Photosensitive element, method for forming resist pattern, and method for producing wiring board

The photosensitive element with optimized compositions forms resist patterns with superior adhesion and plated copper wiring properties, addressing the challenge of fine wiring pattern formation in existing technologies.

KR103045262B1Active Publication Date: 2026-11-06ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020240108956
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-08-21
Filing Date
2024-08-14
Publication Date
2026-11-06
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Existing photosensitive elements struggle to form resist patterns with both excellent adhesion to the substrate and plated copper wiring formation properties, particularly for fine wiring patterns of 7 μm or less.

Method used

A photosensitive element comprising a support film and a photosensitive resin layer with specific compositions, including an alkali-soluble polymer, a compound with ethylenically unsaturated bonds, and a non-imidazole photopolymerization initiator, with optimized content ratios and components to enhance adhesion and plated copper wiring formation.

Benefits of technology

The solution enables the formation of resist patterns with excellent adhesion and plated copper wiring properties, allowing for the creation of fine, independent lines with retention after plating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024088627641-PAT00013_ABST
    Figure 112024088627641-PAT00013_ABST
Patent Text Reader

Abstract

(Problem) Provides a photosensitive element capable of forming a resist pattern with excellent adhesion to a substrate and plated copper wiring formation properties. (Solution) A photosensitive element comprising a support film and a photosensitive resin layer including a photosensitive resin composition, The above photosensitive resin composition comprises the following components based on the total solid mass of the photosensitive resin composition: (A) Alkali-soluble polymer: 30 to 70 mass% ; (B) Compound having ethylenically unsaturated bonds: 20 to 60 mass%; and (C) Non-imidazole photopolymerization initiator: 4.0 to 10.0 mass% ; Includes, The content of the constituent unit derived from benzyl (meth)acrylate in the above component (A) is 40 mass% or more with respect to the total of component (A), and A photosensitive element in which the content of a compound having two molecules having ethylenically unsaturated bonds in the above component (B) is 80 mass% or more with respect to the entire component (B).
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a photosensitive element and a method for forming a resist pattern. Background Technology

[0002] Printed circuit boards are generally manufactured using a photolithography process. In photolithography, first, a film containing a photosensitive resin composition is formed on a substrate, and then a resist pattern is formed by performing pattern exposure and development on the film. Subsequently, a conductor pattern is formed by etching or plating treatment. After that, a predetermined wiring pattern is formed on the substrate by removing the resist pattern on the substrate.

[0003] Recently, with the miniaturization and high-density increase of electronic devices, finer wiring patterns than conventional ones are required. In relation to this requirement, MSAP (Modified Semi Additive Process) and SAP (Semi Additive Process) are attracting attention. In these methods, in order to form fine wiring, it is desired to form a resist pattern with both adhesion and resolution of 7 μm or less, for example. In relation to the aspect of forming such a resist pattern, Patent Document 1 discloses a photosensitive resin composition comprising a binder polymer, a photopolymerizable compound, a photopolymerization initiator, and an anthracene-based sensitizer, wherein the binder polymer comprises a polymer (a) having a hydroxyalkyl (meth)acrylate unit and a styrene or styrene derivative unit, and the content of the styrene or styrene derivative unit is 40 mass% or more. In addition, Patent Document 1 discloses a photosensitive element having a photosensitive resin layer formed using such a photosensitive resin composition on a support. Prior art literature

[0004] International Patent Publication No. 2021 / 193232 The problem to be solved

[0005] However, in the photosensitive element of Patent Document 1, it was difficult to form a resist pattern that combines the adhesion of the resist pattern to the substrate with the formation of plated copper wiring.

[0006] Therefore, the object of the present invention is to provide a photosensitive element capable of forming a resist pattern with excellent adhesion to a substrate and excellent plated copper wiring formation properties. Furthermore, the object of the present invention is to provide a method for forming a resist pattern using such a photosensitive element. means of solving the problem

[0007] [1]

[0008] A photosensitive element comprising a support film and a photosensitive resin layer including a photosensitive resin composition,

[0009] The above photosensitive resin composition comprises the following components based on the total solid mass of the photosensitive resin composition:

[0010] (A) Alkali-soluble polymer: 30 to 70 mass% ;

[0011] (B) Compound having ethylenically unsaturated bonds: 20 to 60 mass%; and

[0012] (C) Non-imidazole photopolymerization initiator: 4.0 to 10.0 mass% ;

[0013] Includes,

[0014] The content of the constituent unit derived from benzyl (meth)acrylate in the above component (A) is 40 mass% or more with respect to the total of component (A), and

[0015] A photosensitive element in which the content of a compound having two molecules having ethylenically unsaturated bonds in the above component (B) is 80 mass% or more with respect to the entire component (B).

[0016] [2]

[0017] The photosensitive element described in Item 1, wherein the content of the above (C) component is 4.50 mass% or more with respect to the total solid mass of the photosensitive resin composition.

[0018] [3]

[0019] A photosensitive element described in Item 1 or 2, wherein the content of the above (C) component is 4.75 mass% or more with respect to the total solid mass of the photosensitive resin composition.

[0020] [4]

[0021] A photosensitive element described in any one of items 1 to 3, wherein the content of the above (C) component is 5.25 mass% or more with respect to the total solid mass of the photosensitive resin composition.

[0022] [5]

[0023] A photosensitive element described in any one of items 1 to 4, wherein the content of the above (C) component is 6.00 mass% or more with respect to the total solid mass of the photosensitive resin composition.

[0024] [6]

[0025] A photosensitive element described in any one of items 1 to 5, wherein the content of a constituent unit derived from benzyl (meth)acrylate in the above component (A) is 50 weight% or more with respect to the total component (A).

[0026] [7]

[0027] A photosensitive element described in any one of items 1 to 6, wherein the content of a constituent unit derived from benzyl (meth)acrylate in the above component (A) is 60 weight% or more with respect to the total component (A).

[0028] [8]

[0029] A photosensitive element described in any one of items 1 to 7, wherein the content of a compound having two of the above-mentioned ethylenically unsaturated bonds is 90 mass% or more with respect to the total of (B) components.

[0030] [9]

[0031] A compound having two of the above-mentioned ethylenically unsaturated bonds is of the following general formula (II):

[0032] [Chemical Formula 1]

[0033]

[0034] (during food, R 2 are, each independently, a hydrogen atom or a methyl group, and X 2 O and Y 2 O is, each independently, an oxyethylene group or an oxypropylene group, m3, m4, n2, and n3 are, each independently, integers from 0 to 40, m3 + m4 is from 1 to 40, and n2 + n3 is from 0 to 20.

[0035] A photosensitive element described in any one of items 1 to 8, comprising a compound represented by .

[0036]

[10]

[0037] A photosensitive element described in Item 9, wherein the content of the compound represented by the above general formula (II) is 90 mass% or more with respect to the total of component (B).

[0038]

[11]

[0039] A compound having two of the above-mentioned ethylenically unsaturated bonds among the molecules is,

[0040] A compound in which the average value of n2+n3+m3+m4 in the above general formula (II) is 10 or less, and

[0041] A photosensitive element described in item 9 or 10 comprising a compound in which the average value of n2 + n3 + m3 + m4 in the above general formula (II) is 15 or more.

[0042]

[12]

[0043] With respect to the total solid mass of the photosensitive resin composition, the above (C) component is included in an amount of 5.0 mass% or more, and

[0044] The absorbance (Y) at a wavelength of 365 nm at a film thickness of 25 μm of the above photosensitive resin layer is 0.35 or less, and

[0045] The contribution (X) of the absorbance of the above (C) component to the above absorbance (Y) is 40% or more, and

[0046] The above contribution (X) is the following equation (1):

[0047] X (%) = 100×εc / absorbance (Y) of photosensitive resin layer ··· (1)

[0048] ε : Change in absorbance per 1 mass% of component (C)

[0049] c: Content of component (C) relative to the total mass of the solid components of the photosensitive resin composition (mass%)

[0050] A photosensitive element described in any one of items 1 to 11, produced by

[0051]

[13]

[0052] A photosensitive element described in Item 12, having a contribution (X) of 55% or more.

[0053]

[14]

[0054] A photosensitive element described in Item 12 or 13, having a contribution (X) of 65% or more.

[0055]

[15]

[0056] A photosensitive element described in any one of items 12 to 14, having a contribution (X) of 85% or more.

[0057]

[16]

[0058] A photosensitive element described in any one of items 12 to 15, having an absorbance (Y) of 0.30 or less.

[0059]

[17]

[0060] A photosensitive element described in any one of items 12 to 16, having an absorbance (Y) of 0.25 or less.

[0061]

[18]

[0062] The above photosensitive resin composition is,

[0063] (D) Other photopolymerization initiators

[0064] Including additionally,

[0065] The above (D) component comprises at least one selected from the group consisting of benzophenone compounds, pyrazolin compounds, anthracene compounds and coumarin compounds, a photosensitive element described in any one of items 1 to 17.

[0066]

[19]

[0067] The above photosensitive resin composition further comprises (D) other photopolymerization initiators, and

[0068] The above (D) component comprises at least one selected from the group consisting of benzophenone compounds and pyrazolin compounds, a photosensitive element as described in Item 18.

[0069]

[20]

[0070] The above photosensitive resin composition is,

[0071] (E) Polymerization inhibitor

[0072] A photosensitive element described in any one of items 1 to 19, additionally comprising

[0073]

[21]

[0074] The photosensitive element described in Item 20, further comprising phenothiazine and / or tert-butylcatechol as the polymerization inhibitor (E) above.

[0075]

[22]

[0076] The photosensitive element described in item 20 or 21, wherein the content of the polymerization inhibitor (E) above is 50 to 500 ppm with respect to the total solid mass of the photosensitive resin composition.

[0077]

[23]

[0078] A photosensitive element described in any one of items 1 to 22, wherein the absorbance of the above-mentioned support film at 365 nm is 0.1 or less.

[0079]

[24]

[0080] A photosensitive element described in any one of items 1 to 23, additionally equipped with a protective film.

[0081]

[25]

[0082] A method for forming a resist pattern using a photosensitive element described in any one of items 1 to 24,

[0083] The following process:

[0084] Process of laminating a photosensitive element onto a substrate;

[0085] A process of exposing a photosensitive resin layer of the stacked photosensitive element; and

[0086] A process for developing the above photosensitive resin layer after exposure;

[0087] A method for forming a resist pattern, comprising

[0088]

[26]

[0089] A photosensitive element roll formed by winding a photosensitive element described in any one of items 1 to 24.

[0090]

[27]

[0091] A process of forming a resist pattern on a substrate using a photosensitive element described in any one of items 1 to 24, and

[0092] A process for forming a conductor pattern by etching or plating a substrate having a resist pattern formed thereon, and

[0093] Process of peeling a resist pattern from a substrate

[0094] A method for manufacturing a wiring board, comprising

[0095]

[28]

[0096] A process of forming a resist pattern on a substrate made of a metal film insulating plate using a photosensitive element described in any one of items 1 to 24, and

[0097] A process for forming a conductor pattern by plating a substrate having a resist pattern formed thereon, and

[0098] A process for peeling a resist pattern from a substrate, and

[0099] Process of removing conductor layers other than the above conductor pattern

[0100] A method for manufacturing a wiring board comprising in this order.

[0101]

[29]

[0102] A method for manufacturing a wiring board as described in Item 28, forming a wiring board having a conductor pattern with a width of 10 μm or less. Effects of the invention

[0103] The present invention can provide a photosensitive element capable of forming a resist pattern with excellent adhesion of the resist pattern and plated copper wiring formation properties. In addition, the present invention can provide a method for forming a resist pattern using such a photosensitive element. Brief explanation of the drawing

[0104] FIG. 1 is a plan view for explaining an example of a “foreign substance” assumed by the present embodiment. FIG. 2 is a plan view showing the configuration of a mask pattern related to the present embodiment. FIG. 3 is a plan view showing the configuration of a mask pattern related to the present embodiment. FIG. 4 is a plan view showing the configuration of a mask pattern related to the present embodiment. FIG. 5 is a drawing showing an example of an observed image related to the present embodiment. FIG. 6 is a drawing showing an example of an observed image related to the present embodiment. Specific details for implementing the invention

[0105] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0106] The present invention is not limited to this embodiment but can be implemented with various modifications within the scope of its gist.

[0107] In this specification, where multiple structures represented by the same reference numeral exist within the same formula, unless otherwise specified, each structure may be selected independently, and may be identical or different from one another. In the same specification, where multiple structures represented by the same reference numeral exist within different formulas, unless otherwise specified, each structure may be selected independently, and may be identical or different from one another. In this specification, various measurements are performed based on the methods described in the embodiments unless specifically mentioned otherwise.

