Super cpacitor and manufactuing method making the same
The supercapacitor design with nickel and silver layers on a carbon-based support addresses storage capacity and durability issues by stabilizing electrode materials, achieving improved performance and longevity.
Patent Information
- Application Number
- KR1020250018931
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-02-13
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2045-02-13
AI Technical Summary
Existing supercapacitors face challenges in improving storage capacity and durability during long-term use, particularly due to issues with electrode material compatibility and deposition methods.
A supercapacitor design featuring a first electrode with a nickel-containing layer on a carbon-based support, formed via electrochemical deposition, and a second layer of silver-containing composition created through microplasma treatment, without the use of adhesives, enhancing interfacial properties and conductivity.
The method significantly improves electric charging capacity and durability by stabilizing nickel and silver deposition, resulting in enhanced storage capacity and charge/discharge speed, with long-term stability demonstrated through 8,500 cycles.
Smart Images

Figure 112025017024140-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a supercapacitor and a method for manufacturing the same. Background Technology
[0003] With energy issues mounting globally due to continuous population growth, concerns regarding energy production and consumption have become a major challenge for humanity. The finiteness of energy that can be produced from fossil fuels such as coal, wood, oil, and natural gas, along with the negative environmental impacts caused by these fuels, are urging the development of various solutions for the production and storage of eco-friendly energy.
[0004] To meet these energy demands and requirements, batteries and supercapacitors are emerging as promising alternatives for sustainable energy storage solutions as next-generation power devices. In particular, supercapacitors offer various advantages such as high energy, power density, rapid charging and discharging capabilities, excellent durability, appropriate size, and low weight; consequently, extensive research is currently underway in related fields to improve their performance.
[0005] To improve the performance of supercapacitors, it is necessary to thoroughly understand and control the surface characteristics of the materials used. Furthermore, various studies are underway to find eco-friendly materials that can enhance cost efficiency and achieve higher charge storage capacities by investing further in synthesis methods and manufacturing technologies for supercapacitor materials to expand related businesses and develop low-cost manufacturing techniques. Prior art literature
[0007] Republic of Korea Published Patent No. 10-2023-0084018 The problem to be solved
[0008] The supercapacitor of the present invention and the method for manufacturing the same aim to improve the storage capacity of the supercapacitor and obtain high durability even during long-term use of the supercapacitor by using supercapacitor electrodes made of nickel and silver. means of solving the problem
[0010] To solve the above objective, the present invention provides a supercapacitor comprising: a first electrode; a second electrode facing the first electrode; and a separator provided between the first electrode and the second electrode, wherein the first electrode is provided on a carbon-based support and comprises a first layer containing nickel and a second layer provided on the first layer and comprising silver.
[0011] Furthermore, the present invention provides a super capacitor in which the first layer and the second layer are in contact with each other.
[0012] Furthermore, the present invention provides a supercapacitor in which the second layer comprises either silver nanoparticles or silver nanosheets.
[0013] Furthermore, the present invention provides a supercapacitor in which the surface of the carbon-based support is hydrophilic.
[0014] Furthermore, the present invention provides a supercapacitor in which the first layer is formed on the carbon-based support through electrochemical deposition (ECD).
[0015] Furthermore, the present invention provides a supercapacitor formed on the first layer by forming a microplasma in a solution containing silver for the second layer.
[0016] Furthermore, the present invention provides a method for manufacturing a supercapacitor comprising the steps of: forming a first layer containing nickel on a carbon-based support using electrochemical deposition (ECD); and forming a second layer containing silver by forming a microplasma on the first layer.
[0017] Furthermore, the present invention provides a method for manufacturing a supercapacitor that further comprises the step of treating an acid on one surface of the carbon-based support.
[0018] Furthermore, the present invention provides a method for manufacturing a supercapacitor in which the concentration of acid treated on one surface of the carbon-based support is 5 M or more and 10 M or less.
