Asphalt composition for road paving and road paving device using the same
The road paving device with a detachable frame and integrated modules addresses fluidity and width adjustment issues, ensuring rapid curing and uniform coating, improving crack resistance and surface protection for flexible road paving.
Patent Information
- Application Number
- KR1020250210449
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-12-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-12-26
AI Technical Summary
Conventional asphalt compositions and application vehicles fail to provide sufficient fluidity before spraying, rapid hardening after application, and do not adequately respond to varying road widths or conditions, lacking integrated leveling functions, leading to inefficient and ineffective road paving.
A road paving device with a detachable main frame and subframe system, adjustable working width, and integrated spray nozzles, along with a scraper and stirrer, ensures flexible application and rapid curing, while incorporating a brush module with a rotating screw and roller brush for uniform coating.
The device allows for adjustable working width, rapid curing, and uniform coating, enhancing crack resistance and surface protection, enabling flexible response to various road conditions and construction methods.
Smart Images

Figure 112025147142831-PAT00005_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an asphalt composition for road paving and a road paving device using the same. More specifically, the invention relates to an asphalt composition for road paving and a road paving device using the same, which includes a coating module capable of exhibiting sufficient fluidity before road paving, rapidly curing after road paving to exhibit excellent workability, providing excellent crack resistance performance after curing, as well as surface protection functions such as self-healing performance, slip resistance, and aging delay, and allowing the working width to be varied to flexibly respond to various road widths or conditions with a single vehicle, while simultaneously changing the function of the working device according to various construction methods. Background Technology
[0002] Asphalt paved on roads undergoes embrittlement over time due to molecular cleavage by ultraviolet rays and oxides, such as ketones and carboxylic acids, generated by oxidation reactions between oxygen and asphalt hydrocarbons, leading to the occurrence of cracks.
[0003] In particular, asphalt-based road pavements subjected to environmental loads such as temperature changes and vehicle traffic loads experience rapid degradation of their physical properties, which can easily lead to cracking. Consequently, preventive maintenance of road pavements is being emphasized, and methods such as fog seal and sand seal are being used as surface treatment techniques for this purpose.
[0004] The fog seal method refers to a technique that revitalizes the road surface by thinly spraying emulsified asphalt onto the surface of asphalt pavement to fill small cracks and voids.
[0005] The sand seal method refers to a technique in which emulsified asphalt is sprayed and then a thin layer of sand is spread over it; this increases surface friction and enhances the interlocking of aggregates.
[0006] The asphalt composition (emulsified asphalt) used in this road pavement surface treatment method must satisfy the following conditions.
[0007] First, sufficient fluidity must be ensured before spraying on the road pavement to enable efficient spraying operations by equipment.
[0008] Second, rapid hardening must occur after spraying on the road pavement to enable prompt traffic opening.
[0009] However, there was a problem in that the asphalt compositions used in the conventional fog seal method did not satisfy these conditions, or even if they did, their performance was poor.
[0010] In addition to the aforementioned asphalt composition, the asphalt application vehicle for applying the asphalt composition to the road is generally configured such that it is mounted on a vehicle and moves from a tank containing asphalt to a nozzle module installed at the rear of the vehicle to spray the asphalt composition.
[0011] However, in the case of such asphalt coating vehicles, there is a problem in that they are susceptible to various factors such as the shape, width, and slope of the road, and in cases where the coating method is complex, such as when multiple compositions are applied sequentially, the process inevitably proceeds with a second coating after the first coating is performed using the coating vehicle.
[0012] Furthermore, most conventional asphalt composition coating vehicles focus on asphalt spraying functions; however, there are relatively few coating vehicles that also include leveling functions using scrapers, and technological development in this regard is also insufficient. Consequently, there is a disadvantage in that it is difficult to respond organically to situations requiring the application of the various coating methods mentioned above. The problem to be solved
[0013] The objective of the present invention is to provide an asphalt composition for road paving and a road paving device using the same, which includes a coating module capable of varying the working width to flexibly respond to various road widths or conditions with a single vehicle, rather than simply applying the asphalt composition on the road, and simultaneously changing the function of the working device according to various construction methods. means of solving the problem
[0014] A road paving device using an asphalt composition for road paving according to one embodiment of the present invention comprises a main frame that is detachably installed at the rear of a vehicle, a subframe coupled to at least one side of the main frame and moving in a direction perpendicular to the driving direction of the vehicle to vary the working width, and a plurality of spray nozzles installed on the main frame and the subframe and spraying an asphalt composition onto the road surface, wherein the asphalt composition comprises 100 parts by weight of emulsified asphalt mixed with scleroglucan, 10 to 60 parts by weight of sand, and 5 to 40 parts by weight of a modifier.
[0015] In addition, the subframe is jointly connected to at least one side of the mainframe, so that during operation, the subframe can rotate from the mainframe to expand the working width.
[0016] In addition, the subframe is positioned parallel to the main frame when not in operation, and when in operation, it can be rotated from the joint of the main frame by any one of the preset angles of 90°, 120°, 145°, 150°, or 180° to expand the working width.
[0017] In addition, the subframe is slidably coupled to the main frame, allowing the working width to be varied while performing linear reciprocating motion.
[0018] In addition, the subframe can be expanded and contracted in steps by a length corresponding to a preset working width from a sliding guide installed on the main frame.
[0019] Additionally, the device further includes a storage unit for receiving an asphalt composition for road paving and a stirrer that stirs the interior of the storage unit at a regular interval, wherein the stirrer includes a central shaft penetrating the interior of the storage unit and an auxiliary shaft that rotates together in conjunction with the rotation of the central shaft, and a plurality of stirring blades vertically connected to the central shaft and the auxiliary shaft are axially connected to each shaft and rotate, and the central stirring blade connected to the central shaft and the auxiliary stirring blade connected to the auxiliary shaft can be axially rotated so as not to interfere with each other.
[0020] In addition, it may further include a scraper installed adjacent to the rear of the main frame to level the asphalt composition applied from the plurality of spray nozzles.
[0021] In addition, it may further include a lifting unit installed at the rear of the vehicle and adjusting the height of the main frame from the road surface.
[0022] In addition, it may further include a vertical frame that is formed to extend from both sides of the main frame toward the rear of the vehicle and mounted on the vehicle, and has a plurality of spray nozzles installed for applying an asphalt composition to the side of the road surface.