[0108] In this specification, the upper or lower limit of a numerical range described in steps may be substituted with the upper or lower limit of a numerical range described in another corresponding step, or may be substituted with the corresponding value described in the examples. Regarding the term "process," it is included in this term not only when it is an independent process, but also when it cannot be clearly distinguished from other processes, provided that the function of the process is achieved.

[0109] In the drawings, scales, shapes, and lengths may be exaggerated to enhance clarity. In this specification, various measurements are performed based on the methods described in the embodiments unless otherwise specifically stated.

[0110] [First Embodiment]

[0111] [Photosensitive element]

[0112] The present embodiment is a photosensitive element comprising a support film and a photosensitive resin layer comprising a photosensitive resin composition.

[0113] Herein, the photosensitive resin composition comprises the following components with respect to the total solid mass of the photosensitive resin composition:

[0114] (A) Alkali-soluble polymer: 30 to 70 mass% ;

[0115] (B) Compound having ethylenically unsaturated bonds: 20 to 60 mass%; and

[0116] (C) Non-imidazole photopolymerization initiator: 4.0 to 10.0 mass% ;

[0117] Includes,

[0118] (A) The content of constituent units derived from benzyl (meth)acrylate in component (A) is 40 mass% or more with respect to the total of component (A), and

[0119] (B) The content of the compound having two molecules with ethylenically unsaturated bonds in the component is 80 mass% or more with respect to the total of the component (B).

[0120] According to the present embodiment, it is possible to form a resist pattern with excellent adhesion and plated copper wiring formation properties.

[0121] In addition, according to one preferred embodiment of the present invention, as described in the example, it is possible to form a resist pattern with excellent adhesion of the resist pattern, formation of plated copper wiring, formation of independent fine lines, and retention of independent fine lines after plating.

[0122] Hereinafter, in this specification, the above (A) to (C) are simply referred to as “Component (A)” to “Component (C)”. The same applies to (D) to (F) described later.

[0123] (A) Component ~ (F) Component, in addition, the raw materials of these components may be used as a single type or two or more types may be used in combination.

[0124] The photosensitive element comprises a support film and a photosensitive resin layer comprising a photosensitive resin composition. In addition to the support film and the photosensitive resin layer, the photosensitive element may have other layers. Examples of other layers include an intermediate layer formed between the support film and the photosensitive resin layer, a protective film formed on the side opposite to the support film in the photosensitive resin layer, and a release layer formed between the protective film and the photosensitive resin layer.

[0125] The photosensitive element is configured, for example, by having a photosensitive resin layer directly laminated onto a support film and also by having an intermediate layer interposed on the support film. The photosensitive resin layer may be one layer or two or more layers.

[0126] The photosensitive element is preferably a dry film resist or a transfer film, and more preferably a dry film resist, from the viewpoint that it facilitates the significant exertion of the effects of the present embodiment.

[0127] <Jiji Film>

[0128] The support film is a layer or film for supporting a photosensitive resin layer, and is preferably a transparent film that transmits active light.

[0129] Examples of materials for transparent films include synthetic resins such as polyethylene, polypropylene, polycarbonate, and polyethylene terephthalate. Among these, polyethylene terephthalate is preferred in terms of having appropriate flexibility and strength.

[0130] From the perspective of ensuring excellent adhesion of the resist pattern, the absorbance of the support film at a wavelength of 365 nm is preferably 0.3 or less, more preferably 0.2 or less, more preferably 0.1 or less, and most preferably 0.08 or less. The absorbance is 0 or greater.

[0131] As a support film, it is desirable to use a film with minimal internal foreign matter, i.e., a high-quality film. Preferably, high-quality films include PET films synthesized using Ti-based catalysts, PET films with a small diameter and low content of the lubricant, PET films containing the lubricant on only one side of the film, thin-film PET films, PET films with smoothing treatment performed on at least one side, and PET films with harmonization treatment such as plasma treatment performed on at least one side. By using a high-quality film, the light to be exposed can be irradiated onto the photosensitive resin layer without being blocked by internal foreign matter, and thus, it becomes easier to realize a resist pattern with excellent resolution.

[0132] The film thickness of the support film is preferably 5 to 25 μm, and more preferably 6 to 20 μm. As the film thickness of the support film decreases, the number of internal foreign substances tends to decrease, and therefore, it is easier to prevent a decrease in the resolution of the resist pattern. On the other hand, if the film thickness is less than 5 μm, elongation deformation in the winding direction due to tension during the coating and winding manufacturing processes is prone to occur, and tearing due to minute scratches is also prone to occur. As a result, the strength of the film is likely to be insufficient, and consequently, wrinkles are likely to form during lamination.

[0133] Smoothing treatment using a calendering device or the like may be performed on at least one side of the support film. By doing so, the surface roughness of one side of the support film, particularly the side in contact with the photosensitive resin layer, can be reduced, and in this case, it becomes easier to exhibit the effects of the present invention.

[0134] The haze of the support film is preferably 0.01 to 1.5%, more preferably 0.01 to 1.2%, and even more preferably 0.01 to 0.95%, from the perspective of improving the parallelism of light rays irradiated onto the photosensitive resin layer and from the perspective of being able to achieve excellent resolution.

[0135] <Photosensitive resin layer>

[0136] The photosensitive resin layer includes a photosensitive resin composition.

[0137] The photosensitive resin composition comprises the following components based on the total solid mass of the photosensitive resin composition:

[0138] (A) Alkali-soluble polymer: 30 to 70 mass% ;

[0139] (B) Compound having ethylenically unsaturated bonds: 20 to 60 mass%; and

[0140] (C) Non-imidazole photopolymerization initiator: 4.0 to 10.0 mass% ;

[0141] Includes

[0142] The photosensitive resin composition may optionally include component (D) (another photopolymerization initiator) and component (E) (a polymerization inhibitor), and may also optionally include component (F) (an antioxidant, a stabilizer, a base dye, and a plasticizer, etc.). Component (F) is an other component other than components (A) to (E).

[0143] Here, regarding the photosensitive resin composition, "solid content" corresponds to the component excluding the solvent among components (A) to (F) included in the photosensitive resin composition.

[0144] ≪(A) Component: Alkali-soluble polymer≫

[0145] (A) The component preferably has a monomer component composed of the first monomer described below, and more preferably has a monomer component composed of at least one type of the first monomer and at least one type of the second monomer described below. The content of the repeating unit of the component (A) is,

[0146] (A) In the case where only one type of alkali-soluble polymer is included as a component, it refers to the copolymerization ratio of repeating units, and

[0147] (A) When two or more alkali-soluble polymers are used as components, the weighted average value of the copolymerization ratio of repeating units is indicated by the ratio of the content of each alkali-soluble polymer.

[0148] The first monomer is a monomer having a carboxyl group in the molecule and also having at least one polymerizable unsaturated group in the molecule. Examples of the first monomer include (meth)acrylic acid, fumaric acid, cinnamic acid, crotonic acid, itaconic acid, 4-vinylbenzoic acid, maleic anhydride, maleic acid semiester, etc. Among these, (meth)acrylic acid is preferred, and methacrylic acid is more preferred, from the perspective that the adhesion and resolution of the resist pattern are easily excellent.

[0149] Additionally, in this specification, “(meth)acrylic acid” means acrylic acid or methacrylic acid, “(meth)acryloyl group” means acryloyl group or methacryloyl group, and “(meth)acrylate” means “acrylate” or “methacrylate”.

[0150] The content of the first monomer is preferably 10 to 50 mass% based on the total mass of the total monomer components. Setting the content to 10 mass% or more is preferable from the viewpoint that the adhesion and resolution of the resist pattern are excellent, 15 mass% or more is more preferable, 18 mass% or more is even more preferable, 21 mass% or more is even more preferable, 23 mass% or more is particularly preferable, and 25 mass% or more is most preferable. Setting the content to 50 mass% or less is preferable from the viewpoint that the adhesion and resolution of the resist pattern are excellent, 35 mass% or less is more preferable, 30 mass% or less is even more preferable, 29 mass% or less is particularly preferable, and 27 mass% or less is most preferable.

[0151] When using two or more types of the first monomer, it is preferable that the sum of the contents of each is within the above range.

[0152] The second monomer is non-acidic and is also a monomer having at least one polymerizable unsaturated group in the molecule.

[0153] As for the second monomer, it is preferable to include a compound having an aromatic structure from the perspective of easily achieving excellent adhesion and resolution of the resist pattern. By including such a compound as the second monomer, it is easy to suppress swelling of the photosensitive resin layer during development, and thus, it is easy to obtain a cured film with excellent adhesion and resolution of the resist pattern. The content of the constituent unit derived from the compound having an aromatic structure is preferably 40 to 90 mass% based on the total mass of the total monomer components. Setting the content to 40 mass% or more is preferable from the perspective of easily achieving excellent adhesion and resolution of the resist pattern, 45 mass% or more is more preferable, 50 mass% or more is even more preferable, 55 mass% or more is even more preferable, and 60 mass% or more is particularly preferable. Setting the content to 90 mass% or less is preferable from the perspective of excellent developability, and 85 mass% or less is more preferable.

[0154] When using two or more compounds having an aromatic structure as the second monomer, it is preferable that the sum of the contents of each is within the above range.

[0155] Examples of compounds having an aromatic structure include benzyl (meth)acrylate, styrene, methylstyrene, vinyltoluene, tert-butoxystyrene, acetoxystyrene, styrene dimer, and styrene trimer, styrene derivatives, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl (meth)acrylate.

[0156] In the present embodiment, the compound having an aromatic structure preferably includes benzyl (meth)acrylate. The content of benzyl (meth)acrylate, based on the total mass of the total monomer components, may be 40 mass% or more, 45 mass% or more, 50 mass% or more, more preferably 55 mass% or more, even more preferably 60 mass% or more, and particularly preferably 70 mass% or more, from the perspective of excellent plating copper wiring formation and independent fine wire retention after plating. Additionally, the content of benzyl (meth)acrylate is preferably 90 mass% or less, and more preferably 85 mass% or less, from the perspective of excellent adhesion of the resist pattern.

[0157] Two or more compounds having an aromatic structure may be used, and in this case, the compounds may be a combination of styrene and benzyl (meth)acrylate. It is preferable that the total content of styrene and benzyl (meth)acrylate be 50 to 90 mass% based on the total mass of the monomer components.

[0158] In alkali-soluble polymers, when the content of a compound having an aromatic structure (e.g., benzyl (meth)acrylate) is high, it is easy to reduce the number of foreign substances in the photosensitive element.

[0159] When comprising a copolymer as an alkali-soluble polymer that substantially contains only (meth)acrylic acid and benzyl (meth)acrylate as monomer components (in other words, the content of monomer components derived from (meth)acrylic acid and monomer components derived from benzyl (meth)acrylate in the copolymer is 95 mass% or more), from the perspective of the balance of developability, adhesion, and resolution, the content of (meth)acrylic acid in the copolymer is preferably 15 mass% or more and 25 mass% or less, based on the total mass of all monomer components, and more preferably 17 mass% or more and 23 mass% or less. Since benzyl (meth)acrylate is relatively hydrophilic compared to alkyl (meth)acrylates and styrene, the above excellent effects are easily obtained.

[0160] Examples of foreign substances in a photosensitive resin composition are shown in FIG. 1. In the drawing, the photosensitive resin layer is indicated by number “101”, and the foreign substance is indicated by number “110”. Examples of foreign substances (110) include, for instance, precipitates of a size of several to several tens of μm (precipitates (111) shown in FIG. 1) or bubbles of a size of several tens of μm (bubbles (112) shown in FIG. 1) formed around precipitates of a size of several μm as nuclei; etc. Foreign substances can be observed with the naked eye or with an optical microscope.

[0161] As a developmental trend, it is possible to consider including a relatively large amount of component (C) in the photosensitive resin composition. On the other hand, when the content of component (C) is high, compatibility with other components in the photosensitive resin composition is likely to deteriorate, and therefore, it is thought that such foreign matter (110) occurs in the photosensitive resin layer (101) during film formation. However, when the content of a compound having an aromatic structure (e.g., benzyl(meth)acrylate) in component (A) is high, compatibility between the (C) nonimidazole photopolymerization initiator and the photosensitive resin composition is likely to improve. Thus, even if the design includes a relatively large amount of component (C) in the photosensitive resin composition, it is easy to prevent the occurrence of component (C) in the photosensitive resin composition, and therefore, it is thought that it is easy to reduce the number of foreign matter.

[0162] It is also preferable that the second monomer includes a compound having a hydroxyl group. By having a constituent unit derived from such a compound, it becomes easier to control the developability of the photosensitive resin layer, and thus, it becomes easier to obtain a cured film with excellent adhesion and resolution of the resist pattern. The second monomer may include both a compound having an aromatic structure and a compound having a hydroxyl group.