[0019] Furthermore, the present invention provides a method for manufacturing a supercapacitor in which the time for forming the microplasma is 300 seconds or more and 1200 seconds or less. Effects of the invention
[0021] The supercapacitor according to the present invention and the method for manufacturing the same have the effect of improving the electric charging capacity and increasing the durability of the supercapacitor electrode by depositing nickel on the surface of a carbon cloth using an electrochemical deposition method, thereby more stably fixing nickel on the surface of the carbon cloth, and depositing silver by forming a microplasma. Brief explanation of the drawing
[0023] FIG. 1 is a schematic diagram of a supercapacitor according to one embodiment of the present invention. FIGS. 2a to 2c are process diagrams for manufacturing the first electrode of a supercapacitor according to one embodiment of the present invention. FIGS. 3a to 3d are TEM images of the first electrode of a supercapacitor according to a comparative example and an embodiment of the present invention. Figure 4 is a graph showing the current according to the voltage potential of Comparative Examples 1 to 3 and the Example. FIG. 5 is a graph showing the voltage potential over time of Comparative Examples 1 to 3 and the Example. FIG. 6 is a graph showing the relative capacitance of Comparative Examples 1 to 3 and the Examples. FIG. 7 is a graph showing the characteristics of each electrode according to electrochemical impedance spectroscopy (EIS) of Comparative Examples 1 to 3 and the Examples. FIG. 8 is a graph for verifying the cycle stability of a supercapacitor according to one embodiment of the present invention. FIG. 9 shows a supercapacitor according to one embodiment of the present invention. FIGS. 10a to 10d are graphs comparing the initial state of a supercapacitor according to one embodiment of the present invention and the state after performing 8,500 GDC cycles. Specific details for implementing the invention
[0024] The present invention will be described in detail below.
[0025] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.
[0026] The terms used herein are for describing the embodiments and are not intended to limit the invention. In this specification, the singular form includes the plural form unless specifically stated otherwise in the text. As used herein, "comprises" and / or "comprising" do not exclude the presence or addition of one or more other components in addition to the components mentioned.
[0027] FIG. 1 is a schematic diagram of a supercapacitor according to one embodiment of the present invention.
[0028] As can be seen in FIG. 1, a supercapacitor according to one embodiment of the present invention may comprise a first electrode, a second electrode, a separator, and an electrolyte solution.
[0029] In this case, the first electrode (100) and the second electrode (200) may face each other, and the separator (300) may be provided between the first electrode (100) and the second electrode (200), and the electrolyte solution may be provided between the first electrode (100) and the second electrode (200), and the electrolyte in the electrolyte solution may pass through the separator (300).
[0030] The first electrode (100) may be, for example, an anode, and the second electrode (200) may be, for example, a cathode, but is not limited thereto.
[0031] According to one embodiment of the present invention, the first electrode (100) may comprise a carbon-based support (110), a first layer (120) provided on the carbon-based support (110) and comprising a nickel-containing composition, and a second layer (130) provided on the first layer (120) and comprising a silver-containing composition.
[0032] FIGS. 2a to 2c are process diagrams for manufacturing the first electrode of a supercapacitor according to an embodiment of the present invention. In this case, FIGS. 2a to 2c are enlarged views of the first electrode of a supercapacitor according to an embodiment of the present invention.
[0033] FIGS. 3a to 3d are TEM images of the first electrode of a supercapacitor according to a comparative example and an embodiment of the present invention. In this case, FIGS. 3a and 3b relate to the surface of a supercapacitor according to a comparative example, where the comparative example of FIG. 3a relates to a case where silver is deposited on a carbon cloth without treating it with a separate plasma, and FIG. 3b relates to a case where silver is deposited on a carbon cloth by forming a plasma using argon gas. FIGS. 3c and 3d relate to the surface of the first electrode of a supercapacitor according to an embodiment of the present invention. FIG. 3c relates to a case where nickel is deposited on a carbon cloth using chemical electrodeposition (ECD), and FIG. 3d relates to a case where silver is deposited by forming a plasma using argon gas in the embodiment of FIG. 3c.
[0034] First, as can be seen in FIG. 2a, the first electrode (100) may be a carbon-based support (110), for example, a carbon cloth (CC). Since the surface of the carbon-based support (110) is hydrophobic, the interfacial properties of the surface of the carbon-based support (110) can be changed to hydrophilic by performing an acid treatment on the carbon-based support (110) using an acid activation approach to facilitate the formation of the first layer (120) containing the nickel-containing composition. Through the acid activation approach, the nickel-containing composition can be more easily adsorbed onto the surface of the carbon-based support (110).
[0035] For example, the acid treatment can be performed by treating the carbon-based support (110) with a nitric acid (HNO3) solution. In this case, the concentration of the nitric acid (HNO3) solution may be 5 M or more and 10 M or less. When the concentration of the nitric acid (HNO3) solution is 5 M or more and 10 M or less, the hydrophilic properties of the surface of the carbon-based support (110) may be improved.