[0023] In addition, the injection radius of the asphalt composition sprayed from the injection nozzle installed on the vertical frame may be formed to be smaller than the injection radius of the asphalt composition sprayed from the injection nozzle installed on the main frame.
[0024] In addition, the injection nozzle installed on the vertical frame can be installed so as to be inclined toward the center of the vehicle.
[0025] A road paving device using an asphalt composition for road paving according to another embodiment of the present invention comprises: a brush module body installed adjacent to a mounting plate that includes a discharge part for discharging an asphalt composition and is installed so as to be detachably attached to the rear of a vehicle; a guide inclined part located below the discharge part and formed to be inclined downward so that the discharged asphalt composition flows down; a rotary screw positioned perpendicular to the driving direction of the vehicle adjacent to the bottom of the guide inclined part and conveying the asphalt composition flowing down to both sides through rotational driving; and a roller brush positioned parallel to the rear of the rotary screw and uniformly finishing the surface of the asphalt composition applied to the road surface, wherein the asphalt composition consists of 100 parts by weight of emulsified asphalt mixed with scleroglucan, 10 to 60 parts by weight of sand, and 5 to 40 parts by weight of a modifier.
[0026] In addition, the above-mentioned rotating screw is formed as a reverse screw in which the spiral directions on both sides are opposite with respect to the center, so that the asphalt composition introduced into the center can be spread to both sides.
[0027] In addition, it may further include a stirring paddle formed to protrude radially from the center of the rotation axis of the rotating screw so that the asphalt composition falling from the discharge section is stirred without clumping.
[0028] In addition, to maintain a constant separation distance between the roller brush and the road surface by a preset distance, support wheels installed on both sides of the bottom of the brush module body and rotating in contact with the road surface may be further included.
[0029] In addition, it may further include a discharge screw installed inside the discharge section and stirring the discharged asphalt composition so that it does not clump together.
[0030] An asphalt composition for road paving according to one embodiment of the present invention may consist of 100 parts by weight of emulsified asphalt mixed with scleroglucan, 10 to 60 parts by weight of sand, and 5 to 40 parts by weight of a modifier.
[0031] In addition, the emulsified asphalt mixed with the scleroglucan may consist of 100 parts by weight of asphalt, 30 to 70 parts by weight of an emulsion mixed with scleroglucan, and 0.5 to 10 parts by weight of a UV curing agent.
[0032] In addition, the asphalt may consist of one or more selected from the group consisting of straight asphalt, modified asphalt, and a colorless petroleum resin binder. Effects of the invention
[0033] A road paving device using an asphalt composition for road paving according to the present invention has the advantage of being able to freely adjust the working width to suit the construction section, ranging from a narrow shoulder to a wide road width, through a spraying module capable of varying the working width, and to flexibly respond to construction situations or application methods by selecting and applying the spraying module. Brief explanation of the drawing
[0034] FIG. 1 is a schematic perspective view of a road paving device using an asphalt composition for road paving according to one embodiment of the present invention. FIG. 2 is a side view of a road paving device using an asphalt composition for road paving. FIG. 3 is a detailed cross-sectional view of a stirrer in a storage section of a road paving device using an asphalt composition for road paving. FIG. 4 is an operating state diagram according to one embodiment of a frame with a spray nozzle installed thereon, in a road paving device using an asphalt composition for road paving. FIG. 5 is an operating state diagram according to another embodiment of a frame with a spray nozzle installed thereon, in a road paving device using an asphalt composition for road paving. FIG. 6 is a detailed view of a road paving device using an asphalt composition for road paving, with a scraper installed. FIG. 7 is an operating state diagram according to another embodiment of FIG. 4. FIG. 8 is a diagram showing the specific operating state of the lifting unit in a road paving device using an asphalt composition for road paving. FIG. 9 is a schematic perspective view of a road paving device using an asphalt composition for road paving according to another embodiment of the present invention. FIG. 10 is a detailed drawing showing the internal configuration of a road paving device using an asphalt composition for road paving according to another embodiment of the present invention. FIG. 11 is a cross-sectional view of FIG. 10. FIG. 12 is a side cross-sectional view of FIG. 10. FIG. 13 is a side cross-sectional view of another embodiment of FIG. 12. Specific details for implementing the invention
[0035] Hereinafter, preferred embodiments of the present invention and the physical properties of each component are described in detail. This description is intended to be sufficient for a person skilled in the art to easily practice the invention, and does not imply that the technical scope and concept of the present invention are limited thereby.
[0037] FIG. 1 is a schematic perspective view of a road paving device according to one embodiment of the present invention, and FIG. 2 is a side view of a road paving device according to the present invention.
[0038] Referring to FIGS. 1 and 2, the road paving device of the present invention is mounted on the rear of a vehicle (10) and driven. A storage unit (20) for receiving an asphalt composition is mounted on the vehicle (10), and the road paving device of the present invention may further include a mounting plate (40) comprising a transfer unit (30) for transferring the asphalt composition from the storage unit (20) to the road paving device of the present invention and a discharge unit (41) mounted on the rear of the vehicle for discharging the asphalt composition to the main frame (100) of the road paving device.
[0039] The asphalt composition delivered to the main frame (100) through the discharge unit (41) is sprayed onto the road surface through the spraying device disclosed in the present invention.
[0040] The above injection device mainly comprises a main frame (100) that is detachably installed at the rear of a vehicle (10), a pair of sub-frames (200) that are movably coupled to both the left and right sides of the main frame (100) to expand and contract the overall working width, and a plurality of injection nozzles (110, 210) that are respectively installed on the main frame (100) and the sub-frames (200) to spray an asphalt composition.
[0041] Here, the asphalt composition may consist of 100 parts by weight of emulsified asphalt mixed with scleroglucan, 10 to 60 parts by weight of sand, and 5 to 40 parts by weight of a modifier, which will be described later.
[0042] In addition, a lifting unit (300) is provided to raise the main frame (100) to a desired height from the road surface.
[0043] FIG. 8 illustrates a specific operating state diagram of the lifting unit, wherein the lifting unit (300) is installed on the vehicle through a connecting part (310) that is coupled to the rear of the vehicle (10), more specifically to both sides of the mounting plate (40), and is a device for adjusting the height of the entire main frame (100) from the road surface, and can be implemented as an actuator in the form of a hydraulic or pneumatic cylinder.