[0163] The compound having the above-mentioned hydroxyl group is preferably a hydroxyalkyl (meth)acrylate. As for the hydroxyalkyl (meth)acrylate, it is preferably 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, or 4-hydroxybutyl (meth)acrylate, and more preferably 2-hydroxyethyl methacrylate. These are relatively easy to obtain, easy to control developability, and easy to realize a resist pattern with excellent adhesion and resolution.

[0164] (A) The content of the compound having a hydroxyl group in the component is preferably 1.0 to 20 mass% based on the total mass of the monomer components, more preferably 1 to 10 mass%, and even more preferably 1 to 6 mass%, from the view that the adhesion and developability of the resist pattern are excellent.

[0165] When using two or more compounds having hydroxyl groups, it is preferable that the sum of the contents of each is within the above range.

[0166] The second monomer may further include a polymerizable compound that is different from either a compound having an aromatic structure or a compound having a hydroxyl group.

[0167] Polymerizable compounds distinct from either compounds having an aromatic structure or compounds having a hydroxyl group include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dicyclofentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, ethylcarbitol (meth)acrylate. Examples include (meth)acrylates such as methoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolane-4-yl)methyl (meth)acrylate, cyclic trimethylolpropaneformal (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate; esters of vinyl alcohols such as vinyl acetate; and (meth)acrylonitrile.

[0168] (A) The weight average molecular weight Mw of the component is preferably 10,000 to 60,000. A weight average molecular weight Mw of 60,000 or less is preferred from the viewpoint that it is easy to realize flexibility, resolution, and developability of the resist pattern, and from the same viewpoint, 55,000 or less is more preferred, and less than 50,000 is more preferred. From the same viewpoint, the weight average molecular weight Mw is preferably 10,000 or more, 14,000 or more is more preferred, and 25,000 or more is more preferred.

[0169] (A) The polydispersity of the component (weight average molecular weight Mw / number average molecular weight Mn) is preferably 1.0 to 6.0, more preferably 1.0 to 5.0, even more preferably 1.0 to 4.0, and particularly preferably 1.0 to 3.0.

[0170] (A) As described above, the component may be used as a single type or in combination of two or more types. When two or more types are used in combination, it is preferable that the molecular weight and polydispersity of the monomers in the plurality of (A) components be selected such that the weighted average value when the content ratio is treated as weight falls within the above range.

[0171] (A) Component may be synthesized by mixing a single or multiple monomers and a radical polymerization initiator in a solution diluted with a solvent, and then heating and stirring. The solvent mentioned herein is, for example, acetone, methyl ethyl ketone, isopropanol, etc., and the radical polymerization initiator mentioned herein is, for example, benzoyl peroxide, azoisobutyronitrile, etc. In some cases, Component (A) may be synthesized by adding a portion of the mixture dropwise to the reaction solution. In some cases, after synthesizing Component (A), additional solvent may be added to adjust the concentration to a desired level. As a method for synthesizing Component (A), bulk polymerization, suspension polymerization, or emulsion polymerization may be used in addition to solution polymerization. Furthermore, Component (A) may be synthesized by living radical polymerization.

[0172] (A) The ratio of the content of component to the total solid mass of the photosensitive resin composition may be 30 mass% or more, 35 mass% or more, 40 mass% or more, 45 mass% or more, or 50 mass% or more. In addition, the above content may be 70 mass% or less, 65 mass% or less, or 60 mass% or less.

[0173] Setting the ratio of the content of component (A) to the total solid mass of the photosensitive resin composition to 70 mass% or less is desirable from the perspective of controlling the development time in a desirable way, and setting it to 30 mass% or more is desirable from the perspective of suppressing the seepage of the photosensitive resin layer from the cross-section of the film.

[0174] ≪(B) Component: Compound having ethylenically unsaturated bonds≫

[0175] (B) The component is a compound having at least one ethylenically unsaturated bond among the molecules.

[0176] (B) The component preferably comprises a compound having two or more molecules having ethylenically unsaturated bonds. For example, the component (B) comprises a compound having two molecules having ethylenically unsaturated bonds.

[0177] However, component (B) may include a compound having three ethylenically unsaturated bonds in the molecule, and may also include a compound having four, five, or six ethylenically unsaturated bonds in the molecule.

[0178] (B) The content of a compound having two molecules having ethylenically unsaturated bonds in the component (B) may be 80 mass% or more with respect to the total component (B) from the viewpoint of excellent independent line forming ability, preferably 85 mass% or more, and more preferably 90 mass% or more. In addition, the above content may be 100 mass% or less than 100 mass% with respect to the total component (B).

[0179] (B) Among the components, compounds having two ethylenically unsaturated bonds in a molecule may be, for example, compounds having a bisphenol backbone. The “compounds having a bisphenol backbone” mentioned here also include compounds having a hydrogenated bisphenol backbone.

[0180] (B) The component preferably comprises a compound containing a (meth)acryloyl group (also referred to as a “(meth)acrylate compound” in this specification), and more preferably comprises a (meth)acrylate compound having two or more functional groups (a compound having two or more (meth)acryloyl groups in one molecule).

[0181] (B) When a component contains a (meth)acrylate compound, it may contain only a difunctional (meth)acrylate compound, or it may contain a difunctional (meth)acrylate compound and a (meth)acrylate compound with three or more functions. The (meth)acrylate compound may include, for example, tetrafunctional, pentafunctional, or hexafunctional (meth)acrylate compounds.

[0182] (B) When component (B) includes a (meth)acrylate compound, the content of the difunctional (meth)acrylate compound may be 80 mass% or more with respect to the total of component (B) for excellent independent wire formation ability, preferably 85 mass% or more, and more preferably 90 mass% or more. In addition, the content may be 100 mass% or less than 100 mass% with respect to the total of component (B).

[0183] (B) When the component includes a compound having three or more molecules having ethylenically unsaturated bonds, the content of the compound may be 20 mass% or less, 15 mass% or less, or 10 mass% or less with respect to the total of the component (B). In addition, the content may be 1 mass% or more, or 5 mass% or more with respect to the total of the component (B).

[0184] (B) When component (B) contains a (meth)acrylate compound with three or more functional groups, the content of the compound may be 20 mass% or less, 15 mass% or less, or 10 mass% or less with respect to the total of component (B) in order to ensure excellent adhesion and developability of the resist pattern.

[0185] As for difunctional (meth)acrylate compounds, for example,

[0186] Alkyl di(meth)acrylate,

[0187] 1,3-Bis(meth)acryloyloxy-2-propanol,

[0188] The following general formula (I):

[0189] [Chemical Formula 2]

[0190]

[0191] {In the food, R 1 Each is independently a hydrogen atom or a methyl group, and X 1 O and Y 1 O is, each independently, an oxyalkylene group having 2 to 4 carbon atoms; m1, m2, and n1 are, each independently, integers from 0 to 40; m1 + m2 is 1 to 40; and n1 is 0 to 20.

[0192] Polyalkylene glycol di(meth)acrylate represented by,

[0193] Tricyclodecanol di(meth)acrylate,

[0194] The following general formula (II):

[0195] [Chemical Formula 3]

[0196]

[0197] {In the food, R 2 are, each independently, a hydrogen atom or a methyl group, and X 2 O and Y 2 O is, each independently, an oxyethylene group or an oxypropylene group, m3, m4, n2, and n3 are, each independently, integers from 0 to 40, m3 + m4 is from 1 to 40, and n2 + n3 is from 0 to 20.

[0198] Examples include bisphenol A type di(meth)acrylates represented by.

[0199] As for the polyalkylene glycol di(meth)acrylate represented by the above formula (I), R 1 = methyl group, m1 + m2 = 6 (average value), n1 = 12 (average value), X 1O is an oxyethylene group, Y 1 Examples include vinyl compounds in which O is an oxypropylene group (manufactured by Resonac, product name "FA-024M").

[0200] Bisphenol A type di(meth)acrylate compounds represented by the above general formula (II) include BPE-200 (R 2 = Methyl group, X 2 O = oxyethylene group, m3+m4 = 4, n2 = n3 = 0), BPE-500 (R 2 = methyl group, X 2 O = oxyethylene group, m3+m4 = 10, n2 = n3 = 0), BPE-900 (R 2 = methyl group, X 2 O = oxyethylene group, m3 + m4 = 17, n2 = n3 = 0) (The above, manufactured by Shinnakamura Chemical Industry Co., Ltd., product name), FA-321M (R 2 = methyl group, X 2 O = oxyethylene group, m3+m4 = 10, n2 = n3 = 0), FA-P321M (R 2 = Methyl group, X 2 O = oxypropylene group, m3 + m4 = 10, n2 = n3 = 0) (Above, manufactured by Resonac, product name), FA-P323M (R 2 = Methyl group, X 2 O = oxypropylene group, Y 2 Examples include O = oxyethylene group, m3 + m4 = 4, n2 + n3 = 30) (The above, manufactured by Resonac, product name).

[0201] (B) The component preferably comprises a bisphenol A type di(meth)acrylate compound represented by the general formula (II) above, in order to easily improve the adhesion, resolution, plating copper wiring formation, and independent fine line formation of the resist pattern. The content of the compound is preferably 1 mass% or more with respect to the total component (B), more preferably 20 mass% or more, even more preferably 50% or more, particularly preferably 80% or more, and most preferably 90% or more. Since the compound has a high aromatic ring ratio, using such a compound ensures good compatibility with benzyl(meth)acrylate, and thus, the plating copper wiring formation and independent fine line formation are easily improved.

[0202] In the compound represented by the above general formula (II), from the perspective that the adhesion and resolution of the resist pattern are likely to be excellent, it is preferable that the average value of n2 + n3 + m3 + m4 of the compound included in the photosensitive resin composition is 20 or less, and more preferable that it is 15 or less. In addition, the average value of n2 + n3 + m3 + m4 of the compound included in the photosensitive resin composition may be 2 or more, it is preferable that it exceeds 4, and more preferable that it exceeds 10.

[0203] Bisphenol A type di(meth)acrylate compounds are more preferably included in the bisphenol A type di(meth)acrylate having an average value of n2+n3+m3+m4 of 10 or less, and in the bisphenol A type di(meth)acrylate having an average value of n2+n3+m3+m4 of 15 or more, from the viewpoint that independent wire formation is easily achieved.

[0204] In addition, the number of structural units of oxyethylene or oxypropylene groups represents an integer value in a single molecule and a rational number, which is an average value, in an aggregate of multiple molecules.

[0205] Commercially available difunctional (meth)acrylate compounds include, for example, NK ester (registered trademark) A-HD-N, A-NOD-N, A-DOD-N, A-NPG, 701A, A-200, A-400, A-600, A-1000, APG-200, APG-400, APG-700, A-PTMG65, A-DCP, ABE-300, A-BPE-4, A-BPE-10, A-BPE-20, HD-N, NOD-N, DOD-N, NPG, 701, 2G, 3G, 4G, 9G, 14G, 23G, 9PG, DCP, BPE-80N, BPE-100, BPE-200, BPE-500, BPE-900, BPE-1300N, NK Oligo (Registered Trademark) UA-4200, UA-160TM, UA-290TM, UA-W2A, UA-4400, UA-122P, U-200PA (all manufactured by Shinnakamura Chemical Industry Co., Ltd.), Light Acrylate (Registered Trademark) 3EG-A, 4EG-A, 9EG-A, 14EG-A, PTMGA-250, NP-A, MPD-A, 1.6HX-A, 1.9ND-A, DCP-A, BP-4 EAL, BP-4PA, HPP-A, Light Ester G-201P (all manufactured by Kyoei Chemical Co., Ltd.), Pancreel (registered trademark) FA-124AS, FA-023M, FA-121M, FA-124M, FA-125M, FA-129AS, FA-137M, FA-220M, FA-222A, FA-240A, FA-240M, FA-320M, FA-3218M, FA-321A, FA-321M, FA-324A, FA-731A, FA-P240A, FA-P270A, FA-PTG9A, FA-PTG9M, FA-PTG28A, etc. FA-PTG49A (Manufactured by Resonac), DPGDA, HDDA, TPGDA, EBECRYL 145, EBECRYL 150, PEG400DA, EBECRYL 11, IRR 214-K, EBECRYL 130, EBECRYL PEG200DMA (Manufactured by Daicel AllNex), SR212, SR213, SR230, SR238F, SR259, SR268, SR272, SR306H, SR344, SR349, SR508, CD560, CD561, CD564, SR601, SR602, SR610, SR833S, SR9003, SR9045, SR9209, SR205, SR206, Examples include SR209, SR210, SR214, SR231, SR239, SR248, SR252, SR297, SR348, SR480, CD540, CD541, CD542, SR603, SR644, SR9036 (all manufactured by Arkema), KAYARAD (registered trademark) NPGDA, PEG400DA, FM-400, R-167, HX-220, HX-620, R-551, R-712, R-604, R-684 (all manufactured by Japan Explosives Co., Ltd.).

