Polymer composition, lubricating oil additive, viscosity index improver, lubricating oil composition, method for manufacturing a polymer composition, and method for manufacturing a macro monomer
A (meth)acrylic copolymer-based polymer composition with tailored molecular weight distribution and scattering properties addresses the issue of viscosity loss in lubricants, enhancing viscosity index and solubility across temperature variations.
Patent Information
- Application Number
- KR1020227027599
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-25
- Filing Date
- 2021-03-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-03-25
AI Technical Summary
Conventional lubricant compositions fail to maintain viscosity across a wide temperature range, particularly experiencing a loss at high temperatures, and existing viscosity index improvers do not provide sufficient improvement.
A polymer composition comprising a (meth)acrylic copolymer with specific molecular weight distribution and scattering characteristics, including constituent units from alkyl methacrylate, alkyl acrylate, and alkoxyalkyl (meth)acrylate, which enhances viscosity index improvement.
The polymer composition maintains viscosity effectively across varying temperatures, providing improved viscosity index and solubility in base oils, even under high shear conditions.
Smart Images

Figure R1020227027599_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a polymer composition used in engine oil, etc., a lubricating oil additive, a viscosity index improver, a lubricating oil composition, a method for manufacturing a polymer composition, and a method for manufacturing a macro monomer.
[0002] The present application claims priority based on Japanese Patent Application No. 2020-055130 filed in Japan on March 25, 2020, and Japanese Patent Application No. 2020-055131 filed in Japan on March 25, 2020, and incorporates the contents thereof herein. Background Technology
[0003] Lubricant compositions used for engine oils, gear oils, etc., in automobiles, require a constant viscosity capable of protecting components over a wide range from low to high temperatures.
[0004] However, conventional lubricant compositions lose viscosity at high temperatures and fail to exhibit their original performance. Furthermore, in response to the recent trend toward lower fuel consumption, there is a demand for lubricants that reduce viscosity within the practical temperature range while suppressing the decrease in viscosity at high temperatures (improving the viscosity index).
[0005] For this reason, for example, Patent Document 1 and Patent Document 2 describe a viscosity index improver comprising a (meth)acrylate-based polymer having a long-chain alkyl group. Prior art literature
[0006] Japanese Patent Publication No. 2013-203913 and Japanese Patent Publication No. Hei 10-298576 The problem to be solved
[0007] However, the method described in Patent Document 1 and Patent Document 2 does not provide sufficient improvement in viscosity index.
[0008] The present invention aims to solve these problems. means of solving the problem
[0009] The gist of the present invention is a polymer composition comprising a (meth)acrylic copolymer A, wherein the (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from an alkyl methacrylate a1 having 5 to 14 carbon atoms of an alkyl group, a constituent unit derived from an alkyl acrylate a2 having 5 to 14 carbon atoms of an alkyl group, and a constituent unit derived from an alkyl acrylate a3 having 1 to 4 carbon atoms of an alkyl group.
[0010] The gist of the present invention is that, as a polymer composition, the differential distribution value in the differential molecular weight distribution curve of the polymer composition measured by gel permeation chromatography satisfies the following Equation 1, and the magnitude q of the scattering vector of small-angle X-ray scattering at 25°C of the following base oil solution at 35 wt% of the polymer composition is 0.07 nm -1 2nm or more -1 In the following range, the maximum value of scattering intensity after standardization is 40cm -1 It is in the polymer composition of the above.
[0011] dMp30 / dMp≥0.65 ···1
[0012] ·dMp30: Differential distribution value of molecular weight corresponding to 30% of the peak top molecular weight measured by gel permeation chromatography.
[0013] ·dMp: Differential distribution value of peak-top molecular weight measured by gel permeation chromatography.
[0014] · Base oil: API standard Group III or Group III plus
[0015] [1]
[0016] As a polymer composition,
[0017] The differential distribution value represented by Formula 1 below in the differential molecular weight distribution curve of the polymer composition measured by gel permeation chromatography is 0.65 or higher, preferably 0.70 or higher and 1.0 or lower, more preferably 0.75 or higher and 1.0 or lower, and even more preferably 0.80 or higher and 1.0 or lower.
[0018] The magnitude q of the scattering vector of small-angle X-ray scattering at 25°C for the following base oil solution at 35 wt% of the above polymer composition is 0.07 nm -1 2nm or more -1 In the following range, the maximum value of scattering intensity after standardization is 40cm -1 That is all, 40cm -1 Over 1100cm -1 The following is more preferable, and 60cm -1 Over 500cm -1 The following is more preferable, and 80cm -1 Over 450cm -1 A polymer composition that is more preferable as follows.
[0019] dMp30 / dMp ···1
[0020] ·dMp30: Differential distribution value of molecular weight corresponding to 30% of the peak top molecular weight measured by gel permeation chromatography.
[0021] ·dMp: Differential distribution value of peak-top molecular weight measured by gel permeation chromatography.
[0022] · Base oil: API standard Group III or Group III plus
[0023] [2]
[0024] The above polymer composition is a polymer composition comprising (meth)acrylic copolymer A, and
[0025] The polymer composition described in [1], wherein the (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from alkyl methacrylate a1 having 5 to 14 carbon atoms of an alkyl group, a constituent unit derived from alkyl acrylate a2 having 5 to 14 carbon atoms of an alkyl group, and a constituent unit derived from alkyl acrylate a3 having 1 to 4 carbon atoms of an alkyl group.
[0026] [3]
[0027] The polymer composition described in [2], wherein, with respect to the total mass of the (meth)acrylic copolymer A, the content of the constituent unit derived from the alkyl methacrylate a1 is preferably 1 mass% or more and 50 mass% or less, more preferably 5 mass% or more and 45 mass% or less, and even more preferably 10 mass% or more and 40 mass% or less.
[0028] [4]
[0029] A polymer composition comprising (meth)acrylic copolymer A,
[0030] The above (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from alkyl methacrylate a1 having 5 to 14 carbon atoms in an alkyl group, a constituent unit derived from alkyl acrylate a2 having 5 to 14 carbon atoms in an alkyl group, and a constituent unit derived from alkyl acrylate a3 having 1 to 4 carbon atoms in an alkyl group, and
[0031] A polymer composition wherein, in the above (meth)acrylic copolymer A, the constituent unit derived from the above alkyl methacrylate a1 is preferably 1 mass% or more and 50 mass% or less with respect to the total mass of the above (meth)acrylic copolymer A, is more preferably 5 mass% or more and 45 mass% or less, and even more preferably 10 mass% or more and 40 mass% or less.
[0032] [5]
[0033] A polymer composition described in any one of [2] to [4], wherein, in the above (meth)acrylic copolymer, the content of the constituent unit derived from the alkyl acrylate a2 is preferably 1 mass% or more and 50 mass% or less with respect to the total mass of the above (meth)acrylic copolymer A, is more preferably 5 mass% or more and 45 mass% or less, and even more preferably 10 mass% or more and 40 mass% or less.
[0034] [6]
[0035] A polymer composition described in any one of [2] to [5], wherein, in the above (meth)acrylic copolymer A, the content of the constituent unit derived from the alkyl acrylate a3 with respect to the total mass of the above (meth)acrylic copolymer A is preferably 30 mass% or more and 80 mass% or less, more preferably 35 mass% or more and 75 mass% or less, and even more preferably 40 mass% or more and 70 mass% or less.
[0036] [7]
[0037] A polymer composition comprising (meth)acrylic copolymer A,
[0038] The above (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from alkyl methacrylate a1 having 5 to 14 carbon atoms in an alkyl group, a constituent unit derived from alkyl acrylate a2 having 5 to 14 carbon atoms in an alkyl group, and a constituent unit derived from alkyl acrylate a3 having 1 to 4 carbon atoms in an alkyl group, and
[0039] A polymer composition wherein, in the above (meth)acrylic copolymer A, the content of the constituent unit derived from the alkyl acrylate a3 with respect to the total mass of the above (meth)acrylic copolymer A is preferably 30 mass% or more and 80 mass% or less, more preferably 35 mass% or more and 75 mass% or less, and even more preferably 40 mass% or more and 70 mass% or less.
[0040] [8]
[0041] The polymer composition described in [7], wherein, with respect to the total mass of the (meth)acrylic copolymer A, the content of the constituent unit derived from the alkyl acrylate a2 is preferably 1 mass% or more and 50 mass% or less, more preferably 5 mass% or more and 45 mass% or less, and even more preferably 10 mass% or more and 40 mass% or less.
[0042] [9]
[0043] A polymer composition described in any one of claims [2] to [8], wherein the above (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from alkoxyalkyl (meth)acrylate a4.
[0044]
[10]
[0045] The polymer composition described in [9], wherein, with respect to the total mass of the (meth)acrylic copolymer A, the content of the constituent unit derived from the alkoxyalkyl (meth)acrylate a4 is preferably 1 mass% or more and 30 mass% or less, more preferably 3 mass% or more and 25 mass% or less, and even more preferably 5 mass% or more and 20 mass% or less.
