A method for solidifying radioactive spent ion exchange resin using phosphoric acid-based geopolymer raw materials and solidified radioactive waste ion exchange resin resulting therefrom
A method using metakaolin and phosphoric acid to solidify spent ion exchange resins into a geopolymer body addresses the challenge of solidifying organic radioactive waste, achieving high compressive strength and efficient disposal.
Patent Information
- Application Number
- KR1020240096340
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Existing methods struggle to efficiently solidify spent radioactive ion exchange resins into a stable, high-compressive-strength form suitable for disposal in radioactive waste facilities, due to their organic nature and potential for cracking or detachment from cement solidification.
A method involving mixing radioactive spent ion exchange resin with metakaolin and phosphoric acid as an acidic activator, followed by curing, to create a phosphoric acid-based geopolymer solidified body with optimized ratios and conditions to enhance compressive strength and loading capacity.
The method achieves a compressive strength exceeding the acceptance criteria of radioactive waste disposal facilities while maximizing waste loading, ensuring structural integrity and minimizing leaching risks.
Smart Images

Figure 112024079356628-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for solidifying radioactive waste using a phosphoric acid-based geopolymer raw material and a radioactive waste solidified body according to the same. Specifically, it relates to a method for solidifying radioactive waste, such as spent radioactive ion exchange resin, into a phosphoric acid-based geopolymer solidified body having a compressive strength higher than the acceptance criteria of a radioactive waste disposal facility while maximizing the loading rate of the radioactive waste when disposing of radioactive waste by solidification. Background Technology
[0003] Generally, most of the reactor devices and equipment at nuclear power plants that must be decommissioned after reaching the end of their lifespan are contaminated with radioactive materials.
[0004] As such, buildings, facilities, machinery, structures, etc., contaminated with radioactive materials cannot be simply buried or incinerated; they must be disposed of in accordance with the regulations of the Atomic Energy Act and the Environment Act after undergoing volume reduction treatments, such as decontamination and cutting, to remove the radioactive materials.
[0005] In accordance with these processing regulations, low- and intermediate-level radioactive waste, such as radioactive concentrated waste liquid powder generated at nuclear power plants, radioactive spent ion exchange resins, and radioactive acidic waste liquid generated through chemical decontamination processes, is solidified with solidifying materials such as cement (concrete), paraffin, asphalt, and geopolymer to be safely stored in a fixed form and placed in storage drums.
[0006] These radioactive wastes are permanently disposed of in radioactive waste disposal facilities. Since it is important to ensure stable solidification treatment to prevent immobilized radionuclides contained in the disposed waste from leaking into the nearby environment, it is common practice to stabilize low- and intermediate-level radioactive waste by solidifying it using cement.
[0007] However, in the case of spent radioactive ion exchange resins, which account for more than 90% of Korea's low- and intermediate-level radioactive waste along with radioactive concentrated waste liquid, there is a problem in that cement solidification is difficult because they are composed of organic materials and emit high radioactivity depending on the radionuclide. In particular, due to the characteristics of organic ion exchange resins that absorb water and expand easily, problems such as the detachment of the cement solidification body or the occurrence of cracks after solidification are continuously being reported.
[0008] To overcome the limitations of cement, methods such as solidifying into organic polymer solids, disposing of spent radioactive ion exchange resins by turning them into liquid using the Fenton process, and solidifying by grinding after drying have been proposed. However, these methods have not been adopted due to issues such as economic feasibility, heterogeneity of the solidified material, and the possibility of generating secondary waste. Consequently, spent radioactive ion exchange resins are currently being temporarily stored inside nuclear power plants.
[0010] Accordingly, there is an urgent need for research on methods to maximize the loading rate of radioactive waste, such as spent radioactive ion exchange resins, while simultaneously solidifying it into a solidified body with compressive strength higher than the acceptance standards of radioactive waste disposal facilities.