[0206] Examples of (meth)acrylate compounds with three or more functions include trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, isocyanuric acid tri(meth)acrylate, pentaerythritol (tri / tetra)(meth)acrylate, ditrimethylolpropane (tetra / penta / hexa)(meth)acrylate, dipentaerythritol (tetra / penta / hexa)(meth)acrylate, etc.

[0207] (Meth)acrylate compounds with three or more functions,

[0208] An alcohol having three or more groups capable of adding alkylene oxide groups within the molecule as a central backbone, to which alkylene oxide groups such as ethylene oxide, propylene oxide, or butylene oxide are added, and

[0209] (Met)acrylic acid

[0210] It may also be a compound obtained by forming (meth)acrylate from.

[0211] Examples of such compounds include, for instance, trimethylolpropane alkylene oxide modified tri(meth)acrylate, glycerin alkylene oxide modified tri(meth)acrylate, alkylene oxide modified pentaerythritol (tri / tetra)(meth)acrylate, alkylene oxide modified ditrimethylolpropane (tetra / penta / hexa)(meth)acrylate, alkylene oxide modified dipentaerythritol (tetra / penta / hexa)(meth)acrylate, alkylene oxide modified isocyanuric acid tri(meth)acrylate, etc.

[0212] As for (meth)acrylate compounds with three or more functionalities, alkylene oxide-modified pentaerythritol (tri / tetra)(meth)acrylate may be included in view of excellent developability.

[0213] Commercially available (meth)acrylate compounds with three or more functions include, for example, NK esters (registered trademarks) A-TMPT, A-TMPT-9EO, AT-20E, A-GLY-3E, A-GLY-9E, A-GLY-20E, A-9300, A-9200YN, A-TMM-3, A-TMM-3L, A-TMM-3LM-N, A-TMMT, ATM-35E, AD-TMP, A-DPH, A-9550, A-DPH-12E, TPOA-50, NK oligos (registered trademarks) UA-7100, UA-1100H, U-6LPA, UA-33H, U-10HA, U-10PA, U-15HA (the above, Shin-Nakamura Chemical) Manufactured by Industrial Co.), Light Acrylate (Registered Trademark) TMP-A, cPE-3A, PE-4A, DPE-6A (all, manufactured by Kyoei Chemical Co.), FA-731A (manufactured by Resonac), TMPTA, EBECRYL 160S, OTA 480, PETIA, PETRA, EBECRYL 40, PETA, EBECRYL 140, EBECRYL 1140, EBECRYL 1142, DPHA, EBECRYL 895, EBECRYL 896, EBECRYL TMPTMA (all, manufactured by Daicel AllNex), SR351S, SR368, SR415, SR444, SR454, SR492, SR499, CD501, SR502, SR9020, D9021, Examples include SR9035, SR295, SR355, SR399, SR494, SR9041 (all manufactured by Arkema), KAYARAD (registered trademark) GPO-303, TMPTA, THE-330, TPA-330, PET-30, T-1420(T), RP-1040, DPHA, DPEA-12, D-310, DPCA-20 (all manufactured by Japan Explosives Co., Ltd.).

[0214] Based on the above, an example of component (B) usable in the present embodiment is as follows. However, component (B) used in the present embodiment is not limited to the following compounds.

[0215] Dimethacrylate of polyethylene glycol obtained by adding an average of 2 moles of ethylene oxide to each end of bisphenol A (manufactured by Shinnakamura Chemical Industry, product name BPE-200);

[0216] Dimethacrylate of polyethylene glycol obtained by adding an average of 5 moles of ethylene oxide to each end of bisphenol A (manufactured by Shinnakamura Chemical Industry, product name BPE-500);

[0217] Dimethacrylate of polyethylene glycol, to which an average of 2 moles of propylene oxide and an average of 15 moles of ethylene oxide are added to each end of bisphenol A, respectively;

[0218] Tetramethacrylate, in which an average of 1 mole of ethylene oxide is added to each of the four ends of pentaerythritol;

[0219] Hexamethacrylates obtained by adding an average of 2 moles of ethylene oxide to each of the six ends of dipentaerythritol; and

[0220] Dimethacrylate of polyethylene glycol, in which an average of 5 moles of ethylene oxide are added to each end of hydrogenated bisphenol A.

[0221] With respect to the total solid mass in the photosensitive resin composition, the content of component (B) is 20 mass% or more, preferably 25 mass% or more, more preferably 30 mass% or more, and even more preferably 35 mass% or more, from the perspective of excellent sensitivity, tackiness, and tracking ability. In addition, from the perspective of excellent edge fusion ability, tackiness, and resolution, it is 60 mass% or less, preferably 50 mass% or less, more preferably 45 mass% or less, and even more preferably 42 mass% or less.

[0222] The term "internal edge fusion" as used herein refers to a characteristic that suppresses the overflow of the resist during storage of the photosensitive element roll, and in this case, the smaller the amount of overflow, the more desirable it is. Additionally, the term "tackiness" as used herein refers to the adhesiveness of the photosensitive resin composition.

[0223] From the perspective of excellent edge fusion properties, tackiness, and resolution, the value of the content of component (A) relative to the content of component (B) (i.e., content of component (A) / value of the content of component (B)) is preferably 1.6 or less, more preferably 1.5 or less, and even more preferably 1.4 or less. This value is preferably 0.7 or more, more preferably 0.8 or more, even more preferably 0.9 or more, and particularly preferably 1.0 or more.

[0224] It is preferable that the number of ethylenically unsaturated bonds per 100 g of solid content of the photosensitive resin composition be 0.1 to 0.3 moles. By having 0.1 moles or more, it is easy to prevent the photosensitive resin component from leaching out from the cured resist pattern during the rinsing process after development, and furthermore, to prevent contamination of the rinsing process. By having 0.3 moles or less, it becomes difficult for defects or further detachment of the cured resist pattern to occur during the rinsing process after development, and thus, it is easy to prevent contamination of the rinsing process.

[0225] The number of ethylenically unsaturated bonds per 100 g of solid content of the photosensitive resin composition is preferably 0.1 mole or more, more preferably 0.11 mole or more, even more preferably 0.12 mole or more, and particularly preferably 0.13 mole or more. In addition, the number of such ethylenically unsaturated bonds is preferably 0.3 mole or less, more preferably 0.28 mole or less, even more preferably 0.25 mole or less, particularly preferably 0.22 mole or less, 0.20 mole or less, or 0.18 mole or less, and most preferably 0.15 mole or less.

[0226] The number of ethylenically unsaturated bonds per 100 g of solid content of the photosensitive resin composition is preferably 0.1 to 0.25 mol, more preferably 0.1 to 0.2 mol, even more preferably 0.11 to 0.2 mol, and particularly preferably 0.11 to 0.15 mol.

[0227] ≪(C) Ingredient: Non-imidazole photopolymerization initiator≫

[0228] (C) Component is a photopolymerization initiator having a non-imidazole structure.

[0229] (C) The content of component is 4.00 mass% or more with respect to the total solid mass of the photosensitive resin composition. From the perspective of facilitating excellent adhesion of the resist pattern, it is preferable to have 4.25 mass% or more or 4.50 mass% or more, more preferably 4.75 mass% or more, even more preferably 5.00 mass% or more, even more preferably 5.25 mass% or more, particularly preferably 5.75 mass% or more, and most preferably 6.00 mass% or more. Additionally, from the perspective of facilitating the reduction of the number of foreign substances, the above content is preferably 10.0 mass% or less, more preferably 9.00 mass% or less, and even more preferably 8.00 mass% or less.

[0230] (C) As for the component, for example, a lofin dimer, that is, a dimer of a compound having a lofin structure (a compound having a 2,4,5-triarylimidazole backbone).

[0231] Lopine dimers, that is, dimers of 2,4,5-triarylimidazole, include 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer {alias: 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole}, 2,2',5-tris-(o-chlorophenyl)-4-(3,4-dimethoxyphenyl)-4',5'-diphenylbiimidazole, 2,4-bis-(o-chlorophenyl)-5-(3,4-dimethoxyphenyl)-diphenylbiimidazole, 2,4,5-tris-(o-chlorophenyl)-diphenylbiimidazole, 2-(o-chlorophenyl)-bis-4,5-(3,4-dimethoxyphenyl)-biimidazole, 2,2'-Bis-(2-fluorophenyl)-4,4',5,5'-Tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,3-difluoromethylphenyl)-4,4',5,5'-Tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,4-difluorophenyl)-4,4',5,5'-Tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,5-difluorophenyl)-4,4',5,5'-Tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,6-difluorophenyl)-4,4',5,5'-Tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,3,4-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,3,5-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,3,6-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,4,5-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-Bis-(2,4,6-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,3,4,5-tetrafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,3,4,6-tetrafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, and 2,2'-bis-(2,3,4,5,6-pentafluorophenyl)-4,4',5,Examples include 5'-tetrakis-(3-methoxyphenyl)-biimidazole, etc.

[0232] From the perspective of ensuring excellent adhesion and resolution of the resist pattern, component (C) is preferably composed of a lopin dimer, and among them, it is more preferable to include a 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer.

[0233] ≪(D) ​​Component: Other photopolymerization initiators≫

[0234] (D) Components may include, for example, N-aryl-α-amino acid compounds, quinone compounds, aromatic ketone compounds, anthracene derivatives, acetophenone compounds, acylphosphine oxide compounds, benzoin compounds, benzoin ether compounds, dialkyl ketal compounds, thioxantone compounds, dialkylaminobenzoic acid ester compounds, oxime ester compounds, acridin compounds, pyrazolin derivatives, N-aryl amino acid ester compounds, coumarin derivatives, and halogen compounds.

[0235] Examples of aromatic ketone compounds include benzophenone compounds. Examples of benzophenone compounds include benzophenone, mihler ketone [4,4'-bis(dimethylamino)benzophenone], 4-methoxy-4'-dimethylaminobenzophenone, etc. Among aromatic ketone compounds, 4,4'-bis(diethylamino)benzophenone is preferred in terms of excellent sensitizing effect and adhesion.

[0236] That is, the photosensitive resin composition preferably comprises (D) at least one selected from the group consisting of benzophenone compounds, pyrazolin compounds, anthracene compounds, and coumarin compounds.

[0237] In this specification, "anthracene derivative" refers to both anthracene and compounds derived therefrom. Examples of anthracene derivatives include anthracene, 9,10-dialcocyanthracene, 9,10-dimethoxycyanthracene, 9,10-diethoxycyanthracene, 9,10-dibutoxycyanthracene, 9,10-diphenylanthracene, 2-ethylanthraquinone, octaethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 10-phenyl-9-anthraceboronic acid, etc. In terms of excellent saturation effect and adhesion, 9,10-dibutoxycyanthracene, 9,10-diphenylanthracene, and 10-phenyl-9-anthraceneboronic acid are preferred, and in particular, 9,10-diphenylanthracene and 10-phenyl-9-anthraceneboronic acid are preferred.

[0238] As for pyrazolin derivatives, 1-phenyl-3-(4-tert-butyl-styryl)-5-(4-tert-butyl-phenyl)-pyrazolin, 1-phenyl-3-(4-biphenyl)-5-(4-tert-butyl-phenyl)-pyrazolin, 1-phenyl-3-(4-biphenyl)-5-(4-tert-octyl-phenyl)-pyrazolin, and 1-phenyl-3-(4-methoxystyryl)-5-(4-methoxyphenyl)-pyrazolin are preferred in terms of excellent adhesion and rectangularity of the resist pattern.

[0239] When the photosensitive resin composition includes component (D), it is preferable to include any one of a benzophenone compound, a pyrazolin compound, anthracene compound, and a coumarin compound for excellent storage stability, and it is more preferable to include any one of a benzophenone compound and a pyrazolin compound.

[0240] (D) The content of component (D) is preferably 0 to 0.5 mass% with respect to the total solid mass of the photosensitive resin composition, more preferably 0 to 0.1 mass%, even more preferably 0 to 0.05 mass%, and particularly preferably 0 to 0.025 mass%. By adjusting the content of component (D) to within the above range, it is easy to reduce the absorbance in the region other than the exposure wavelength, thereby making it easy to improve storage stability.

[0241] ≪(E) Ingredient: Polymerization Inhibitor≫

[0242] (E) Examples of components include phenothiazine, p-methoxyphenol, hydroquinone, pyrogallol, naphthylamine, tert-butylcatechol, cuprous chloride, 2,6-di-tert-butyl-p-cresol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), triethyleneglycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], aluminum nitrosophenylhydroxyamine salt (e.g., aluminum salt to which 3 moles of nitrosophenylhydroxyamine are added), diphenylnitrosamine, etc. Among these, an aluminum salt to which 3 moles of triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate] or nitrosophenylhydroxylamine are added is preferred.

