Cobalt-containing metal foam element and method of manufacturing the same
By alloying metallic cobalt or nickel-cobalt foams with aluminum to form a stable aluminum oxide layer, the method addresses the adhesion issues of catalytic coatings, enhancing catalyst stability and durability, suitable for industrial use.
Patent Information
- Application Number
- KR1020227009196
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-25
- Filing Date
- 2020-09-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Existing methods for manufacturing metal foam-supported catalysts face challenges in achieving stable adhesion of catalytic active coatings, leading to separation of fragments under mechanical stress and reduced catalyst life, particularly in flow-through reactors, and require complex equipment and expensive reagents.
A method involving the use of metallic cobalt or nickel-cobalt alloy foams, alloyed with aluminum-containing powder at controlled temperatures to form a stable aluminum oxide layer, followed by application of a catalytic active layer, ensuring strong adhesion and mechanical stability.
The method produces a catalyst with excellent adhesion and mechanical stability, reducing the risk of catalyst failure and plant disruption, while being cost-effective and suitable for mass production.
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing a supported catalyst, comprising the steps of: coating a metal foam made of metallic cobalt, an alloy of nickel and cobalt, or an array of overlapping layers of nickel and cobalt with aluminum; subsequently heat treating to achieve alloy formation between the metal foam and aluminum; subsequently oxidizing the aluminum surface; and applying a catalytic active layer comprising at least one supporting oxide and at least one catalytic active component. The present invention also relates to the use of the supported catalyst obtained by the above method and chemical modifications thereof. Background Technology
[0002] The use of metal foams as supports for catalytic active coatings is known from the prior art. Catalytic active coatings on metallic supports typically consist of a supporting oxide that increases the micro-surface area and a catalytic active metal applied to the supporting oxide (see, e.g., WO 9511752 A1). Although the monolithic supported catalyst thus obtained can be used for various applications, its usability is limited because the catalytic active coating, which is mainly composed of oxide components, does not adhere very well to the metal support. In the case of mechanical stress and potentially also when the supported catalyst is operated in a flow-through reactor, poor adhesion leads to the separation of fragments of the catalytic active layer, which in turn results in a reduction in catalyst life due to the separated solid particles and a potential interruption of plant operation.
[0003] An alternative is to use a sol-gel process to coat metal foams as catalyst supports. However, this process carries a high potential for risk and requires the use of specialized, difficult-to-handle equipment and expensive reagents.
[0004] Another process for manufacturing metal foam-supported catalysts in the prior art utilizes the ability to generate a relatively stable oxide layer on a metal surface by atomic layer deposition (ALD). For example, US 20120329889 A1 discloses a method for manufacturing a metal foam-supported catalyst for Fischer-Tropsch synthesis, which involves preparing a thin Al2O3 film on a metal foam using atomic layer deposition (ALD), followed by an oxide coating by dip coating, drying, and subsequent calcination. US 20120329889 A1 explicitly mentions the difficulty of achieving a stable bond between the metal foam surface and the oxide coating (see paragraphs
[0068] and
[0069] ), which is achieved by applying an oxide intermediate layer by ALD. However, the method disclosed in US 20120329889 A1 requires a very complex apparatus. The problem to be solved
[0005] In light of the limited accessibility to stable metal foam-supported catalysts, the present invention aims to provide a method suitable for mass production that is as simple as possible and suitable for manufacturing a support catalyst having a catalyst coating from a catalyst-inert metal foam. In such a catalyst, the pores provided by the foam base structure must not be clogged, and the catalyst coating must be as simple as possible to apply, yet possess the characteristic of adhering very well to the metal foam. The method of the present invention and the product obtainable through this method meet these requirements. means of solving the problem
[0006] A method according to the present invention for manufacturing a supporting catalyst comprises the following steps:
[0007] (a) providing a metal foam A made of metallic cobalt, an alloy of nickel and cobalt, or an array of overlapping layers of nickel and cobalt,
[0008] (b) a step of obtaining metal foam AX by applying aluminum-containing powder MP to metal foam A,
[0009] (c) a step of obtaining metal foam B by heat-treating metal foam AX to achieve the formation of an alloy between metal foam A and aluminum-containing powder MP, wherein
[0010] The maximum temperature in the heat treatment of metal foam AX is within the range of 680 to 715℃, and
[0011] A step of obtaining the metal foam B, wherein the total duration of heat treatment in a temperature range of 680 to 715℃ is 5 to 240 seconds,
[0012] (d) a step of obtaining metal foam C by oxidizing metal foam B,
[0013] (e) A step of obtaining a supported catalyst by applying a catalytic active layer comprising at least one supporting oxide and at least one catalytic active component to at least a portion of the surface of metal foam C.
