine, etc., and one or more of these may be used. Among these, water is preferred in terms of environmental burden and recoverability.
[0077] The volatile fraction of the film-forming solution (the ratio of volatile components, such as liquid media, that are removed by volatilization or evaporation during film formation, contained in the film-forming solution) varies depending on the film-forming method, film-forming conditions, etc., but generally, it is preferable to be within the range of 50 to 95 mass%, and more preferable to be within the range of 55 to 90 mass%. When the volatile fraction of the film-forming solution is 50 mass% or higher, the viscosity of the film-forming solution does not become excessively high, and filtration and degassing during the preparation of the film-forming solution are carried out smoothly, making it easier to manufacture a film with fewer foreign substances or defects. On the other hand, when the volatile fraction of the film-forming solution is 95 mass% or lower, the concentration of the film-forming solution does not become excessively low, making it easier to manufacture an industrial film.
[0078] It is preferable that the film-forming solution contains a surfactant. By including a surfactant, film-forming properties are improved, which suppresses the occurrence of non-uniformity in film thickness and facilitates the peeling of the film from the metal roll or belt used for film formation. When a PVA film is manufactured from a film-forming solution containing a surfactant, the film may contain the surfactant. The type of surfactant is not particularly limited, but anionic surfactants or nonionic surfactants are preferred from the perspective of peelability from the metal roll or belt.
[0079] Anionic surfactants include, for example, carboxylic acid types such as potassium laurate; sulfate ester types such as polyoxyethylene lauryl ether sulfate, sodium alkyl sulfate, potassium alkyl sulfate, ammonium alkyl sulfate, triethanolamine alkyl sulfate, sodium polyoxyethylene alkyl ether sulfate, sodium polyoxypropylene alkyl ether sulfate, sodium polyoxyethylene alkylphenyl ether sulfate, octyl sulfate, etc.; sulfonic acid types such as sodium alkyl sulfonate, potassium alkyl sulfonate, ammonium alkyl sulfonate, triethanolamine alkyl sulfonic acid, sodium alkylbenzene sulfonate, disodium dodecyl diphenyl ether disulfonic acid, sodium alkyl naphthalene sulfonate, disodium alkyl sulfosuccinate, sodium polyoxyethylene alkyl sulfosuccinate, dodecylbenzene sulfonate, etc. Phosphate ester types such as sodium alkyl phosphate ester, potassium alkyl phosphate ester, ammonium alkyl phosphate ester, triethanolamine alkyl phosphate ester, sodium polyoxyethylene alkyl ether phosphate ester, sodium polyoxypropylene alkyl ether phosphate ester, and sodium polyoxyethylene alkylphenyl ether phosphate ester are preferred.
[0080] As nonionic surfactants, for example, alkyl ether type such as polyoxyethylene oleyl ether; alkylphenyl ether type such as polyoxyethylene octylphenyl ether; alkyl ester type such as polyoxyethylene laurate; alkylamine type such as polyoxyethylene laurylamino ether; alkylamide type such as polyoxyethylene lauric acid amide; polypropylene glycol ether type such as polyoxyethylene polyoxypropylene ether; alkanolamide type such as lauric acid diethanolamide, oleic acid diethanolamide; and allylphenyl ether type such as polyoxyalkylene allylphenyl ether are preferred.
[0081] These surfactants can be used as a single type or in combination of two or more types.
[0082] When the film-forming solution contains a surfactant, the content thereof is preferably within the range of 0.01 to 0.5 parts by mass relative to 100 parts by mass of PVA (A) contained in the film-forming solution, more preferably within the range of 0.02 to 0.3 parts by mass, and particularly preferably within the range of 0.05 to 0.2 parts by mass. When the content thereof is 0.01 parts by mass or more, the film-forming properties and peelability are further improved. On the other hand, when the content thereof is 0.5 parts by mass or less, it is possible to suppress the surfactant from bleeding out onto the surface of the PVA film and causing blocking, which would lead to a decrease in handling properties.
[0083] Examples of film-forming methods for forming a PVA film using the above-mentioned film-forming solution include the casting method, extrusion method, wet method, and gel method. These film-forming methods may be adopted individually or in combination of two or more. Among these film-forming methods, the casting method and the extrusion method are preferred in that they yield a PVA film used for manufacturing a polarizing film with uniform thickness and width and good physical properties. The formed PVA film may be subjected to drying or heat treatment as necessary.
[0084] As an example of a specific method for manufacturing a PVA film used in the manufacture of the polarizing film of the present invention, for instance, a T-shaped slit die, a hopper plate, an I-die, a rip coater die, etc., may be used to uniformly discharge or spread the film-forming liquid onto the circumferential surface of a first rotating heated roll (or belt) located at the uppermost side, and to dry the film by evaporating volatile components from one side of the film discharged or spread onto the circumferential surface of the first roll (or belt), and then to further dry it on the circumferential surface of one or more rotating heated rolls arranged downstream, or to further dry it by passing it through a hot air drying device, and then to wind it by a winding device. Drying by heated rolls and drying by a hot air drying device may be carried out in an appropriate combination. In addition, a multilayer PVA film may be formed by forming a layer made of PVA (A) on one side of a substrate film composed of a single resin layer.
[0085] The method for manufacturing the polarizing film of the present invention is not particularly limited. A preferred manufacturing method is a method for manufacturing a polarizing film comprising a dyeing treatment in which a PVA film is dyed with a dichroic pigment and a stretching treatment in which the film is uniaxially stretched, wherein the film is immersed in an aqueous solution containing a boric acid crosslinking agent, and then immersed in an aqueous solution containing a boron-containing compound (B). In addition to the dyeing treatment and the stretching treatment, the PVA film may additionally undergo swelling treatment, boric acid crosslinking treatment, fixation treatment, washing treatment, drying treatment, heat treatment, etc., as needed. The order of each treatment is not particularly limited, and one or more treatments may be performed simultaneously. Furthermore, one or more of each treatment may be performed two or more times.