[0243] (E) In terms of excellent adhesion of the resist pattern and storage stability, the component preferably comprises any one of phenothiazine, p-methoxyphenol, tert-butylcatechol, and 2,6-di-tert-butyl-p-cresol, and more preferably comprises phenothiazine and / or tert-butylcatechol.

[0244] (E) The content of the component is preferably 10 to 5000 ppm with respect to the total solid mass of the photosensitive resin composition, with respect to excellent resolution of the resist pattern and plating copper wiring formation ability, more preferably 10 to 1000 ppm, even more preferably 50 to 1000 ppm, and particularly preferably 50 to 500 ppm.

[0245] ≪(F) Other Components≫

[0246] The photosensitive resin composition may include component (F) as desired. Examples of component (F) include base dyes, antioxidants, stabilizers, colorimetric dyes, and plasticizers. Additionally, the photosensitive resin composition may include various solvents as component (F).

[0247] base dye

[0248] Examples of base dyes include, for instance, Diamond Green [CAS number (hereinafter the same): 633-03-4] (e.g., Aizen Diamond Green GH, trade name, manufactured by Hodogaya Chemical Industry Co., Ltd.), Fuchsin [632-99-5], Methyl Violet [603-47-4], Methyl Green [82-94-0], Victoria Blue B [2580-56-5], Basic Blue 7 [2390-60-5] (e.g., Aizen Victoria Pure Blue BOH, trade name, manufactured by Hodogaya Chemical Industry Co., Ltd.), Rhodamine B [81-88-9], Rhodamine 6G [989-38-8], Basic Yellow 2 [2465-27-2], etc. Among these, Diamond Green is preferred from the perspective of improving tintability, color stability, and exposure contrast.

[0249] The content of the base dye is preferably 0.001 to 3 mass%, more preferably 0.01 to 2 mass%, and even more preferably 0.04 to 1 mass% with respect to the total solid mass of the photosensitive resin composition. The content of the base dye is preferably greater than or equal to the lower limit value above from the viewpoint of obtaining good colorability, while on the other hand, it is preferably less than or equal to the upper limit value above from the viewpoint of maintaining the sensitivity of the photosensitive resin layer.

[0250] antioxidants

[0251] Examples of antioxidants include triphenylphosphite (e.g., manufactured by ADEKA, trade name: TPP), tris(2,4-di-tert-butylphenyl)phosphite (e.g., manufactured by ADEKA, trade name: 2112), tris(monononylphenyl)phosphite (e.g., manufactured by ADEKA, trade name: 1178), bis(monononylphenyl)-dinonylphenylphosphite (e.g., manufactured by ADEKA, trade name: 329K), etc.

[0252] The content of the antioxidant is preferably 0.01 to 0.8 mass% with respect to the total solid mass of the photosensitive resin composition, and more preferably 0.01 to 0.3 mass%. The content of the antioxidant is preferably greater than or equal to the lower limit value above from the perspective of expressing good color stability of the resist pattern and also improving the sensitivity of the photosensitive resin layer. On the other hand, it is preferably less than or equal to the upper limit value above from the perspective of expressing good color stability while suppressing the color development of the resist pattern.

[0253] stabilizer

[0254] A stabilizer can be used to improve the thermal stability of the photosensitive resin composition. Examples of stabilizers include at least one of an alkylene oxide compound having a glycidyl group and a benzotriazole compound.

[0255] Examples of alkylene oxide compounds having a glycidyl group include, for example, neopentyl glycol diglycidyl ether (e.g., Epollite 1500NP manufactured by Kyoei Chemical Co.), nonaethylene glycol diglycidyl ether (e.g., Epollite 400E manufactured by Kyoei Chemical Co.), bisphenol A-propylene oxide 2 molar adduct diglycidyl ether (e.g., Epollite 3002 manufactured by Kyoei Chemical Co.), 1,6-hexanediol diglycidyl ether (e.g., Epollite 1600 manufactured by Kyoei Chemical Co.).

[0256] Examples of benzotriazole compounds include carboxybenzotriazole, 1,2,3-benzotriazole, 1-chloro-1,2,3-benzotriazole, 1-(N,N-bis(2-ethylhexyl)aminomethyl)-1,2,3-benzotriazole, 1-(N,N-bis(2-ethylhexyl)aminomethyl)-1,2,3-tolyltriazole, 1-(N,N-bis-2-hydroxyethyl)aminomethyl)-1,2,3-benzotriazole, 1-(N,N-bis(2-ethylhexyl)aminomethyl)-5-carboxy-1,2,3-benzotriazole, etc.

[0257] The total content of the antioxidant, the alkylene oxide compound having a glycidyl group, and the benzotriazole compound in the photosensitive resin composition is preferably 0.001 to 3 mass% and more preferably 0.05 to 1 mass% with respect to the total solid mass of the photosensitive resin composition.

[0258] Colorimetric dyes

[0259] The photosensitive resin composition may include a colorimetric dye that develops color upon light irradiation. As for colorimetric dyes, for example, a combination of a leuco dye and a halogen compound is known. Examples of leuco dyes include tris(4-dimethylamino-2-methylphenyl)methane [leucocrystalline violet], tris(4-dimethylamino-2-methylphenyl)methane [leucomalachite green], etc. Examples of halogen compounds include amyl bromide, isoamyl bromide, isobutylene bromide, ethylene bromide, diphenylmethyl bromide, benzal bromide, methylene bromide, tribromomethylphenylsulfone, carbon tetrabromide, tris(2,3-dibromopropyl)phosphate, trichloroacetamide, amyl iodide, isobutyl iodide, 1,1,1-trichloro-2,2-bis(p-chlorophenyl)ethane, hexachloroethane, etc.

[0260] plasticizer

[0261] The photosensitive resin composition may include additives such as plasticizers in the photosensitive resin layer. Examples of this type of additive include phthalate esters such as diethyl phthalate, o-toluenesulfonamide, p-toluenesulfonamide, tributyl citrate, triethyl citrate, triethyl acetyl citrate, tri-n-propyl acetyl citrate, tri-n-butyl acetyl citrate, polypropylene glycol, polyethylene glycol, polyethylene glycol alkyl ether, polypropylene glycol alkyl ether, etc.

[0262] <Composition of Photosensitive Resin Layer>

[0263] The film thickness of the photosensitive resin layer is preferably 3 to 100 μm, and specifically, preferred upper limits of the film thickness include 7 μm, 15 μm, 25 μm, 40 μm, 60 μm, etc. In one embodiment, the preferred upper limit of the film thickness is 50 μm. As the film thickness approaches 3 μm, resolution is more likely to improve, and as it approaches 100 μm, film strength is more likely to improve. Accordingly, the film thickness of the photosensitive resin layer can be appropriately selected according to the application of the photosensitive element, as well as the application of the resist pattern or final product obtained using the photosensitive element. When the formed resist pattern is used in a plating formation process, the film thickness is preferably 10 to 30 μm, and more preferably 15 to 27 μm.

[0264] In this embodiment, the absorbance (Y) at a wavelength of 365 nm at a film thickness of 25 μm of the photosensitive resin layer is 0.35 or less. Accordingly, storage stability and the rectangularity of the resist pattern are likely to be excellent, and the adhesion of the resist pattern is also likely to be excellent. From the same perspective, such absorbance is preferably 0.3 or less, more preferably 0.2 or less, more preferably 0.18 or less, and particularly preferably 0.16 or less. Such absorbance may be 0 or greater, and from the perspective of obtaining a photosensitive resin layer composition with good photoreactivity and excellent sensitivity, it is preferably 0.11 or greater.

[0265] Generally, the absorbance of a photosensitive resin layer can be measured using a spectrophotometer by placing a substrate on which the photosensitive resin layer is formed as a reference. Additionally, the absorbance can generally be measured by referring to JIS K 0115 (2004). When using a spectrophotometer, the absorbance of the photosensitive resin layer can be calculated by converting the result measured using only the substrate into a reference. In the case of the photosensitive element described below, a support film may be used as the substrate. The absorbance measured by the above method is a value derived by including the amount of light scattered by the photosensitive resin layer and the substrate. The "absorbance" referred to in this embodiment is a value derived using the method described in the <Absorbance> item of the example.

[0266] In one mode,

[0267] With respect to the total solid mass of the photosensitive resin composition, it contains 5.0 mass% or more of component (C), and

[0268] The absorbance (Y) at a wavelength of 365 nm at a film thickness of 25 μm of the photosensitive resin layer is 0.35 or less, and

[0269] It is desirable that the contribution (X) of the absorbance of component (C) to the absorbance (Y) is 40% or more.

[0270] In this embodiment, the contribution (X) is the following formula (1):

[0271] X (%) = 100×εc / absorbance (Y) of photosensitive resin layer ··· (1)

[0272] ε : Change in absorbance per 1 mass% of component (C)

[0273] c: Content of component (C) in the total solid components of the photosensitive resin composition (mass%)

[0274] It is produced by.

[0275] ε can be obtained by the following method.

[0276] A photosensitive resin composition is prepared by adding component (C) in different amounts to 100 parts by mass of the total of component (A) and component (B), and each is coated onto a substrate to a film thickness of 25 μm, and the absorbance of the resulting photosensitive resin layer is measured. The results obtained are plotted with the content of component (C) (mass%) based on the total solid mass of the photosensitive resin composition as the X-axis and the absorbance of the photosensitive resin layer (Y) as the Y-axis. The data obtained by this is linearly approximated to obtain a straight line with a predetermined slope. The slope of this straight line corresponds to the change in absorbance value ε per 1 mass% of component (C) at that content.

[0277] The component (A) used at this time preferably contains methacrylic acid, styrene, benzyl methacrylate, 2-hydroxyl methacrylate, and methyl methacrylate in any proportion. The component (B) preferably contains bisphenol A type di(meth)acrylate such as FA-321M. Since these components have low absorbance at 365 nm, they are suitable for accurately measuring the change in absorbance value ε per 1 mass% of component (C).

[0278] The contribution (X) is preferably 45% or more, more preferably 55% or more, more preferably 65% ​​or more, and particularly preferably 85% or more from the perspective of excellent storage stability. It is thought that as the value (X) increases, the increase / decrease effect by additives other than component (C) is easily suppressed, and thus the reactivity to long-wavelength light such as yellow light is easily reduced, thereby improving storage stability.

[0279] Means of increasing the contribution (X) include, for example, increasing the content of component (C), decreasing the content of component (D), or decreasing the content of other components that have absorption at 365 nm.

[0280] When the photosensitive resin composition includes a plurality of (C) components, the contribution (X) is obtained as follows.

[0281] That is, as component (C), when components (C-1) to (Cn) are included (n is an integer greater than or equal to 2), the change in absorbance values ​​ε1 to ε per 1 mass% for each n , furthermore, derive contributions (X-1) ~ (Xn).

[0282] And, the sum of the obtained contributions (X-1) to (Xn) is treated as the contribution (X) in this embodiment.

[0283] <Protective Film>

[0284] The photosensitive element may be provided with a protective film. The support film, the photosensitive resin layer, and the protective film may be laminated in this order.

[0285] The protective film can be laminated on the photosensitive resin layer side of the laminate of the support film and the photosensitive resin layer, and functions as a cover.

[0286] When the adhesion between the photosensitive resin layer and the protective film is sufficiently smaller than the adhesion between the photosensitive resin layer and the support film, the protective film can be easily peeled off from the photosensitive resin layer. For example, polyethylene film, polypropylene film, stretched polypropylene film, polyester film, etc., can be preferably used as the protective film. A release layer may be formed on the surface of the protective film.

[0287] The film thickness of the protective film is preferably 10 to 100 μm, and more preferably 10 to 50 μm. Examples of protective films include Alphen (registered trademark) EM-501, E-200, E-201F, FG-201, MA-411 (all manufactured by Oji F-Tex Co.), Torepan (registered trademark) KW37, 2578, 2548, 2500, YM17S, Serafil (registered trademark) PJ271, PJ111, HP2, PJ101, WZ, MDA, MFA, TK07, BKE, BX8A, SY (all manufactured by Toray Co.), GF-18, GF-818, GF-858 (all manufactured by Tamapoly Co.), etc.

[0288] [Photosensitive Element Roll]

[0289] An additional aspect of the present embodiment is a photosensitive element roll formed by winding the photosensitive element.

[0290] The photosensitive element roll may be equipped with a core for winding a long photosensitive element, or it may not have a core.

[0291] [Method for manufacturing a photosensitive element]

[0292] The photosensitive element related to the present embodiment as described above can be manufactured by a method as shown below. That is, an additional aspect of the present embodiment is a method for manufacturing a photosensitive element.

