Eco-friendly organic and inorganic binders and semi-combustible fireproof insulation materials impregnated therewit
A semi-noncombustible organic-inorganic binder for fire doors, using a water-soluble acrylic resin and inorganic components, addresses eco-friendliness and insulation needs, ensuring rapid adhesion and fire resistance with maintained strength and thermal performance.
Patent Information
- Application Number
- KR1020240113182
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Existing insulation materials for fire doors lack eco-friendliness, strength, and effective thermal insulation and heat shielding properties, necessitating the development of a semi-fireproof organic-inorganic binder composition that adheres quickly and provides excellent space-filling and soundproofing effects.
A semi-noncombustible organic-inorganic binder composed of a water-soluble acrylic resin, bentonite, perlite, calcium carbonate, and additives like dispersants and curing agents, which is applied via a spray method to glass fibers, ensuring rapid adhesion and fire resistance.
The binder provides excellent adhesion, flame resistance, and maintains strength and thermal insulation performance, suitable for fire doors and other building materials, with minimal moisture impact and high thermal conductivity.
Smart Images

Figure 112024092063527-PAT00004_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an eco-friendly semi-fireproof organic-inorganic binder composition and a semi-fireproof insulation material for fire doors impregnated therewith. Specifically, the invention relates to an eco-friendly semi-fireproof organic-inorganic binder composition and an insulation material for fire doors impregnated therewith, which is composed of a semi-fireproof material that is excellent in thermal insulation performance and soundproofing effect due to its ability to adhere to the surface of an adhesive in a short period of time, thereby enabling installation without cutting the insulation material, and also has good space-filling and filling properties for buildings. Background Technology
[0002] Non-combustible insulation materials for buildings with improved thermal insulation performance are characterized by not burning easily or minimizing the propagation of flames in the event of a fire. These materials can significantly enhance the fire safety of buildings, and representative non-combustible insulation materials include mineral wool, glass wool, calcium silicate, aerogel, and inorganic foam insulation. Furthermore, due to recent advancements in domestic and international construction technology, the performance requirements for insulation materials are gradually becoming higher. Additionally, as laws and regulations in developed countries tend to become standardized, the required physical properties of insulation materials, depending on their type and application, are also becoming more universal.
[0003] Therefore, in order to respond to environmental regulations, research and development regarding improved non-combustibility and eco-friendly insulation materials is actively being carried out in the insulation industry. In particular, since it is very important for insulation materials for fire doors to have sufficient strength to prevent twisting or bending while providing thermal insulation and heat shielding functions, organic and inorganic binders impregnated into fire doors are required to be eco-friendly and possess sufficient strength and thermal insulation and heat shielding functions.
[0004] Regarding prior art related to insulation materials for fire doors, Korean published patent No. 2020-0107415 discloses a technology relating to an insulation material for fire doors with excellent thermal insulation and heat shielding properties, comprising a core material mixed with fumed silica powder, expanded perlite powder, an opacifying agent, and inorganic fibers between a lower outer shell and an upper outer shell woven with glass fibers, and stitching four corners where the lower outer shell and the upper outer shell meet; and Korean registered patent No. 1412523 discloses a fireproof insulation material for fire doors manufactured by heat-pressing molding with a molding machine and then naturally drying a mixture obtained by mixing expanded vermiculite, non-expanded vermiculite, porous silica powder, an IR opacifying agent, sodium silicate, and fast-setting cement, and comprises a fiber tube (100) formed by weaving a plurality of ultrafine inorganic fibers (20) into a tube having a diameter of 10 mm to 30 mm; A fiber plate (200) formed in the shape of a plate, wherein the space between the plurality of ultrafine inorganic fibers (20) forming the fiber tube (100) is filled with an inorganic binder (110); and the plurality of fiber tubes (100) are stacked to form a plate. A fire door insulation board made of glass fiber