[0086] Swelling treatment can be performed by immersing the PVA film in water. The temperature of the water in which the film is immersed is preferably within the range of 20 to 40°C, more preferably within the range of 22 to 38°C, and even more preferably within the range of 25 to 35°C. In addition, the immersion time is preferably within the range of, for example, 0.1 to 5 minutes, and more preferably within the range of 0.2 to 3 minutes. Furthermore, the water in which the film is immersed is not limited to pure water, but may be an aqueous solution in which various components are dissolved, or a mixture of water and a hydrophilic medium.
[0087] The dyeing treatment can be performed by contacting a PVA film with a dichroic pigment. It is common to use iodine-based pigments or dichroic dyes as the dichroic pigment. The dyeing treatment may be performed at any stage before, during, or after the stretching treatment. The dyeing treatment is generally performed by immersing the PVA film in a dyeing bath containing iodine and potassium iodide (especially an aqueous solution) or a solution containing multiple dichroic dyes (especially an aqueous solution). The concentration of iodine in the dyeing bath is preferably within the range of 0.01 to 0.5 mass%, and the concentration of potassium iodide is preferably within the range of 0.01 to 10 mass%. In addition, the temperature of the dyeing bath is preferably 20 to 50°C, particularly 25 to 40°C. The preferred dyeing time is 0.2 to 5 minutes. When using dichroic dyes, water-based dyes are preferred. Additionally, the dye concentration in the dyeing bath is preferably 0.001 to 10 mass%. Furthermore, dyeing aids may be used as needed, and inorganic salts such as sodium sulfate or surfactants may be used. When using sodium sulfate, 0.1 to 10 mass% is preferred. The dyeing temperature is preferably 30 to 80°C. Specific dichroic dyes include C.I. Direct Yellow 28, C.I. Direct Orange 39, C.I. Direct Yellow 12, C.I. Direct Yellow 44, C.I. Direct Orange 26, C.I. Direct Orange 71, C.I. Direct Orange 107, C.I. Direct Red 2, C.I. Direct Red 31, C.I. Direct Red 79, C.I. Examples include Direct Red 81, C.I. Direct Red 247, C.I. Direct Green 80, C.I. Direct Green 59, etc., and dichroic dyes developed for manufacturing polarizers are preferred.
[0088] Boric acid crosslinking treatment can be performed by immersing a PVA film in an aqueous solution containing a boric acid crosslinking agent. By performing boric acid crosslinking treatment on the PVA film, the PVA molecular chains are crosslinked, and the orientation of the PVA molecular chains is improved. As a result, since the orientation of the dichroic pigment adsorbed on the PVA film is improved, the optical performance of the resulting polarizing film is enhanced. From this perspective, it is more preferable to perform the boric acid crosslinking treatment after the dyeing treatment and before the stretching treatment. As the boric acid crosslinking agent, one or more types of boron-containing inorganic compounds such as boric acid and borates such as borax may be used, and it is preferable that the boric acid crosslinking agent be boric acid for ease of handling. In order to maintain sufficient stretchability, the concentration of the boric acid crosslinking agent in the aqueous solution containing the boric acid crosslinking agent is preferably 1 to 10 mass%, and more preferably 2 to 7 mass%. If the concentration of the boric acid crosslinking agent exceeds 10 mass%, there is a risk that crosslinking will proceed excessively and the stretchability will decrease. In addition, if the concentration of the boric acid crosslinking agent is less than 1 mass%, there is a risk that the orientation of the dichroic pigment adsorbed on the PVA film will not be sufficiently improved, and the polarization performance of the resulting polarizing film will not be sufficiently improved. The aqueous solution containing the boric acid crosslinking agent may contain an auxiliary agent such as potassium iodide. The concentration of the boron-containing compound (B) in the aqueous solution containing the boric acid crosslinking agent is preferably 2.0 mass% or less, more preferably 0.5 mass% or less, and even more preferably 0.1 mass%, and it is particularly preferable that the aqueous solution does not substantially contain the boron-containing compound (B). In addition, in an aqueous solution containing a boric acid crosslinking agent, the ratio of the concentration (mass%) of the boron-containing compound (B) to the concentration (mass%) of the boric acid crosslinking agent [boron-containing compound (B) / boric acid crosslinking agent] is preferably less than 1, more preferably 0.5 or less, even more preferably 0.25 or less, and particularly preferably 0.1 or less.In terms of efficiently crosslinking boric acid, the temperature of the aqueous solution containing the boric acid crosslinking agent is preferably 20 to 50 ℃, and particularly preferably 25 to 40 ℃.
[0089] In the manufacturing method of the present invention, immersion of the PVA film in an aqueous solution containing a boric acid crosslinking agent may be performed in any treatment, but it is preferable to perform it in the boric acid crosslinking treatment. In addition, immersion of the PVA film in an aqueous solution containing a boric acid crosslinking agent may be performed in multiple treatments.
[0090] Apart from the stretching treatment described below, the PVA film may be stretched (pre-stretched) during or between each of the treatments described above. In this way, the total stretching ratio of the pre-stretching performed prior to the stretching treatment (a ratio obtained by multiplying the stretching ratio in each treatment) is preferably 1.5 times or more, more preferably 2.0 times or more, and even more preferably 2.5 times or more, based on the original length of the raw material PVA film before stretching, from the perspective of the optical performance of the obtained polarizing film. Meanwhile, the said total stretching ratio is preferably 4.0 times or less, and more preferably 3.5 times or less. The stretching ratio in the swelling treatment is preferably 1.05 to 2.5 times. The stretching ratio in the dyeing treatment is preferably 1.1 to 2.5 times. The stretching ratio in the boron crosslinking treatment is preferably 1.1 to 2.5 times.