[0046]
[11]
[0047] A polymer composition described in any one of [1] to
[10] , wherein the differential distribution value represented by the following formula in the differential molecular weight distribution curve measured by gel permeation chromatography is 0.65 or higher, preferably 0.70 or higher and 1.0 or lower, more preferably 0.75 or higher and 1.0 or lower, and even more preferably 0.80 or higher and 1.0 or lower.
[0048] dMp30 / dMp ···1
[0049] ·dMp30: Differential distribution value of molecular weight corresponding to 30% of the peak top molecular weight.
[0050] ·dMp: Differential distribution value of peak top molecular weight.
[0051]
[12]
[0052] The size of the scattering vector q=0.1nm of small-angle X-ray scattering at 100°C for a 35wt% base oil solution of the above polymer composition, which is API standard Group III or Group III Plus. -1 The scattering intensity after standardization in is 1cm -1 It is desirable to be at least 1.5cm -1 Over 100.0cm -1 It is more desirable to be less than 2cm -1 Over 50.0cm -1 A polymer composition described in any one of [1] to
[11] , which is more preferably the following.
[0053]
[13]
[0054] A polymer composition described in any one of [1] to
[12] , wherein the mass average molecular weight of the polymer composition, measured by gel permeation chromatography, is preferably 50,000 or more and 200,000 or less, more preferably 100,000 or more and 150,000 or less, and even more preferably 150,000 or more and 100,000 or less.
[0055]
[14]
[0056] A polymer composition described in any one of claims [1] to
[13] , wherein the molecular weight distribution of the polymer composition, measured by gel permeation chromatography, is preferably 5 or more and 20 or less, more preferably 6 or more and 18 or less, and even more preferably 7 or more and 15 or less.
[0057]
[15]
[0058] A polymer composition described in any one of [2] to
[14] , wherein the above (meth)acrylic copolymer A is a graft copolymer.
[0059]
[16]
[0060] The above graft copolymer comprises a constituent unit derived from a vinyl radical polymerizable monomer m1 and a constituent unit derived from a macromonomer M other than the vinyl radical polymerizable monomer m1, as described in
[15] .
[0061]
[17]
[0062] The above-described vinyl radical polymerizable monomer m1 is an alkyl acrylate a2 having 5 to 14 carbon atoms in the alkyl group and an alkyl acrylate a3 having 1 to 4 carbon atoms in the alkyl group, a polymer composition described in
[16] .
[0063]
[18]
[0064] The above-mentioned macromonomer M comprises a constituent unit derived from the vinyl radical polymerizable monomer m2, a polymer composition as described in
[16] or
[17] .
[0065]
[19]
[0066] The above vinyl radical polymerizable monomer m2 comprises an alkyl methacrylate a1 having 5 to 14 carbon atoms in the alkyl group, a polymer composition described in
[18] .
[0067]
[20]
[0068] A polymer composition described in any one of
[16] to
[19] , wherein the above macromonomer M has the structure of Formula 2 below.
[0069]
[0070] (during food, X 1 To X n-1 Each independently represents a hydrogen atom, a methyl group, or a CH2OH, and Y 1 to Y n Each represents a substituent that independently binds to the vinyl group of the vinyl radical polymerizable monomer m2. Z represents a terminal group, and n represents an integer from 2 to 10,000.
[0071]
[21]
[0072] A polymer composition described in any one of claims
[16] to
[20] , wherein the number average molecular weight of the above macromonomer M, measured by gel permeation chromatography, is preferably 500 to 30000, more preferably 1000 to 25000, and particularly preferably 2000 to 20000.
[0073]
[22]
[0074] A lubricating oil additive comprising a polymer composition described in any one of [1] to
[21] .
[0075]
[23]
[0076] A viscosity index improver comprising a polymer composition described in any one of [1] to
[21] .
[0077]
[24]
[0078] A lubricating oil composition comprising a polymer composition described in any one of [1] to
[21] .
[0079]
[25]
[0080] A method for preparing a polymer composition by polymerizing a monomer mixture comprising a macro monomer and a vinyl radical polymerizable monomer in a base oil,
[0081] A method for preparing a polymer composition described in any one of [1] to
[21] , wherein the above macromonomer is a macromonomer polymerized in a base oil.
[0082]
[26]
[0083] A method for preparing a polymer composition described in
[25] using an α-methylstyrene dimer as a chain transfer agent.
[0084]
[27]
[0085] A method for producing a macromonomer by polymerizing a monomer mixture containing a vinyl radical polymerizable monomer using a cobalt chain transfer agent in a base oil.
[0086]
[28]
[0087]
[20] or
[21] The above polymer composition and a lubricating oil composition comprising a base oil. Effects of the invention
[0088] According to the present invention, a polymer composition, a lubricant additive, a viscosity index improver, and a lubricant composition with a high viscosity index improvement effect can be provided.
[0089] In addition, according to the method for manufacturing a polymer composition of the present invention, a polymer composition with a high viscosity index improvement effect can be manufactured.
[0090] In addition, according to the method for manufacturing a macro monomer of the present invention, a macro monomer capable of producing a polymer composition with a high viscosity index improvement effect can be manufactured. Brief explanation of the drawing
[0091] Figure 1 is a differential molecular weight distribution curve of the polymer composition of the present invention prepared in Example 2. Specific details for implementing the invention
[0092] The polymer composition of the present invention satisfies the following Equation 1 for the differential distribution value in the differential molecular weight distribution curve of the polymer composition measured by gel permeation chromatography (GPC).
[0093] dMp30 / dMp≥0.65 ···1
[0094] ·dMp30: Differential distribution value of molecular weight corresponding to 30% of the peak top molecular weight measured by gel permeation chromatography.
[0095] ·dMp: Differential distribution value of peak-top molecular weight measured by GPC.
[0096] The polymer composition of the present invention is a mixture of polymers with different structures, such as low molecular weight diblock copolymers or high molecular weight graft copolymers, and the fine molecular weight distribution curve has a broad distribution and has multiple peaks or shoulders. By satisfying Formula 1 above, the polymer composition of the present invention indicates the presence of a graft copolymer that contributes to the improvement of the viscosity index. In terms of the improvement of the viscosity index, the dMp30 / dMp is more preferably 0.70 or higher, and even more preferably 0.75 or higher. More specifically, the dMp30 / dMp is preferably 0.70 or higher and 2.0 or lower, more preferably 0.75 or higher and 1.5 or lower, and even more preferably 0.80 or higher and 1.0 or lower.
[0097] The polymer composition of the present invention has a scattering vector magnitude q of small-angle X-ray scattering at 25°C of a 35 wt% base oil solution of the polymer composition, which is 0.07 nm -1 2nm or more -1 In the following range, the maximum value of scattering intensity after standardization is 40cm -1 That is all. More specifically, the maximum value of the scattering intensity after the above standardization is 40 cm -1 Over 1100cm -1 The following is more preferable, and 60cm -1 Over 500cm -1 The following is more preferable, and 80cm -1 Over 450cm -1 The following is more desirable.
[0098] The magnitude q of the scattering vector of the above small-angle X-ray scattering is the reciprocal of the interparticle distance in the base oil solution, and while the scattering intensity represents the degree of particulate matter, the polymer composition of the present invention has a maximum scattering intensity of 40 cm after normalization. -1 If the above, the polymer exists dispersed in a fine particle structure in the base oil at 25°C, and the increase in viscosity of the base oil at low temperatures can be suppressed.
[0099] In addition, the above base oil is an API (American Petroleum Institute) standard Group III or Group III Plus base oil. The Group III base oil is a mineral oil with a viscosity index (VI) ≥ 120, saturated hydrocarbon content (Vol.%) ≥ 90, and sulfur content (MASS%) ≤ 0.03, and the Group III Plus base oil is a mineral oil with a viscosity index (VI) ≥ 135, saturated hydrocarbon content (Vol.%) ≥ 90, and sulfur content (MASS%) ≤ 0.03.
[0100] In addition, the polymer composition of the present invention has a scattering vector magnitude q=0.1nm of small-angle X-ray scattering at 100°C of a base oil solution of 35 wt% of the polymer composition. -1 The scattering intensity after standardization in is 1cm -1 It is desirable to be at least 1.5cm -1 More than 10.0cm -1 It is more desirable to be less than 2cm -1 Over 9.0cm -1 It is more desirable that it be less than or equal to 1 cm. After the above standardization, the scattering intensity is 1 cm -1 As a result, even at 100°C, the polymer is not completely dissolved in the base oil and a partially shrunken structure remains, and thus, even under high temperature (150°C) and high shear conditions, the viscosity is easily improved.
[0101] In addition, the mass average molecular weight of the polymer composition measured by GPC is preferably 50,000 or more and 2,000,000 or less, more preferably 100,000 or more and 150,000 or less, and even more preferably 150,000 or more and 100,000 or less, in order to ensure good solubility and viscosity index with respect to base oil.
[0102] In addition, the molecular weight distribution of the polymer composition measured by GPC is preferably 5 or more and 20 or less, more preferably 6 or more and 18 or less, and even more preferably 7 or more and 15 or less, in order to ensure good solubility and viscosity index with respect to base oil.