[0036] Next, as can be seen in FIG. 2b, in order to form the first electrode (100), the first layer (120) containing a nickel-containing composition can be formed on the carbon-based support (110).
[0037] According to one embodiment of the present invention, electrochemical deposition (ECD) may be used to adsorb the nickel-containing composition onto the carbon-based support (110). In this case, a thin nickel layer may be formed on the surface of the carbon-based support (110), for example, a carbon cloth, despite surface incompatibility between the carbon-based support and the metal ions.
[0038] As can be seen from FIGS. 3a to 3c, in the case of the comparative example of FIGS. 3a and 3b, it can be seen that the silver ions are not finely deposited on the carbon cloth due to the hydrophobicity of the carbon cloth surface and the incompatibility between the carbon cloth and the metal ions, for example, silver ions.
[0039] On the other hand, in the case of FIG. 3c, the first electrode of the supercapacitor according to one embodiment of the present invention can be seen to have the nickel-containing composition densely deposited on the surface of the carbon cloth.
[0040] As can be seen from FIGS. 3a to 3c, when the interfacial properties of the carbon cloth surface are changed to hydrophilic through an acid activation approach and metal ions, such as nickel ions, are deposited through electrochemical deposition (ECD), it can be confirmed that the nickel-containing composition is more easily deposited on the surface of the carbon-based support.
[0041] Next, as can be seen again in FIG. 2c, a second layer (130) containing a silver-containing composition can be formed on the first layer (120) containing the nickel-containing composition.
[0042] According to one embodiment of the present invention, the second layer (130) containing the silver-containing composition can be formed by forming a solution containing silver ions and a microplasma on the carbon-based support (110) on which the first layer (120) is formed.
[0043] The microplasma may be formed, for example, using argon gas. In this case, the microplasma may be formed on the carbon-based support (110) on which the first layer (120) is formed for a duration of 300 seconds or more and 1200 seconds or less. If the microplasma is formed for less than 300 seconds, silver may not be sufficiently deposited on the first layer (120), and if the microplasma is formed for more than 1200 seconds, the reaction may not proceed further, and additional silver may not be deposited.
[0044] Furthermore, since the second layer (130) containing the silver-containing composition is formed directly on the first layer (120) through the micro-plasma treatment, the second layer (130) can be formed on the first layer (120) without a separate adhesive member, for example, a binder. Accordingly, the first layer (120) containing the nickel-containing composition and the second layer (130) containing the silver-containing composition can come into contact with each other.
[0045] Since the first layer (120) and the second layer (130) are formed without a separate adhesive member, such as a binder, and are configured to come into contact with each other, the electrical conductivity characteristics between the first layer (120) and the second layer (130) can be improved compared to the case where an adhesive member is formed. This can improve the electrical conductivity characteristics of a supercapacitor according to one embodiment of the present invention.
[0046] As can be seen in FIG. 3d, the nickel-containing composition is deposited on the carbon-based support, and the silver-containing composition is deposited thereon. Through this, it can be seen that the silver-containing composition is densely formed on the first layer containing the nickel-containing composition through the microplasma treatment.
[0047] In this case, by forming the second layer containing the silver-containing composition, the storage capacity and charge / discharge speed of the supercapacitor according to one embodiment of the present invention can be significantly improved.
[0048] Below, we will examine in more detail the performance of the first electrode formed by the supercapacitor manufacturing method according to one embodiment of the present invention.
[0049] FIGS. 4 to 7 are graphs showing the performance of a first electrode formed by a method for manufacturing a supercapacitor according to a comparative example and an embodiment of the present invention under a 3-electrode system. In the 3-electrode system implemented in FIGS. 4 to 7, silver / silver chloride (Ag / AgCl) was used as the counter electrode and platinum (Pt) was used as the auxiliary electrode, and the electrochemical characteristics of each working electrode were tested by changing the working electrode. At this time, the characteristics of each working electrode according to the comparative example and the embodiment were measured using the PGSTAT204N workstation model of Metrohm Autolab.
[0050] Comparative Example 1 (CC@AgWOP) A silver-containing composition was deposited on the carbon cloth without depositing a separate nickel-containing composition. In this case, the silver-containing composition was deposited on the carbon cloth without separate plasma treatment.