[0091] The stretching treatment may be performed using either a wet stretching method or a dry stretching method. In the case of the wet stretching method, stretching is performed in an aqueous solution. Stretching may also be performed in the dyeing bath or an aqueous boric acid solution as described above. In the case of the dry stretching method, stretching treatment may be performed at room temperature, while heating, or in the air using a PVA film after absorption. Among these, the wet stretching method is preferred, and stretching treatment is more preferred to be performed in an aqueous solution containing boric acid. The concentration of boric acid in the aqueous boric acid solution is preferably within the range of 0.5 to 6 mass%, and more preferably within the range of 1 to 5 mass%. Additionally, the aqueous boric acid solution may contain potassium iodide, and its concentration is preferably within the range of 0.01 to 10 mass%. In the stretching treatment, the stretching temperature is preferably 30°C or higher, more preferably 40°C or higher, and even more preferably 50°C or higher. Meanwhile, the stretching temperature is preferably 90°C or lower, more preferably 80°C or lower, and even more preferably 70°C or lower. In addition, the stretching ratio in the stretching treatment is preferably 2.0 to 4.0 times. From the perspective of the optical performance of the obtained polarizing film, the said stretching ratio is more preferably 2.2 times or higher. Meanwhile, the said stretching ratio is more preferably 3.5 times or lower. Furthermore, regarding the optical performance of the obtained polarizing film, the total stretching ratio up to the fixing treatment described later is preferably 5 times or higher, and more preferably 5.5 times or higher, based on the original length of the raw material PVA film before stretching. Although there is no particular upper limit for the stretching ratio, it is preferable that the stretching ratio be 8 times or lower.
[0092] When performing a stretching treatment on a long PVA film, there are no particular restrictions on the direction of uniaxial stretching, and uniaxial stretching in the long length direction, transverse uniaxial stretching, or so-called inclined stretching can be employed; however, uniaxial stretching in the long length direction is preferred in that a polarizing film with excellent optical performance is obtained. Uniaxial stretching in the long length direction can be performed by using a stretching device equipped with a plurality of rolls parallel to each other and changing the peripheral speed between each roll. Meanwhile, transverse uniaxial stretching can be performed using a tenter-type stretching machine.
[0093] In manufacturing a polarizing film, it is desirable to perform a fixation treatment after the stretching treatment to strengthen the adsorption of dichroic pigments (such as iodine-based pigments) onto the PVA film. As the fixation treatment bath used for the fixation treatment, an aqueous solution containing a boron-containing compound (B) is preferably used. Additionally, if necessary, boric acid, iodine compounds, metal compounds, etc., may be further added to the fixation treatment bath. The temperature of the fixation treatment bath is preferably 35°C to 80°C. On the other hand, if the temperature of the fixation treatment bath exceeds 80°C, the polarizing film may melt in the fixation treatment bath, or wrinkles may form on the polarizing film, resulting in a decrease in polarization performance. The above temperature is more preferably 75°C or lower, and even more preferably 70°C or lower. The stretching ratio in the fixation treatment is preferably 1.3 times or lower, more preferably 1.2 times or lower, and even more preferably less than 1.1 times.
[0094] After immersing the PVA film in an aqueous solution containing a boric acid crosslinking agent, a boron-containing compound (B) may be adsorbed onto the PVA film during any of the processes of dyeing, stretching, or fixing. It is preferable to adsorb the boron-containing compound (B) onto the PVA film during the fixing process after stretching, as this allows for the efficient removal of unnecessary iodine-based pigments and suppresses the cutting of the PVA film during stretching. The boron-containing compound (B) may be used as a single type or as a mixture of two or more types. In order to rapidly proceed the substitution reaction between the boron-containing compound (B) and boric acid (C) on the surface of the PVA film, the concentration of the boron-containing compound (B) in the aqueous solution used for adsorption of the boron-containing compound (B) needs to be 1.5 to 5.0 mass%. If the above concentration is lower than 1.5 mass%, the adsorption of the boron-containing compound (B) onto the surface of the PVA film is delayed. The above concentration is preferably 2.0 mass% or higher, and more preferably 2.5 mass% or higher. Meanwhile, if the above concentration is higher than 5.0 mass%, the boron-containing compound (B) is excessively adsorbed on the surface of the PVA film, making it difficult for the substitution reaction between the boron-containing compound (B) and boric acid (C) to proceed. In addition, there is a risk that precipitates of the boron-containing compound (B) will form on the surface of the resulting polarizing film, thereby degrading optical performance. For this reason, the concentration of the boron-containing compound (B) is preferably 4.5 mass% or lower, and more preferably 4.0 mass% or lower. The concentration of the boric acid crosslinking agent in the aqueous solution containing the boron-containing compound (B) is preferably 1.5 mass% or less, more preferably 1.0 mass% or less, even more preferably 0.5 mass% or less, particularly preferably 0.1 mass% or less, and most preferably the aqueous solution does not substantially contain the boric acid crosslinking agent.In addition, in the aqueous solution containing the boron-containing compound (B), the ratio of the concentration of the boric acid crosslinking agent (mass%) to the concentration of the boron-containing compound (B) [boric acid crosslinking agent / boron-containing compound (B)] is preferably less than 1, more preferably 0.5 or less, even more preferably 0.25 or less, and particularly preferably 0.1 or less.