[0014] Nickel foams, in which aluminum is first applied, alloyed, and then partially leached out, are known from the prior art as an alternative to typical Raney-type catalysts (see, for example, EP 2764916 A1). The foam thus obtained is an activated all-metal Raney-type catalyst commonly used in hydrogenation reactions.
[0015] In addition, metal foams in which aluminum is applied first and then oxidized after alloying are known from the prior art (see Wen-Wen Zeng et al. “Synthesis and Compression Characteristics of Oxidation-Resistant Ni-Al Foams”, Acta metallurgica Sinica, volume 30, No. 10, October 1, 2017, pp. 965-972). However, in the process of Wen-Wen Zeng et al., the entire cross-section of the metal foam is alloyed with aluminum (see Conclusion, p. 972), whereas in the process of the present invention, alloy formation is limited to the upper layer of the metal foam, leaving a non-alloyed region in the central region of the metal foam.
[0016] Experimental results related to the present invention demonstrate that the selection of temperature conditions for heat treatment for alloy formation significantly influences the results. The method according to the present invention limits alloy formation to the upper layer of the metal foam, allowing unalloyed regions to remain in the central region of the metal foam. The presence of these unalloyed regions particularly affects the mechanical stability of the obtained support catalyst. The fracture / compressive strength decreases significantly as the degree of alloying and complete alloying of the metal foam increases, resulting in a very brittle support catalyst that tends to fracture under mechanical stress. Since continuously operating fixed-bed reactors used on an industrial scale can have fixed-bed volumes of up to 100 m³, this fact is of considerable practical importance, meaning that depending on the bulk density and height of the fixed bed used, there may potentially be multiple metric tons weighed on the lower layer. If the support catalyst used to form the fixed bed lacks sufficient mechanical stability and durability to support such weights for thousands of operating hours, this can lead to failure of the support structure and, consequently, mechanical failure of the catalytic active region (catalyst failure). Broken material can be discharged from the reactor along with the fluid into adjacent plant components and / or cause caking in the fixed bed. In both cases, significant disruption to plant operation occurs.
[0017] In the context of the present invention, metal foam A is understood to mean a metal body in the form of a foam. Metal bodies in the form of foam are disclosed, for example, in Ullmann's Encyclopedia of Industrial Chemistry, section "Metallic Foams" (published online July 15, 2012, DOI: 10.1002 / 14356007.c16_c01.pub2). Metal foams having different morphological characteristics, namely pore size and shape, layer thickness, areal density, geometric surface area, porosity, etc., are suitable in principle. Preferably, metal foam A has a g / m³ of 400 to 1500 g / m³ 2It has a density in the range of 400 to 3000 µm, preferably 400 to 800 µm, and a thickness in the range of 0.5 to 10 mm, preferably 1.0 to 5.0 mm. Manufacturing can be carried out in a manner known in itself. For example, a foam made of an organic polymer can be initially coated with a metal and then removed by pyrolysis to mass-produce metal foams. To coat with at least one first metal or its precursor, the foam made of the organic polymer may be contacted with a solution or suspension containing the first metal. This can be carried out, for example, by spraying or dipping. Deposition by chemical vapor deposition (CVD) is also possible. Polymer foams suitable for manufacturing molded articles in the form of foams preferably have a pore size in the range of 100 to 5000 µm, more preferably 450 to 4000 µm, and particularly 450 to 3000 µm. A suitable polymer foam preferably has a layer thickness of 0.5 to 10 mm, more preferably 1.0 to 5.0 mm. A suitable polymer foam preferably has a density of 300 to 1200 kg / m³. The specific surface area is preferably in the range of 100 to 20,000 m² / m³, more preferably 1,000 to 6,000 m² / m³. The pore size is preferably in the range of 0.50 to 0.95.
[0018] The metal foam A used in step (a) of the method according to the present invention may have any desired shape, for example, a cube, a rectangular prism, a cylinder, etc. Alternatively, the metal foam may be formed as, for example, a monolith.
[0019] The aluminum-containing powder MP may be applied in various ways in step (b) of the method according to the present invention, for example by contacting a metal foam A with the composition of the aluminum-containing powder MP by rolling or dipping, or by applying the composition of the aluminum-containing powder MP by spraying, scattering, or pouring. The composition of the aluminum-containing powder MP for this purpose may be in the form of a suspension or a powder.
[0020] In step (b) of the method according to the present invention, the actual application of the composition of the aluminum-containing powder MP to the metal foam A is preferably preceded by pre-impregnating the metal foam A with a binder. Impregnation can be achieved, for example, by spraying the binder or by dipping the metal foam A into the binder, but is not limited to these options. Thus, it is possible to apply the composition of the metal-containing powder MP to the metal foam A prepared in this way.