[0051] Comparative Example 2 (CC@AgWP): A silver-containing composition was deposited on the carbon cloth without depositing a separate nickel-containing composition. In this case, the silver-containing composition was deposited on the carbon cloth by performing micro-plasma treatment using argon gas.
[0052] Comparative Example 3 (NiCC) A nickel-containing composition was deposited on a carbon cloth.
[0053] Example (NiCC@AgWP) : As a first electrode according to an embodiment of the present invention, a carbon cloth was treated by applying ultrasound in deionization water, acetone, and ethanol for 30 minutes each, and the treated carbon cloth was acid-treated through a hydrothermal process in a 6M nitric acid (HNO3) solution at a temperature of 90°C for 4 hours. The acid-treated carbon cloth was washed several times with deionization water and ethanol until the pH reached 7, and then dried at a temperature of 80°C for 10 hours. After that, nickel nanoseeds were deposited on the carbon cloth substrate by an electrochemical deposition method. Furthermore, a 0.02M silver solution was prepared on the carbon cloth substrate on which the nickel nanoseeds were deposited to form a microplasma containing argon (Ar) gas for 10 minutes, and the first electrode was washed with deionization water and then dried at a temperature of 80°C for 10 hours. Meanwhile, the microplasma was operated using an AC power supply with a maximum voltage of 6 kV and a frequency of 12 kHz, and argon (Ar) gas was introduced at a rate of about 1.5 L / min to form the plasma.
[0054] Figure 4 is a graph showing the current according to the voltage potential of Comparative Examples 1 to 3 and the Example.
[0055] As can be seen in Figure 4, when comparing Comparative Example 1 and Comparative Example 2, it can be confirmed that the area of the CV curve in Comparative Example 2 is relatively larger than that in Comparative Example 1. Through this, it can be confirmed that the capacitance characteristics of the electrode are improved when a silver-containing composition is deposited on a carbon cloth using a microplasma with argon gas.
[0056] Next, it can be confirmed that the area of the CV curve in the embodiment of the present invention is relatively the largest compared to Comparative Examples 1 to 3. This confirms that the capacitance characteristics are most improved in the embodiment of the present invention compared to Comparative Examples 1 to 3.
[0057] FIG. 5 is a graph showing the voltage potential over time for Comparative Examples 1 to 3 and the Example. In this case, FIG. 5 is a graph relating to galvanosthetic charge-discharge (GCD), and 1 mA / cm² 2 This shows the discharge profile of a galvanosthetic charge-discharge cycle at a constant current density.
[0058] As can be seen in Fig. 5, when comparing Comparative Example 1 and Comparative Example 2, it can be confirmed that the redox strength is higher when a silver-containing composition is deposited on a carbon cloth using a microplasma with argon gas.
[0059] Compared to Comparative Examples 1 to 3, it can be confirmed that the electrochemical performance of the carbon cloth containing the nickel-containing composition and the silver-containing composition in the embodiment of the present invention is improved.
[0060] FIG. 6 is a graph showing the relative capacitance of Comparative Examples 1 to 3 and the Examples.
[0061] As can be seen in FIG. 6, it can be confirmed that the capacitance of the embodiment of the present invention is the highest compared to Comparative Examples 1 to 3.
[0062] FIG. 7 is a graph showing the characteristics of each electrode according to electrochemical impedance spectroscopy (EIS) of Comparative Examples 1 to 3 and the Examples.
[0063] As can be seen in Fig. 7, it can be confirmed that no semicircular shape is observed in Comparative Example 2, Comparative Example 3 and the Example, which indicates that the resistance to charge transfer at the interface between each electrode and the electrolyte is minimized.
[0064] Referring to FIGS. 4 to 7, it can be seen that the electrochemical characteristics of a supercapacitor according to one embodiment of the present invention are improved when using the first electrode according to the embodiment.
[0065] FIGS. 8 to 11 are graphs showing the performance of a supercapacitor according to one embodiment of the present invention under a 2-electrode system. In this case, the first electrode was applied as the example (NiCC@AgWP) in FIGS. 4 to 7 above, the second electrode was applied as a carbon cloth utilizing bio-derived carbon, a polypropylene film was used as a separator, and a 3M potassium hydroxide (KOH) solution was used as the electrolyte.