[0095] In addition, regarding the improvement of optical performance, it is preferable that the aqueous solution containing the boron-containing compound (B) contains an auxiliary agent of iodide, such as potassium iodide, and the concentration of said iodide is preferably 0.5 to 15 mass%. It is also preferable that the temperature of the aqueous solution containing the boron-containing compound (B) is 35 to 80°C. If the temperature is below 35°C, the substitution rate between the boron-containing compound (B) and boric acid (C) slows down, and there is a risk that the effect of improving polarization performance will be insufficient. It is more preferable that the temperature is 40°C or higher, and even more preferable that it is 45°C or higher. On the other hand, if the temperature is excessively high, there is a risk that the PVA film will dissolve in the aqueous solution or wrinkles will form on the resulting polarizing film, thereby degrading the polarization performance. For this reason, it is more preferable that the temperature is 75°C or lower, and even more preferable that it is 70°C or lower. The time for immersing the PVA film in the above aqueous solution is preferably 5 to 400 seconds. The above time is more preferably 10 seconds or more, more preferably 15 seconds or more, and particularly preferably 20 seconds or more. Meanwhile, the above time is more preferably 350 seconds or less, more preferably 250 seconds or less, particularly preferably 150 seconds or less, and most preferably 70 seconds or less.
[0096] Methods for adsorbing a boron-containing compound (B) onto a PVA film include (1) immersing the PVA film alone in an aqueous solution containing the boron-containing compound (B) without laminating it with a base film, etc., (2) laminating a base film to one side of the PVA film to reduce the occurrence of wrinkles during the fixing process, and then immersing the resulting laminate in the aqueous solution, (3) spraying the aqueous solution containing the boron-containing compound (B) onto the surface of a polarizing film, and (4) applying the aqueous solution to the surface of the PVA film using a roll coated with the aqueous solution, and among these, (1) is preferred. According to method (1), the adsorption of the boron-containing compound (B) from the surface of the PVA film to the center proceeds equally from both sides, which is preferred.
[0097] In the fixation treatment, a method for manufacturing the polarizing film of the present invention by adsorbing a boron-containing compound (B) onto a PVA film is preferably a method of performing swelling treatment, stretching treatment, and fixation treatment in this order, and a method of performing swelling treatment, boric acid crosslinking treatment, stretching treatment, and fixation treatment in this order, and the latter is more preferable. After performing these treatments, at least one treatment selected from the group consisting of washing treatment, drying treatment, and heat treatment may be performed as needed. After adsorbing the boron-containing compound (B) onto the PVA film, it is preferable not to immerse the PVA film in an aqueous solution containing a boric acid crosslinking agent.
[0098] Cleaning treatment is generally performed by immersing the film in distilled water, pure water, an aqueous solution, etc. At this time, for the sake of improving optical performance, it is preferable to use an aqueous solution containing an iodide such as potassium iodide as an auxiliary agent, and it is preferable to set the concentration of said iodide to 0.5 to 10 mass%. In addition, the temperature of the aqueous solution during cleaning treatment is generally 5 to 50°C, 10 to 45°C is preferable, and 15 to 40°C is more preferable. From an economic perspective, it is not desirable for the temperature of the aqueous solution to be excessively low, and if the temperature of the aqueous solution is excessively high, optical performance may deteriorate.
[0099] Although the conditions for the drying treatment are not particularly limited, it is preferable to perform drying at a temperature within the range of 30 to 150 ℃, particularly within the range of 50 to 130 ℃. By drying at a temperature within the above range, it is easy to obtain a polarizing film with excellent dimensional stability.
[0100] By performing heat treatment after drying, a polarizing film with even better dimensional stability can be obtained. Here, heat treatment refers to a process in which a polarizing film with a moisture content of 5% or less after drying is further heated to improve the dimensional stability of the polarizing film. Although the conditions for heat treatment are not particularly limited, it is preferable to perform heat treatment within the range of 60°C to 150°C, particularly within the range of 70°C to 150°C. If heat treatment is performed at a temperature lower than 60°C, the dimensional stabilization effect by heat treatment is insufficient, and if heat treatment is performed at a temperature higher than 150°C, severe reddening may occur in the polarizing film.
[0101] It is preferable that the transmittance of the polarizing film of the present invention obtained in this way is 42.0% or higher, and the degree of polarization is 99.85% or higher. If the transmittance of the polarizing film is less than 42.0%, there is a risk that the brightness of the obtained LCD will be insufficient. The transmittance is more preferably 43.0% or higher, and even more preferably 43.5% or higher. Meanwhile, the transmittance is typically 48% or lower. In addition, an LCD panel with high image quality is obtained by having a degree of polarization of 99.85% or higher. It is more preferable that the degree of polarization is 99.9% or higher. The transmittance and degree of polarization of the polarizing film are measured by the method described in the examples described below.
[0102] The polarizing film of the present invention is typically used as a polarizing plate by laminating a protective film, which is optically transparent and also has mechanical strength, onto both or one side thereof. As the protective film, tricellulose acetate (TAC) film, cellulose acetate-butyric acid (CAB) film, acrylic film, polyester film, etc. are used. In addition, as the adhesive for lamination, PVA-based adhesive or UV-curing adhesive may be used.
[0103] The polarizing plate obtained as described above may be laminated with a phase difference film, a viewing angle enhancement film, a brightness enhancement film, etc. In addition, after coating the polarizing plate with an adhesive such as an acrylic-based adhesive, it may be laminated with a glass substrate and used as a component of an LCD.
[0104] Examples
[0105] The present invention will be specifically explained by the following examples, but the present invention is not limited in any way by these examples. In addition, each evaluation method employed in the following examples and comparative examples is shown below.