[0293] This manufacturing method is,

[0294] A method for manufacturing a photosensitive element comprising a support film and a photosensitive resin layer, comprising the following process:

[0295] A process for preparing a combination solution of a photosensitive resin composition by mixing (A) an alkali-soluble polymer, (B) a compound having ethylenically unsaturated bonds, and (C) a nonimidazole photopolymerization initiator and a solvent (combination process);

[0296] A process of applying the above combination solution onto a support film (application process); and

[0297] A process of obtaining a photosensitive resin layer by heating a coated support film (process of forming a photosensitive resin layer);

[0298] Includes

[0299] <Assembly Process>

[0300] In this process, the above-described components (A), (B), and (C) are mixed with a solvent to prepare a combination solution of a photosensitive resin composition.

[0301] Suitable solvents include ketones, such as methyl ethyl ketone (MEK), and alcohols, such as methanol, ethanol, and isopropyl alcohol. A single solvent may be used, or a mixture of two or more solvents may be used.

[0302] The solvent content is preferably in the range of 30 to 60 mass%, more preferably 33 to 55 mass%, and even more preferably 35 to 57 mass% with respect to the total amount of the photosensitive resin composition.

[0303] It is preferable to mix a solvent into the photosensitive resin composition so that the viscosity of the combination solution of the photosensitive resin composition is 500 to 4000 mPa·sec at 25°C. The viscosity can be measured at 25°C using a Brookfield viscometer (manufactured by ECO, model number DVNext).

[0304] <Coating Process>

[0305] In this process, the above-mentioned combination solution is applied onto a support film.

[0306] For the application of the combination solution to the support film, conventional methods such as applying with a roll coater, spin coater, bar coater, blade coater, curtain coater, and screen printer, or spraying with a spray coater, may be used.

[0307] <Photosensitive Resin Layer Formation Process>

[0308] In this process, a photosensitive resin layer is obtained by heating a support film coated with the above-mentioned combination solution. Specifically, in this process, a photosensitive resin layer containing a photosensitive resin composition is formed on a support film by removing the solvent in the combination solution through heat distillation.

[0309] The heating temperature of the support film is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 90°C or higher. Heating to 90°C or higher accelerates the evaporation of the solvent contained in the mixture, thereby improving the production efficiency of the photosensitive element. Additionally, the heating temperature of the support film is preferably 140°C or lower, more preferably 130°C or lower, and even more preferably 120°C or lower. By maintaining the temperature at 140°C or lower, it is easy to prevent the progression of thermal polymerization of the photosensitive resin composition. The heating time of the support film is preferably 1 to 10 minutes.

[0310] <Protection Process>

[0311] A method for manufacturing a photosensitive element, after the process of forming the photosensitive resin layer,

[0312] Process of laminating a protective film onto a photosensitive resin layer (protection process)

[0313] You may have it.

[0314] [Method for forming a resist pattern]

[0315] An additional aspect of the present embodiment is a method for forming a resist pattern.

[0316] This method is the following process:

[0317] A process of laminating photosensitive elements onto a substrate (lamination process);

[0318] A process for exposing a photosensitive resin layer of a stacked photosensitive element (exposure process); and

[0319] (4) A process for developing a photosensitive resin layer after exposure;

[0320] Includes

[0321] <Lamination Process>

[0322] In this process, a photosensitive element is laminated onto a substrate. Specifically, if the photosensitive element includes a protective film, the protective film is peeled off from the photosensitive element, and then a photosensitive resin layer is heat-pressed onto the substrate using a laminator. Examples of substrate materials include copper, stainless steel (SUS), glass, indium tin oxide (ITO), etc. Additionally, these substrates may be metal film insulating plates in which a conductive layer made of copper, stainless steel (SUS), etc., is formed on an insulating layer, such as a copper-clad laminate. Before heat-pressing the photosensitive resin layer onto the substrate, the surface of the substrate may be cleaned, for example, with an aqueous H2SO4 solution with a concentration of about 10 mass% and pure water.

[0323] Heat pressing can be performed, for example, by using a laminator equipped with rolls, or by passing a laminate of a substrate and a photosensitive resin layer between the rolls one or more times (hereinafter referred to as lamination). The heating temperature of the rolls during lamination is, for example, 40 to 160°C. In addition, the substrate may be preheated to 40 to 80°C before performing lamination. Heat pressing may be performed under a reduced pressure environment.

[0324] <Photolithography Process>

[0325] In this process, the photosensitive resin layer of the laminated photosensitive element is exposed. Exposure can be performed using an exposure machine, or, if desired, after peeling off the support film. When exposing with a photomask, the exposure amount is determined by the light source illuminance and exposure time, and these may be measured by a photometer.

[0326] This process may be carried out by direct imaging exposure. In direct imaging exposure, exposure is performed directly by a direct drawing device without using a photomask. As a light source, a semiconductor laser with a wavelength of 350 to 410 nm or an ultra-high pressure mercury lamp is used. When the drawing pattern is controlled by a computer, the amount of exposure is determined by the illuminance of the exposure light source and the moving speed of the substrate.

[0327] The light irradiation method used in the photolithography process is preferably at least one type selected from projection lithography, proximity lithography, contact lithography, direct imaging lithography, and electron beam direct projection, and it is more preferable to perform the process using projection lithography or direct imaging lithography.

[0328] <Heating Process (Post-exposure heating process)>

[0329] A method for forming a resist pattern, between the exposure process and the development process,

[0330] A process of heating a photosensitive resin layer and a substrate after exposure (heating process)

[0331] It may have a heating temperature of about 30 to about 200°C, more preferably 30 to 150°C, and even more preferably 35 to 120°C. By carrying out this process, it is easy to realize improvements in the adhesion and resolution of the resist pattern. For heating, a heating furnace using a hot air, infrared, or far-infrared method may be used, and a constant temperature bath, hot plate, hot air dryer, infrared dryer, hot roll, etc. may also be used.

[0332] The elapsed time from the exposure process to the heating process, for example, the elapsed time from the point when the exposure is stopped to the point when heating is started, is preferably 10 to 600 seconds, and more preferably 20 to 300 seconds. The elapsed time from the point when heating is started to the point when heating is stopped is preferably 1 to 120 seconds, and more preferably 5 to 60 seconds.

[0333] <Development Process>

[0334] In this process, the photosensitive resin layer after exposure is developed. Specifically, unexposed or exposed portions in the photosensitive resin layer after exposure are removed using a developing device and a developing solution. If a support film is present on the photosensitive resin layer after exposure, it is preferable to remove it before performing this process. Examples of the developing solution include a developing solution containing an alkaline aqueous solution. By this process, unexposed or exposed portions are removed, thereby obtaining a resist pattern.

[0335] As for the alkaline aqueous solution, aqueous solutions such as Na2CO3, K2CO3, and tetramethylammonium hydroxide are preferred. The alkaline aqueous solution is selected according to the characteristics of the photosensitive resin layer, and generally, an aqueous Na2CO3 solution with a concentration of 0.2 to 2 mass% is used. The alkaline aqueous solution may contain a surfactant and an antifoaming agent, and may also contain a small amount of solvent to promote development. During the development process, it is preferable to maintain the temperature of the developer solution constant within the range of 20 to 40°C.

[0336] <Washing Process>

[0337] The method for forming a resist pattern is, after the development process,

[0338] Washing process of resist pattern and substrate (washing process)

[0339] It may have. According to this process, the amount of developer remaining on the resist pattern and substrate can be reduced. The rinsing water is selected in accordance with the characteristics of the photosensitive resin layer, in addition to pure water and industrial water. Among these, it is preferable to include a polyvalent metal salt such as MgSO4 at a concentration of 0.001 to 1 mass% from the perspective of excellent rectangularity and resolution of the resist pattern. In the rinsing process, it is preferable to maintain the temperature of the rinsing water constant within the range of 20 to 40°C.

[0340] <Heating Process (Heating Process After Development)>

[0341] A method for forming a resist pattern, after a developing process or a washing process,

[0342] A process of further heating the resist pattern and substrate at 60 to 300 ℃ (heating process)

[0343] It may have. By carrying out this process, the chemical resistance of the resist pattern can be improved. For the heating process, a heating furnace using hot air, infrared rays, or far-infrared rays may be used.

[0344] [Method for manufacturing a wiring board]

[0345] One aspect of the present embodiment is a method for manufacturing a wiring board.

[0346] This method is the following process:

[0347] A process of forming a resist pattern on a substrate using the above-mentioned photosensitive element (resist pattern formation process), and

[0348] A process for forming a conductor pattern by etching or plating a substrate having a resist pattern formed thereon (conductor pattern formation process); and

[0349] Process of peeling off a resist pattern from a substrate (peeling process);

[0350] Includes

[0351] In addition, one aspect of the present embodiment is the following process:

[0352] A process of forming a resist pattern on a substrate made of a metal film insulating plate using the above-mentioned photosensitive element (resist pattern formation process), and

[0353] A process for forming a conductor pattern by plating a substrate having a resist pattern formed thereon (conductor pattern formation process), and

[0354] A process for peeling off a resist pattern from a substrate (peeling process) and,

[0355] Process of removing conductor layers other than the conductor pattern (conductor layer removal process)

[0356] This is a method for manufacturing a wiring board that includes the following in this order.

[0357] Among these, the resist pattern formation process is the same as described above in the [Method for forming a resist pattern], so the explanation here is omitted.

[0358] <Conductor Pattern Formation Process>

[0359] In this process, a conductor pattern is formed by etching or plating a substrate on which a resist pattern is formed. The conductor pattern can be formed by using, for example, a metal plate or a metal film insulating plate as the substrate, and by etching or plating the surface of the substrate (for example, a copper surface) exposed by development.

[0360] (Plating method)

[0361] Methods for forming a conductor pattern by plating are, for example, as follows.

[0362] After the development process, the substrate is immersed in an acidic degreasing bath, such as a 1 to 50 mass% aqueous sulfuric acid solution, at 20 to 60°C for 1 to 60 minutes. After rinsing the immersed substrate with water, it is immersed in an aqueous sulfuric acid solution with a concentration of 1 to 50 mass% at room temperature for 1 to 60 minutes.

[0363] In addition, an aqueous solution containing copper sulfate at a concentration of 1 to 15 mass%, sulfuric acid at a concentration of 0.1 to 30 mass%, and hydrochloric acid at a concentration of 1 to 1000 ppm is prepared, and

[0364] Next, a copper sulfate plating solution is prepared by additionally mixing 0.01 to 40 ml / l and 1 to 200 ml / l of a brightener (in one embodiment, manufactured by Atotech Co., Ltd.: Caparacid HL and Caparacid GS), respectively.

[0365] Using the prepared copper sulfate plating solution, by a Haring cell uniform plating device (manufactured by Yamamoto Plating Test Engineers Co., Ltd.), at an applied current density of 0.1 to 10 A / dm² 2 Plating is performed for 1 to 300 minutes. By doing so, a conductor pattern can be formed.

[0366] The thickness of the copper plating film can be appropriately changed according to the thickness of the resist pattern. For example, the thickness of the copper plating film is preferably in the range of 1 μm or more, and also the thickness of the resist pattern (μm) - 2 μm or less. In this specification, the thickness of the resist pattern refers to the thickness of the photosensitive resin layer after curing.

[0367] <Peeling Process>

[0368] In this process, the resist pattern is peeled off from the substrate. By using an aqueous solution that has stronger alkalinity than the developer, the resist pattern is easily peeled off from the substrate. By carrying out this process, a wiring board (e.g., a printed circuit board) having a desired wiring pattern can be obtained.

[0369] Examples of an alkaline aqueous solution for stripping (hereinafter also referred to as "stripping solution") include an aqueous solution of NaOH or KOH at a concentration of 2 to 5 mass%, or an organic amine-based stripping solution. The stripping solution may contain a small amount of a water-soluble solvent. Examples of water-soluble solvents include alcohol. The temperature of the stripping solution is preferably within the range of 40 to 70°C, and the immersion time in the stripping solution is preferably 1 to 30 minutes.

[0370] <Conductor Layer Removal Process>

[0371] When a conductor pattern is formed by plating on a metal film insulating plate, a conductor pattern is formed on the conductor layer of the metal film insulating plate. Therefore, from the perspective of insulating between conductor patterns, it is desirable to remove the conductor layer other than the conductor pattern. Examples of such removal methods include etching after peeling off the resist pattern.

[0372] Photosensitive elements are used in the manufacture of printed circuit boards; the manufacture of lead frames for IC chip mounting; precision machining of metal foils such as metal masks; the manufacture of packages such as Ball Grid Arrays (BGA) and Chip Size Packages (CSP); the manufacture of tape substrates such as Chip on Film (COF) and Tape Automated Bonding (TAB); the manufacture of semiconductor bumps; and the manufacture of barriers for flat panel displays such as ITO electrodes, address electrodes, and electromagnetic shields.