[0103] In addition, the above molecular weight distribution is a value calculated as mass average molecular weight (Mw) / number average molecular weight (Mn).
[0104] In addition, the polymer composition of the present invention preferably comprises (meth)acrylic copolymer A.
[0105] The above (meth)acrylic copolymer A means a copolymer in which at least a portion of the constituent units are derived from (meth)acrylic monomers. (meth)acrylic copolymer A may further include constituent units derived from monomers other than (meth)acrylic monomers (e.g., styrene).
[0106] As the above (meth)acrylic monomer, for example, (meth)acrylates containing a carboxyl group such as (meth)acrylic acid, succinic acid 2-(meth)acryloyloxyethyl, maleic acid 2-(meth)acryloyloxyethyl, phthalic acid 2-(meth)acryloyloxyethyl, hexahydrophthalic acid 2-(meth)acryloyloxyethyl; Methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, i-propyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, s-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl methacrylate, n-heptyl methacrylate, n-octyl methacrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-undecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, isoamyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, (Meth)acrylates having an alkyl group, such as behenyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, i-nonyl (meth)acrylate, i-decyl (meth)acrylate, 3-i-propylheptyl (meth)acrylate, i-undecyl (meth)acrylate, 2-t-butylheptyl (meth)acrylate, i-dodecyl (meth)acrylate, i-tridecyl (meth)acrylate, i-tetradecyl (meth)acrylate; (Meth)acrylates having hydroxyl groups, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, glycerin mono(meth)acrylate, ethylene glycol mono(meth)acrylate, propylene glycol mono(meth)acrylate);Methacrylates having a cyclic alkyl group, such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenoxyethyl (meth)acrylate, dicyclofentanyl (meth)acrylate, adamantyl (meth)acrylate, etc.; (Meth)acrylates having an aromatic ring structure such as phenyl(meth)acrylate, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, phenoxydiethylene glycol(meth)acrylate, phenoxypolyethylene glycol(meth)acrylate, nonylphenoxypolyethylene glycol(meth)acrylate, phenoxypolypropylene glycol(meth)acrylate, phenylphenyl(meth)acrylate, phenylphenoxyethyl(meth)acrylate, phenoxybenzyl(meth)acrylate, phenylbenzyl(meth)acrylate, naphthyl(meth)acrylate, (1-naphthyl)methyl(meth)acrylate; (meth)acrylates having a heterocyclic ring structure such as tetrahydrofurfuryl(meth)acrylate, glycidyl(meth)acrylate, (meth)acryloylmorpholine; Examples include alkoxyalkyl (meth)acrylates such as methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, butoxyethyl (meth)acrylate, 2-ethylhexyl diethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate; and 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 2-(meth)acryloyloxyethyl acid phosphate, trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and (meth)acrylamide. Two or more of these may be used in combination.
[0107] In addition, the above (meth)acrylic copolymer A is preferably a copolymer comprising a constituent unit derived from alkyl methacrylate a1 having 5 to 14 carbon atoms of an alkyl group, a constituent unit derived from alkyl acrylate a2 having 5 to 14 carbon atoms of an alkyl group, and a constituent unit derived from alkyl acrylate a3 having 1 to 4 carbon atoms of an alkyl group.
[0108] As the above alkyl methacrylate a1, for example, a methacrylate having a straight-chain alkyl group such as n-pentyl methacrylate, n-hexyl methacrylate, n-heptyl methacrylate, n-octyl methacrylate, n-nonyl methacrylate, n-decyl methacrylate, n-undecyl methacrylate, n-dodecyl methacrylate, n-tridecyl methacrylate, n-tetradecyl methacrylate; Examples include methacrylates having branched alkyl groups such as isoamyl methacrylate, 2-ethylhexyl methacrylate, i-nonyl methacrylate, i-decyl methacrylate, 3-i-propylheptyl methacrylate, i-undecyl methacrylate, 2-t-butylheptyl methacrylate, i-dodecyl methacrylate, i-tridecyl methacrylate, and i-tetradecyl methacrylate; and methacrylates having cyclic alkyl groups such as cyclopentyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, dicyclopentenyl methacrylate, dicyclopentenoxyethyl methacrylate, dicyclofentanyl methacrylate, and adamantyl methacrylate. Two or more of these may be used in combination.
[0109] In addition, a straight-chain or branched alkyl methacrylate having 8 to 14 carbon atoms is preferred in that it has an excellent effect of improving the viscosity index, a straight-chain or branched alkyl methacrylate having 10 to 14 carbon atoms is more preferred, and a straight-chain or branched alkyl methacrylate having 12 to 14 carbon atoms is even more preferred.
[0110] In addition, with respect to the solubility and viscosity index with respect to the base oil being good, the constituent unit derived from the alkyl methacrylate a1 is preferably 1 mass% or more and 50 mass% or less with respect to the total mass of the (meth)acrylic copolymer A, more preferably 5 mass% or more and 45 mass% or less, and even more preferably 10 mass% or more and 40 mass% or less.
[0111] In addition, in this specification, the content of a constituent unit can be calculated from the input amount of the monomer constituting each constituent unit.
[0112] As the above alkyl acrylate a2, for example, an acrylate having a straight-chain alkyl group such as n-pentyl acrylate, n-hexyl acrylate, n-heptyl acrylate, n-octyl acrylate, n-nonyl acrylate, n-decyl acrylate, n-undecyl acrylate, n-dodecyl acrylate, n-tridecyl acrylate, n-tetradecyl acrylate; an acrylate having a branched alkyl group such as i-amyl acrylate, 2-ethylhexyl acrylate, i-nonyl acrylate, i-decyl acrylate, 3-i-propylheptyl acrylate, i-undecyl acrylate, 2-t-butylheptyl acrylate, i-dodecyl acrylate, i-tridecyl acrylate, i-tetradecyl acrylate; Examples include acrylates having cyclic alkyl groups, such as cyclopentyl acrylate, cyclohexyl acrylate, isobornyl acrylate, dicyclopentenyl acrylate, dicyclopentenoxyethyl acrylate, dicyclopentanyl acrylate, and adamantyl acrylate. Two or more of these may be used in combination.
[0113] In addition, a straight-chain or branched alkyl acrylate having 8 to 14 carbon atoms is preferred in that it has an excellent effect of improving the viscosity index, a straight-chain or branched alkyl acrylate having 10 to 14 carbon atoms is more preferred, and a straight-chain or branched alkyl acrylate having 12 to 14 carbon atoms is even more preferred.
[0114] In addition, with respect to the solubility and viscosity index with respect to the base oil being good, the constituent unit derived from the alkyl acrylate a2 is preferably 1 mass% or more and 50 mass% or less with respect to the total mass of the (meth)acrylic copolymer A, more preferably 5 mass% or more and 45 mass% or less, and even more preferably 10 mass% or more and 40 mass% or less.
[0115] Examples of the above alkyl acrylate a3 include acrylates having straight-chain alkyl groups such as methyl acrylate, ethyl acrylate, n-propyl acrylate, and n-butyl acrylate; and acrylates having branched alkyl groups such as i-propyl acrylate, i-butyl acrylate, t-butyl acrylate, and s-butyl acrylate. Two or more of these may be used in combination.
[0116] In addition, alkyl acrylates having 2 to 4 carbon atoms are preferred in that they have an excellent effect of improving the viscosity index, alkyl acrylates having 3 to 4 carbon atoms are more preferred, and alkyl acrylates having 4 carbon atoms are even more preferred.
[0117] In addition, in order to ensure good solubility and viscosity index with respect to base oil, the constituent unit derived from the alkyl acrylate a3 is preferably 30 mass% or more and 80 mass% or less with respect to the total mass of the (meth)acrylic copolymer A, more preferably 35 mass% or more and 75 mass% or less, and even more preferably 40 mass% or more and 70 mass% or less.
[0118] In addition, the above (meth)acrylic copolymer A may include constituent units derived from alkoxyalkyl (meth)acrylate a4 in addition to the above alkyl methacrylate a1, the above alkyl acrylate a2, and the above alkyl acrylate a3 in order to adjust solubility or viscosity index with respect to base oil.
[0119] Examples of the above alkoxyalkyl (meth)acrylate a4 include methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, butoxyethyl (meth)acrylate, 2-ethylhexyl diethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, etc. Two or more of these may be used in combination.
[0120] In addition, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, and butoxyethyl (meth)acrylate are preferred in that they have an excellent effect of improving the viscosity index, methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate are more preferred, and methoxyethyl (meth)acrylate is even more preferred.
[0121] In addition, with respect to the solubility and viscosity index with respect to the base oil being good, the constituent unit derived from the alkoxyalkyl (meth)acrylate a4 is preferably 1 mass% or more and 30 mass% or less with respect to the total mass of the (meth)acrylic copolymer A, more preferably 3 mass% or more and 25 mass% or less, and even more preferably 5 mass% or more and 20 mass% or less.