material is disclosed, comprising a plurality of fiber tubes (100) forming the fiber board (200) and a perlite foam particle (210) filled in the space between them, and a basic unit (300) formed by stacking a plurality of fiber boards (200). Additionally, Korean registered patent No. 1162562 discloses a non-combustible high-performance insulation material having a thermal conductivity value of 0.025 W / mK or less, comprising 40 to 99 weight% of silica powder, 0.5 to 20 weight% of reinforcing fibers consisting of organic fibers alone or a mixture of organic and inorganic fibers, and 0 to 50 weight% of a radiant heat blocking additive and reinforcing material, which is dry-mixed and press-molded, and then wrapped (1 to 2 times) on six sides with a heat-shrink film. Prior art literature
[0005] Korean Published Patent No. 2020-0107415 Korean Registered Patent No. 1412523 Korean Published Patent No. 2022-0129753 Korean Registered Patent No. 1162562 The problem to be solved
[0006] The problem to be solved by the present invention is to provide an eco-friendly organic-inorganic binder composition and a semi-fireproof insulation material for fire doors using the same. This invention is an improvement upon Patent Application No. 2023-93988, which was developed and filed by the inventor. More specifically, the purpose is to provide a semi-fireproof organic-inorganic binder in which an eco-friendly water-soluble organic binder is combined with an inorganic insulation material for the manufacture of a semi-fireproof insulation material for fire doors, and a semi-fireproof insulation material for fire door interiors using the same. means of solving the problem
[0007] As a means of solving the problem, the semi-noncombustible organic-inorganic binder for fire doors is composed of a water-soluble organic binder, a water-soluble inorganic binder, a dispersant, a viscosity modifier, a pH modifier, an auxiliary flame retardant, and a curing agent.
[0008] To examine this in detail, one embodiment of the semi-noncombustible organic-inorganic binder for fire doors according to the present invention comprises a water-soluble acrylic resin composition as an organic binder composed of an acrylic copolymer, poly(acrylamide), polyvinylpyrrolidone, polyvinyl alcohol, and an ethylene-vinyl alcohol copolymer, an inorganic binder composed of bentonite, perlite, and calcium carbonate, and additives composed of a dispersant, a viscosity modifier, a pH modifier, an auxiliary flame retardant, and a curing agent.
[0009] An organic-inorganic binder composition is prepared by composing an organic-inorganic binder composition with a composition ratio of 200 parts by weight of an inorganic binder, 5 to 10 parts by weight of a dispersant, 2 to 5 parts by weight of a viscosity modifier, 3 to 5 parts by weight of a pH modifier, 30 to 45 parts by weight of an auxiliary flame retardant, and 20 to 30 parts by weight of a water-soluble curing agent, based on 100 parts by weight of a water-soluble acrylic resin composition, and then mixing 30 to 50 parts by weight of the above organic-inorganic binder composition with 100 parts by weight of water to produce an eco-friendly organic-inorganic binder having a solid content of 35 to 45% by weight, a viscosity of 2,000 to 4,000 cps, and a pH of 5.5 to 7.5.
[0010] The water-soluble acrylic resin composition according to the present invention is an acrylic resin prepared by polymerizing monomers of alkyl acrylates having 6 to 12 carbon atoms as a main component to enhance adhesion and strength, and contains many polar groups such as hydroxyl, carboxyl, sulfonic acid, amino, amide, methylol, oxyethylene, etc. in the molecular chain.
[0011] The bentonite, perlite, and calcium carbonate according to the present invention are heat-resistant inorganic ceramic components selected to ensure non-combustibility, and bentonite has good affinity and dispersibility with water, which improves the storage stability of the binder, while perlite has the characteristic of having a low expansion / shrinkage rate due to heat.
[0012] In addition, bentonite, perlite, and calcium carbonate are used as raw materials mixed with water-soluble acrylic binders and are inorganic materials added to control viscosity and mitigate fire hazards. In particular, perlite is a material that has pores, making it resistant to fire, as well as having improved thermal conductivity and excellent durability against moisture.
[0013] Bentonite has the property of absorbing up to 10 times its own volume of water when it comes into contact with moisture, which has the advantage of being able to control viscosity, non-flammability, and enhance the strength characteristics of products.
[0014] Calcium carbonate has the property of generating heat upon contact with moisture or heat, which has an excellent effect on improving drying speed and product strength.