[0044] The above lifting unit (300) can set an optimal spraying pattern by adjusting the distance between the spray nozzle (110, 210) and the road surface during operation, and can control the coating thickness by adjusting the pressure applied to the road surface, and when not in operation, it lifts the main frame (100) high from the ground so as not to interfere with the vehicle (10) driving.
[0045] FIG. 3 is a detailed cross-sectional view illustrating a stirrer (20a) inside a storage unit (20) according to the present invention.
[0046] The storage unit (20) receives a pre-mixed asphalt composition. Since this asphalt composition may settle or harden during transport or while waiting for work, a stirrer (20a) is installed inside the storage unit (20) to stir the composition inside at regular intervals.
[0047] The above-mentioned stirrer (20a) includes a central shaft (21) that penetrates the interior of the storage unit (20) and an auxiliary shaft (23) that rotates together with the rotation of the central shaft (21), and a plurality of stirring blades (22, 24) vertically connected to the central shaft (21) and the auxiliary shaft (23) are axially connected to each shaft and can rotate.
[0048] Specifically, as illustrated in FIG. 3, the upper pulleys of the central shaft (21) and the auxiliary shaft (23) can be connected by a belt (25) so that they can rotate together in conjunction. A plurality of auxiliary stirring blades (24) are also vertically connected to the auxiliary shaft (23) and rotate axially.
[0049] At this time, the central stirring blade (22) and the auxiliary stirring blade (24) are arranged at different heights or rotated at different phases so that they are designed to rotate axially without interfering with each other when the stirrer (20a) rotates. Through this, the asphalt composition inside the storage unit (20) can be efficiently stirred without any blind spots.
[0050] The injection device, which is a core component of the present invention, is a device installed at the rear of a vehicle (10) to inject an asphalt composition, and includes a main frame (100) and a subframe (200).
[0051] The main frame (100) is a central frame fixed to the rear of the chassis of the vehicle (10), and the sub-frame (200) is coupled to at least one side of the main frame (100) and moves in the road width direction perpendicular to the driving direction of the vehicle (10) to vary the overall working width. A plurality of injection nozzles (110) are installed on the main frame (100), and a plurality of injection nozzles (210) are installed on the sub-frame (200).
[0052] The present invention includes various embodiments depending on the way the subframe (200) is coupled to and moved to the main frame (100).
[0053] FIG. 4 is an operating state diagram of a folding device according to the first embodiment of the present invention. In this embodiment, the sub-frame (200) is connected to the side of the main frame (100) so as to be rotatable.
[0054] FIG. 4(a) illustrates a state of operation when not working or working on a narrow width. In this state, the subframe (200) is folded parallel to (or at a specific angle to) the mainframe (100).
[0055] FIG. 4(b) illustrates the state during operation. The operator uses a driving means, such as a hydraulic or pneumatic cylinder (not shown in the drawing), to rotate the subframe (200) from the mainframe (100) to extend the working width.
[0056] At this time, the rotation angle can be set in various ways as needed. As shown in FIG. 4(b), it may be rotated to 180° to be aligned with the main frame (100) to secure the maximum working width, or as shown in FIG. 7, it may be fixed by rotating only to a preset intermediate angle such as 90° or 120°, 145°, 150°, etc. to correspond to curved sections of the road or specific widths.
[0057] Preferably, the spray nozzle (210) installed on the subframe (200) may be formed with a smaller spray radius than the spray nozzle (110) installed on the mainframe (100) in order to precisely control the spray pattern at the edge of the working width. Additionally, it may be installed at a predetermined angle toward the center of the vehicle to prevent the sprayed asphalt from scattering outward and to apply it accurately to the road surface boundary.
[0058] FIG. 5 is an operating state diagram of a sliding device according to another embodiment of the present invention. In this embodiment, the subframe (200) is slidably coupled to the main frame (100).
[0059] Specifically, a sliding guide (120) (e.g., a guide rail) is installed on the main frame (100), and the subframe (200) performs a linear reciprocating motion along the sliding guide (120). FIG. 5 sequentially shows the process in which the subframe (200) is pulled out in the direction of the arrow by a driving means from a state where the working width is minimized (top), thereby expanding the working width in multiple stages.
[0060] Unlike the hinge method, this structure has the advantage of being able to continuously or precisely expand and contract the working width in pre-set steps.
[0061] FIG. 6 is a detailed view of the state in which a scraper (400) according to the present invention is installed.
[0062] The device of the present invention may include not only a function of spraying an asphalt composition (110, 210), but also a function of immediately leveling the sprayed composition.
[0063] To this end, a scraper (400) is installed adjacent to the rear of the main frame (100). The scraper (400) is in the shape of a thin plate made of rubber or urethane material and performs a leveling or leveling function by adhering to the road surface and spreading the asphalt composition sprayed from a plurality of spray nozzles (110, 210) evenly to a certain thickness.
[0064] When the subframe (200) is extended, the scraper (400) may also be extended together, or a separate scraper may be moved together behind the subframe (200).
[0065] The scraper (400) can be attached to the rear of the vehicle by means of a mounting part (410) that is attached to the mounting plate (40) in a detachable manner.
[0067] A road paving device using an asphalt composition for road paving according to another embodiment of the present invention comprises: a brush module body (500) installed adjacent to a mounting plate (40) that is detachably installed at the rear of a vehicle and includes a discharge section (41) from which an asphalt composition is discharged; a guide inclined section (520) located below the discharge section (41) and formed to be inclined downward so that the discharged asphalt composition flows down; a rotating screw (530) positioned perpendicular to the driving direction of the vehicle adjacent to the bottom of the guide inclined section (520) and conveying the asphalt composition flowing down to both sides through rotational driving; and a roller brush (540) positioned parallel to the rear of the rotating screw (530) and uniformly finishing the surface of the asphalt composition applied to the road surface.
[0068] The brush module body (500) has connecting plates (510) formed on both sides so that it can be detachably mounted to the rear of the vehicle. The connecting plates (510) can be coupled to the connecting plate insertion groove (11) formed at the rear of the vehicle by a sliding method or other method.
[0069] The brush module body (500) includes a guide slope (520) located below the discharge section (41) and guiding the asphalt composition discharged through the discharge section (41) to flow down onto the road. The guide slope (520), which is inclined downward, prevents the asphalt composition from accumulating at a specific point by allowing it to flow downward due to gravity, and performs the function of guiding the asphalt composition toward the rotating screw (530) described later.