[0012] (Patent Document 1) KR 10-2375027 B
[0013] (Patent Document 2) KR 10-2181217 B The problem to be solved
[0015] In order to solve the problems associated with the aforementioned conventional technology, we propose a method for disposing of radioactive waste, such as spent radioactive ion exchange resins, by solidification that maximizes the loading rate of the radioactive waste while simultaneously solidifying it into a solidified body having a compressive strength higher than the acceptance criteria of a radioactive waste disposal facility. means of solving the problem
[0017] In order to solve the problems according to the prior art described above, the method for solidifying radioactive spent ion exchange resin according to the present invention comprises: (a) a step of generating a mixture in which radioactive spent ion exchange resin, metakaolin, water, and an acidic activator are mixed; and (b) a step of curing the mixture.
[0018] The above acidic activator may be phosphoric acid (H3PO4).
[0020] Preferably, the ratio of the weight of the combined water and the water contained in the acid activator to the weight of the remainder excluding the water and the water contained in the acid activator in the mixture may be 0.6 to 1.3.
[0022] Preferably, the weight of the radioactive spent ion exchange resin per 100 weight parts of the mixture may be 10 to 50.
[0024] Preferably, the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture may be 0.6 to 1.2.
[0026] Preferably, the molar concentration of phosphorus in the phosphoric acid may be 8 to 12 mol / L.
[0028] Preferably, the ratio of the weight of the combined water and the water contained in the acid activator to the weight of the remainder excluding the water and the water contained in the acid activator in the mixture may be 0.6 to 0.8.
[0030] Preferably, the weight of the radioactive spent ion exchange resin per 100 weight parts of the mixture may be 40 to 50.
[0032] Preferably, the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture may be 0.6 to 0.8.
[0034] Preferably, the molar concentration of phosphorus in the phosphoric acid may be 8 to 12 mol / L.
[0036] Preferably, the ratio of the weight of the combined water and the water contained in the acid activator to the weight of the remainder excluding the water and the water contained in the acid activator in the mixture may be 0.65 to 0.75.
[0038] Preferably, the weight of the radioactive spent ion exchange resin per 100 weight parts of the mixture may be 45 to 50.
[0040] Preferably, the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture may be 0.65 to 0.75.
[0042] Preferably, the molar concentration of phosphorus in the phosphoric acid may be 8 to 12 mol / L.
[0044] Preferably, in step (b), the mixture may be cured for 5 to 7 days.
[0046] Preferably, in step (b), the mixture may be cured at room temperature for 4.5 to 5.5 days, and then cured at 55 to 65°C for 0.5 to 1.5 days.
[0048] In order to solve the problems according to the prior art described above, the radioactive waste ion exchange resin solidified body according to the present invention may be a radioactive waste ion exchange resin solidified body manufactured according to the radioactive waste ion exchange resin solidification method described above.
[0050] In order to solve the problems according to the prior art described above, the method for treating radioactive spent ion exchange resin according to the present invention comprises: (c) a step of generating a mixture of radioactive spent ion exchange resin, metakaolin, water, and an acidic activator; and (d) a step of curing the mixture.
[0051] The above acidic activator may be phosphoric acid (H3PO4).
[0053] Preferably, the ratio of the weight of the combined water containing the water and the water containing the acid activator to the weight of the remainder excluding the water and the water containing the acid activator in the mixture is 0.65 to 0.75, and
[0054] The weight of the radioactive waste ion exchange resin may be 45 to 50 parts per 100 parts by weight of the above mixture.