[0122] In addition, the above (meth)acrylic copolymer A may include constituent units derived from other vinyl radical polymerizable monomers in addition to the above alkyl methacrylate a1, the above alkyl acrylate a2, the above alkyl acrylate a3, and the above alkoxyalkyl (meth)acrylate a4 in order to adjust solubility or viscosity index with respect to base oil.
[0123] Other vinyl radical polymerizable monomers include vinyl compounds such as styrene or vinyl acetate; (meth)acrylates containing a carboxyl group such as (meth)acrylic acid, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl maleate, 2-(meth)acryloyloxyethyl phthalate, and 2-(meth)acryloyloxyethyl hexahydrophthalate; and alkyl methacrylates having 1 to 4 carbon atoms such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, i-propyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, and s-butyl methacrylate. Alkyl (meth)acrylates having 15 or more carbon atoms in an alkyl group, such as cetyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; (meth)acrylates having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, glycerin mono(meth)acrylate, ethylene glycol mono(meth)acrylate, and propylene glycol mono(meth)acrylate; (Meth)acrylates having an aromatic ring structure such as phenyl(meth)acrylate, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, phenoxydiethylene glycol(meth)acrylate, phenoxypolyethylene glycol(meth)acrylate, nonylphenoxypolyethylene glycol(meth)acrylate, phenoxypolypropylene glycol(meth)acrylate, phenylphenyl(meth)acrylate, phenylphenoxyethyl(meth)acrylate, phenoxybenzyl(meth)acrylate, phenylbenzyl(meth)acrylate, naphthyl(meth)acrylate, (1-naphthyl)methyl(meth)acrylate; (meth)acrylates having a heterocyclic ring structure such as tetrahydrofurfuryl(meth)acrylate, glycidyl(meth)acrylate, (meth)acryloylmorpholine;;Examples include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 2-(meth)acryloyloxyethyl acid phosphate, trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, (meth)acrylamide, etc. Two or more of these may be used in combination.
[0124] The above (meth)acrylic copolymer A may be a block copolymer, a random copolymer, or a graft copolymer. Among these, it is preferable to be a graft copolymer, as the viscosity index can be improved by including multiple constituent units with different solubility in base oil. The above graft copolymer preferably includes a constituent unit derived from a vinyl radical polymerizable monomer m1 and a constituent unit derived from a macromonomer M other than m1. In addition, two or more types of macromonomer M may be used in combination. It is preferable to include a constituent unit derived from macromonomer M as a branch component of the above graft copolymer. It is preferable to include a constituent unit derived from the monomer m1 described below as a stem component of the above graft copolymer.
[0125] Examples of the above monomer m1 include styrene, vinyl acetate, (meth)acrylate compounds, etc. Examples of (meth)acrylate compounds include the above alkyl methacrylate a1, the above alkyl acrylate a2, and the above alkyl acrylate a3.
[0126] Other (meth)acrylate compounds include, for example, (meth)acrylates containing a carboxyl group such as (meth)acrylic acid, succinic acid 2-(meth)acryloyloxyethyl, maleic acid 2-(meth)acryloyloxyethyl, phthalic acid 2-(meth)acryloyloxyethyl, hexahydrophthalic acid 2-(meth)acryloyloxyethyl; and alkyl methacrylates having 1 to 4 carbon atoms, such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, i-propyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, and s-butyl methacrylate. Alkyl (meth)acrylates having 15 or more carbon atoms in an alkyl group, such as cetyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; (meth)acrylates having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, glycerin mono(meth)acrylate, ethylene glycol mono(meth)acrylate, and propylene glycol mono(meth)acrylate; (Meth)acrylates having an aromatic ring structure such as phenyl(meth)acrylate, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, phenoxydiethylene glycol(meth)acrylate, phenoxypolyethylene glycol(meth)acrylate, nonylphenoxypolyethylene glycol(meth)acrylate, phenoxypolypropylene glycol(meth)acrylate, phenylphenyl(meth)acrylate, phenylphenoxyethyl(meth)acrylate, phenoxybenzyl(meth)acrylate, phenylbenzyl(meth)acrylate, naphthyl(meth)acrylate, (1-naphthyl)methyl(meth)acrylate; (meth)acrylates having a heterocyclic ring structure such as tetrahydrofurfuryl(meth)acrylate, glycidyl(meth)acrylate, (meth)acryloylmorpholine; Alkoxy(meth)acrylates such as methoxyethyl(meth)acrylate, ethoxyethyl(meth)acrylate, butoxyethyl(meth)acrylate, etc.;Examples include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 2-(meth)acryloyloxyethyl acid phosphate, trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, (meth)acrylamide, etc. Two or more of these may be used in combination.
[0127] In addition, the alkyl methacrylate a1, the alkyl acrylate a2, and the alkyl acrylate a3 may be included in either one of the monomer m1 and the macromonomer M, or in both; however, in terms of ease of adjusting solubility in base oil, it is preferable that the vinyl radical polymerizable monomer m1 is the alkyl acrylate a2 and the alkyl acrylate a3.
[0128] In addition, the above macromonomer M is not particularly limited as long as it is a polymer having a radical polymerizable group, but from the degree of design regarding solubility in base oil, it is preferable that it be a compound having a radical polymerizable group at the terminal end and containing two or more constituent units derived from monomer m2 having a vinyl radical polymerizable group. As the above monomer m2, examples include the same vinyl radical polymerizable monomer listed as monomer m1. It is preferable that the above monomer m2 includes an alkyl methacrylate having 5 or more carbon atoms in the alkyl group for excellent viscosity index improvement effect, and it is even more preferable that it includes the above alkyl methacrylate a1 for excellent solubility in base oil.
[0129] In addition, the above macromonomer M is preferably of the structure represented by the following Formula 2 in terms of radical polymerization compatibility with the above monomer m1.
[0130]
[0131] (during food, X 1To X n-1 Each represents a hydrogen atom, a methyl group, or a CH2OH independently. 1 to Y n It is a substituent that binds to the vinyl group of the (m2) component, which is a monomer constituent unit, for example, OR 1 , halogen atom, COR 2 , COOR 3 , CN, CONR 4 R 5 , NHCOR 6 , or R 7 Represents, and R 1 to R 7 Each represents independently a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group, a cyclic ether group, a heteroaryl group, etc. Z represents a terminal group, and n represents an integer from 2 to 10000. In addition, Z of the terminal group may include a hydrogen atom and a group derived from a radical polymerization initiator, similar to the terminal groups of polymers obtained by known radical polymerization.
[0132] In terms of having good solubility and viscosity index with respect to base oil, the number average molecular weight of the macro monomer M measured by gel permeation chromatography is preferably 500 to 30000, more preferably 1000 to 25000, and particularly preferably 2000 to 20000.
[0133] The above macromonomer M may be used as prepared by a known method or as a commercially available one. Examples of methods for preparing the above macromonomer M include, for instance, a method of preparing it using a cobalt chain transfer agent (U.S. Patent No. 4680352), a method of using an α-substituted unsaturated compound such as α-bromomethylstyrene as a chain transfer agent (International Publication No. 88 / 04304), a method of chemically bonding a polymerizable group (Japanese Patent Publication No. Sho 60-133007 and U.S. Patent No. 5147952), and a method by pyrolysis (Japanese Patent Publication No. Hei 11-240854).
[0134] A method using a cobalt chain transfer agent is preferable in that it involves fewer manufacturing process steps and utilizes a catalyst with a high chain transfer constant. Since the cobalt chain transfer agent has a high chain transfer constant, macromonomers with controlled molecular weight can be obtained with the addition of a small amount.
[0135] As a cobalt chain transfer agent, a known cobalt complex may be used. The amount of the cobalt chain transfer agent is preferably 0.00001 to 0.1 parts by mass per 100 parts by mass of vinyl radical polymerizable monomer m2, more preferably 0.00005 to 0.05 parts by mass, and particularly preferably 0.0001 to 0.02 parts by mass.
[0136] The polymer composition of the present invention preferably has a total light transmittance of 85 to 95% when measured by the method described below in the examples, 88 to 93% is more preferable, and 90 to 93% is more preferable.
[0137] The polymer composition of the present invention, when measured by the method described below in the examples, has a viscosity index (VI) calculated by the method of JIS-K2283-1993 that is preferably 200 to 300, more preferably 205 to 300, and even more preferably 210 to 300.
[0138] Method for preparing a polymer composition
[0139] Next, an example of a method for preparing a polymer composition of the present invention is presented.
[0140] The polymer composition of the present invention can be prepared by polymerizing a monomer mixture comprising a macro monomer and a vinyl radical polymerizable monomer other than the macro monomer in a base oil using a known method.
[0141] Other examples of methods for preparing polymer compositions of the present invention are shown below.
[0142] The polymer composition of the present invention can be prepared by polymerizing a monomer mixture comprising the alkyl methacrylate a1, the alkyl acrylate a2, and the alkyl acrylate a3 in a base oil using a known method.
[0143] Examples of the above base oils include mineral base oils refined from crude oil or synthetic oils chemically synthesized. Examples of commercially available base oils include API standard Group III base oils such as SK Rublicant’s YUBASE3, and API standard Group III plus base oils such as SK Rublicant’s YUBASE4.