[0021] Alternatively, it is possible to apply the composition of the aluminum-containing powder MP and the binder in a single step. To this end, the composition of the aluminum-containing powder MP is suspended in the liquid binder itself before application, or the composition of the aluminum-containing powder MP and the binder are suspended in an auxiliary liquid F.
[0022] The binder is a composition that can be completely converted into a gaseous product by heat treatment within a temperature range of 100 to 400°C, comprising an organic compound that promotes the adhesion of the composition of aluminum-containing powder MP to the metal foam. The organic compound is preferably selected from the group consisting of polyethyleneimine (PEI), polyvinylpyrrolidone (PVP), ethylene glycol, and mixtures of these compounds. PEI is particularly preferred. The molecular weight of polyethyleneimine is preferably in the range of 10,000 to 1,300,000 g / mol. The molecular weight of polyethyleneimine (PEI) is preferably in the range of 700,000 to 800,000 g / mol.
[0023] The auxiliary fluid F must be capable of forming a suspension of the composition of the binder and the aluminum-containing powder MP and must be completely converted into a gaseous product by heat treatment within a temperature range of 100 to 400°C. The auxiliary fluid F is preferably selected from water, ethylene glycol, PVP, and mixtures of these compounds. When the auxiliary fluid is used, the binder is typically suspended in water at a concentration within the range of 1% to 10% by weight, followed by the suspension of the composition of the aluminum-containing powder MP in this suspension.
[0024] The aluminum-containing powder MP used in step (b) of the method according to the present invention may also contain fine aluminum, but may also contain additives that contribute to increasing fluidity or water stability. These additives must be able to be completely converted into gaseous products by heat treatment in a temperature range of 100 to 400°C.
[0025] It is preferable that the aluminum-containing powder MP has an aluminum content in the range of 80% to 99.8% by weight. It is preferable that the powder has aluminum particles with a particle size of 5 µm or more and 200 µm or less. It is particularly preferable that 95% of the aluminum particles have a particle size of 5 µm or more and 75 µm or less. The aluminum-containing powder MP may contain aluminum components in an oxidized form in addition to aluminum components in elemental form. This oxidized fraction is typically in the form of oxidized compounds, e.g., oxides, hydroxides, and / or carbonates. The mass ratio of oxidized aluminum is typically in the range of 0.05% to 10% by weight of the total mass of the aluminum-containing powder MP.
[0026] In step (c) of the method according to the present invention, heat treatment is performed to achieve the formation of one or more alloys.
[0027] Experimental results related to the present invention show that the selection of temperature conditions for heat treatment for alloy formation has a significant effect on the process of alloy formation. The method according to the present invention limits alloy formation to the upper layer of the metal foam, so that unalloyed regions remain in the central region of the metal foam.
[0028] In step (c) of the method according to the present invention, metal foam AX is heat-treated to achieve the formation of an alloy between metal foam A and aluminum-containing powder MP to obtain metal foam B, the maximum temperature of the heat treatment of metal foam AX is in the range of 680 to 715°C, and the total duration of the heat treatment in the temperature range of 680 to 715°C is 5 to 240 seconds.
[0029] The heat treatment typically involves heating the metal foam AX in stages, followed by cooling it to room temperature. The heat treatment is performed under an inert gas or under reducing conditions. Reducing conditions are understood to mean the presence of a gas mixture containing hydrogen and at least one gas that is inert under reaction conditions. A suitable example is a gas mixture containing 50 volume% N2 and 50 volume% H2. The inert gas used is preferably nitrogen. Heating can be achieved, for example, in a belt furnace. Suitable heating rates are in the range of 10 to 200 K / min, preferably 20 to 180 K / min. During the heat treatment, the temperature is typically first increased from room temperature to about 300 to 400°C, and moisture and organic components are removed from the coating at this temperature for about 2 to 30 minutes. Then, the temperature is increased to a range of 680 to 715°C, thereby obtaining alloy formation between the metal foam A and the aluminum-containing powder MP. Next, the metal foam is quenched by contact with an inert gas environment at a temperature of about 200°C.