[0015] The dispersant in the present invention is ABDM (Alkyl benzyl dimethyl ammonium chloride), a water-soluble dispersant capable of preventing phase separation between inorganic substances and an aqueous solution (water). The present invention relates to an organic acid pH regulator composed of 40 to 50 weight% water, 10 to 40 weight% sodium acetate, 1 to 6 weight% adipic acid, 6 to 10 weight% citric acid, and 1 to 20 weight% glacial acetic acid, in order to improve product shelf life by enhancing antibacterial activity as well as pH control. It has the advantages of excellent antibacterial effect and the ability to improve shelf life without affecting product quality. This is a water-soluble product that utilizes water, and since organic substances such as mold may occur, especially during the hot and humid rainy season and summer, it is possible to secure antibacterial properties and shelf life through pH control. In particular, when inorganic substances are stirred in an aqueous solution, it helps them dissolve well, thereby affecting the uniform particle size of the product.
[0016] The semi-noncombustible insulation material for fire doors according to the present invention is a spray-type insulation board capable of a spray or impregnation coating method. The main component, the inorganic fiber, mainly consists of glass fiber, mineral wool, and ceramic wool. These are crushed into various sizes, and long fibers (25–50 mm) and short fibers (5.0–20 mm) are mixed in a 5:5 ratio. Then, a dust suppressant (dust oil) is sprayed to suppress airborne dust during installation. As the main component of a water-soluble binder and a hardener are simultaneously sprayed into the atmosphere through a discharge port, the organic-inorganic blended binder and hardener are simultaneously sprayed into the air onto the bonding surface of the spray-type insulation board to be insulated. Upon attachment, crosslinking occurs due to the electrostatic attraction between cations and anions based on chemical ionic bonding, which allows for adhesion and curing simultaneously. Over time It has the characteristic that hardness and adhesion increase as the contained moisture evaporates over time. Effects of the invention
[0017] The semi-noncombustible organic-inorganic binder according to the present invention exhibits excellent adhesion between glass fibers used as insulation for fire doors and demonstrates flame resistance, making it particularly suitable as a binder when manufacturing insulation for fire doors. However, it is not limited to this and can be applied to building materials and interior / exterior materials vulnerable to fire. It can be used for various purposes such as ceilings, walls, windows and doors, interior wall finishing materials, hot and cold water protection covers, interior finishing materials, portable toilets, and livestock sheds.
[0018] In addition, the thermal insulation material for fire doors according to the present invention exhibits characteristics of a semi-noncombustible grade, including minimal changes in strength and thickness, minimal reduction in initial strength due to moisture, and excellent flame resistance. Brief explanation of the drawing
[0019] Fig. 1: This is a fire door board of the present invention. Fig. 2: This is a test report on organic volatile organic compounds (VOCs) of the organic-inorganic binder of the present invention. Fig. 3: This is a test report on the compressive strength of the present invention. Fig. 4: This is a test report on the hot shrinkage of the present invention. Fig. 5: This is a test report on the thermal conductivity of the thermal insulation material for fire doors according to the present invention. Fig. 6: This is a test report on the non-combustibility of the thermal insulation material for fire doors according to the present invention. Fig. 7: This is a test report on the water repellency of the organic-inorganic binder of the present invention. Fig. 8: This is a test report on organic volatile organic compounds (VOCs) of the organic-inorganic binder board of the present invention. Specific details for implementing the invention
[0020] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. In describing the present invention, detailed descriptions of related known functions or configurations are omitted if it is determined that such detailed descriptions may unnecessarily obscure the essence of the present invention. Furthermore, terms described below are defined considering their functions in the present invention, and these may vary depending on the intentions of users or operators or judicial precedents. Therefore, such definitions should be based on the content throughout this specification. Although the eco-friendly organic-inorganic binder composition according to the present invention and the semi-noncombustible thermal insulation material for fire doors impregnated therewith are described in more detail, the present invention is not limited by the contents and embodiments described below.