[0070] A rotating screw (530) is positioned adjacent to the bottom of the above-mentioned guide inclined section (520). The rotating screw (530) is positioned lengthwise in a horizontal direction perpendicular to the vehicle's driving direction and is made rotatable by a driving motor.
[0071] Here, the rotary screw (530) is formed as a reverse screw with the spiral directions on both sides opposite to the center. Accordingly, the asphalt composition dropped from the central discharge section (41) is transported by spreading from the center to both ends by the rotation of the rotary screw (530). Through this, a uniform amount of composition can be supplied across the entire width of the brush module body (500) without the need for a separate width expansion device.
[0072] Additionally, a stirring paddle (531) may be further included, which is formed to protrude radially from the center of the rotation axis of the rotating screw (530) so that the asphalt composition falling from the discharge section (41) is stirred without clumping. The stirring paddle (531) is configured to physically and strongly stir the high-viscosity asphalt composition. If the falling speed of the asphalt composition falling from the discharge section (41) and the conveying speed of the asphalt composition being conveyed left and right by the rotating screw (530) are not properly controlled, the asphalt composition may harden or clump. To prevent this, by adding a separate stirring paddle (531) in addition to the screw, the asphalt composition can be guided not to clump between the screw blades and the left and right conveying efficiency can be increased.
[0073] Additionally, a roller brush (540) may be positioned parallel to the rear of the rotating screw (530). The asphalt composition that is primarily laid on the floor by passing through the rotating screw (530) can be finished flat and simultaneously have fine bubbles removed as the surface is swept by the rotation of the roller brush (540) positioned at the rear.
[0074] At this time, in order to maintain a uniform coating thickness, it is important to maintain a gap between the roller brush (540) and the road surface. To this end, support wheels (550) that rotate in contact with the road surface are installed on both sides of the bottom of the brush module body (500). The support wheels (550) rotate together with the vehicle's movement by directly contacting the road surface, and by supporting the roller brush (540) so that it is spaced at a constant distance from the road surface by a preset distance, it is possible to ensure that the coating is applied at a constant thickness despite vehicle vibrations or unevenness of the road surface.
[0075] In addition, it may further include a discharge screw (43) installed inside the discharge section (41) and stirring the discharged asphalt composition so that it does not clump together.
[0076] As mentioned above, the asphalt composition has viscosity and needs to be physically stirred continuously. However, clogging may occur during the discharge process from the discharge unit (41), so a discharge unit screw (43) may be installed to prevent this.
[0077] The discharge screw (43) rotates around an axis perpendicular to the direction in which the asphalt composition is discharged, pushing the asphalt composition downward and stirring it at the same time so that it flows smoothly into the brush module body (500) without clumping.
[0079] Next, the asphalt composition is described in detail.
[0080] The above asphalt composition consists of scleroglucan-mixed emulsified asphalt, sand, and a modifier, and preferably consists of 100 parts by weight of scleroglucan-mixed emulsified asphalt, 10 to 60 parts by weight of sand, and 5 to 40 parts by weight of a modifier.
[0081] The above-mentioned emulsified asphalt mixed with scleroglucan consists of 100 parts by weight of asphalt, 25 to 400 parts by weight of an emulsion mixed with scleroglucan, and 0.5 to 10 parts by weight of a UV curing agent. Since scleroglucan is mixed, it not only exhibits excellent tackiness but also improves durability and waterproofing performance.
[0082] At this time, it is preferable that the asphalt consists of one or more selected from the group consisting of straight asphalt, modified asphalt, and a colorless petroleum resin binder.
[0083] At this time, the straight asphalt is a residue obtained by distilling crude oil, has excellent adhesiveness and water resistance, and is mainly used for road paving, roofing manufacturing, and waterproofing work. In the present invention, it is preferable to use one with a penetration depth of 5 to 130 mm.
[0084] In addition, the above modified asphalt (PMA) is a product that improves performance by adding a modifying material to general asphalt, and may consist of one of SBS modified asphalt, SBR modified asphalt, or EVA modified asphalt, and plays a role in suppressing deformation and cracking in high and low temperature environments and improving durability. In one embodiment, the above modifying material may be synthetic rubber powder, polyethylene, polypropylene, EVA, etc., having a particle size of 0.1 to 0.5 millimeters, and the above synthetic rubber powder is preferably composed of one or more selected from the group consisting of butadiene rubber, nitrile butadiene rubber, and ethylene propylene diene rubber.
[0085] In addition, it is preferable that the synthetic rubber powder be contained in an amount of 5 to 20 parts by weight per 100 parts by weight of asphalt, and the synthetic rubber powder composed of the above components plays a role in improving the crack resistance performance of the modified asphalt.
[0086] If the particle size of the synthetic rubber powder is less than 0.1 millimeters or the content of the synthetic rubber powder is less than 5 parts by weight, the above effect is negligible, and if the particle size of the synthetic rubber powder exceeds 0.5 millimeters or the content of the synthetic rubber powder exceeds 20 parts by weight, the above effect is not significantly improved, and the mechanical properties of the paved road may deteriorate excessively, which is undesirable.
[0087] In addition, when a colorless petroleum resin binder is applied as described above, an asphalt composition for road paving that imparts various colors to the surface of existing asphalt can be provided, and it can be applied in various cases such as anti-slip, marking of child protection zones, marking of speed bumps, and when warnings with text or images are required on the road surface.
[0088] Here, in the case of an asphalt composition for road paving to which the colorless petroleum resin binder is applied, it may consist of 100 parts by weight of colorless petroleum resin, 0.63 to 70 parts by weight of process oil or flux oil, 0.63 to 50 parts by weight of wax or paraffin, 6.25 to 50 parts by weight of natural vegetable oil, 0.13 to 20 parts by weight of vegetable emulsifier or cationic emulsifier, and 0.13 to 6 parts by weight of antioxidant.
[0089] The above petroleum resin is a factor that determines the basic adhesive performance and strength of the asphalt binder, and can be expressed in a desired color when mixed with pigment. The above petroleum resin may be any one selected from aliphatic petroleum resin, aromatic petroleum resin, or coumarone-indene-based petroleum resin, or a mixture thereof.