[0030] In the case of the metals related to the present invention, to limit alloy formation to the upper region of the metal foam and leave an unalloyed region within the metal foam, the maximum temperature of the heat treatment of the metal foam AX in step (c) needs to be in the range of 680 to 715°C, and the total duration of the heat treatment in the temperature range of 680 to 715°C needs to be 5 to 240 seconds. Although the duration of the heat treatment may compensate to some extent for the level of the maximum treatment temperature and vice versa, the frequency of experiments achieving alloy formation in the upper region of the metal foam while leaving unalloyed regions within the metal foam decreases sharply when the maximum temperature of the heat treatment deviates from the temperature range of 680 to 715°C and / or the duration of the heat treatment in the temperature range of 680 to 715°C deviates from 5 to 240 seconds. If the maximum temperature is too high and / or the metal foam remains in the maximum temperature region for too long, this can cause alloy formation to advance to the lowest depth of the metal foam, preventing any non-alloyed regions from remaining. If the maximum temperature is too low and / or the metal foam does not remain in the maximum temperature region for a sufficiently long time, alloy formation does not begin at all.
[0031] In step (c) of the method according to the present invention, the heat treatment of the metal foam induces the formation of an aluminum-containing phase. The mass ratio of metal foam B to metal foam A, V, V = m (metal foam B) / m (metal foam A), is a measure of how much aluminum is alloyed in the foam in step (c) of the method according to the present invention. In a preferred embodiment, the mass ratio of metal foam B to metal foam A, V, V = m (metal foam B) / m (metal foam A) is in the range of 1.1:1 to 1.5:1. In another preferred embodiment, the mass ratio of metal foam B to metal foam A, V, V = m (metal foam B) / m (metal foam A) is in the range of 1.2:1 to 1.4:1.
[0032] In step (d) of the method according to the present invention, metal foam C is produced by performing an oxidation treatment on metal foam B.
[0033] The purpose of the oxidative treatment of metal foam B in step (d) of the method according to the present invention is to impart an external aluminum oxide layer to the aluminum present on the surface of metal foam B. This purpose can be achieved, for example, by exposing metal foam B in a heated state to an oxidizing gas atmosphere (e.g., air) or by contacting it with an alkaline solution, for example, through the initial surface formation of aluminum hydroxide on metal foam B, and by converting aluminum hydroxide into aluminum oxide through heat treatment under oxidizing conditions.
[0034] To expose the heated metal foam B to an oxidizing gas atmosphere, for example, it is sufficient to heat the metal foam to an appropriate temperature inside the furnace through the introduction of air.
[0035] When metal foam B is heated by the inflow of air without prior formation of aluminum hydroxide, the selected temperature should be 200°C to 1200°C, or 200°C to 1000°C, or 200°C to 750°C. According to the present invention, thermal oxidation is preferably performed in air at a temperature of 200°C to 700°C for 1 to 60 minutes.
[0036] If aluminum hydroxide is first formed on the surface of metal foam B by performing only heat treatment after contact with, for example, an alkaline solution, at least a portion of the aluminum present on the surface is converted into aluminum hydroxide, and subsequently, at least a portion of the aluminum hydroxide formed on the surface is converted into aluminum oxide.
[0037] Converting at least a portion of the aluminum present on the surface into aluminum hydroxide is preferably achieved by contacting the metal foam with an alkaline aqueous solution.
[0038] The alkaline aqueous solution comprises sodium hydroxide, potassium hydroxide, lithium hydroxide, or a combination thereof at a concentration of 0.05 wt% to 30 wt%, preferably 0.5 wt% to 5 wt%, and metal foam B is contacted with the alkaline aqueous solution for 5 to 120 minutes, preferably 30 minutes or less, more preferably 10 minutes or less. This treatment may occur within a temperature range of 10°C to 110°C. It is preferable to treat at 20°C (room temperature).
[0039] This leads to the thermal conversion of at least a portion of the superficially formed aluminum hydroxide into aluminum oxide in an oxidizing atmosphere. This is carried out by applying heat from 20°C (room temperature) to 700°C for 1 minute to 8 hours by the introduction of air. According to the present invention, thermal oxidation is preferably carried out in air at a temperature of 200°C to 700°C for 1 to 60 minutes.
[0040] Metal foam C serves as a support for a suitable catalyst that can be specifically selected for a particular reaction to be catalyzed.
[0041] In step (e) of the method according to the present invention, a catalytic active layer comprising at least one support oxide and at least one catalytic active component is applied to at least a portion of the surface of a metal foam C to obtain a support catalyst.
[0042] A catalytic active layer according to the present invention can be particularly easily provided in the metal foam C according to the present invention, because the aluminum oxide skin formed on the surface of the metal foam C ensures excellent bonding of the supporting oxide and provides long durability and lifespan, as well as very high mechanical stability, especially wear resistance.
[0043] A catalytic active layer comprising at least one supporting oxide and at least one catalytic active component can be applied to metal foam C, for example, by drawing in or pumping a coating suspension through the continuous cavities of open-pore metal foam C. This is possible because, in terms of the continuous cavities of metal foam C and high dimensional stability, metal foam C is similar to monolithic substrates used in automotive exhaust catalysts. The coating suspension may also be applied by dipping (referred to as "dip coating") or spraying (referred to as "spray coating"). In principle, which of the application processes known in the prior art is preferred depends, first, on the composition and flow characteristics of the coating suspension, and second, on the actual structure of the metal foam according to the present invention. Dip coating has the greatest possible tolerance to various characteristics of the coating suspension and is therefore suitable for coating all metal foams of the present invention.