[0056] Preferably, the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture is 0.65 to 0.75, and
[0057] The molar concentration of phosphorus in the above phosphoric acid may be 8 to 12 mol / L. Effects of the invention
[0059] Due to the above-described means of solving the problem, radioactive waste ion exchange resins can be efficiently solidified and disposed of using a solidified body, etc., according to a solidification method that maintains a compressive strength higher than the acceptance criteria of a radioactive waste disposal facility, minimizes the occurrence of problems associated with conventional technology, and maximizes the loading rate of radioactive waste. Brief explanation of the drawing
[0061] FIG. 1 is a drawing illustrating an example of a mixing ratio for manufacturing a geopolymer solidified body according to the present invention. FIG. 2 is a schematic diagram illustrating the process of preparing a radioactive spent ion exchange resin sample used to manufacture a geopolymer solidified body according to the present invention. FIGS. 3 to 8 are drawings illustrating test data for a geopolymer solidified body according to the present invention. Specific details for implementing the invention
[0062] Hereinafter, preferred embodiments of the method according to the present invention will be described with reference to the accompanying drawings. In this process, the thickness of lines or the size of components depicted in the drawings may be exaggerated for clarity and convenience of explanation. Furthermore, the terms described below are defined considering their functions in the present invention, and these may vary depending on the intention or convention of the user or operator. Therefore, the definitions of these terms should be based on the content throughout this specification.
[0064] Referring to FIGS. 1 to 8, a method for solidifying a radioactive spent ion exchange resin into a geopolymer solidified body using raw materials for manufacturing a phosphoric acid-based geopolymer is described.
[0065] A mixture of radioactive spent ion exchange resin, metakaolin, water, and an acidic activator can be produced, and subsequently, the mixture produced in this way can be cured to produce a solidified geopolymer body in which the radioactive spent ion exchange resin is solidified.
[0066] Here, the acidic activator can be phosphoric acid (H3PO4).
[0068] Among the mixing ratios of the mixture, the weight ratio of water to the remainder is examined first.
[0069] The ratio of the weight of water (L) containing water and acid activator to the weight of the remainder (S) excluding water and acid activator contained in the mixture may be 0.6 to 1.3. That is, the L / S ratio may be 0.6 to 1.3, where L is the combined weight of water and acid activator contained in the mixture, and S is the weight of the remainder excluding water and acid activator contained in the mixture.
[0070] More preferably, the L / S ratio may be 0.6 to 0.8, and even more preferably 0.65 to 0.75.
[0071] Next, regarding the weight of the radioactive spent ion exchange resin mixed into the mixture, the weight of the radioactive spent ion exchange resin per 100 parts by weight of the total mixture may be 10 to 50. More preferably, it may be 40 to 50. Even more preferably, it may be 45 to 50.
[0072] Next, regarding the ratio of the molar concentrations of aluminum and phosphorus in the mixture, the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture may be 0.6 to 1.2. More preferably, it may be 0.6 to 0.8. Even more preferably, it may be 0.65 to 0.75.
[0073] Next, the molar concentration of phosphorus in the phosphoric acid mixed as an oxidation activator may be 8 to 12 mol / L.
[0075] Regarding the curing conditions, the mixture mixed at the above-described mixing ratio can be cured for 5 to 7 days. Specifically, the mixture can be cured at room temperature for 4.5 to 5.5 days, and then cured at 55 to 65°C for 0.5 to 1.5 days.
[0077] Explain the experiment and the experimental results.
[0078] FIG. 1 relates to the mixing ratio and curing conditions of a mixture for manufacturing a geopolymer solidified body in which radioactive spent ion exchange resin is solidified.
[0079] In Figure 1, P molarity represents the concentration of phosphorus in phosphoric acid, which is an acidic activator. In the Liquid / Solid ratio, Liquid represents the weight of the water in the mixture combined with the water contained in the acidic activator, and Solid represents the weight of the remainder excluding the water in the mixture combined with the water contained in the acidic activator.
[0080] The P / Al molarity ratio represents the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture, and the waste loading (wt%) represents the weight percentage of spent radioactive ion exchange resin mixed in the mixture (loading rate of spent radioactive ion exchange resin).