[0090] In addition, it contains 0.63 to 70 parts by weight of process oil or flux oil, and the process oil or flux oil enables stable mixing with petroleum resin, controls the viscosity of the colorless petroleum resin binder, and improves fluidity, thereby ensuring ease of asphalt production and construction.
[0091] If the content of the above process oil or flux oil is less than 0.63 parts by weight, the viscosity control effect is negligible and workability may be reduced, and if it exceeds 70 parts by weight, the softening point of the binder is excessively lowered, which may weaken heat resistance and deformation resistance, so it is undesirable.
[0092] In addition, 0.63 to 50 parts by weight of wax or paraffin are included for the purpose of reinforcing the viscosity of the binder and improving heat resistance, especially at high temperatures; if less than 0.63 parts by weight, the effect of reinforcing heat resistance may be insufficient, and if more than 50 parts by weight, flexibility at low temperatures decreases and cracking may occur.
[0093] Next, to impart eco-friendly characteristics and improve workability, it contains 6.25 to 50 parts by weight of natural vegetable oil. The natural vegetable oil is eco-friendly in that it partially replaces conventional petroleum-based oils to reduce the generation of volatile organic compounds (VOCs) and uses renewable raw materials, and it has an appropriate viscosity, providing excellent workability when mixed with petroleum resin. If the content of the natural vegetable oil is less than 6.25 parts by weight, the eco-friendly effect is negligible, and if it exceeds 50 parts by weight, the mechanical properties of the binder may deteriorate, which is undesirable.
[0094] In addition, plant-based emulsifiers or cationic emulsifiers are included during the manufacture of emulsified asphalt to ensure emulsion stability and impart dispersibility to each component. In particular, the use of cationic emulsifiers can enhance adhesion to the aggregate surface, and by maintaining a stable mixture of water and oil components, the emulsifier improves the storage stability of the composition and ensures uniform quality.
[0095] If the content of the above emulsifier or cationic emulsifier is less than 0.13, the emulsion stability effect is negligible, and if it exceeds 20 parts by weight, it may cause excessive bubble generation or deterioration of physical properties.
[0096] In addition, 0.13 to 6 parts by weight of an antioxidant are included to prevent oxidation of the binder and improve long-term durability. During the asphalt production and construction stages, oxidation caused by heat and ultraviolet rays leads to cracking or delamination; the antioxidant suppresses this oxidation reaction, thereby maintaining the performance of the binder and improving durability.
[0097] If the content of the above antioxidant is less than 0.13, the effect of improving durability is negligible, and if it exceeds 6 parts by weight, it is undesirable as it may have a negative effect on physical properties.
[0099] In addition, the emulsion mixed with the scleroglucan contains 30 to 70 parts by weight and preferably consists of 100 parts by weight of deionized water, 0.05 to 5 parts by weight of an emulsifier, 0.01 to 5 parts by weight of scleroglucan, and 0.01 to 2 parts by weight of protic acid.
[0100] The above deionized water (DI water) is produced by an electrochemical method in which tap water or distilled water is passed through an electrically charged resin, that is, an ion exchange resin having positive and negative charges. It is desirable to use deionized water from which dissolved ions and minerals have been removed in order to maximize the characteristics and effects of the emulsifier.
[0101] In addition, the above emulsifier is formed by mixing 25 to 400 parts by weight of a slow-curing emulsifier with 100 parts by weight of a fast-curing cationic emulsifier, wherein the fast-curing cationic emulsifier is composed of one or a mixture of an alkylamine emulsifier or an alkyl polyamine emulsifier, and the slow-curing emulsifier is composed of one or a mixture of a quaternary ammonium salt emulsifier or a lignoamine cationic emulsifier, and the curing speed of the asphalt composition can be controlled by adjusting the mixing ratio of the fast-curing cationic emulsifier and the slow-curing emulsifier.
[0102] In addition, the scleroglucan contained in the above emulsion is a biopolymer extracted from contractile bacteria and is composed of a polymer consisting of glucose units, which is mixed into the above emulsified asphalt to improve the strength and durability of the paved road surface and suppress damage to the paved road caused by snow, rain, or high heat, thereby providing the effect of extending the lifespan of the paved road.
[0103] In addition, the above proton acid is a chemical substance produced in petrochemical processes, mainly using ethylene as a raw material and obtained through the reaction of ethylene and oxygen. It is water-soluble and, when mixed with an emulsifier, exhibits useful effects in various chemical processes as follows.
[0104] First, it enhances the performance of emulsifiers by strengthening the role of mixing water with other substances. Second, it improves the function of breaking down ions in water and facilitates chemical reactions occurring in water more effectively, exhibiting significant effects particularly in chemical reactions where inter-ionic interactions are critical.
[0105] In addition, the above-mentioned UV curing agent is contained in an amount of 0.5 to 10 parts by weight and is composed of 1,6-hexanediol diacrylate. It removes hydrogen radicals from molecules forming asphalt or polymers added to asphalt, and forms molecular radicals that react with each other to form cross-links, thereby providing a paved road with excellent heat resistance and chemical resistance as well as improved mechanical properties.
[0106] If the content of the above UV curing agent is less than 0.5 parts by weight, the above effect is negligible, and if the content of the above UV curing agent exceeds 10 parts by weight, the above effect is not significantly improved, and it is undesirable because the impact resistance may actually decrease after moisture is removed from the emulsified asphalt due to excessive crosslinking reaction.
[0108] The above sand contains 10 to 60 parts by weight and is composed of one or more selected from the group consisting of quartz sand, basalt, limestone, granite, blast furnace slag, electric furnace slag, and washed sand, preferably having a particle size of 10 to 100 mesh.
[0109] Sand exhibiting the above-mentioned composition and particle size acts as aggregate to extend the lifespan of asphalt roads, and since the emulsified asphalt mixed with scleroglucan as described above has excellent adsorption performance on the surface of sand, material separation does not occur before and after application, thereby enabling the formation of a very stable coating layer on the road surface.
[0110] If the sand content is less than 10 parts by weight or the sand particle size exceeds 100 mesh, the above effect is negligible, and if the sand content exceeds 60 parts by weight or the sand particle size is less than 10 mesh, it is undesirable because the sand can easily detach from the emulsified asphalt.
[0112] The above modifier is contained in an amount of 5 to 40 parts by weight and is formed by mixing 50 to 80 parts by weight of a filler with 100 parts by weight of an ethylene methyl acrylic acid copolymer. The modifier composed of the above components not only improves the durability and adhesion of the asphalt composition for road paving but also serves to provide self-healing performance.