[0144] In addition, the monomer mixture may also contain a macromonomer M. The macromonomer M is preferably a macromonomer obtained by polymerizing a monomer mixture containing a vinyl radical polymerizable monomer using a cobalt chain transfer agent in the base oil. Since the cobalt chain transfer agent has a high chain transfer constant, a macromonomer with a controlled molecular weight can be obtained by adding a small amount. In addition, the macromonomer preferably contains the alkyl methacrylate α1 as a constituent unit.
[0145] As the above vinyl radical polymerizable monomer, the above polymerizable monomer m1 may be cited, and it is preferable to include the above alkyl acrylate a2 and the above alkyl acrylate a3.
[0146] In the present invention, by polymerizing a monomer mixture comprising the above macromonomer and a vinyl radical polymerizable monomer other than the above macromonomer, a polymer composition of the present invention is obtained, which is a mixture of polymers with different structures, such as a diblock copolymer or a graft copolymer.
[0147] In addition, polymerization can be carried out under known conditions, but it is preferable to use α-methylstyrene dimer as a chain transfer agent because it has a particularly excellent effect in suppressing heat during polymerization.
[0148] Lubricant Additives
[0149] The polymer composition comprising the (meth)acrylic copolymer A of the present invention can be used as a lubricant additive to be added to lubricants such as engine oil, gear oil, and hydraulic fluid used in mobility, such as industrial machinery, robots, and automobiles.
[0150] As base oils such as engine oil, gear oil, and hydraulic oil mentioned above, examples include mineral-based base oils refined from crude oil or chemically synthesized synthetic oils. Examples of commercially available base oils include API standard Group III base oils such as SK Rublicant’s YUBASE3, and API standard Group III Plus base oils such as SK Rublicant’s YUBASE4.
[0151] Examples of lubricant additives include, for instance, antioxidants, viscosity index improvers, pour point depressants, detergent dispersants, corrosion inhibitors, rust inhibitors, extreme pressure agents, lubricity improvers, defoaming agents, emulsifiers, anti-wear agents, friction modifiers, antifungal agents, anti-emulsifiers, etc.
[0152] Viscosity Index Improver
[0153] In addition, the polymer composition of the present invention can be used as a viscosity index improver for the lubricating oil.
[0154] For viscosity index improvers, it is preferable that the degree of increase in kinematic viscosity upon addition is greater at high temperatures and smaller at low temperatures. Generally, it is known that viscosity index improvers containing (meth)acrylate-based polymers do not completely dissolve at low temperatures and form a fine particle structure, and as solubility improves with increasing temperature, the polymer chains widen and exhibit the aforementioned functions. As an indicator of the performance of a viscosity index improver, a viscosity index calculated from kinematic viscosity at low temperatures (e.g., 40°C) and high temperatures (e.g., 100°C) is used.
[0155] The viscosity index is a value measured by the method of JIS-K2283-1993, and the higher the value, the smaller the change in viscosity due to temperature. In addition, in recent years, high values for viscosity index improvers are required for viscosity at high temperatures (150°C) and high shear conditions (HTHS 150°C viscosity). Therefore, it is desirable that the viscosity improver does not completely dissolve at 100°C and is expected to have a viscosity improvement effect even at higher temperatures. The dissolution state at 100°C can be evaluated, for example, by small-angle X-ray scattering (SAXS).
[0156] Lubricating Oil Composition
[0157] A lubricating oil composition comprising the polymer composition of the present invention may contain various additives in addition to the polymer composition of the present invention. Other additives may include antioxidants, viscosity index improvers, pour point depressants, detergent dispersants, corrosion inhibitors, rust inhibitors, extreme pressure agents, oiliness improvers, defoaming agents, emulsifiers, anti-wear agents, friction modifiers, antifungal agents, anti-emulsifiers, etc.
[0158] The content of the polymer composition of the present invention included in the above lubricating oil composition is preferably 0.01 to 30 mass% when the total mass of the lubricating oil composition is 100 mass%, more preferably 0.05 to 25 mass%, and most preferably 0.1 to 20 mass%. By making the content of the polymer composition 0.01 mass% or more, the viscosity index of the lubricating oil composition is improved, and by making it 30 mass% or less, the kinematic viscosity of the lubricating oil composition at low temperatures is suppressed, thereby improving fuel efficiency.
[0159] Examples
[0160] The present invention will be explained in more detail below through examples and comparative examples. Additionally, "parts" in the examples represent "parts by mass." Evaluations were measured by the following methods.
[0161] <Molecular weight of polymer composition>
[0162] Measurements were performed using gel permeation chromatography (GPC) (HLC-8320 manufactured by Toso Co., Ltd.). After preparing 0.2 mass% of the tetrahydrofuran solution of the polymer composition, 10 μl of the solution was injected into a device equipped with two columns manufactured by Toso Co., Ltd. (TSKgelSuperHZM-H, inner diameter 6.0 mm, length 15 cm) and a TSKguardcolumn SuperHZ-H (inner diameter 4.6 mm, length 3.5 cm). Measurements were performed under conditions of a flow rate of 0.5 ml / min, eluent: tetrahydrofuran (stabilizer BHT), and column temperature: 40°C, and the mass average molecular weight (Mw), number average molecular weight (Mn), and peak top molecular weight (Mp) were calculated by converting to standard polystyrene.
[0163] <Molecular weight of macromonomer M>
[0164] Measurements were performed using gel permeation chromatography (GPC) (HLC-8320 manufactured by Toso Co., Ltd.). After preparing 0.2 mass% of a tetrahydrofuran solution of macromonomer M, 10 μl of the solution was injected into a device equipped with columns manufactured by Toso Co., Ltd. (TSKgel SuperHZM-M (inner diameter 4.6 mm, length 15 cm), HZM-M (inner diameter 4.6 mm, length 15 cm), HZ-2000 (inner diameter 4.6 mm, length 15 cm), TSKguardcolumn SuperHZ-L (inner diameter 4.6 mm, length 3.5 cm). Measurements were performed under conditions of flow rate: 0.35 ml / min, eluent: tetrahydrofuran (stabilizer BHT), and column temperature: 40°C, and the mass average molecular weight (Mw) and number average molecular weight (Mn) were calculated by standard polystyrene conversion.
[0165] Small-angle X-ray scattering measurement (SAXS)
[0166] A base oil solution containing 35 mass% of the polymer composition obtained in the example was placed in a 2 mmφ quartz capillary, and small-angle X-ray scattering measurements were performed at measurement temperatures of 25°C and 100°C.
[0167] Small-angle X-ray scattering measurements were performed using the SAXSpoint 2.0 system manufactured by AntonPaar. For the small-angle X-ray scattering measurement conditions, Cu Kα (wavelength 1.54 Å) X-rays were used, the exposure time was set to 30 min (10 min × 3 times), the measurement environment was set to vacuum, and the camera length was set to 570 mm.
[0168] A one-dimensional scattering profile was obtained by irradiating a capillary sample of a base oil solution of a (meth)acrylic copolymer with X-rays. In addition, the same measurement as above was performed on a 2 mmφ quartz capillary containing only base oil for background correction.
[0169] Background correction is performed on the one-dimensional scattering profile obtained from the above procedure. Specifically, the one-dimensional scattering profile of the base oil alone is obtained by subtracting the one-dimensional scattering profile of each sample with transmittance correction, thereby obtaining the one-dimensional scattering profile after background correction.
[0170] Next, absolute scattering intensity correction of the one-dimensional scattering profile was performed in accordance with Journal of Physics: Conference Series 247 (2010) 012005. Specifically, as a sample for absolute scattering intensity correction, small-angle X-ray scattering measurements were performed without placing glass carbon in a capillary tube under the same analysis conditions as above to obtain the one-dimensional scattering profile of glass carbon. Next, the one-dimensional scattering profile of glass carbon after background correction was obtained by subtracting the one-dimensional scattering profile without a sample from the one-dimensional scattering profile of glass carbon after transmittance correction. The one-dimensional scattering profile of glass carbon after background correction was divided by thickness (cm) and exposure time (S) to acquire the scattering profile ST per unit thickness and unit time.
[0171] Next, prepare the differential scattering cross-section of glassy carbon disclosed by the National Institute of Standards and Technology (NIST), and this is 0.1 nm -1 ≤q≤1nm -1 For each q in the range, the scattering profile ST is divided to obtain the coefficient value for each q. The average value of these coefficient values is used as the scale factor for calculating the differential scattering cross-section. Next, the one-dimensional scattering profile of the base oil solution of each polymer composition after background correction is corrected to the scattering intensity per unit thickness and unit time by dividing it by the capillary diameter (cm) and exposure time (s), and the scattering intensity after normalization (differential scattering cross-section (cm²)) is obtained by multiplying it by the scale factor obtained by the above method. -1 A scattering profile was obtained after )) and normalization.