[0106] <Calculation of total boron element content (T), etc. in polarizing film>
[0107] The mass [A (g)] of a polarizing film conditioned at 23 ℃ and 50 % RH for 16 hours was measured, and the polarizing film was dissolved in 20 mL of distilled water to a mass of 0.005 mass%. The aqueous solution in which the polarizing film was dissolved was used as the measurement sample, and its mass [B (g)] was measured. The boron concentration [C (ppm)], potassium concentration [D (ppm)], and iodine concentration [E (ppm)] of the measurement sample were measured using a multi-type ICP emission analyzer (ICP) manufactured by Shimadzu Corporation. Subsequently, the values calculated by substituting the measured values into the following equations (1), (2), and (3) were defined as the total boron element content (mass%), total potassium element content (mass%), and total iodine element content (mass%) in the polarizing film.
[0108] Total boron element content (T, mass%) in polarizing film
[0109] = [(C × 10 -6 × B) / A] × 100 (1)
[0110] Total potassium element content in polarizing film (F, mass%)
[0111] = [(D × 10 -6 × B) / A] × 100 (2)
[0112] Total iodine element content in polarizing film (G, mass%)
[0113] = [(E × 10 -6 × B) / A] × 100 (3)
[0114] <Calculation of Moisture Content (H, mass%) in Polarizing Film>
[0115] About 0.1 g of a polarizing film that had been heated at 23 ℃ and 50 % RH for 16 hours was cut, and its mass [X (g)] was measured. After drying the polarizing film in a dryer at 105 ℃ for 16 hours, the mass [Y (g)] of the polarizing film was measured. The obtained values were substituted into the following equation (4) to calculate the moisture content in the polarizing film.
[0116] Moisture content (H, mass%) in polarizing film
[0117] = (X - Y) / X × 100 (4)
[0118] < Boron element content derived from boron-containing compound (B) in polarizing film (b t Measurement of )
[0119] A solution in which a polarizing film is dissolved in heavy water to a concentration of 0.003 mass% and then concentrated to 0.15 mass% using a rotary evaporator 1 It was used as a sample for H-NMR measurement. 1 H-NMR (JNM-AL400, manufactured by Nihon Electronics Co., Ltd.: 400 MHz) measurements were performed at 80 ℃, and the number of integrated cycles was set to 256. The results were analyzed using ALICE2 (manufactured by Nihon Electronics Co., Ltd.) according to the following method. The obtained from the measurement 1For the H-NMR chart, the phase was adjusted to make the baseline smooth, and the baseline correction was performed automatically by setting the average point to 20. Next, the peak of the heavy water, which is the measurement solvent, was automatically set as a reference at the position of 4.65 ppm. Then, as shown in Fig. 2, the hydrogen peak of the hydrocarbon group included in the boron-containing compound (B) was integrated, and the peak area (Area I) was calculated. At this time, the sum of the hydrogen peak areas of the hydrocarbon group included in the boron-containing compound (B) that do not overlap with the hydrogen peak of PVA (Area J) was used as the standard for the peak area, and the value of Area J was set so that the number of hydrogens in the corresponding hydrocarbon group of the boron-containing compound (B) was equal to the value of Area J. Next, the hydrogen peak in the range of 1.6 to 2.4 ppm was considered as the sum of the hydrogen peak derived from the methylene group of PVA and the hydrogen peak of the hydrocarbon group contained in the boron-containing compound (B) that overlaps with the hydrogen peak derived from the methylene group of PVA, and the peak area (area K) was calculated. Then, the area L was calculated by subtracting the number of hydrogens of the hydrocarbon group of the boron-containing compound (B) that overlaps with the hydrogen peak of the methylene group derived from PVA from the area K. The values obtained by these methods were substituted into the following equation (5) to calculate the content of organic groups derived from the boron-containing compound (B) (M, mass parts) per 100 mass parts of PVA (A). In addition, the boron content (N, mass parts) derived from the boron-containing compound (B) per 100 mass parts of PVA (A) was calculated by substituting the values into the following equation (6). In addition, in the following formulas (5) and (6), O is the number of hydrogens in the hydrocarbon group contained in the boron-containing compound (B) that does not overlap with the peak of PVA, P is the number of borons per molecule of the boron-containing compound (B), and Q is the number of organic groups of the boron-containing compound (B).Then, by substituting each calculated value into Equation (7), the boron element content (b) derived from the boron-containing compound (B) in the polarizing film is obtained. t , mass %) was calculated. In addition, Equations (5), (6), and (7) are used when using non-modified PVA, and when using modified PVA as a raw material, it is necessary to appropriately modify Equations (5), (6), and (7).
[0120] Content of organic groups derived from boron-containing compounds (B) per 100 parts by mass of PVA (A) (M, parts by mass)
[0121] ={(Area J / O) / (Area L / 2)}× (Q / 44.0526) × 100 (5)
[0122] Boron element content (N, parts by mass) derived from boron-containing compound (B) per 100 parts by mass of PVA (A)
[0123] ={(Area J / O) / (Area L / 2)}× (10.811 × P / 44.0526) × 100 (6)
[0124] Boron element content derived from boron-containing compound (B) in polarizing film (b t , mass%)
[0125] = N × 1 / (100 + M) × (100 - T - F - G - H) (7)
[0126] In the formula, 10.811 is the atomic weight of boron, and 44.0526 is the molecular weight per mole of repeating unit of unmodified PVA. Also, of Fig. 2 1 The H-NMR chart was obtained by measuring the polarizing film of Example 1.