[0113] The above ethylene methylacrylic acid copolymer contains about 4 to 15% of methylacrylic acid or methylacrylate salt, and exhibits the characteristic that as the amount of methylacrylate decreases, the metal adhesion, stiffness, and permeability decrease, while the adhesive strength increases.
[0114] The above ethylene methyl acrylic acid copolymer has excellent mechanical properties because when the ionically crosslinked molecules are heated, the crosslinking bonds are broken and heat sealing properties are exhibited, and when cooled, they become ionically crosslinked again and become rigid. In addition, it has excellent oil and cold resistance, and excellent resistance to strong acids, strong alkalis, grease, oil, organic solvents, and water.
[0115] The above ethylene-methylacrylic acid copolymer is a polymer copolymerized with ethylene and (meth)acrylic acid, in which ions such as zinc, sodium, potassium, calcium, and ammonium are cross-linked to the carboxyl group, and the carboxy anions act as reversible cross-links between supramolecular network polymer chains due to the electrostatic attraction of neutralizing cations such as zinc, sodium, potassium, calcium, and ammonium.
[0116] That is, the above ethylene methyl acrylic acid copolymer forms a supramolecular composite network due to the characteristic that the rubber having thermoplastic reversible covalent bonds and the molecular chains are ionically bonded within the asphalt, thereby exhibiting the effect of providing self-healing performance for external damage such as cracks or scratches and microcracks that occur in the asphalt.
[0117] In addition, the above filler is contained in an amount of 50 to 80 parts by weight and is preferably composed of one or more selected from the group consisting of talc, calcium carbonate, pulp, silicon dioxide, limestone, magnesium silicate, and slaked lime. The filler composed of the above components improves the compatibility between the asphalt component and the ethylene methyl acrylic acid copolymer by increasing bonding strength and imparting polarity, and exhibits the effect of increasing adhesive strength.
[0118] If the content of the above-mentioned modifier is less than 5 parts by weight, the above effect is negligible, and if the content of the above-mentioned modifier exceeds 40 parts by weight, the above effect is not significantly improved, and the content of emulsified asphalt or sand is reduced excessively, which is undesirable because the mechanical properties of the paved road may actually deteriorate.
[0120] In addition, the asphalt composition for road paving may further contain 0.001 to 5 parts by weight of a phase change material per 100 parts by weight of the emulsified asphalt mixed with the scleroglucan, and the phase change material is preferably formed by encapsulating one or more selected from the group consisting of n-hexadecane, n-heptadecane, n-octadecane, n-nonadecane, n-eicosan, n-heneicosan, n-docosan, n-tricosan, n-tetracosan, capric acid, lauric acid, stearic acid, palmitic acid, and hexadecanol with melanin.
[0121] Phase change materials composed of the above components control the phase change temperature of asphalt, thereby suppressing damage to the asphalt caused by low or high temperatures and improving durability.
[0122] In addition, the phase change materials listed above are encapsulated with melamine components, exhibiting excellent stability and heat resistance, which allows for the provision of phase change effects over a long period.
[0123] If the content of the above-mentioned phase change material is less than 0.001 parts by weight, the above-mentioned effect is negligible, and if the content of the above-mentioned phase change material exceeds 5 parts by weight, the above-mentioned effect is not significantly improved, and the mechanical properties of the paved road made of the asphalt composition for road paving may be excessively degraded, which is undesirable.
[0125] In addition, a road paving surface treatment method using an asphalt composition for road paving composed of the above components comprises the steps of: preparing an asphalt composition for road paving by mixing the emulsified asphalt mixed with the above-mentioned scleroglucan, sand, and a modifier; and spraying the asphalt composition for road paving onto the surface of the road pavement.
[0126] At this time, the above spraying may be performed by spraying with a spraying device such as a sprayer, or by direct application with a coating device such as a roller.
[0127] In addition, the surface treatment process described above can be repeated 1 to 3 times, and the paving thickness of the asphalt composition for road paving per step is preferably 1 to 2 millimeters, and the total paving thickness is more preferably formed to be 1 to 5 millimeters.
[0128] In other words, the asphalt composition disclosed in the present invention differs from the conventional fog seal method, which sprays only emulsified asphalt on the surface of a paved road, or the sand seal method, which sprays emulsified asphalt first and then sprays sand on top of it, in terms of paving components and process, in that the asphalt composition mixed with emulsified asphalt and sand is sprayed onto the surface of a paved road.
[0130] Hereinafter, the method for manufacturing the asphalt composition disclosed in the present invention and the physical properties of a paved road to which the asphalt composition manufactured by the method is applied will be explained with reference to examples.
[0132] <Preparation Example 1> Preparation of Modified Asphalt
[0133] Modified asphalt was prepared by mixing 100 parts by weight of asphalt and 12 parts by weight of synthetic rubber (nitrile butadiene rubber with a particle size of 0.1 to 0.5 millimeters) powder.
[0135] <Preparation Example 2> Preparation of an emulsion mixed with scleroglucan
[0136] An emulsion was prepared by mixing 100 parts by weight of deionized water, 2.5 parts by weight of an emulsifier (a mixture of alkylamine and quaternary ammonium salt in a 1:1 ratio by weight), 2.5 parts by weight of scleroglucan, and 1 part by weight of proton acid.
[0138] <Preparation Example 3> Preparation of emulsified asphalt mixed with scleroglucan
[0139] Scleroglucan-mixed emulsified asphalt was prepared by mixing 100 parts by weight of modified asphalt prepared through Preparation Example 1, 50 parts by weight of an emulsion mixed with scleroglucan prepared through Preparation Example 2, and 5 parts by weight of a UV curing agent (1,6-hexanediol diacrylate).
[0141] <Preparation Example 4> Preparation of Modifier
[0142] A modifier was prepared by mixing 65 parts by weight of a filler (silicon dioxide and limestone mixed in a 1:1 weight ratio) with 100 parts by weight of an ethylene methyl acrylic acid copolymer.
[0144] <Example 1>
[0145] An asphalt composition for road paving was prepared by stirring 100 parts by weight of emulsified asphalt mixed with scleroglucan prepared through Preparation Example 3, 35 parts by weight of sand, and 25 parts by weight of a modifier prepared through Preparation Example 4.