[0044] According to the present invention, after contact with a coating suspension, the coated metal foam is calcined in step (e) to obtain a supporting catalyst. The catalytic active layer according to the present invention comprises at least one supporting oxide. For the purposes of the present invention, the supporting oxide is typically 50 to 200 m 2 It is an inorganic oxide having a high specific surface area of 1 / g. This supporting oxide has multiple functions in the finished catalyst: firstly, it serves to increase, at a microscopic level, the macroscopic, i.e., geometric surface area provided by the metal foam of the present invention, which is referred to in the context of the present invention as the contact area between the reaction medium and the catalyst. Secondly, it itself can interact with catalytic active species to influence the reaction process. For example, the selection of the supporting oxide influences the selectivity of complex hydrogenation reactions in which multiple functional groups of the organic substrate molecule can react with hydrogen. Additionally, it provides a microscopic surface on which catalytic active components are distributed. It also forms a matrix on which additional functional components and additives that serve to tune specific catalytic functions may be distributed when the catalyst is customized for a specific application.
[0045] The supporting oxide is preferably selected from the group consisting of aluminum oxide, silicon dioxide, titanium oxide, and mixtures thereof.
[0046] A transition metal or a transition metal compound is used as a catalytic active component of the catalytic active layer, and the transition metal is preferably selected from the group consisting of iron, ruthenium, osmium, cobalt, rhodium, iridium, nickel, palladium, platinum, cerium, copper, silver, gold, and mixtures thereof.
[0047] As additional functional components and additives, the catalytic layer may preferably comprise an inorganic oxide selected from oxides of alkaline earth metals, oxides of transition metals, oxides of rare earths, oxides of aluminum and gallium, oxides of silicon, germanium and tin, and / or mixtures thereof.
[0048] The catalytic active layer according to the present invention may comprise one or more supporting oxides, one or more catalytic active components, and optionally additionally functional components and additives.
[0049] To apply a catalyst to the metal foam of the present invention, a coating suspension is prepared by introducing components into water. The catalyst components are applied to the supporting oxide by pre-impregnating the supporting oxide with a suitable metal salt solution (precursor solution), by adding the precursor solution directly to the coating suspension, and optionally by precipitation or chemically induced deposition or decomposition of the precursor compound on the already suspended supporting oxide(s). Functional components and additives may also be introduced in this manner or added directly as solid oxides. Alternatively, it is possible to add all components of the catalyst generated from a soluble precursor by a re-impregnation method after the supporting oxide has been applied to the metal foam of the present invention. The choice of the preparation method is determined by the characteristics of the resulting catalyst to be established and the target composition.
[0050] In step (e) of the method of the present invention, fixation of the catalytic active layer applied to the metal foam is preferably achieved by calcination in air.
[0051] According to the present invention, calcination is performed in air at a temperature of 200°C to 800°C for 1 minute to 8 hours. According to the present invention, calcination is preferably performed in air at a temperature of 200°C to 680°C for 1 to 480 minutes. Particularly preferably, calcination is performed in air at a temperature of 300°C to 650°C for 1 to 480 minutes.
[0052] According to the present invention, the thermal oxidation of step d) is preferably performed in air at a temperature of 200°C to 680°C for 1 to 60 minutes, and the calcination of step e) is preferably performed in air at a temperature of 200°C to 680°C for 1 to 480 minutes.
[0053] The method for manufacturing a support catalyst according to the present invention significantly reduces manufacturing costs compared to conventional methods. In addition, the metal foam of the present invention forms a pure aluminum oxide layer that acts as a barrier to diffusion between the support material and the catalyst layer due to an excess of Al on the surface.
[0054] The aluminum oxide on the surface of the metal foam and the aluminum oxide-based catalyst layer as a supporting oxide constitute a system of the same type. Therefore, the coefficient of expansion is similar, flaking under thermal stress is minimal, and the compound stability following calcination is excellent.
[0055] In addition to the method according to the present invention for producing a supporting catalyst, the present invention also provides the use of the supporting catalyst and the catalyst in chemical modification that can be obtained by these methods.