[0081] Figure 2 illustrates the conditions under which the radioactive spent ion exchange resin sample used in the experiment was prepared. The prepared radioactive spent ion exchange resin sample used was a radioactive spent ion exchange resin sample saturated with water. In the Liquid / Solid ratio in Figure 1, Liquid is the weight of water contained in the mixture and the acidic activator, and is the weight of water in the radioactive spent ion exchange resin without water. In Figure 1, Solid is the weight of the remainder containing water in the radioactive spent ion exchange resin.
[0082] Figure 3 shows the compressive strength of each sample (for each geopolymer solidified according to the mixing ratio shown in Figure 1) at an L / S ratio (Liquid / Solid ratio in Figure 1) of 1.2.
[0083] Figure 3 shows that the compressive strength of the geopolymer solidified without mixing radioactive spent ion exchange resin (Spent IER loading (wt%) = 0) is significantly higher than that of the other samples (geopolymer solidified with mixing radioactive spent ion exchange resin, Spent IER loading (wt%) = 10, 20, 30, 40, 50).
[0084] Radioactive spent ion exchange resins have low mechanical strength, which is attributed to the porous structure of the radioactive spent ion exchange resins. For this reason, the compressive strength of a geopolymer solidified with radioactive spent ion exchange resins mixed in a porous structure appears to be lower than that of a geopolymer solidified without radioactive spent ion exchange resins mixed in.
[0085] In Figure 3, except for the case where the loading rate is 50 wt%, the remaining samples show a compressive strength exceeding 3.445 MPa, which is the acceptance criterion for radioactive waste disposal facilities.
[0086] Figure 4 shows the compressive strength of the samples according to each L / S ratio. When the L / S ratio is 0.7, the compressive strength is higher than when the L / S ratio is 1.2, and even when the loading rate of spent radioactive ion exchange resin is 50 wt%, the compressive strength exceeds the acceptance standard compressive strength (3.445 MPa) for radioactive waste disposal facilities.
[0087] Looking at Figures 3 and 4, it appears that the L / S ratio affects the compressive strength of the manufactured geopolymer solidified body. This suggests that as the amount of water mixed into the mixture increases (as the L / S ratio increases), the concentration of the acidic activator is diluted, and consequently, the compressive strength of the geopolymer solidified body decreases.
[0088] Gamma irradiation, water immersion, and thermal cycling tests, which are acceptance criteria tests for radioactive waste disposal facilities, were conducted on the geopolymer solidified body manufactured according to the present invention. Figure 5 shows the compressive strength of the geopolymer solidified body according to loading ratio before the test (control) and after the test (gamma irradiation, water immersion, thermal cycling). Considering the standard deviation of the compressive strength, it appears that the acceptance criteria tests did not induce structural decomposition of the geopolymer solidified body. Gamma rays can cause changes in the structure of organic materials, but it appears that there is no effect on the geopolymer solidified body manufactured according to the present invention. The geopolymer solidified body according to the present invention exhibits excellent water resistance and stability against freezing and thawing.
[0089] Figure 6 shows the leachability index. Cobalt (Co), cesium (Cs), and scrotonium (Sr) show a leachability index that satisfies the acceptance criteria for radioactive waste disposal facilities, which must be higher than 6.0 according to ANSI / ANS. Silicon (Si), aluminum (Al), and phosphorus (P), which are the main components of the geopolymer solidified material, show a good leachability index of 12 or higher, which is much higher than the acceptance criteria for radioactive waste disposal facilities, which must be higher than 6.0 according to ANSI / ANS. In the case of the leaching index of cobalt (Co), cesium (Cs), and scrotonium (Sr), the leaching index is lower than that of the alkali-based geopolymer solidified by the radioactive waste ion exchange resin. This is because the alkali-based geopolymer solidified exhibits a high leaching index by effectively preventing the movement of positively charged nuclides through the attractive force between the structural negative charge and positively charged nuclides, whereas the phosphoric acid-based geopolymer solidified appears to cause a low leaching index due to the repulsive force between the positive charge and positively charged nuclides in the geopolymer solidified.