[0127] < Boron element concentration (b o ), boron element concentration (b i ), boron element concentration (c o ) and boron element concentration (c i Output of )
[0128] The concentration of boron elements derived from boron-containing compounds (B) in a polarizing film was measured using a gas cluster ion beam gun-equipped X-ray photoelectron spectrometer (manufactured by ALVAC PY Inc.: PHI5000 VersaProbe II) (GCIB-XPS). For the measurement, a polarizing film that had been conditioned for at least 16 hours at approximately 23°C and 40% RH was used. Under conditions of a sputter ion source Ar2500+, an acceleration voltage of 10 keV, and a current of 30 nA, sputtering was performed over a range of 1 mm × 1 mm while neutralizing, and X-ray photoelectron spectroscopic measurements (XPS measurements) were performed. XPS measurements were performed using monochromatic Al as the X-ray source, with an X-ray spot diameter of 200 μm and an X-ray output of 15 kV and 50 W, and five types of detection elements were selected: carbon, boron, oxygen, iodine, and potassium. In addition, when using dichroic dyes as dichroic pigments, it is necessary to appropriately select elements such as nitrogen and sulfur contained in the dichroic dyes as detection elements. Next, using the analysis software "MultiPak" (manufactured by ALVAC PY Co., Ltd.), the boron element concentration (a, atomic %) at each depth of the polarizing film was calculated based on the bonding energy of CC and CH bonds, which is 284.8 eV. After that, for the XPS spectra at each depth, the binding energy attributable to boron in boric acid (C) and the binding energy attributable to boron in boron-containing compound (B) were appropriately set, and peak separation was performed using the least squares method with a pseudo-forkt function using the table calculation software “Microsoft 2010” (manufactured by Microsoft Corporation). In addition, a linear function calculated from the average intensity of the XPS spectra at 187 to 189 eV and the average intensity of the XPS spectra at 195 to 197 eV was used as a baseline.In this way, the ratio (b, %) of the peak area of boron from boron-containing compound (B) to the sum of the peak area of boron from boric acid (C) and the peak area of boron from boron-containing compound (B) was calculated, and by substituting this into the following formula (8), the concentration of boron element from boron-containing compound (B) at each depth and the concentration of boron element from boric acid (C) at each depth were calculated.
[0129] Elemental boron concentration (atomic%) derived from boron-containing compound (B)
[0130] = a × b × 10 -2 (8)
[0131] Elemental boron concentration (atomic%) derived from boric acid (C)
[0132] = a × (100 - b) × 10 -2 (9)
[0133] In addition, the binding energy originating from boron in the boron-containing compound (B) varies depending on the structure of the said compound. Therefore, it is necessary to set the said binding energy appropriately according to the type of boron-containing compound (B). For example, if the boron-containing compound (B) is n-propylboronic acid, it is around 191.5 eV. Also, when performing peak separation using the least squares method with a pseudo-Forkt function, the Laurent function ratio of boric acid is set to 0.241, and 2 1 / 2 × σ was set to 0.916. In addition, the Laurent content and full width at half maximum of the boron-containing compound (B) also vary depending on the structure of the compound. Therefore, depending on the type of compound, the Laurent content and 2 1 / 2 It is necessary to set × σ appropriately. If the boron-containing compound (B) is n-propylboronic acid, the Laurent content is 0.000, 2 1 / 2 × σ was set to 0.769.
[0134] By this method, the boron element concentration (atomic %) derived from the boron-containing compound (B) and the boron element concentration (atomic %) derived from boric acid (C) were each calculated at each depth from one surface of the polarizing film to the center. Specifically, the etching range was set so that the etching rate was approximately 16 to 26 nm / min, and a total of 14 measurements were performed while etching from one surface of the polarizing film to the center, and the boron element concentration (atomic %) derived from the boron-containing compound (B) and the boron element concentration (atomic %) derived from boric acid (C) were each calculated at each measurement, that is, at each depth. Then, the same measurements were performed from the other surface of the polarizing film, and the boron element concentration (atomic%) derived from the boron-containing compound (B) and the boron element concentration (atomic%) derived from boric acid (C) at each depth were calculated, respectively. Subsequently, the average value of the boron element concentration derived from the boron-containing compound (B) calculated in the range up to 7.5% of the total thickness from the surface of the polarizing film inward was the boron element concentration derived from the boron-containing compound (B) (b o , atomic %), and the average value of the boron element concentration (atomic %) derived from boric acid (C) calculated within the said range is the boron element concentration (c) derived from boric acid (C). o , atomic %) was used.
[0135] Also, the average value of the boron element concentration derived from the boron-containing compound (B) calculated in the range of up to 7.5% of the total thickness from the center to the outside of the polarizing film is the boron element concentration derived from the boron-containing compound (B) (b i , atomic %), and the average value of the boron element concentration derived from boric acid (C) calculated within the said range is the boron element concentration derived from boric acid (C) (c i , atomic %). In addition, to minimize error, measurements from the outermost surface where sputtering was not performed were excluded, and the average concentration (co ) and (b o ) was produced.
[0136] <Optical Performance of Polarizing Films>
[0137] A rectangular sample measuring 4 cm in length direction × 2 cm in width direction was taken from the center of the polarizing film in the width and length directions, and the parallel transmittance and cross-Nicole transmittance of the polarizing film were measured using an integrating sphere-equipped spectrophotometer V-7100 (manufactured by Nihon Bunko Co., Ltd.) and an automatic polarizing film measuring device VAP-7070S (manufactured by Nihon Bunko Co., Ltd.) equipped with a Glen Taylor polarizer. Here, the measurement wavelength range was set to 380 to 780 nm, and the transmittance when the vibration direction of the polarizing light incident on the polarizing film through the Glen Taylor polarizer was parallel to the transmission axis of the polarizing film was defined as parallel transmittance, and the transmittance when it was perpendicular to the transmission axis of the polarizing film was defined as cross-Nicole transmittance. Afterwards, using the “Polarizing Film Evaluation Program” (manufactured by Nihon Bunko Co., Ltd.), visual sensitivity correction was performed in the visible light region of a 2° field of view with a C light source using the aforementioned parallel transmittance and cross-Nicole transmittance in accordance with JIS Z 8722 (Method for Measuring Object Color), and the single transmittance and degree of polarization of the polarizing film were calculated, and these two values were obtained as the optical characteristics of the polarizing film.