[0056] The support catalyst according to the present invention can be advantageously used, for example, in a chemical fixed-bed process. Specific details for implementing the invention
[0057] Examples of Co foam
[0058] 1. Provision of metal foam
[0059] Six metal foams made of cobalt (af) were provided (manufacturer: AATM, dimensions: 100 mm x 100 mm x 2 mm, weight per unit area: 1000 g / m², average pore diameter: 580 μm), which were manufactured by electrolytically depositing cobalt into a polyurethane foam and then pyrolyzing the plastic components.
[0060] 2. Applications of Aluminum
[0061] Next, a binder solution (2.5 wt% polyethyleneimine in water) was first sprayed onto metal foams a, b, c, d, e, and f, and then powdered aluminum (Manufacturer: AMG, average particle size: < 63 µm, containing 3 wt% added ethylenebis(stearamide)) was applied as a dry powder (approx. 400 g / m²). 2 It was applied in the form of ).
[0062] 3. Heat treatment
[0063] Next, metal foams a, b, c, d, and e were heat-treated in a furnace under a nitrogen atmosphere. First, the furnace was heated from room temperature to a maximum temperature within about 15 minutes, maintained for a certain period of time, and then quenched by contacting it with a nitrogen atmosphere at 200°C.
[0064] Maximum temperature of metal foams a, d, and e:
[0065] 700℃ for 2 minutes
[0066] Temperature progression of metal foam b:
[0067] 600℃ for 2 minutes
[0068] Temperature progression of metal foam c:
[0069] 750℃ for 2 minutes
[0070] 4. Determination of the degree of alloying
[0071] Next, the degree of alloy formation in the metal foams was determined. This was done by examining the cross-sections of the metal foams using a microscope and a scanning electron microscope. In metal foams a, d, and e, surface alloy formation occurred but had non-alloy regions remaining within the metal foam, whereas in the case of metal foam b, no alloy formation occurred, and in the case of metal foam c, alloy formation was so advanced that no non-alloy regions remained within the metal foam.
[0072] 5. Oxidation Treatment
[0073] Next, oxidation treatment was performed on metal foams a and d.
[0074] Metal foam a was exposed to an oxidizing gas atmosphere while heated. This was achieved by heating the metal foam to 700°C in a furnace with the introduction of air.
[0075] Metal foam d was first brought into contact with an alkaline solution (5 wt% aqueous NaOH at 20°C for 10 minutes). A white precipitate formed on the foam. The precipitate was aluminum converted into aluminum hydroxide. Subsequently, metal foam d was dried in air. The dried metal foam with the white precipitate was pre-oxidized in a preheated furnace at 700°C in a normal atmosphere, at which point the aluminum hydroxide was converted into aluminum oxide.
[0076] Oxidative pretreatment has multiple functions:
[0077] - Protection of supporting material against additional oxidation
[0078] - Adhesion promoter between metal and ceramic systems
[0079] - Diffusion barrier of alloying elements on the supporting material into the catalytic ceramic layer.
[0080] 6. Comparison Processing
[0081] An aluminum oxide layer was provided to a metal foam f that had previously remained in an untreated state, as described in the prior art (see WO95 / 11752A1, Example 3). This was accomplished by completely immersing the metal foam f in a saturated sodium aluminate solution for 3 hours, then tilting it back and forth in deionized water until the hydrolysis reaction subsided, and finally heating it at 500°C for 3 hours under the inflow of air.
[0082] 7. Application of the catalytic active layer
[0083] Next, a catalytic active layer was applied to metal foams a, d, e, and f by spraying. This was accomplished by wetting the metal foams with water. Subsequently, a 2.5% polyethyleneimine suspension was stirred with high surface area χ-aluminum oxide. A mixture of water / polyethyleneimine and aluminum oxide was sprayed. After spraying, a drying process was carried out in air inside a drying oven at 140°C for 30 minutes. For calcination, the samples were baked in a furnace at 650°C for 5 hours. The coating, drying, and calcination processes were repeated several times until the desired amount of coating was applied.
[0084] 8. Investigation of the obtained support catalyst
[0085] Finally, the obtained support catalysts were examined, in particular, to investigate the resistance of the catalytic active layer on the metal foam to mechanical stress. In many cases, a scratch test can be performed to determine the quality of adhesion of the oxidative catalytic active layer to the support foam. However, in the case of the present invention, this test is impossible due to the irregular structure of the foam. Therefore, the mechanical stability of the catalytic active layer was investigated by a temperature change test, which provides a measure of the quality of adhesion of the oxide layer to the support foam. This was performed by heating metal foams a, d, e, and f to 500°C and then quenching them in cold water. Subsequently, the amount of loss, which is the mass of the catalytic layer detached from each sample, was determined by filtration, drying, and weighing of the detached material.