[0147] <Example 2>
[0148] The process was carried out in the same manner as in Example 1 above, but an asphalt composition for road paving was prepared by mixing 100 parts by weight of emulsified asphalt mixed with scleroglucan, 10 parts by weight of sand, and 5 parts by weight of a modifier.
[0150] <Example 3>
[0151] The process was carried out in the same manner as in Example 1 above, but a road paving asphalt composition was prepared by mixing 100 parts by weight of emulsified asphalt mixed with scleroglucan, 60 parts by weight of sand, and 40 parts by weight of a modifier.
[0153] <Example 4>
[0154] The process was carried out in the same manner as in Example 1 above, but an asphalt composition for road paving was prepared by further mixing 2.5 parts by weight of a phase change material (n-docosan encapsulated with melamine) with 100 parts by weight of the emulsified asphalt mixed with scleroglucan.
[0156] <Example 5>
[0157] The process was carried out in the same manner as in Example 2 above, but an asphalt composition for road paving was prepared by further mixing 2.5 parts by weight of a phase change material (n-docosan encapsulated with melamine) with 100 parts by weight of the emulsified asphalt mixed with scleroglucan.
[0159] <Example 6>
[0160] The process was carried out in the same manner as in Example 3 above, but an asphalt composition for road paving was prepared by further mixing 2.5 parts by weight of a phase change material (n-docosan encapsulated with melamine) with 100 parts by weight of the emulsified asphalt mixed with scleroglucan.
[0162] <Comparative Example 1>
[0163] Asphalt (PG 64-22).
[0165] <Comparative Example 2>
[0166] RSC Emulsified Asphalt.
[0168] <Comparative Example 3>
[0169] Modified RSC emulsified asphalt.
[0171] <Comparative Example 4>
[0172] The process was carried out in the same manner as in Example 1 above, but an asphalt composition for road paving was prepared by mixing 100 parts by weight of emulsified asphalt mixed with scleroglucan, 35 parts by weight of sand, and 3 parts by weight of a modifier.
[0174] <Comparative Example 5>
[0175] The process was carried out in the same manner as in Example 1 above, but an asphalt composition for road paving was prepared by mixing 100 parts by weight of emulsified asphalt mixed with scleroglucan, 35 parts by weight of sand, and 60 parts by weight of a modifier.
[0177] The skid resistance of the asphalt compositions for road paving prepared through the above Examples 1 to 3 and Comparative Examples 1 to 5 was measured and is shown in Table 1 below.
[0178] {However, skid resistance was measured in accordance with the KS F 2375 test method, and for Examples 1 to 3 and Comparative Examples 4 to 5, skid resistance was measured after road paving via simultaneous laying, while for Comparative Examples 1 to 3, skid resistance was measured after road paving using the sand seal method.}
[0179]
[0180]
[0181] As shown in Table 1 above, it can be seen that the asphalt composition for road paving prepared through Examples 1 to 3 provides a paved road exhibiting superior slip resistance compared to the asphalt composition for road paving prepared through Comparative Examples 1 to 4.
[0183] In addition, the adhesive strength of the asphalt compositions for road paving prepared through Examples 1 to 3 and Comparative Examples 1 to 5 was measured and is shown in Table 2 below.
[0184] {However, adhesive strength was measured using a PATTI (Pneumatic Adhesion Tensil Testing Instrument) in accordance with the standards of AASHTO TP91.}
[0185] Table 2
[0186]
[0187] As shown in Table 2 above, it can be seen that the asphalt composition for road paving prepared through Examples 1 to 3 exhibits superior adhesive strength compared to the asphalt composition for road paving prepared through Comparative Examples 1 to 4.
[0189] In addition, the abrasion resistance of the asphalt compositions for road paving prepared through Examples 1 to 3 and Comparative Examples 1 to 5 was measured and is shown in Table 3 below.
[0190] {However, wear resistance was determined using the method of measuring the amount of wear after an abrasion test according to ASTM 3910.}
[0191] Table 3
[0192]
[0193] As shown in Table 3 above, it can be seen that the asphalt composition for road paving prepared through Examples 1 to 3 exhibits superior wear resistance compared to the asphalt composition for road paving prepared through Comparative Examples 1 to 5.
[0194] In particular, as shown in Comparative Example 5, it can be seen that wear resistance is actually reduced when an excessive amount of modifier and phase change material components are used.
[0196] In addition, the heat generation of the asphalt compositions for road paving prepared through Examples 4 to 6 and Comparative Examples 1 to 5 was measured and is shown in Table 4 below.
[0197] {However, the calorific value was measured using the test method of ASTM D3286 and a calorific value tester.}
[0198] Table 4
[0199]
[0200] As shown in Table 4 above, it can be seen that the asphalt composition for road paving produced through Examples 4 to 6 has an appropriate amount of phase change material mixed in, and exhibits a superior heat generation compared to the asphalt composition for road paving produced through Comparative Examples 1 to 5.
[0202] Accordingly, the asphalt composition for road paving disclosed in the present invention and the road paving method using the composition provide a paved road that exhibits sufficient fluidity before road paving, hardens rapidly after road paving to exhibit excellent workability, and not only exhibits excellent crack resistance performance but also self-healing performance after hardening.