[0021] The eco-friendly organic-inorganic binder according to the present invention is composed of an organic-inorganic binder composition comprising 200 parts by weight of an inorganic binder, 5 to 10 parts by weight of a dispersant, 2 to 5 parts by weight of a viscosity modifier, 3 to 5 parts by weight of a pH modifier, and 30 to 45 parts by weight of an auxiliary flame retardant, based on 100 parts by weight of a water-soluble acrylic resin composition, and then 30 to 50 parts by weight of the above organic-inorganic binder composition and 5 to 10 parts by weight of a water-soluble curing agent are mixed with 100 parts by weight of water to form an eco-friendly organic-inorganic binder having a solid content of 35 to 45% by weight, a viscosity of 2,000 to 4,000 cps, and a pH of 5.5 to 7.5.
[0022] The water-soluble acrylic resin composition according to the present invention is a product based on an acrylic resin that is soluble in water and used for various purposes. It is prepared by polymerizing monomers of alkyl acrylates having 6 to 12 alkyl groups as shown in <Chemical Formula 1> below, and is a polymer resin widely known as an acrylic resin containing many polar groups such as hydroxyl, carboxyl, sulfonic acid, amino, amide, methylol, oxyethylene, etc., in its molecular chain, so it can be easily selected and used.
[0023]
[0024] The above acrylic binder has high adhesion strength with inorganic materials such as glass fiber, mineral wool, and carbon fiber. In order to synthesize a binder capable of shortening the curing speed, the most basic method involves inducing a crosslinking reaction through ionic bonding by the combination of COO- ions contained in polyvinyl terminal groups with Na+, Ca+, Ba+, K+, NH+, and Mg+ cations, and the improvement in adhesion strength can be achieved by increasing the crosslinking density.
[0025] In addition, based on the above-mentioned water-soluble binder and hardener, and since the angle at which the binder and inorganic fibers are attached to fire doors, walls, roofs, etc., must be 60° or more from the floor, a fast curing speed and instantaneous adhesion are required, and the hardener has the structure of <Chemical Formula 2> below, and a viscosity of 200 to 400 cps is suitable.
[0026] <Chemical Formula 2>
[0027] Bentonite, perlite, and calcium carbonate are heat-resistant inorganic ceramic components selected to ensure non-combustibility. Bentonite has good affinity and dispersibility with water, which improves the storage stability of the binder, while perlite has the characteristic of having a low expansion / shrinkage rate due to heat.
[0028] The above bentonite, perlite, and calcium carbonate are used as raw materials mixed with a water-soluble acrylic binder and are inorganic materials added to control viscosity and mitigate fire hazards. In particular, perlite has pores, making it resistant to fire, as well as a material with improved thermal conductivity and excellent durability against moisture.
[0029] The dispersant according to the present invention is used to prevent the phenomenon of layer separation between the inorganic ceramic component and the aqueous solution, and ABDM (Alkyl benzyl dimethyl ammonium ahlorid), a water-soluble dispersant, is used.
[0030] In order to improve the shelf life of a product by controlling pH and enhancing antibacterial power, the present invention uses an organic acid pH regulator composed of 40 to 50 weight% water, sodium acetate, 10 to 40 weight% carboxyl groups, 1 to 6 weight% adipic acid, 6 to 10 weight% citric acid, and 1 to 20 weight% glacial acetic acid. This provides the advantage of having excellent antibacterial effects and improving shelf life without affecting the quality of the product.
[0031] And. The fire-resistant semi-noncombustible thermal insulation material using an eco-friendly organic-inorganic binder according to the present invention
[0032] 1). A first process of preparing a glass long fiber mat (1) by cutting the glass long fibers into a certain size,
[0033] 2). A second process of preparing an organic-inorganic binder composition comprising 200 parts by weight of an inorganic binder, 5 to 10 parts by weight of a dispersant, 2 to 5 parts by weight of a viscosity modifier, 3 to 5 parts by weight of a pH modifier, and 30 to 45 parts by weight of an auxiliary flame retardant, based on 100 parts by weight of a water-soluble acrylic resin composition in the glass long fiber mat of the first process, and then mixing 30 to 50 parts by weight of the above organic-inorganic binder composition and 5 to 10 parts by weight of a water-soluble curing agent with 100 parts by weight of water to produce an eco-friendly organic-inorganic binder having a solid content of 35 to 45% by weight, a viscosity of 2,000 to 4,000 cps, and a pH of 5.5 to 7.5; and
[0034] 3). The binder-impregnated glass long fiber mat (2) of the second process is first pre-dried, and then dried while being pressed by a heat press at 220 to 250°C to produce a semi-fireproof insulation material for fire doors through a third process.