[0172] <Viscosity Index (VI)>
[0173] Evaluation was performed using a fully automatic simple kinematic viscometer (manufactured by Cannon, product name: Simple-VIS type) in accordance with ASTM D7279 (D445) method. The kinematic viscosity (Vk100) at 100°C of the polymer composition obtained in this example was 6.5 mm 2 The concentration was adjusted with YUBASE4 to be / s, and the kinematic viscosity (Vk40) at 40°C of the polymer composition with adjusted concentration was also measured.
[0174] Using the obtained “Vk100” and “Vk40”, the viscosity index (VI) was calculated according to the method of JIS-K2283-1993.
[0175] <Solubility in base oils>
[0176] A base oil solution containing 35 mass% of the polymer obtained in this example was placed between two 1 mm thick sheets of glass using a 2 mm thick silicone rubber as a gasket, and the total light transmittance was measured using a haze meter (product name: HM-150 type, manufactured by Murakami Shikisai Kijutsu Genkyujo).
[0177] [Preparation Example 1]
[0178] (Synthesis of Co complex (cobalt chain transfer agent))
[0179] In a synthesis apparatus equipped with a stirring device, 2.00 g (8.03 mmol) of cobalt(II) acetate tetrahydrate (Wako Junyakus, Wako Special Grade) and 3.86 g (16.1 mmol) of diphenylglyoxime (Tokyo Kasei, EP Grade) and 100 ml of diethyl ether, which had been deoxygenated by nitrogen bubbling beforehand, were added under a nitrogen atmosphere and stirred at 25°C for 2 hours.
[0180] Next, 20 ml of trifluoroboron diethyl ether complex (manufactured by Tokyo Kasei Co., Ltd., EP grade) was added and stirred for 6 hours. The resulting mixture was filtered, the solid was washed with diethyl ether, and dried at 20°C for 12 hours at a pressure of 100 MPa or less to obtain 5.02 g (7.93 mmol, yield 99 mass%) of a dark brown solid Co complex (1).
[0181] [Preparation Example 2]
[0182] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 50 parts of YUBASE4, 50 parts of acrylic ester SL (manufactured by Mitsubishi Chemical, trade name: Acrylic ester SL, a mixture of an alkyl methacrylate having 12 carbon atoms in the alkyl group and an alkyl methacrylate having 13 carbon atoms in the alkyl group), and 0.0015 parts of the Co complex prepared in Preparation Example 1 were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. After raising the liquid temperature to 85°C, a mixture containing acrylic ester SL (50 parts) and 0.5 parts of 1,1,3,3-tetramethylbutylperoxy2-ethylhexanoate (manufactured by Nichiyu, trade name: Perocta O), a polymerization initiator, was added dropwise over a period of 4 hours. In addition, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (35 parts) and perocta O (0.4 parts) was added, and the temperature was raised to 95°C. After maintaining the liquid temperature at 95°C for 4 hours, it was cooled to obtain a YUBASE4 solution containing 54 mass% of macromonomer M1. The GPC results of the obtained macromonomer are shown in Table 1.
[0183] [Preparation Examples 3 to 5]
[0184] Macromonomers M2 to M4 were obtained in the same manner as in Preparation Example 2, except that the amount of Co complex was changed as shown in Table 1. The results of GPC are shown in Table 1.
[0185] [Preparation Example 6]
[0186] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 40 parts of YUBASE4, 98 parts of acrylic ester SL, 2 parts of methyl methacrylate (manufactured by Mitsubishi Chemical, trade name: Acrylic Ester M), 0.003 parts of the Co complex prepared in Preparation Example 1, and 0.1 parts of t-butylperoxy-2-ethylhexanoate (manufactured by Nichiyu, trade name: Perbutyl O) as a polymerization initiator were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 90°C and maintained at 90°C for 2.5 hours. Subsequently, a mixture containing YUBASE4 (20 parts) and Perbutyl O (0.7 parts) was added dropwise over 1 hour, and the liquid temperature was raised to 105°C. After maintaining at 105°C for 1 hour, YUBASE4 (30 parts) was added and cooled to obtain a YUBASE4 solution containing 52.6 mass% of macromonomer M5. The GPC results of the obtained macromonomer are shown in Table 1.
[0187] [Preparation Example 7]
[0188] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 60 parts of YUBASE4, 98 parts of acrylic ester SL, 2 parts of methyl methacrylate, 0.005 parts of the Co complex prepared in Preparation Example 1, and 0.1 parts of t-amylperoxy2-ethylhexanoate (manufactured by Arkma Yoshitomi Co., Ltd., trade name Luperox 575) as a polymerization initiator were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 90°C and maintained at 90°C for 2.5 hours. Subsequently, a mixture containing YUBASE4 (10 parts) and perbutyl O (0.7 parts) was added dropwise over 1 hour, and the liquid temperature was raised to 105°C. After maintaining at 105°C for 1 hour, YUBASE4 (20 parts) was added and cooled to obtain a YUBASE4 solution containing 52.6 mass% of macromonomer M6. The results of the GPC of the obtained macromonomer are shown in Table 1.
[0189] <Example 1>
[0190] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 78.7 parts of YUBASE4, 25 parts of acrylic ester SL, 52 parts of n-butyl acrylate (manufactured by Mitsubishi Chemical, trade name: nBA), 23 parts of lauryl acrylate (manufactured by Osaka Yuki Chemical, trade name: LA), 0.03 parts of t-butylperoxy-2-ethylhexanoate (manufactured by Nichiyu, trade name: Perbutyl O) as a polymerization initiator, and 0.03 parts of α-methylstyrene dimer (manufactured by Nichiyu, trade name: Nopromer MSD) as a chain transfer agent were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C and maintained at 85°C for 2 hours, after which a mixture of YUBASE4 (40 parts) and perbutyl O (0.015 parts) was added dropwise over 2 hours. Additionally, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (67 parts) and perocta O (0.5 parts) was added, and the temperature was raised to 95°C. After maintaining the liquid temperature at 95°C for 1 hour, the solution was cooled to obtain a solution containing 35 mass% of a (meth)acrylic copolymer. The evaluation results of the obtained polymer composition are shown in Table 2.
[0191] <Example 2>
[0192] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 38.2 parts of YUBASE3, 46.3 parts of a YUBASE4 solution of macromonomer M1 obtained in Preparation Example 2, 52 parts of n-butyl acrylate, 23 parts of lauryl acrylate, 0.015 parts of perbutyl O as a polymerization initiator, and 0.04 parts of nopromer MSD as a chain transfer agent were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C and maintained at 85°C for 2 hours, after which a mixture of YUBASE3 (42 parts) and perbutyl O (0.015 parts) was added dropwise over 2 hours. In addition, after maintaining at 85°C for 1 hour, a mixture containing YUBASE3 (67.5 parts) and Perocta O (0.5 parts) was added, the temperature was raised to 95°C, and the liquid temperature was maintained at 95°C for 1 hour. After adding YUBASE3 (16.7 parts), the solution was cooled to obtain a solution containing 35 mass% of a (meth)acrylic copolymer. The evaluation results of the obtained polymer composition are shown in Table 2.
[0193] <Example 3>
[0194] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 7.6 parts of YUBASE4, 46.3 parts of a YUBASE4 solution of macromonomer M2 obtained in Preparation Example 3, 52 parts of n-butyl acrylate, 23 parts of lauryl acrylate, 0.015 parts of perbutyl O as a polymerization initiator, and 0.03 parts of nopromer MSD as a chain transfer agent were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C and maintained at 85°C for 2 hours, after which a mixture of YUBASE4 (42 parts) and perbutyl O (0.015 parts) was added dropwise over 2 hours. In addition, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (67.5 parts) and perocta O (0.5 parts) was added, the temperature was raised to 95°C, and the liquid temperature was maintained at 95°C for 1 hour. After adding YUBASE4 (46.7 parts), the solution was cooled to obtain a YUBASE4 solution containing 35 mass% of the polymer composition. The evaluation results of each obtained polymer composition are shown in Table 2.
[0195] <Example 7>
[0196] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 12.5 parts of YUBASE4, 37 parts of a YUBASE4 solution of macromonomer M2 obtained in Preparation Example 3, 56 parts of n-butyl acrylate, 24 parts of lauryl acrylate, 0.015 parts of perbutyl O as a polymerization initiator, and 0.04 parts of nopromer MSD as a chain transfer agent were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C and maintained at 85°C for 2 hours, after which a mixture of YUBASE4 (42 parts) and perbutyl O (0.015 parts) was added dropwise over 2 hours. In addition, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (67.5 parts) and Perocta O (0.5 parts) was added, the temperature was raised to 95°C, and the liquid temperature was maintained at 95°C for 1 hour. After adding YUBASE4 (46.7 parts), the solution was cooled to obtain a solution containing 35 mass% of a (meth)acrylic copolymer. The evaluation results of the obtained polymer composition are shown in Table 3.