[0204] Although the present invention has been described above with reference to preferred embodiments, those skilled in the art or those with ordinary knowledge in the relevant technical field will understand that various modifications and changes can be made to the invention without departing from the spirit and technical scope of the invention as set forth in the claims below. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be determined by the claims. Explanation of the symbols
[0205] 10 : Vehicle 20 : Storage section 20a : Stirrer 21: Central shaft 22 : Central stirring blade 23: Auxiliary shaft 24: Auxiliary stirring blade 25 : Belt 30 : Transfer section 40 : Mounting plate 41 : Discharge section 43 : Discharge screw 100 : Main frame 110 : Spray nozzle 120 : Sliding guide 200 : Subframe 210 : Spray nozzle 300 : Lifting unit 310 : Connection part 400 : Scraper 410 : Mounting part 500 : Brush module main body 510 : Connecting plate 520: Guide slope 530: Rotary screw 531 : Stirring paddle 540: Roller Brush 550: Support wheel
Claims
Claim 1 A main frame installed to be detachably attached to the rear of the vehicle; a subframe coupled to at least one side of the main frame and moving perpendicular to the vehicle's driving direction to vary the working width; and a plurality of spray nozzles installed on the main frame and subframe and spraying an asphalt composition onto the road surface; wherein the asphalt composition comprises 100 parts by weight of emulsified asphalt mixed with scleroglucan, 10 to 60 parts by weight of sand, 5 to 40 parts by weight of a modifier, and 0.001 to 5 parts by weight of a phase change material; wherein the emulsified asphalt mixed with scleroglucan comprises 100 parts by weight of asphalt, 30 to 70 parts by weight of an emulsion mixed with scleroglucan, and 0.5 to 10 parts by weight of a UV curing agent; wherein the UV curing agent comprises 1,6-hexanediol diacrylate; wherein the modifier comprises 50 to 80 parts by weight of a filler mixed with 100 parts by weight of an ethylenemethylacrylic acid copolymer; wherein the filler comprises one or more selected from the group consisting of talc, pulp, silicon dioxide, and magnesium silicate; and A road paving device using an asphalt composition, characterized in that the phase change material is formed by encapsulating one or more selected from the group consisting of n-docosan, n-tricosan, n-tetracosan, capric acid, lauric acid, stearic acid, palmitic acid, and hexadecanol with melamine, the injection radius of the asphalt composition sprayed from the injection nozzle installed on the subframe is formed to be smaller than the injection radius of the asphalt composition sprayed from the injection nozzle installed on the mainframe, and the injection nozzle installed on the subframe is installed so as to be inclined toward the center of the vehicle. Claim 2 A road paving device using an asphalt composition for road paving according to claim 1, wherein the subframe is jointly connected to at least one side of the mainframe, and during operation, the subframe rotates from the mainframe to expand the working width. Claim 3 A road paving device using an asphalt composition for road paving according to claim 2, characterized in that the subframe is positioned parallel to the main frame when not in operation, and when in operation, is rotated by any one of a preset angles of 90°, 120°, 145°, 150°, or 180° from the joint of the main frame to expand the working width. Claim 4 A road paving device using an asphalt composition for road paving, characterized in that, in claim 1, the subframe is slidably coupled to the main frame and varies the working width while performing linear reciprocating motion. Claim 5 A road paving device using an asphalt composition for road paving according to claim 4, wherein the subframe is expanded and contracted in stages by a length corresponding to a preset working width from a sliding guide installed on the main frame. Claim 6 A road paving device using an asphalt composition for road paving according to claim 1, further comprising a storage unit for receiving an asphalt composition for road paving and a stirrer for stirring the interior of the storage unit at a certain period, wherein the stirrer comprises a central shaft penetrating the interior of the storage unit and an auxiliary shaft that rotates together in conjunction with the rotation of the central shaft, and wherein a plurality of stirring blades vertically connected to the central shaft and the auxiliary shaft are axially connected to each shaft and rotate, and wherein the central stirring blade connected to the central shaft and the auxiliary stirring blade connected to the auxiliary shaft are axially rotated so as not to interfere with each other. Claim 7 A road paving device using an asphalt composition for road paving, characterized in that, in claim 1, it further comprises a scraper installed adjacent to the rear of the main frame for leveling the asphalt composition applied from the plurality of spray nozzles. Claim 8 A road paving device using an asphalt composition for road paving, characterized in that, in claim 1, it further includes a lifting unit installed at the rear of a vehicle and adjusting the height of the main frame from the road surface. Claim 9 delete Claim 10 delete Claim 11 A brush module body installed adjacent to a mounting plate that is detachably installed at the rear of a vehicle and includes a discharge section for discharging an asphalt composition; a guide slope section located below the discharge section and formed to be inclined downward so that the discharged asphalt composition flows down; and a rotary screw positioned perpendicular to the vehicle's driving direction adjacent to the bottom of the guide slope section and transporting the asphalt composition flowing down to both sides through rotational drive. and a roller brush arranged parallel to the rear of the rotary screw and uniformly finishing the surface of an asphalt composition applied to a road surface; wherein the asphalt composition comprises 100 parts by weight of emulsified asphalt mixed with scleroglucan, 10 to 60 parts by weight of sand, 5 to 40 parts by weight of a modifier, and 0.001 to 5 parts by weight of a phase change material; wherein the emulsified asphalt mixed with scleroglucan comprises 100 parts by weight of asphalt, 30 to 70 parts by weight of an emulsion mixed with scleroglucan, and 0.5 to 10 parts by weight of a UV curing agent; wherein the UV curing agent comprises 1,6-hexanediol diacrylate; wherein the modifier comprises 50 to 80 parts by weight of a filler mixed with 100 parts by weight of an ethylenemethylacrylic acid copolymer; and wherein the filler comprises one or more selected from the group consisting of talc, pulp, silicon dioxide, and magnesium silicate. A road paving device using an asphalt composition for road paving, characterized in that the phase change material is formed by encapsulating one or more selected from the group consisting of n-docosan, n-tricosan, n-tetracosan, capric acid, lauric acid, stearic acid, palmitic acid, and hexadecanol with melamine, the guide inclined portion is configured to prevent the discharged asphalt composition from accumulating at a specific point and to guide the asphalt composition toward the rotating screw side, and further includes a discharge screw installed inside the discharge portion to agitate the discharged asphalt composition so as not to clump together. Claim 12 A road paving device using an asphalt composition for road paving according to claim 11, wherein the rotating screw is formed as a reverse screw with the spiral directions on both sides opposite with respect to the center, and spreads the asphalt composition introduced into the center to both sides. Claim 13 A road paving device using an asphalt composition for road paving according to claim 11, further comprising a stirring paddle formed to protrude radially from the center of the rotation axis of the rotating screw so as to stir the asphalt composition falling from the discharge section without clumping. Claim 14 A road paving device using an asphalt composition for road paving, characterized in that, in order to maintain a constant separation distance between the roller brush and the road surface by a preset distance, it further includes support wheels installed on both sides of the lower part of the brush module body and rotating in contact with the road surface. Claim 15 delete Claim 16 delete Claim 17 delete Claim 18 delete
Citation Information
Patent Citations
Stirring and mixing drum
CN219897751U
Spraying device of finisher
JP1999152709A
Device for heating and spraying modified rubber and modified asphalt to coat a surface
KR101371104B1
Apparatus for spreading ground reinforcing materials
KR1020170124887A
Storage stable, light coloured emulsions from low penetration grade clear binders