[0066] FIG. 8 is a graph for verifying the cycle stability of a supercapacitor according to an embodiment of the present invention, showing the capacitance retention and Columbia efficiency according to the number of cycles. In this case, the graph in FIG. 8 is 20 mA / cm 2 The cycle was carried out under a constant current density.
[0067] As can be seen in FIG. 8, even after 8,500 consecutive GCD cycles, the supercapacitor according to one embodiment of the present invention maintains 80% of its initial capacitance and has a relatively high column ratio efficiency of 86%. This confirms that the supercapacitor according to one embodiment of the present invention has excellent durability.
[0068] FIG. 9 shows a supercapacitor according to one embodiment of the present invention.
[0069] As can be seen in FIG. 9, the supercapacitor according to one embodiment of the present invention exhibits excellent flexibility and can be confirmed to perform its function even in a bent state and be connected to a light-emitting diode to supply power.
[0070] FIGS. 10a to 10d are graphs comparing the initial state of a supercapacitor according to one embodiment of the present invention and the state after performing 8,500 GDC cycles. In this case, FIG. 10a relates to the X-ray diffraction (XRD) experimental results of a supercapacitor according to one embodiment of the present invention, and the experiment was conducted within the 2θ scan range of 10-90° using Cu Kα (λ = 0.15405 nm) radiation of the Empyrean XRD system of PANanalytical. In addition, FIGS. 10b to 10c relate to experimental results of X-ray photoelectronic analysis (XPS) of a supercapacitor according to one embodiment of the present invention, and are graphs analyzing the elemental composition and the chemical and electronic states of atoms within the material at 12 kV using monochromatic AlKα radiation at 1486.6 eV with the Theta probe K-ALPA+XPS system of Thermo Fisher Scientific.
[0071] As can be seen in FIG. 10a, it can be confirmed that the peak positions of the embodiment (NiCC@AgWP) in the initial state (before) and after performing 8,500 GDC cycles according to one embodiment of the present invention remain almost the same, except for the peak at 37.2°.
[0072] As can be seen in FIGS. 10b to 10d, it can be confirmed that nickel and silver are still present on the surface of the carbon cloth even after 8,500 GDC cycles have been performed in the supercapacitor according to one embodiment of the present invention. This indicates that the long-term durability of the supercapacitor according to one embodiment of the present invention is excellent even after 8,500 GDC cycles have been performed.
[0074] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will understand that other specific forms can be easily modified without altering the technical spirit or essential features of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.
[0075] The scope of the present invention is defined by the claims set forth below, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of the present invention. Explanation of the symbols
[0077] 100: First electrode 110: Carbon-based support 120: 1st floor 130: 2nd floor 200: Second electrode 300: Separator
Claims
Claim 1 A supercapacitor comprising: a first electrode; a second electrode facing the first electrode; and a separator provided between the first electrode and the second electrode, wherein the first electrode comprises a carbon-based support having a hydrophilic functional group formed on its surface; a first layer comprising a nickel nanoseed provided on the surface of the support; and a second layer laminated on the first layer and comprising one or more of silver nanoparticles and silver nanosheets, wherein the first layer and the second layer are in physical contact with each other to form an interface. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 A supercapacitor according to claim 1, wherein the first layer is formed by forming nickel nanoseeds on the carbon-based support via electrochemical deposition (ECD). Claim 6 In claim 1, the second layer is a supercapacitor formed on the first layer by forming a microplasma in a silver-containing solution. Claim 7 A method for manufacturing a supercapacitor comprising: a step of forming a first layer containing nickel on a carbon-based support using electrochemical deposition (ECD); and a step of forming a second layer containing silver by forming a microplasma on the first layer, wherein a hydrophilic functional group is formed on the surface of the carbon-based support, the first layer contains nickel nanoseeds, the second layer contains one or more of silver nanoparticles and silver nanosheets, and the first layer and the second layer are in physical contact with each other to form an interface. Claim 8 A method for manufacturing a supercapacitor according to claim 7, further comprising the step of treating an acid on one surface of the carbon-based support. Claim 9 A method for manufacturing a supercapacitor according to claim 8, wherein the concentration of acid treated on one surface of the carbon-based support is 5 M or more and 10 M or less. Claim 10 A method for manufacturing a supercapacitor according to claim 7, wherein the time for forming the microplasma is 300 seconds or more and 1200 seconds or less.