[0197] <Example 8>
[0198] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 74 parts of a YUBASE4 solution of macromonomer M2 obtained in Preparation Example 3, 42 parts of n-butyl acrylate, 18 parts of lauryl acrylate, 0.015 parts of perbutyl O as a polymerization initiator, and 0.02 parts of nopromer MSD as a chain transfer agent were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C and maintained at 85°C for 2 hours, after which a mixture of YUBASE4 (42 parts) and perbutyl O (0.015 parts) was added dropwise over 2 hours. Additionally, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (67.5 parts) and perocta O (0.5 parts) was added, the temperature was raised to 95°C, and the liquid temperature was maintained at 95°C for 1 hour. After adding YUBASE4 (42.2 parts), the mixture was cooled to obtain a solution containing 35 mass% of a (meth)acrylic copolymer. The evaluation results of the obtained polymer composition are shown in Table 3.
[0199] <Example 13>
[0200] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 40 parts of YUBASE4, 47.6 parts of a YUBASE4 solution of macromonomer M5 obtained in Preparation Example 6, 52 parts of n-butyl acrylate, 23 parts of lauryl acrylate, 0.03 parts of Luperox 575 as a polymerization initiator, and 0.03 parts of Nopromer MSD as a chain transfer agent were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C and maintained at 85°C for 3.5 hours, after which a mixture of YUBASE4 (42 parts) and Luperox 575 (0.015 parts) was added dropwise over 2 hours. In addition, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (20 parts) and Luperox 575 (0.5 parts) was added dropwise over 1 hour, then the liquid temperature was raised to 110°C and maintained at 110°C for 1 hour. After adding YUBASE4 (61.1 parts), the solution was cooled to obtain a YUBASE4 solution containing 35 mass% of the polymer composition. The evaluation results of each obtained polymer composition are shown in Table 4.
[0201] <Example 14>
[0202] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 6.9 parts of YUBASE4, 47.6 parts of a YUBASE4 solution of macromonomer M6 obtained in Preparation Example 7, 52 parts of n-butyl acrylate, 23 parts of lauryl acrylate, 0.015 parts of perbutyl O as a polymerization initiator, and 0.01 parts of nopromer MSD as a chain transfer agent were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C and maintained at 85°C for 2 hours, after which a mixture of YUBASE4 (42 parts) and perbutyl O (0.015 parts) was added dropwise over 2 hours. In addition, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (67.5 parts) and perocta O (0.5 parts) was added, the temperature was raised to 95°C, and the liquid temperature was maintained at 95°C for 1 hour. After adding YUBASE4 (46.7 parts), the solution was cooled to obtain a YUBASE4 solution containing 35 mass% of the polymer composition. The evaluation results of each obtained polymer composition are shown in Table 4.
[0203] <Example 15>
[0204] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 30 parts of YUBASE4 and 47.6 parts of a YUBASE4 solution of macromonomer M6 obtained in Preparation Example 7 were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C, and a mixture containing YUBASE4 (25 parts), n-butyl acrylate (52 parts), lauryl acrylate (23 parts), and Luperox 575 (0.1 parts) as a polymerization initiator was added dropwise over 4 hours. Additionally, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (50 parts) and Luperox 575 (0.5 parts) was added dropwise over 1.5 hours, and the liquid temperature was raised to 110°C. After maintaining at 110°C for 1 hour, YUBASE4 (part 58.1) was added and then cooled to obtain a YUBASE4 solution containing 35 mass% of the polymer composition. The evaluation results of each obtained polymer composition are shown in Table 4.
[0205] <Example 16>
[0206] In a reaction vessel equipped with a stirrer, a cooling tube, and a thermometer, 20 parts of YUBASE4 and 46.3 parts of a YUBASE4 solution of macromonomer M3 obtained in Preparation Example 4 were added, and dissolved oxygen was removed by bubbling nitrogen while stirring. The liquid temperature was raised to 85°C, and a mixture containing YUBASE4 (25 parts), n-butyl acrylate (30 parts), lauryl acrylate (35 parts), 10 parts of 2-methoxyethyl acrylate (manufactured by Osaka Yuki Chemical Co., Ltd., trade name: 2-MTA), and Luperox 575 (0.1 parts) as a polymerization initiator was added dropwise over 4 hours. In addition, after maintaining at 85°C for 1 hour, a mixture containing YUBASE4 (60 parts) and Perox 575 (0.5 parts) was added dropwise over 1.5 hours, and the liquid temperature was raised to 110°C. After maintaining at 110°C for 1 hour, YUBASE4 (59.4 parts) was added and then cooled to obtain a YUBASE4 solution containing 35 mass% of the polymer composition. The evaluation results of each obtained polymer composition are shown in Table 4.
[0207] <Examples 4 to 6, 9 to 12 and Comparative Example 1>
[0208] A polymer composition was obtained in the same manner as in Example 3, except that the type of macro monomer used, the type and amount of monomer, and the amount of α-methylstyrene dimer were changed to the contents of Tables 2 to 5. The evaluation results of each obtained polymer composition are shown in Tables 2 to 5.
[0209] <Examples 17, 18>
[0210] A polymer composition was obtained in the same manner as in Example 16, except that the type of macromonomer used and the type and amount of monomer were changed to the contents of Table 4. The evaluation results of each obtained polymer composition are shown in Table 4.
[0211] <Comparative Examples 2 to 6>
[0212] A polymer composition was obtained in the same manner as in Example 1, except that the type and amount of monomer used and the amount of α-methylstyrene dimer were changed to the contents of Table 5. The evaluation results of each obtained polymer composition are shown in Table 5.
[0213] Comparative Examples 1 to 5 showed a lower viscosity index.
[0214]
[0215]
[0216]
[0217]
[0218]
[0219] The abbreviations in Tables 1 to 5 are as follows.
[0220] · SLMA: A mixture of an alkyl methacrylate having 12 carbon atoms in its alkyl group and an alkyl methacrylate having 13 carbon atoms in its alkyl group (Manufactured by Mitsubishi Chemical, Trade name: Acryester SL)
[0221] ·MMA: Methyl methacrylate (Manufactured by Mitsubishi Chemical, Trade name: Acrylate M)
[0222] · EHA: 2-ethylhexyl acrylate (manufactured by Mitsubishi Chemical, trade name: 2-ethylhexyl acrylic acid)
[0223] ·Co complex: Cobalt chain transfer agent obtained in Preparation Example 1.
[0224] ·α-methylstyrene dimer (Nichiyu, Brand name: Nopromer MSD)
[0225] ·YUBASE3 (API standard Group III base oil, manufactured by SK Rublicant)
[0226] ·YUBASE4 (API standard Group III Plus base oil, manufactured by SK Rublicant)
[0227] · LA: Lauryl Acrylate (Osaka Yuki Kagaku High School Teacher's Product, Product Name: LA)
[0228] ·BA: n-butyl acrylate (manufactured by Mitsubishi Chemical, trade name: butyl acrylate)
[0229] ·EA: Ethyl acrylate (Manufactured by Mitsubishi Chemical, Trade name: Ethyl acrylate)
[0230] · BMA: n-butyl methacrylate (manufactured by Mitsubishi Chemical, trade name: Acrylate B)
[0231] · 2-MTA: 2-Methoxyethyl Acrylate (Manufactured by Osaka Yuki Kagaku High School, Trade Name: 2-MTA) Industrial applicability
[0232] According to the present invention, a polymer composition, a polymer composition, a viscosity index improver, and a lubricant composition with a high viscosity index improvement effect can be provided.
[0233] In addition, according to the method for manufacturing a polymer composition of the present invention, a polymer composition with a high viscosity index improvement effect can be manufactured.
[0234] In addition, according to the method for manufacturing a macro monomer of the present invention, a macro monomer capable of producing a polymer composition with a high viscosity index improvement effect can be manufactured. A polymer composition can be provided.