[0373] It can be used for.

[0374] In addition, unless otherwise specifically mentioned, the values ​​of each of the above-mentioned parameters are measured in accordance with the measurement method in the embodiments described below.

[0375] Examples

[0376] Hereinafter, examples and comparative examples are provided, and the present embodiment is further described. However, the present embodiment is not limited to the following examples, unless it deviates from the gist thereof. In the examples and comparative examples, various physical properties were measured by the following methods.

[0377] [(A) Synthesis of Component]

[0378] The monomer (copolymer component) shown in the table below was mixed with azobisisobutyronitrile in the mixing amounts (unit: parts by mass) shown in the table below, thereby preparing solution (a). 200 g of methyl ethyl ketone and 100 g of ethanol were added to a flask equipped with a stirrer, a reflux condenser, a thermometer, a dropping funnel, and a nitrogen gas inlet tube, and then stirred while blowing nitrogen gas into the flask, and the temperature was raised to 80 ℃. After that, 300 g of the solution (a) was added dropwise into the flask at a constant dropping rate over 4 hours, and then stirred at 80 ℃ for 2 hours.

[0379] Next, 50 parts by mass of a mixture containing 30 parts by mass of methyl ethyl ketone and 20 parts by mass of ethanol was mixed with 0.5 parts by mass of azobisisobutyronitrile to prepare solution (b). 50 g of solution (b) was added dropwise over 10 minutes at a constant dropping rate into a flask containing solution (a), and then stirred for an additional 3 hours at 80°C. In addition, the solution in the flask was heated to 90°C over 30 minutes, then held at 90°C for 2 hours, after which stirring was stopped and the solution was cooled to room temperature (25°C). Thus, solutions of alkali-soluble polymers A1 to A5 were obtained. The weight-average molecular weight (Mw) of alkali-soluble polymers A1 to A5 is shown in the table below.

[0380] The weight-average molecular weight was determined by measuring it by gel permeation chromatography (GPC) and converting it using a calibration curve of standard polystyrene. The conditions for the GPC are shown below.

[0381] (GPC conditions)

[0382] Pump: Japan Spectroscopic Manufacturing PU-4580

[0383] Digester : DG-2080-53

[0384] Column Oven: CO-1560

[0385] Column: Total of 4 items below

[0386] Manufactured by Shodex KF-807 / KF-806M×2 / KF-802.5

[0387] Eluent: Tetrahydrofuran

[0388] Measured temperature: 40 ℃

[0389] Flow rate: 1.00 mL / min

[0390] Detector: Japan Spectroscopic Manufacturing RI-1530

[0391] [Preparation of evaluation samples]

[0392] <Manufacture of Photosensitive Elements>

[0393] Each component and methyl ethyl ketone as defined in the table below were mixed such that the amount of each component as a solid corresponds to the amount indicated in the table below, and the solid content concentration corresponds to 60 mass%. The mixture was then thoroughly stirred to obtain a combination solution of a photosensitive resin composition. The amount of the mixture (parts by mass) is the mass of the non-volatile component (solid content amount). A polyethylene terephthalate film (manufactured by Toray, QS71) with a thickness of 16 μm was used as a support film, and the above combination solution was uniformly applied to its surface using a bar coater. Then, by drying this in a 95°C dryer for 2 minutes and 30 seconds, a photosensitive resin layer with a film thickness of 25 μm was formed. Thus, a photosensitive element was obtained.

[0394] Next, a 19 μm polyethylene film (manufactured by Tamapoly Co., GF-818) was attached as a protective film to the surface of the photosensitive resin layer on the side where the polyethylene terephthalate film was not laminated. The laminate of the support film, the photosensitive resin layer, and the protective film obtained by this was treated as a photosensitive element in this embodiment.

[0395] <Front View>

[0396] A copper-clad laminate with a total thickness of 0.4 mm was prepared by laminating rolled copper foil with a thickness of 18 μm. Then, the surface of the copper-clad laminate was cleaned with a 10 mass% aqueous H2SO4 solution and then cleaned with pure water.

[0397] <Laminate>

[0398] The copper-clad laminate having undergone the above-mentioned front surface was preheated to 50°C. Then, while peeling off the polyethylene film (protective film) of the photosensitive element, a photosensitive resin laminate was laminated onto the copper-clad laminate at a roll temperature of 105°C using a hot roll laminator (manufactured by Asahi Kasei Co., AL-700). By doing so, an evaluation substrate was obtained. Here, the air pressure during lamination was set to 0.35 MPa, and the lamination speed was set to 1.5 m / min.

[0399] <Exposure>

[0400] After 2 hours had passed since lamination, the substrate was exposed to light at a wavelength of 365 nm by a projection exposure machine (UX-23101 manufactured by Ushio Electric Co., Ltd.) with a photomask having a predetermined projection exposure mask pattern interposed therein.

[0401] <Heating>

[0402] The substrate, which had been exposed for 1 minute, was heated for 30 seconds by a blower constant temperature thermostat (manufactured by Yamato Kagaku, DKM600) set to 60°C.

[0403] <Phenomenon>

[0404] A polyethylene terephthalate film (support film) was peeled off from the photosensitive resin layer. Then, using an alkaline developer (manufactured by Fuji Engineering, a developer for dry films), a 1 mass% aqueous solution of Na2CO3 at 30°C was sprayed at a spray pressure of 0.15 MPa over a predetermined period of time to perform development (developing spray). In this embodiment, after the developing spray, a water rinsing spray was additionally performed.

[0405] [Exposure Conditions and Development Conditions]

[0406] <Phenomenon Conditions>

[0407] A substrate having undergone the above <lamination> was prepared, and the above <development> was performed without performing both the above <exposure> and the above <heating>. By doing so, the "shortest development time," which is the shortest time among the times required until the photosensitive resin layer in the unexposed portion is completely dissolved, was measured.

[0408] In this embodiment, the time for the developing spray and the time for the rinsing spray after development were each set to twice the time of the shortest developing time.

[0409] <Exposure Conditions>

[0410] A substrate having undergone the above lamination process was prepared, and exposure was performed using a photomask (refer to FIG. 2) having a mask pattern with a line width (L) / space width (S) (hereinafter simply abbreviated as "L / S") of 8 / 8 (unit: μm). Subsequently, <heating> and <development> were performed to form a resist pattern on the substrate. The formed resist pattern was observed at a magnification of 100x using an optical microscope, thereby obtaining an observation image of the line width of the pattern. The exposure amount at which the line width becomes 8 μm (unit: mJ / cm²) 2 ) was adopted as the optimal exposure amount, and the exposure amount in the following evaluation was all carried out as the optimal exposure amount.

[0411] Figure 2 is a plan view showing an example of the configuration of a mask pattern.

[0412] In the drawing, in the area (100) on the photomask, the area that transmits the exposure light is indicated by reference numeral 10 (transmitting area (10)), and the area that does not transmit the exposure light (slanted area) is indicated by reference numeral 1 (light-blocking area (1)). The light-blocking area (1) has a predetermined width and extends in the X direction, and multiple such light-blocking areas (1) are arranged in the width direction (Y direction) with a predetermined spacing. In this embodiment, since the unexposed portion of the photosensitive resin layer is removed through the <development> process, it is expected that a resist pattern having L / S corresponding to the width (S: space) of the light-blocking area (1) and the width (L: line) of the transmission area (10) is formed by exposing the photosensitive resin layer through a photomask having the mask pattern of FIG. 2, and then heating and developing.

[0413] <Closeness>

[0414] Evaluation was performed using a photomask having a mask pattern (refer to FIG. 3) with an L / S of x / 3x {x = 1 to 15 (varying in 0.5 μm increments)} (unit: μm). Specifically, the photomask was placed over the substrate that had undergone the <front> and <lamination> steps, and the substrate was exposed at an optimal exposure amount. Subsequently, a resist pattern was formed by performing the <heating> and <developing> steps. The formed resist pattern was observed using an optical microscope at a magnification of 100x, thereby obtaining an observation image of the line width of the pattern.

[0415] Figure 3 is a plan view showing an example of the configuration of a mask pattern.

[0416] In the drawing, in the area (100A) on the photomask, the area that transmits the exposure light is indicated by reference numeral 10 (transmitting area), and the area that does not transmit the exposure light (slanted area) is indicated by reference numeral 1 (light-blocking area). The transmitting area (10) has a predetermined width and extends in the x-direction, and multiple such transmitting areas (10) are arranged in the width direction (y-direction) with a predetermined spacing. In this embodiment, since the unexposed portion of the photosensitive resin layer is removed through the <development> process, it is expected that a resist pattern having L / S corresponding to the width (L: line) of the transmitting area (10) and the width (S: space) of the light-blocking area (1) is formed by exposing the photosensitive resin layer through a photomask having the mask pattern of FIG. 3, and then heating and developing.

[0417] In the observed image, the minimum line width at which the line portion (exposed portion) is formed without causing meandering or defects was defined as the value of the “adhesion line width (unit: μm).” A smaller value indicates better adhesion. Adhesion was evaluated according to the following criteria. An evaluation result of B (good) or higher was considered acceptable.

[0418] (metewand)

[0419] A (Significantly Good): Adhesion line width is 3.5 µm or less.

[0420] B (Good): Adhesion line width is greater than 3.5 µm and 4.0 µm or less.

[0421] C (Standard): Adhesion line width is greater than 4.0 µm and less than or equal to 5.0 µm.

[0422] D (Defective): The value of the contact line width is greater than 5.0 μm.

[0423] <Resolution>

[0424] Evaluation was performed using a photomask having a mask pattern (e.g., refer to FIG. 2) in which L / S is x / x {x = 1 to 15 (varying in increments of 0.5 μm)} (unit: μm). That is, the photomask was placed between the substrates that had undergone the <front> and <lamination> steps, and the substrates were exposed at an optimal exposure amount. Subsequently, a resist pattern was formed by performing the <heating> and <developing> steps. The formed resist pattern was observed using an optical microscope at a magnification of 100x, thereby obtaining an observation image of the line width of the pattern. In the observation image, the minimum space width at which the line portion (exposed portion) does not cause meandering or defects, and the space portion (unexposed portion) is removed without residue, was treated as the value of the "resolution space width (unit: μm)." A smaller value indicates better resolution.

[0425] <Independent Line Formation>

[0426] Evaluation was performed using a photomask having a mask pattern (e.g., refer to FIG. 4) with an L / S of x / 200 {x = 1 to 15 (varying in 0.5 μm increments)} (unit: μm). That is, the photomask was placed over the substrate that had undergone the <front> and <lamination> steps and exposed at an optimal exposure amount. Subsequently, a resist pattern was formed by performing the <heating> and <developing> steps. The formed resist pattern was observed using an optical microscope at a magnification of 100x, thereby obtaining an observation image of the line width of the pattern.

[0427] Depending on the mask pattern, the resist lines may be observed to be formed independently, such as when the spacing between adjacent resist lines in the resist pattern is large. In this specification, such resist lines are referred to as "resist independent lines."

[0428] Figure 4 is a plan view showing an example of the configuration of a mask pattern.

[0429] In the drawing, the mask pattern in the area (100B) on the photomask has a wider width (S: space) of the area (1) that does not transmit exposure light compared to the mask pattern in the drawing area (100A) shown in FIG. 3. In the same way as in FIG. 3, it is theoretically expected that a resist pattern having the width (L: line) of the exposure area (10) and a corresponding L / S will be formed based on the mask pattern of the present drawing.

[0430] In the observed image, the minimum line width at which independent resist lines are formed without defects was adopted as the value of "independent line width (unit: μm)." "Independent line formation ability" was evaluated based on the magnitude of the difference between the value of "independent line width" and the value of "close line width" according to the following criteria. The smaller this difference, the better the independent line formation ability.

[0431] (metewand)

[0432] A (Significantly Good): The value of (Independent fine line width) - (Close line width) is 1.0 μm or less.

[0433] B (Good): The value of (independent fine line width) - (close line width) is greater than 1.0 μm and less than or equal to 2.0 μm.

[0434] C (Standard): (Independent fine line width) - (Close line width) is greater than 2.0 μm.

[0435] <Plated Copper Wiring Formability>

[0436] The substrate after the above <development> was cleaned with an acidic cleaner Cupura Pro S2 (ATOTEC) at 35°C for 5 minutes, cleaned with ion-exchanged water at 35°C, cleaned with ion-exchanged water at 25°C, and cleaned with 10% sulfuric acid at 25°C. By doing so, electrolytic copper plating pretreatment was performed on the substrate. Thus, a substrate for evaluating plating resistance after plating pretreatment was obtained.