[0086] The results were as follows:
[0087] Metal foam a and d: 3 mg loss
[0088] Metal foam f: 10mg loss
[0089] Metal foam e: 50mg loss
[0090] The catalytic active layers of metal foams a and d had high resistance to mechanical stress, whereas the resistance of the catalytic active layer of metal foam f was significantly low, and the resistance of the catalytic active layer of metal foam e was very low.
[0091] Examples of NiCo foam
[0092] 1. Provision of metal foam
[0093] Six metal foams (af) made of nickel-cobalt were provided (manufacturer: AATM, dimensions: 100 mm x 100 mm x 2 mm, weight per unit area: 1000 g / m², average pore diameter: 580 µm), which were manufactured by electrolytically depositing nickel into a polyurethane foam, depositing cobalt into the nickel, and then pyrolyzing the plastic components.
[0094] 2. Applications of Aluminum
[0095] Next, a binder solution (2.5 wt% polyethyleneimine in water) was first sprayed onto metal foams a, b, c, d, e, and f, and then powdered aluminum (Manufacturer: AMG, average particle size: < 63 µm, containing 3 wt% added ethylenebis(stearamide)) was applied as a dry powder (approx. 400 g / m²). 2 It was applied in the form of ).
[0096] 3. Heat treatment
[0097] Next, metal foams a, b, c, d, and e were heat-treated in a furnace under a nitrogen atmosphere. First, the furnace was heated from room temperature to a maximum temperature within about 15 minutes, maintained for a certain period of time, and then quenched by contacting it with a nitrogen atmosphere at 200°C.
[0098] Maximum temperature of metal foams a, d, and e:
[0099] 700℃ for 2 minutes
[0100] Temperature progression of metal foam b:
[0101] 600℃ for 2 minutes
[0102] Temperature progression of metal foam c:
[0103] 750℃ for 2 minutes
[0104] 4. Determination of the degree of alloying
[0105] Next, the degree of alloy formation in the metal foams was determined. This was done by examining the cross-sections of the metal foams using a microscope and a scanning electron microscope. In metal foams a, d, and e, surface alloy formation occurred but had non-alloy regions remaining within the metal foam, whereas in the case of metal foam b, no alloy formation occurred, and in the case of metal foam c, alloy formation was so advanced that no non-alloy regions remained within the metal foam.
[0106] 5. Oxidation Treatment
[0107] Next, oxidation treatment was performed on metal foams a and d.
[0108] Metal foam a was exposed to an oxidizing gas atmosphere while heated. This was achieved by heating the metal foam to 700°C in a furnace with the introduction of air.
[0109] Metal foam d was first brought into contact with an alkaline solution (5 wt% aqueous NaOH at 20°C for 10 minutes). A white precipitate formed on the foam. The precipitate was aluminum converted into aluminum hydroxide. Subsequently, metal foam d was dried in air. The dried metal foam with the white precipitate was pre-oxidized in a preheated furnace at 700°C in a normal atmosphere, at which point the aluminum hydroxide was converted into aluminum oxide.
[0110] Oxidative pretreatment has multiple functions:
[0111] - Protection of supporting material against additional oxidation
[0112] - Adhesion promoter between metal and ceramic systems
[0113] - Diffusion barrier of alloying elements on the supporting material into the catalytic ceramic layer.
[0114] 6. Comparison Processing
[0115] An aluminum oxide layer was provided to a metal foam f that had previously remained in an untreated state, as described in the prior art (see WO95 / 11752A1, Example 3). This was accomplished by completely immersing the metal foam f in a saturated sodium aluminate solution for 3 hours, then tilting it back and forth in deionized water until the hydrolysis reaction subsided, and finally heating it at 500°C for 3 hours under the inflow of air.
[0116] 7. Application of the catalytic active layer
[0117] Next, a catalytic active layer was applied to metal foams a, d, e, and f by spraying. This was accomplished by wetting the metal foams with water. Subsequently, a 2.5% polyethyleneimine suspension was stirred with high surface area χ-aluminum oxide. A mixture of water / polyethyleneimine and aluminum oxide was sprayed. After spraying, a drying process was carried out in air inside a drying oven at 140°C for 30 minutes. For calcination, the samples were baked in a furnace at 650°C for 5 hours. The coating, drying, and calcination processes were repeated several times until the desired amount of coating was applied.
[0118] 8. Investigation of the obtained support catalyst
[0119] Finally, the obtained support catalysts were examined, in particular, to investigate the resistance of the catalytic active layer on the metal foam to mechanical stress. In many cases, a scratch test can be performed to determine the quality of adhesion of the oxidative catalytic active layer to the support foam. However, in the case of the present invention, this test is impossible due to the irregular structure of the foam. Therefore, the mechanical stability of the catalytic active layer was investigated by a temperature change test, which provides a measure of the quality of adhesion of the oxide layer to the support foam. This was performed by heating metal foams a, d, e, and f to 500°C and then quenching them in cold water. Subsequently, the amount of loss, which is the mass of the catalytic layer detached from each sample, was determined by filtration, drying, and weighing of the detached material.