[0090] Figure 7 shows the microstructure of the geopolymer solidified body according to the present invention before (control) and after (gamma irradiation, water immersion, thermal cycling) the test was conducted. The radioactive waste disposal acceptance criteria test does not appear to have affected the microstructure of the geopolymer solidified body. All geopolymer solidified bodies exhibit a dense and well-connected microstructure.
[0091] Figure 8 shows XRD analysis data of the geopolymer solidified body according to the present invention before (control) and after (gamma irradiation, water immersion, thermal cycling). Amorphous protrusions appearing at 2 theta 18–35 degrees indicate the geopolymer structure. In the geopolymer solidified body after water immersion and thermal cycling tests, the crystalline structure was not altered, whereas in the geopolymer solidified body after leaching and gamma irradiation tests, aluminum phosphate (AlPO4) crystals were identified as new crystals. Anatase appears to be an impurity contained in metakaolin. Overall, it appears that the amorphous structure is maintained for the geopolymer solidified body manufactured according to the present invention even after the radioactive waste disposal facility acceptance criteria test.
[0093] For the time being, the present specification has been described with reference to embodiments illustrated in the drawings so that those skilled in the art can easily understand and reproduce the present invention; however, this is merely illustrative, and those skilled in the art will understand that various modifications and equivalent alternative embodiments are possible from the embodiments of the present invention. Accordingly, the scope of protection of the present invention should be determined by the claims.
Claims
Claim 1 A method for solidifying a radioactive waste ion exchange resin comprising: (a) a step of producing a mixture of radioactive waste ion exchange resin, metakaolin, water, and an acidic activator; and (b) a step of curing the mixture, wherein the acidic activator is phosphoric acid (H3PO4), and the ratio of the weight of the water combined with the water in the acidic activator to the weight of the remainder excluding the water and the water in the acidic activator in the mixture is 0.6 to 0.
8. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 delete Claim 7 A method for solidifying radioactive spent ion exchange resin according to claim 1, wherein the weight portion of the radioactive spent ion exchange resin is 40 to 50 parts per 100 parts by weight of the mixture. Claim 8 A method for solidifying radioactive spent ion exchange resin according to claim 7, wherein the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture is 0.6 to 0.
8. Claim 9 A method for solidifying radioactive spent ion exchange resin according to claim 8, wherein the molar concentration of phosphorus in the phosphoric acid is 8 to 12 mol / L. Claim 10 A method for solidifying radioactive spent ion exchange resin according to claim 1, wherein the ratio of the weight of the combined water and the water contained in the acidic activator to the weight of the remainder excluding the water and the water contained in the acidic activator in the mixture is 0.65 to 0.
75. Claim 11 A method for solidifying radioactive spent ion exchange resin according to claim 10, wherein the weight portion of the radioactive spent ion exchange resin is 45 to 50 parts per 100 parts by weight of the mixture. Claim 12 A method for solidifying radioactive spent ion exchange resin according to claim 11, wherein the ratio of the molar concentration of phosphorus to the molar concentration of aluminum in the mixture is 0.65 to 0.
75. Claim 13 A method for solidifying radioactive spent ion exchange resin according to claim 12, wherein the molar concentration of phosphorus in the phosphoric acid is 8 to 12 mol / L. Claim 14 A method for solidifying radioactive spent ion exchange resin according to claim 1, wherein in step (b), the mixture is cured for 5 to 7 days. Claim 15 A method for solidifying radioactive spent ion exchange resin according to claim 14, wherein in step (b), the mixture is cured at room temperature for 4.5 to 5.5 days and then cured at 55 to 65°C for 0.5 to 1.5 days. Claim 16 A solidified radioactive waste ion exchange resin body manufactured according to a method for solidifying radioactive waste ion exchange resin according to any one of claims 1, 7 to 15. Claim 17 delete Claim 18 delete Claim 19 delete