[0035] The first process according to the present invention is a process of preparing glass long fibers, which are the material of the insulation material, by cutting them to a certain standard size. Specifically, the glass long fibers are cut into E-glass fibers into a mat with a width of 1m × 1m (width × length) and a thickness of 1.5 to 10mm. When manufacturing insulation material of a larger standard size, it is possible to use the cut glass long fiber mats by laminating them.
[0036] The second process according to the present invention is a process of impregnating the glass long fiber mat of the first process with the environmentally friendly organic-inorganic binder described above. Specifically, it is composed of installing a conveyor in a container of a certain size filled with the environmentally friendly organic-inorganic binder and passing the glass long fiber mat through it at a certain speed to impregnate it with the environmentally friendly organic-inorganic binder.
[0037] The impregnation amount of the above-mentioned environmentally friendly organic-inorganic binder (A) is 2.5 to 3.5 kg / m², and the passing speed is preferably 5 to 20 m / min.
[0038] The third process according to the manufacturing method of the present invention is a process of drying glass long fibers impregnated with an environmentally friendly organic-inorganic binder, and consists of coating or impregnating an environmentally friendly organic-inorganic binder onto a glass long fiber mat, and, as a major process affecting the strength and shape maintenance of the product, pre-drying by microwave and drying by heat press.
[0039] The above pre-drying is performed by passing a glass long fiber mat impregnated with an environmentally friendly organic-inorganic binder (A) through a roller while pressing it to allow the binder to penetrate into the glass long fiber mat, and then pre-drying it at 200 to 300°C by microwave, and the above drying by heat press is performed by drying the pre-dried glass long fiber mat by applying pressure for about 150 to 300 seconds with a heat press heated to 200 to 250°C.
[0040] Below, the environmentally friendly organic-inorganic binder of the present invention and the semi-noncombustible thermal insulation material for fire doors using the same will be explained in more detail through <Examples> and <Test Examples>.
[0041] <Example 1> Preparation of a water-soluble organic-inorganic binder composition
[0042] An organic-inorganic binder composition is prepared by comprising 200 parts by weight of an inorganic binder, 5 to 10 parts by weight of a dispersant, 2 to 5 parts by weight of a viscosity modifier, 3 to 5 parts by weight of a pH modifier, and 30 to 45 parts by weight of an auxiliary flame retardant, based on 100 parts by weight of a water-soluble acrylic resin composition.
[0043] <Example 2> Manufacture of Organic and Inorganic Binders for Fire Doors
[0044] An organic binder for fire doors was prepared by mixing 50 parts by weight of the above water-soluble organic-inorganic binder composition and 5 parts by weight of a water-soluble curing agent with 100 parts by weight of water, having a solid content of 35% by weight, a viscosity of 2,000 to 4,000 cps, and a pH of 5.5 to 7.5.
[0045] <Example 3> Manufacture of insulation material for fire doors
[0046] A semi-noncombustible thermal insulation material for a fire door was manufactured using an E-GLSAA fiber mat with dimensions of 1m × 1m (width × length) and a thickness of 5mm in the semi-noncombustible organic-inorganic binder for a fire door manufactured in <Example 2> above, in the following manner.
[0047] E-glsaa fiber mats are supplied using a conveyor, and then impregnated with the semi-flammable organic-inorganic binder using a spray nozzle with a diameter of 0.2 to 6.0 mm, so that the impregnation amount of the semi-flammable organic-inorganic binder is 3 kg / m². After passing the glass long fiber mat through the impregnated mat while compressing it with a roller, the E-glsaa fiber mat is produced by pre-drying it primarily by maintaining it at 250°C using a microwave. The pre-dried E-glsaa fiber mat is then dried by applying pressure for 250 seconds using a heat press heated to 230°C to produce a semi-flammable insulation material for fire doors.