[0138] <Swelling Degree of PVA Film>
[0139] A PVA film was cut to a size of 5 cm × 10 cm and immersed in 1000 mL of distilled water at 30 ℃ for 30 minutes. Afterward, the PVA film was removed, the moisture on the surface of the PVA film was wiped off with filter paper, and the mass [R (g)] of the PVA film after immersion was measured. Then, the PVA film was dried in a dryer at 105 ℃ for 16 hours, and the mass [S (g)] of the PVA film after drying was measured. The degree of swelling of the PVA film was calculated by substituting the value into the following equation (10).
[0140] Swelling degree (%) = (R / S) × 100 (10)
[0141] [Example 1]
[0142] An aqueous PVA solution was prepared comprising 100 parts by mass of PVA (degree of saponification 99.9%, degree of polymerization 2400), 10 parts by mass of glycerin as a plasticizer, and 0.1 parts by mass of sodium polyoxyethylene lauryl ether sulfate as a surfactant, with a PVA content of 10% by mass. The film obtained by drying the above aqueous PVA solution on a metal roll at 80°C was heat-treated in a hot air dryer (120°C) for 10 minutes, and a PVA film with a thickness of 30 μm and a swelling degree of 200% was obtained.
[0143] A sample measuring 5 cm in width × 9 cm in length was cut from the center of the obtained PVA film in the width direction so that it could be uniaxially stretched over a range of 5 cm in width × 5 cm in length. This sample was immersed in pure water at 30°C for 30 seconds while being uniaxially stretched 1.1 times in the longitudinal direction and subjected to swelling treatment. Subsequently, iodine was adsorbed by immersing the sample in an aqueous solution at 30°C (dyeing treatment bath) containing 0.035 mass% iodine and 3.5 mass% potassium iodide for 60 seconds while being uniaxially stretched 2.2 times (2.4 times overall). Next, the film was immersed in an aqueous solution at 30°C (boric acid crosslinking treatment bath) containing 3.0 mass% boric acid and 3 mass% potassium iodide and uniaxially stretched in the longitudinal direction by 1.2 times (2.7 times total). Furthermore, the film was immersed in an aqueous solution at 60°C (stretching treatment bath) containing 4.0 mass% boric acid and 6 mass% potassium iodide and uniaxially stretched in the longitudinal direction up to 6.0 times total. After the stretching treatment, the film was immersed for 30 seconds in an aqueous solution at 50°C (fixation treatment bath) containing 3.0 mass% n-propylboronic acid and 3.5 mass% potassium iodide as a boron-containing compound (B). During the fixation treatment, the PVA film was not stretched (stretching ratio 1.0 times). Finally, a polarizing film (thickness 13 μm) was prepared by drying at 60 ℃ for 240 seconds.
[0144] The total boron, potassium, and iodine content in the obtained polarizing film were measured and found to be 4.3 mass%, 1.0 mass%, and 5.0 mass%, respectively. Next, the moisture content in the polarizing film was calculated to be 10.0 mass%. And, of the polarizing film 1As a result of measuring and analyzing H-NMR, a hydrogen peak of n-propylboronic acid appeared at 1.1 to 1.3 ppm that did not overlap with the hydrogen peak of PVA, so the peak area (area J) was set to 5. Next, the peak area (area K) of the hydrogen of the methylene group of PVA, which appeared in the range of 1.6 to 2.4 ppm, was calculated. Since the hydrogen peak of the methylene group of PVA overlapped with the hydrogen peak of the C2 hydrocarbon group of n-propylboronic acid, the number of hydrogens of the C2 hydrocarbon group of n-propylboronic acid, 2, was subtracted from the area K to obtain the area L. As a result of substituting these values into the above equations (5), (6), and (7), the boron element content derived from the boron-containing compound (B) in the polarizing film was 0.7 mass%. As a result of measuring and interpreting the XPS spectrum of the polarizing film, the boron element concentration (b) derived from the boron-containing compound (B) in the range of up to 7.5% of the total thickness (surface portion) from the surface to the inside of the polarizing film o ) is 3.1 atomic%, and the concentration of boron element derived from boric acid (C) on the surface (c o ) was 4.6 atomic%. Also, the boron element concentration (b) derived from the boron-containing compound (B) in the range from the center to the outside of the polarizing film, up to 7.5% of the total thickness (central part) i ) is 1.1 atomic %, and the concentration of boron element derived from boric acid (C) in the center (c i ) was 5.7 atomic%.
[0145] As a result of evaluating the optical properties of the polarizing film by the above method, the single transmittance at a polarization degree of 99.9% was 44.85%.
[0146] [Examples 2, 3, Comparative Examples 1–5]
[0147] Polarizing films were prepared in the same manner as in Example 1, except that the composition, temperature, and immersion time of the fixation treatment bath were changed as shown in Table 1, and each measurement and evaluation was performed. In addition, Comparative Example 4 is, 1 In the measurement of H-NMR, the boron-containing compound (B) could not be detected when the number of integration cycles was 256, so the number of integration cycles was changed to 4096.
[0148] [Comparative Example 6]
[0149] This is an example of a polarizing film that does not contain a boron-containing compound (B). A polarizing film was prepared in the same manner as in Example 1, except that an aqueous solution (temperature 30°C) containing 2 mass% of potassium iodide was used as the fixation treatment bath and the immersion time in the fixation treatment bath was changed to 20 seconds, and each measurement and evaluation was performed.