[0437] Next, an aqueous copper sulfate solution with a concentration of 121 g / l was prepared and diluted with sulfuric acid with a concentration of 19 mass% until the volume was 3.6 times. Subsequently, concentrated hydrochloric acid was mixed in an amount resulting in a concentration of 200 ppm. Then, as a brightener, 0.4 ml / l of Caparaside HL and 20 ml / l of Caparaside GS were mixed, respectively, to prepare a copper sulfate plating solution. Finally, regarding the above plating resistance evaluation substrate (6 cm × 12.5 cm), the copper sulfate plating solution was applied using a Haring cell uniform plating apparatus (manufactured by Yamamoto Plating Test Engineers Co., Ltd.) at a voltage of 0.05 V and a current density of 1.0 A / dm² 2 The plating was performed for 45 minutes. Thus, a substrate was obtained after plating. At this time, the thickness of the copper plating film was 20 μm.

[0438] After plating, the substrate was immersed in an amine stripping solution at 50°C for 3 minutes {a 1:1 mixture of R-100S (15 vol%) manufactured by MGC and R-101 (8 vol%) manufactured by MGC}. After removing the substrate, it was washed with ion-exchanged water, and the resist pattern on the substrate was stripped. Subsequently, an evaluation substrate was obtained by air drying. The substrate was observed using an optical microscope at a magnification of 100x, thereby obtaining an observation image.

[0439] In the observed image, the minimum line width at which the plated copper wiring is maintained without peeling, breakage, or collapse in the space area (unexposed area) was adopted as the value of "resolution line width after plating (unit: μm)." The plated copper wiring formability was evaluated based on the following criteria from the magnitude of the difference between the value of "resolution line width after plating" and the value of "resolution space width." The smaller this difference, the better the plated copper wiring formability.

[0440] (metewand)

[0441] A (Good): The value of (sea line width after plating) - (sea space width) is 0 µm.

[0442] B (Standard): The value of (sea line width after plating) - (sea space width) exceeds 0 μm and is 1.0 μm or less.

[0443] C (Defective): The value of (sea line width after plating) - (sea space width) is greater than 1.0 μm.

[0444] FIG. 5 is an example of an observation image that can be obtained in the above <plated copper wiring formation>. FIG. 5(a) shows an example of "falling over" of the plated copper wiring, and FIG. 5(b) shows an example of "peeling and breaking" of the plated copper wiring. In each figure, the plated copper wiring (30) is formed on the substrate (20).

[0445] In FIG. 5(a), some of the plated copper wiring (30A), which should originally be formed by standing upright in a vertical direction, is tilted inward. In this case, in the observation image, the "tilting" is observed as plated copper wiring (30A) that has lost its straightness.

[0446] Additionally, in FIG. 5(b), some of the plated copper wiring (30) is peeled off and broken from the substrate (20). In this case, in the vertical observation image, the "peeling and breaking" is observed as a blank area (dotted line area (S1) in the drawing) where the plated copper wiring is not formed at the location where the plated copper wiring should be formed.

[0447] In addition, regarding “peeling and fracture,” “peeling” refers to a phenomenon in which the entire continuous plated copper wiring is lost from the substrate, and “fracture” refers to a phenomenon in which a part of the continuous plated copper wiring is lost from the substrate.

[0448] <Residualness of Independent Fine Lines After Plating>

[0449] Using the substrate prepared in the evaluation of the above <independent fine line formation ability>, an evaluation substrate was obtained in the same manner as the above <plated copper wiring formation ability>. The substrate was observed at a magnification of 100x using an optical microscope, and an observation image was obtained.

[0450] In the observed image, the minimum line width where no plating erosion (shot) occurred in the area where the resist pattern peeled off was determined and adopted as the "independent fine line plating space width (unit: μm)." The retention of independent fine lines after plating was evaluated based on the following criteria from the magnitude of the difference between the value of the "independent fine line plating space width" and the value of the "independent fine line width." The smaller this difference, the better the retention of independent fine lines after plating.

[0451] (metewand)

[0452] A (Good): The value of (independent fine line plating space width) - (independent fine line width) is 1.0 μm or less.

[0453] B (Standard): The value of (independent fine line plating space width) - (independent fine line line width) exceeds 1.0 μm.

[0454] FIG. 6 is an example of an observation image that can be obtained in the above <independent fine line retention after plating>. In the drawing, plated copper wiring (30) is formed on a substrate (20).

[0455] Meanwhile, the plating is formed on the portion where the resist pattern has been removed by the development process, and therefore, it is desirable that the plating not be eroded in the portion of the resist pattern. In FIG. 6, some of the plated copper wiring (30) is eroded up to the portion where the resist pattern was formed (the dotted line area (S2) in the drawing). The smaller the degree of this erosion, the better the result obtained with respect to the <independent fine wire retention after plating>.

[0456] <Transmittance of photosensitive resin layer>

[0457] The protective film of the photosensitive element was peeled off. Then, using a spectrophotometer U-3010 (manufactured by Hitachi High Technologies Co., Ltd.) and a polyethylene terephthalate film (support film) as a reference, the transmittance (%) of the photosensitive resin layer at a wavelength of 365 nm was measured. The measurement was performed with the slit set to 4 nm and the scan speed set to 600 nm / min.

[0458]

[0459]

[0460]

[0461]

[0462]

[0463]

[0464]

[0465] As can be seen from the table above, in the examples, the evaluation results for <adhesion> and <plated copper wiring formability> were both A or B. That is, in the examples, <adhesion> and <plated copper wiring formability> can be achieved, and in a particularly preferred form, both <independent fine wire formability> and <independent fine wire retention after plating> were satisfactory. Industrial applicability

[0466] By using the photosensitive element according to the present invention, a resist pattern with good adhesion and plated copper wiring formability can be obtained. Such a photosensitive element can be widely used as a photosensitive element for forming resist patterns in printed circuit boards, etc. Explanation of the symbols

[0467] 1: Area that does not transmit exposure light (light-blocking area) 10: Area that transmits exposure light (transmitting area) 20 : Substrate 30: Plated copper wiring 30A: Plated copper wiring 100 : Area on the photomask 100A: Area on the photomask 100B: Area on the photomask 101: Photosensitive resin layer 110 : Foreign object 111 : Precipitate 112 : Bubbles L : Line S : Space S1: Area S2 : Area

Claims

Claim 1 A photosensitive element comprising a support film and a photosensitive resin layer including a photosensitive resin composition, wherein the photosensitive resin composition comprises, with respect to the total solid mass of the photosensitive resin composition, the following components: (A) alkali-soluble polymer: 30 to 70 mass%; (B) compound having ethylenically unsaturated bonds: 20 to 60 mass%; A photosensitive element comprising (C) a non-imidazole photopolymerization initiator: 4.0 to 10.0 mass%; wherein the content of a constituent unit derived from benzyl (meth)acrylate in component (A) is 55 mass% or more with respect to the total of component (A); and the content of a compound having two molecules having ethylenically unsaturated bonds in component (B) is 80 mass% or more with respect to the total of component (B); and wherein the photosensitive resin composition further comprises (E) tert-butylcatechol as a polymerization inhibitor, and the content of the polymerization inhibitor (E) is 50 to 1000 ppm with respect to the total solid mass of the photosensitive resin composition. Claim 2 A photosensitive element according to claim 1, wherein the content of the (C) component is 4.50 mass% or more with respect to the total solid mass of the photosensitive resin composition. Claim 3 A photosensitive element according to claim 1, wherein the content of the (C) component is 4.75 mass% or more with respect to the total solid mass of the photosensitive resin composition. Claim 4 A photosensitive element according to claim 1, wherein the content of the (C) component is 5.25 mass% or more with respect to the total solid mass of the photosensitive resin composition. Claim 5 A photosensitive element according to claim 1, wherein the content of the (C) component is 6.00 mass% or more with respect to the total solid mass of the photosensitive resin composition. Claim 6 delete Claim 7 A photosensitive element according to claim 1, wherein the content of a constituent unit derived from benzyl (meth)acrylate in the above component (A) is 60 weight% or more with respect to the entire component (A). Claim 8 A photosensitive element according to claim 1, wherein the content of a compound having two of the molecules having the ethylenically unsaturated bonds is 90 mass% or more with respect to the total of component (B). Claim 9 In any one of claims 1 to 5, 7 and 8, the compound having two of the ethylenically unsaturated bonds in one molecule is of the following general formula (II): (during food, R 2 are, each independently, a hydrogen atom or a methyl group, and X 2 O and Y 2 A photosensitive element comprising a compound represented as follows: O is each independently an oxyethylene group or an oxypropylene group, m3, m4, n2, and n3 are each independently integers from 0 to 40, m3 + m4 is 1 to 40, and n2 + n3 is 0 to 20. Claim 10 A photosensitive element according to claim 9, wherein the content of the compound represented by the above general formula (II) is 90 mass% or more with respect to the total of component (B). Claim 11 A photosensitive element according to claim 9, wherein the compound having two of the molecules having the above-mentioned ethylenically unsaturated bonds comprises a compound in which the average value of n2+n3+m3+m4 in the above-mentioned general formula (II) is 10 or less, and a compound in which the average value of n2+n3+m3+m4 in the above-mentioned general formula (II) is 15 or more. Claim 12 A photosensitive element according to any one of claims 1 to 5, 7 and 8, wherein the (C) component is included in an amount of 5.0 mass% or more relative to the total solid mass of the photosensitive resin composition, the absorbance (Y) of the photosensitive resin layer at a wavelength of 365 nm at a film thickness of 25 μm is 0.35 or less, and the contribution (X) of the absorbance of the (C) component to the absorbance (Y) is 40% or more, wherein the contribution (X) is calculated by the following formula (1): X (%) = 100 × εc / absorbance (Y) of the photosensitive resin layer ··· (1) ε : value of change in absorbance per 1 mass% of the (C) component c : content (mass%) of the (C) component relative to the total solid mass of the photosensitive resin composition. Claim 13 In claim 12, a photosensitive element in which the contribution (X) is 55% or more. Claim 14 In claim 12, a photosensitive element in which the contribution (X) is 65% or more. Claim 15 In claim 12, a photosensitive element in which the contribution (X) is 85% or more. Claim 16 In claim 12, a photosensitive element having an absorbance (Y) of 0.30 or less. Claim 17 In claim 12, a photosensitive element having an absorbance (Y) of 0.25 or less. Claim 18 A photosensitive element according to any one of claims 1 to 5, 7 and 8, wherein the photosensitive resin composition further comprises (D) other photopolymerization initiator, and the component (D) comprises at least one selected from the group consisting of benzophenone compounds, pyrazolin compounds, anthracene compounds and coumarin compounds. Claim 19 In claim 18, the photosensitive resin composition further comprises (D) other photopolymerization initiator, and the (D) component comprises at least one selected from the group consisting of benzophenone compounds and pyrazolin compounds, a photosensitive element. Claim 20 delete Claim 21 delete Claim 22 A photosensitive element according to claim 1, wherein the content of the polymerization inhibitor (E) is 50 to 500 ppm with respect to the total solid mass of the photosensitive resin composition. Claim 23 A photosensitive element according to any one of claims 1 to 5, 7 and 8, wherein the absorbance of the support film at 365 nm is 0.1 or less. Claim 24 A photosensitive element comprising a protective film in addition to any one of claims 1 to 5, 7 and 8. Claim 25 A method for forming a resist pattern using a photosensitive element described in any one of claims 1 to 5, 7 and 8, comprising the following steps: a step of laminating a photosensitive element onto a substrate; a step of exposing a photosensitive resin layer of the laminated photosensitive element to light; and a step of developing the photosensitive resin layer after exposure. Claim 26 A photosensitive element roll formed by winding a photosensitive element described in any one of claims 1 to 5, 7, and 8. Claim 27 A method for manufacturing a wiring board, comprising: a process of forming a resist pattern on a substrate using a photosensitive element described in any one of claims 1 to 5, 7 and 8; a process of forming a conductor pattern by etching or plating the substrate on which the resist pattern is formed; and a process of peeling the resist pattern from the substrate. Claim 28 A method for manufacturing a wiring board, comprising, in this order: a process of forming a resist pattern on a substrate made of a metal film insulating plate using a photosensitive element described in any one of claims 1 to 5, 7 and 8; a process of forming a conductor pattern by plating the substrate on which the resist pattern is formed; a process of peeling off the resist pattern from the substrate; and a process of removing a conductor layer other than the conductor pattern. Claim 29 A method for manufacturing a wiring board according to claim 28, wherein the wiring board has a conductor pattern with a width of 10 μm or less.

Citation Information

Patent Citations

  • Photosensitive resin composition

    KR1020180019678A

  • Photosensitive resin composition

    KR1020190047146A

  • Photosensitive resin composition

    KR1020220127382A

  • Photosensitive resin composition and method for forming a resist pattern

    KR1020200139227A