Claims
Claim 1 A polymer composition, wherein the polymer composition comprises a (meth)acrylic copolymer A, wherein the (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from an alkyl methacrylate a1 having 5 to 14 carbon atoms in an alkyl group, a constituent unit derived from an alkyl acrylate a2 having 5 to 14 carbon atoms in an alkyl group, and a constituent unit derived from an alkyl acrylate a3 having 1 to 4 carbon atoms in an alkyl group, wherein the (meth)acrylic copolymer A is a graft copolymer, wherein the graft copolymer comprises a constituent unit derived from a vinyl radical polymerizable monomer m1 and a constituent unit derived from a macromonomer M other than the vinyl radical polymerizable monomer m1, wherein the differential distribution value in the differential molecular weight distribution curve of the polymer composition measured by gel permeation chromatography satisfies the following Formula 1, and wherein the following base oil solution of 35 wt% of the polymer composition The magnitude q of the scattering vector for small-angle X-ray scattering at 25°C is 0.07 nm -1 2nm or more -1 In the following range, the maximum value of scattering intensity after standardization is 40cm -1 Polymer composition. dMp30 / dMp≥0.65 ···1 ·dMp30: The differential distribution value of the molecular weight corresponding to 30% of the peak-top molecular weight measured by gel permeation chromatography. ·dMp: The differential distribution value of the peak-top molecular weight measured by gel permeation chromatography. ·Base oil: API standard Group III or Group III Plus Claim 2 In claim 1, the magnitude of the scattering vector q=0.1nm of small-angle X-ray scattering at 100°C of a 35wt% base oil solution of the polymer composition of API standard Group III or Group III Plus -1 The scattering intensity after standardization in is 1cm -1 Polymer composition of the above. Claim 3 A polymer composition comprising a (meth)acrylic copolymer A, wherein the (meth)acrylic copolymer A is a graft copolymer, and the graft copolymer comprises a constituent unit derived from a vinyl radical polymerizable monomer m1 and a constituent unit derived from a macro monomer M other than the vinyl radical polymerizable monomer m1, and wherein the (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from an alkyl methacrylate a1 having 5 to 14 carbon atoms in an alkyl group, a constituent unit derived from an alkyl acrylate a2 having 5 to 14 carbon atoms in an alkyl group, and a constituent unit derived from an alkyl acrylate a3 having 1 to 4 carbon atoms in an alkyl group, and wherein the (meth)acrylic copolymer A comprises 1 to 50 mass% of the constituent unit derived from the alkyl methacrylate a1 based on the total mass of the (meth)acrylic copolymer A. Claim 4 A polymer composition according to claim 3, wherein the (meth)acrylic copolymer A comprises 1 to 50 mass% of a constituent unit derived from the alkyl acrylate a2 with respect to the total mass of the (meth)acrylic copolymer A. Claim 5 A polymer composition for a lubricating oil additive containing a (meth)acrylic copolymer A, wherein the (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from alkyl methacrylate a1 having 5 to 14 carbon atoms in an alkyl group, a constituent unit derived from alkyl acrylate a2 having 5 to 14 carbon atoms in an alkyl group, and a constituent unit derived from alkyl acrylate a3 having 1 to 4 carbon atoms in an alkyl group, wherein the (meth)acrylic copolymer A is a graft copolymer, and with respect to the total mass of the (meth)acrylic copolymer A, the composition comprises 1 to 50 mass% of the constituent unit derived from alkyl methacrylate a1, 1 to 50 mass% of the constituent unit derived from alkyl acrylate a2, and 30 to 80 mass% of the constituent unit derived from alkyl acrylate a3 (provided, the alkyl methacrylate a1 The sum of the content of the constituent unit derived from, the content of the constituent unit derived from the alkyl acrylate a2, and the content of the constituent unit derived from the alkyl acrylate a3 does not exceed 100 mass% with respect to the total mass of the (meth)acrylic copolymer A), polymer composition. Claim 6 A polymer composition according to claim 5, wherein the graft copolymer comprises a constituent unit derived from a vinyl radical polymerizable monomer m1 and a constituent unit derived from a macromonomer M other than the vinyl radical polymerizable monomer m1. Claim 7 A polymer composition for a viscosity index improver containing a (meth)acrylic copolymer A, wherein the (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from alkyl methacrylate a1 having 5 to 14 carbon atoms in the alkyl group, a constituent unit derived from alkyl acrylate a2 having 5 to 14 carbon atoms in the alkyl group, and a constituent unit derived from alkyl acrylate a3 having 1 to 4 carbon atoms in the alkyl group, wherein, based on the total mass of the (meth)acrylic copolymer A, the composition comprises 1 to 50 mass% of the constituent unit derived from alkyl methacrylate a1, 1 to 50 mass% of the constituent unit derived from alkyl acrylate a2, and 30 to 80 mass% of the constituent unit derived from alkyl acrylate a3 (provided, the content of the constituent unit derived from alkyl methacrylate a1 and the composition derived from alkyl acrylate a2 The content of the unit, and the sum of the content of the constituent unit derived from the alkyl acrylate a3, does not exceed 100 mass% with respect to the total mass of the (meth)acrylic copolymer A), polymer composition. Claim 8 A polymer composition according to claim 7, wherein the (meth)acrylic copolymer A is a graft copolymer, and the graft copolymer comprises a constituent unit derived from a vinyl radical polymerizable monomer m1 and a constituent unit derived from a macromonomer M other than the vinyl radical polymerizable monomer m1. Claim 9 A polymer composition for a friction modifier containing a (meth)acrylic copolymer A, wherein the (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from alkyl methacrylate a1 having 5 to 14 carbon atoms in the alkyl group, a constituent unit derived from alkyl acrylate a2 having 5 to 14 carbon atoms in the alkyl group, and a constituent unit derived from alkyl acrylate a3 having 1 to 4 carbon atoms in the alkyl group, wherein, based on the total mass of the (meth)acrylic copolymer A, the composition comprises 1 to 50 mass% of the constituent unit derived from alkyl methacrylate a1, 1 to 50 mass% of the constituent unit derived from alkyl acrylate a2, and 30 to 80 mass% of the constituent unit derived from alkyl acrylate a3 (provided, the content of the constituent unit derived from alkyl methacrylate a1 and the composition derived from alkyl acrylate a2 The content of the unit, and the sum of the content of the constituent unit derived from the alkyl acrylate a3, does not exceed 100 mass% with respect to the total mass of the (meth)acrylic copolymer A), polymer composition. Claim 10 A polymer composition according to claim 9, wherein the (meth)acrylic copolymer A is a graft copolymer, and the graft copolymer comprises a constituent unit derived from a vinyl radical polymerizable monomer m1 and a constituent unit derived from a macromonomer M other than the vinyl radical polymerizable monomer m1. Claim 11 A polymer composition according to any one of claims 3 to 10, wherein the differential distribution value in the differential molecular weight distribution curve measured by gel permeation chromatography satisfies the following Formula 1. dMp30 / dMp≥0.65 ···1 · dMp30: Differential distribution value of the molecular weight corresponding to 30% of the peak top molecular weight. · dMp: Differential distribution value of the peak top molecular weight. Claim 12 A polymer composition according to any one of claims 1 to 4, 6, 8 and 10, wherein the vinyl radical polymerizable monomer m1 comprises an alkyl acrylate a2 having 5 to 14 carbon atoms in an alkyl group and an alkyl acrylate a3 having 1 to 4 carbon atoms in an alkyl group. Claim 13 A polymer composition according to any one of claims 1 to 4, 6, 8 and 10, wherein the macro monomer M comprises a constituent unit derived from a vinyl radical polymerizable monomer m2. Claim 14 A polymer composition according to claim 13, wherein the vinyl radical polymerizable monomer m2 comprises an alkyl methacrylate a1 having 5 to 14 carbon atoms in an alkyl group. Claim 15 A polymer composition according to claim 13, wherein the macro monomer M has the structure of Formula 2 below. During the meal, X 1 To X n-1 Each independently represents a hydrogen atom, a methyl group, or a CH2OH, and Y 1 to Y n OR each independently 1 , halogen atom, COR 2 , COOR 3 , CN, CONR 4 R 5 , NHCOR 6 , or R 7 Represents, and R 1 to R 7 Each represents independently a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group, a cyclic ether group, or a heteroaryl group. Z represents a hydrogen atom or a group derived from a radical polymerization initiator, and n represents an integer from 2 to 10,000. Claim 16 A polymer composition according to any one of claims 1 to 4, 6, 8 and 10, wherein the number average molecular weight of the macro monomer M measured by gel permeation chromatography is 500 to 30,000. Claim 17 A polymer composition according to any one of claims 1 to 10, wherein the (meth)acrylic copolymer A is a copolymer comprising a constituent unit derived from alkoxyalkyl (meth)acrylate a4. Claim 18 A polymer composition according to claim 17, wherein the (meth)acrylic copolymer A comprises 1 to 30 mass% of a constituent unit derived from the alkoxyalkyl (meth)acrylate a4 with respect to the total mass of the (meth)acrylic copolymer A. Claim 19 A polymer composition according to any one of claims 1 to 10, wherein the mass average molecular weight of the polymer composition measured by gel permeation chromatography is 50,000 to 2,000,000. Claim 20 A polymer composition according to any one of claims 1 to 10, wherein the molecular weight distribution of the polymer composition measured by gel permeation chromatography is 5 to 20. Claim 21 A lubricating oil additive comprising a polymer composition described in any one of claims 1 to 10. Claim 22 A viscosity index improver comprising a polymer composition described in any one of claims 1 to 8. Claim 23 A friction modifier comprising a polymer composition described in any one of claims 1 to 6, 9 and 10. Claim 24 A lubricating oil composition comprising a polymer composition described in any one of claims 1 to 10. Claim 25 A method for preparing a polymer composition by polymerizing a monomer mixture comprising a macro monomer and a vinyl radical polymerizable monomer in a base oil, wherein the macro monomer is a macro monomer polymerized in the base oil. A method for preparing a polymer composition as described in any one of claims 1 to 4, 6, 8 and 10. Claim 26 A method for preparing a polymer composition according to claim 25, using an α-methylstyrene dimer as a chain transfer agent. Claim 27 A lubricating oil composition comprising the polymer composition described in any one of claims 1 to 10 and a base oil. Claim 28 delete
Citation Information
Patent Citations
Lubricating oil additive and lubricating oil
JP1995286189A
Lubricating oil
JP1996157855A
Viscosity index improver
JP1998025488A
Impact modifier, its production, and resin composition using same
JP2000355616A
Pour-point depressant and lubricating oil composition
JP2002167591A