[0150] [Comparative Example 7]
[0151] This is an example of a polarizing film that does not contain a boron-containing compound (B). A polarizing film was prepared in the same manner as in Example 1, except that an aqueous solution (temperature 30°C) containing 2 mass% of potassium iodide was used as the fixation treatment bath and the immersion time in the fixation treatment bath was changed to 5 seconds, and each measurement and evaluation was performed.
[0152] In addition, in Examples 2 to 3 and Comparative Examples 1 to 7, iodine was adsorbed by immersing the film in an aqueous solution (dyeing treatment bath) (temperature 30°C) containing 100 parts by mass of potassium iodide to 1 part by mass of iodine for 60 seconds, as in Example 1, while uniaxially stretching it in the longitudinal direction by 2.2 times (2.4 times overall). At this time, the iodine concentration and potassium iodide concentration of the dyeing treatment bath were adjusted so that the polarization degree of the polarizing film after drying was 99.9%. Furthermore, in any of Examples 1 to 3 and Comparative Examples 1 to 7, measurements and evaluations were performed on both surfaces of the polarizing film, and the same results were obtained in all cases. The reason for the same result on both surfaces of the polarizing film is presumed to be that, during the fixation treatment, the adsorption of the boron-containing compound (B) from the surface of the PVA film to the center proceeded equally on both sides.
[0153]
[0154] As shown in Table 1, the polarizing films of Examples 1 to 3 of the present invention have high polarization performance and high single transmittance, so they can meet the demand for high precision in recent electronic devices. Explanation of the symbols
[0155] 1 : Surface 2 : Surface 3 : Center 4 : Central part 5: Hydrogen peak derived from heavy water, the measurement solvent 6: Hydrogen peak derived from the methine group of PVA 7: Hydrogen peak derived from the methylene group of PVA 8: Hydrogen peak derived from a hydrocarbon group contained in the boron-containing compound (B) overlapping with the hydrogen peak derived from PVA 9: Hydrogen peak derived from a hydrocarbon group contained in the boron-containing compound (B) that does not overlap with the hydrogen peak derived from PVA. to , t i , t t : thickness
Claims
Claim 1 A polarizing film comprising polyvinyl alcohol (A), at least one boron-containing compound (B) selected from the group consisting of monoboronic acid represented by the following formula (I) and a compound capable of being converted into the monoboronic acid in the presence of water, and boric acid (C), wherein the boron element content (b) derived from the boron-containing compound (B) t ) is 0.3 to 2.0 mass%, the total boron element content (T) is 3.0 to 7.0 mass%, and also (b for (T). t The ratio of ) (b t / T) is 0.10 to 0.30, and the boron element concentration (b) derived from the boron-containing compound (B) is in the range of up to 7.5% of the total thickness from at least one surface inward. o Polarizing film having 2.2 to 10.0 atomic%. [In Equation (I), R 1 is a monovalent aliphatic group with 1 to 20 carbon atoms, and R 1 The boronic acid group is connected by a boron-carbon bond. Claim 2 In claim 1, the boron element concentration (b) derived from the boron-containing compound (B) in a range of up to 7.5% of the total thickness from the center outward of the polarizing film. i ) is 0.5 to 2.0 atomic %, and also the boron element concentration derived from boric acid (C) (c i A polarizing film having ) 3.5 to 8.0 atomic%. Claim 3 In claim 1, the boron element concentration (c) derived from boric acid (C) in a range of up to 7.5% of the total thickness from the center outward of the polarizing film. i ) for which elemental boron concentration derived from boron-containing compound (B) (b i The ratio of ) (b i / c i Polarizing film with a ) value of 0.01 to 0.
25. Claim 4 In claim 1, the boron element concentration (c) derived from boric acid (C) in a range of up to 7.5% with respect to the total thickness, inwardly from at least one surface of the polarizing film. o Polarizing film having 3.3 to 7.8 atomic%. Claim 5 In claim 1, the boron element concentration (b) derived from a boron-containing compound (B) in a range of up to 7.5% with respect to the total thickness, inwardly from at least one surface of the polarizing film. o ) a boron element concentration (b) derived from a boron-containing compound (B) in a range of up to 7.5% of the total thickness from the center to the outside of the polarizing film. i Polarizing film, higher than ) Claim 6 In claim 1, the boron element concentration (c) derived from boric acid (C) in a range of up to 7.5% with respect to the total thickness, inwardly from at least one surface of the polarizing film. o ) a boron element concentration (c) derived from boric acid (C) in a range of up to 7.5% of the total thickness from the center to the outside of the polarizing film. i Polarizing film lower than ) Claim 7 In claim 1, R 1 This polarizing film is a saturated aliphatic group. Claim 8 In claim 1, R 1 This is a polarizing film that is a straight-chain aliphatic hydrocarbon group. Claim 9 In claim 1, R 1 Polarizing film having 2 to 5 carbon atoms. Claim 10 A polarizing film according to claim 1, wherein the transmittance is 42% or more when the degree of polarization is 99.9% or more. Claim 11 A method for manufacturing a polarizing film according to any one of claims 1 to 10, comprising a dyeing treatment of dyeing a polyvinyl alcohol film with a dichroic dye and a stretching treatment of stretching the film uniaxially, wherein the film is immersed in an aqueous solution containing a boric acid crosslinking agent, and then immersed in an aqueous solution at 35 to 80°C containing 1.5 to 5.0 mass% of a boron-containing compound (B).
Citation Information
Patent Citations
Manufacturing method of polarizer
JP2018180022A
Crosslinking agent for preparing a polarizer and method of preparing a polarizer using the same
KR1020140075154A
Process for Preparing Polarizer
KR1020150052777A
Polarizer, one-side-protected polarizing film, polarizing film including adhesive layer, and image display device and method for continuously manufacturing same
KR1020180103974A
Polarizing film and method for manufacturing same
WO2019146677A1