[0120] The results were as follows:
[0121] Metal foam a and d: 4 mg loss
[0122] Metal foam f: 12mg loss
[0123] Metal foam e: 48mg loss
[0124] The catalytic active layers of metal foams a and d had high resistance to mechanical stress, whereas the resistance of the catalytic active layer of metal foam f was significantly low, and the resistance of the catalytic active layer of metal foam e was very low.
Claims
Claim 1 A method for manufacturing a supported catalyst comprising the following steps: (a) providing a metal foam A made of metallic cobalt, an alloy of nickel and cobalt, or an array of overlapping layers of nickel and cobalt; (b) applying an aluminum-containing powder MP to the metal foam A to obtain a metal foam AX; (c) heat-treating the metal foam AX to achieve the formation of an alloy between the metal foam A and the aluminum-containing powder MP to obtain a metal foam B, wherein the maximum temperature during the heat treatment of the metal foam AX is within the range of 680 to 715°C and the total duration of the heat treatment in the temperature range of 680 to 715°C is 5 to 240 seconds; (d) oxidizing the metal foam B to obtain a metal foam C; (e) forming a catalytic active layer comprising at least one supporting oxide and at least one catalytic active component on the surface of the metal foam C at least Step of obtaining a supporting catalyst by applying it to a part. Claim 2 A method for manufacturing a supporting catalyst, wherein the oxidation treatment of metal foam B in step (d) is selected from - heating metal foam B in contact with an oxidizing gas atmosphere without prior formation of aluminum hydroxide on the surface of the metal foam, and - heating metal foam B in contact with an oxidizing gas atmosphere after aluminum hydroxide has been prior formed on the surface of the metal foam. Claim 3 A method for manufacturing a supporting catalyst according to claim 1, wherein, for the oxidation treatment of metal foam B in step (d), metal foam B is heated by contacting it with an oxidizing gas atmosphere without the prior formation of aluminum hydroxide on the surface of the metal foam. Claim 4 A method for manufacturing a supporting catalyst according to claim 3, wherein heating by contacting with an oxidizing gas atmosphere is performed in air at a temperature of 200°C to 700°C for a period of 1 to 60 minutes. Claim 5 A method for manufacturing a supporting catalyst according to claim 1, wherein for the oxidation treatment of metal foam B in step (d), metal foam B is heated in contact with an oxidizing gas atmosphere after aluminum hydroxide is formed on the surface of the metal foam. Claim 6 A method for manufacturing a supporting catalyst according to claim 5, wherein aluminum hydroxide is formed on the surface by contacting a metal foam with an alkaline aqueous solution. Claim 7 A method for manufacturing a supporting catalyst according to claim 6, wherein the alkaline aqueous solution comprises sodium hydroxide, potassium hydroxide, lithium hydroxide, or a combination thereof, and the metal foam is in contact with the alkaline aqueous solution for a period of 30 minutes or less. Claim 8 A method for manufacturing a supporting catalyst according to claim 5, wherein heating by contacting an oxidizing gas atmosphere after aluminum hydroxide has been formed on the surface of a metal foam body is performed in air at a temperature of 200°C to 700°C for a period of 1 to 60 minutes. Claim 9 A method for manufacturing a supporting catalyst according to claim 1, wherein the supporting oxide of the catalytic active layer applied in step (e) is selected from the group consisting of aluminum oxide, silicon dioxide, titanium oxide, and mixtures thereof. Claim 10 A method for manufacturing a supporting catalyst according to claim 1, wherein the catalytic active component is a transition metal or a transition metal compound, and the transition metal is selected from the group consisting of iron, ruthenium, osmium, cobalt, rhodium, iridium, nickel, palladium, platinum, cerium, copper, silver, gold, and mixtures thereof. Claim 11 A supporting catalyst obtainable by a method according to any one of claims 1 to 10. Claim 12 In claim 11, the support catalyst is a support catalyst used for chemical modification.
Citation Information
Patent Citations
Surface Modified Metallic Foam Body, Process For Its Production And Use Thereof
CN103966473A
Catalyst comprising a metalic support and process for the production of olefins
CN1798717A
Surface modified metallic foam body, process for its production and use thereof
EP2764916A1
Surface modified metal foam, method of making same, and use thereof
JP2016513173A
Method of coating catalyst carrier layer of metal-metal oxide, method of depositing active catalyst particles onto metal substrates for preparing metal monolith catalyst modules, and module thereby
US20040086637A1