[0048] <Test Example 1>
[0049] The results of tests on the human health hazards of the organic-inorganic binder concentrate for fire doors prepared in <Example 2> above, and on the thermal conductivity, compressive strength, and non-flammability of the thermal insulation material for fire doors prepared in <Example 3> above, are shown in [Table 1] below.
[0050]
[0051] In addition, when the solid content of the binder stock solution is 20–25%, the viscosity is 1,600 cps, the dispersion particle size is suitable to be 100 µm or less, and the organic volatile substances of the binder itself are 0.56 µg / m³ 3It was confirmed below that this is an eco-friendly, water-soluble binder that is harmless to the human body. Furthermore, when an insulation board is manufactured using the water-soluble binder of the present invention, the thermal conductivity—the most important characteristic of an insulation material—is 0.038 W / mk, and the hot shrinkage temperature is 786°C, indicating that no deformation occurs due to temperature; additionally, the compressive strength is 355 kPa and the water repellency is 100%. This means that the board does not absorb moisture from surrounding water vapor or rainwater, maintaining its shape, and the thermal conductivity remains constant, thereby exhibiting excellent thermal insulation performance. The evaporative organic volatile matter is 0.52 µg / m³, which is slightly reduced compared to the original binder solution. 3 It indicates, and finally, it is a board that exhibits semi-noncombustible performance indicating fire safety.
Claims
Claim 1 An eco-friendly organic-inorganic binder composition for manufacturing semi-noncombustible thermal insulation for fire doors, characterized by having a solid content of 35 to 45% by weight, a viscosity of 2,000 to 4,000 cps, and a pH of 5.5 to 7.5, prepared by forming an organic-inorganic binder composition comprising 200 parts by weight of an inorganic binder, 5 to 10 parts by weight of a dispersant, 2 to 5 parts by weight of a viscosity modifier, 3 to 5 parts by weight of a pH modifier, and 30 to 45 parts by weight of an auxiliary flame retardant, based on 100 parts by weight of a water-soluble acrylic resin composition, and then mixing 30 to 50 parts by weight of the organic-inorganic binder composition and 5 to 10 parts by weight of a water-soluble curing agent of Formula 2 below, having a viscosity of 200 to 400 cps, based on 100 parts by weight of water. R=Guar gum < Chemical Formula 2 > Claim 2 delete Claim 3 delete Claim 4 1). A first process of preparing a glass long fiber mat by cutting glass long fibers to a predetermined size; 2). A second process of preparing an organic-inorganic binder composition comprising 200 parts by weight of an inorganic binder, 5 to 10 parts by weight of a dispersant, 2 to 5 parts by weight of a viscosity modifier, 3 to 5 parts by weight of a pH modifier, and 30 to 45 parts by weight of an auxiliary flame retardant, based on 100 parts by weight of a water-soluble acrylic resin composition, and then mixing 30 to 50 parts by weight of the organic-inorganic binder composition and 5 to 10 parts by weight of a water-soluble curing agent having a viscosity of 200 to 400 cps with 100 parts by weight of water to produce an eco-friendly organic-inorganic binder having a solid content of 35 to 45% by weight, a viscosity of 2,000 to 4,000 cps, and a pH of 5.5 to 7.5; 3). A semi-noncombustible thermal insulation material for a fire door, characterized by being manufactured by including: a third process of uniformly impregnating the organic / inorganic binder of the second process into the glass long fiber mat of the first process using a spray nozzle, allowing the organic / inorganic binder to penetrate into the interior of the glass long fiber mat, and then pressurizing and drying in a heat press at 220 to 250°C to improve the bonding strength between glass long fibers and form a fire-resistant layer. Claim 5 A semi-noncombustible thermal insulation material for a fire door according to claim 4, characterized in that the spray nozzle of the spray injector has a diameter of 0.2 to 6.0 mm.
Citation Information
Patent Citations
Fiberglass insulation products
JP2023504433A
Water-soluble organic-inorganic binder composition and its construction method
KR102453669B1