Method for manufacturing water-atomized metal powder

The described method addresses the limitations of water atomization by using flat spray nozzles and optimized parameters to produce metal powders with high Fe-based content, fine particle size, and high roundness, achieving efficient amorphization and density for high-frequency applications.

KR103046631B1Active Publication Date: 2026-11-10JFE STEEL CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020237015236
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-18
Filing Date
2021-08-26
Publication Date
2026-11-10
Estimated Expiration
2041-08-26

Smart Images

  • Figure R1020237015236_ABST
    Figure R1020237015236_ABST
Patent Text Reader

Abstract

A method for manufacturing fine water atomized metal powder having a high amorphization rate, high apparent density, and high sphericity, even when the iron-based component content is high. A method for manufacturing water atomized metal powder by spraying cooling water that collides with a molten metal stream falling in a vertical direction and splitting the molten metal stream into metal powder, comprising a process of spraying cooling water from each of three or more cooling water discharge ports spaced apart from the falling molten metal stream at a spreading angle in the range of 5 to 30° with a spray pressure of 10 MPa or more, wherein the droplet diameter of the cooling water is 100 μm or less, the water convergence angle is 5 to 10°, and the water / molten steel ratio is 50 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing water-atomized metal powder. The present invention is particularly suitable for a method for manufacturing water-atomized metal powder of soft magnetic metal powder or iron-based powder for 3D printers, wherein the total content of Fe, Ni, and Co is 76.0 at% or more and 86.0 at% or less in atomic fraction. Background Technology

[0002] The production volume of hybrid vehicles (HV), electric vehicles (EV), and fuel cell vehicles (FCV) is increasing, and there is a demand for lower iron loss, higher efficiency, and miniaturization of the reactors and motor cores used in these vehicles.

[0003] These reactors and motor cores have traditionally been manufactured by laminating thin sheets of electrical steel. Recently, motor cores produced by compression molding using metal powder, which offers a high degree of freedom in shape design, are attracting attention.

[0004] It is believed that amorphizing the metal powder used is effective for reducing iron loss in reactors or motor cores. Additionally, to accommodate high frequencies, it is required to make the particle size of the powder finer.

[0005] Furthermore, in order to miniaturize, lighten, and increase the output of reactors or motors, it is necessary to increase the magnetic flux density of metal powders, and to do so, it is important to increase the concentration of Fe-based elements that may include Ni and Co (increase the total content of iron-based components), and there is a growing demand for amorphous soft magnetic metal powders with an atomic fraction of 76.0 at% or more of Fe-based elements.

[0006] Furthermore, when atomized metal powder is compression-molded and used as a reactor or motor core, low core loss is important for achieving low loss and high efficiency. To achieve this, it is important that the amorphization rate of the atomized metal powder is high, and it is also often influenced by the shape of the atomized metal powder. In other words, core loss tends to be reduced as the shape of the atomized metal powder becomes more spherical. Additionally, there is a close relationship between sphericity and apparent density; the higher the apparent density, the more spherical the powder shape becomes. Recently, for atomized metal powders with small particle sizes, an apparent density of 3.5 g / cm³ or higher is required.

[0007] Also, along with the high frequency of the motor or reactor, the average particle size (D 50 The demand for fine metal powders of less than 50 μm is also increasing.

[0008] Recently, metal powders used in 3D printers have been attracting attention as applications for metal powders other than reactors or motor cores. Metal powders used in 3D printers need to be supplied smoothly, and it is also considered desirable for the sphericity of the powder particles to be 0.90 or higher.

[0009] From the above, the following four performance characteristics are required for water atomized metal powder used as a reactor or motor core.

[0010] 1) In order to miniaturize and increase the performance of the motor, the concentration of Fe-based elements is increased (the total content of iron-based components is increased).

[0011] 2) For low loss and high efficiency, the metal powder is highly amorphous, and also has high apparent density and roundness.

[0012] In addition, due to the increasing demand for atomized metal powder accompanying the increase in HV, EV, and FCV vehicles, the following is required.

[0013] 3) Low cost and high productivity.

[0014] 4) Average particle size corresponding to high frequency (D 50 ) is a metal powder with a thickness of less than 50 μm.

[0015] In addition, regarding atomized metal powder for 3D printing (modeling), 2) and 3) are required, and it is also desirable to satisfy the requirements of 1) and 4). Prior art literature

[0016] Japanese Published Patent Application No. 2001-64704 Japanese Published Patent Application No. 2012-111993 The problem to be solved

[0017] As a means of performing amorphization and shape control of metal powder by the atomization method, the method shown in Patent Document 1 is proposed.

[0018] Patent Document 1 describes obtaining metal powder by splitting molten metal into a gas jet with a spray pressure of 15 to 70 kg / cm², diffusing it while dropping it over a distance of 10 mm to 200 mm, and introducing it into a water stream at an angle of incidence of 30 to 90°. Furthermore, when the angle of incidence is less than 30°, amorphous powder is not obtained, and when the angle of incidence exceeds 90°, powder particles with a shape of low circularity, such as flattened ellipsoids, are observed.

[0019] However, methods for splitting molten metals by atomization include water atomization and gas atomization. Water atomization is a method of obtaining metal powder by spraying cooling water onto molten metals and splitting the molten metal, while gas atomization is a method of spraying inert gas onto molten metals. Patent Document 1 discloses a gas atomization method for the first time, in which the splitting of molten metals is carried out using gas.

[0020] In the water atomization method, the flow of molten steel is divided by a water jet sprayed from a nozzle, and the metal is converted into powder (metal powder), and the metal powder is also cooled by the water jet to obtain atomized metal powder. On the other hand, in the gas atomization method, an inert gas sprayed from a nozzle is used. In the case of the gas atomization method, since the ability to cool the molten steel is low, equipment for separate cooling after atomization is sometimes provided.

[0021] In manufacturing metal powder, the water atomization method has a higher production capacity and lower cost compared to the gas atomization method because it uses only water. However, metal powder produced by the water atomization method has an irregular shape, and in particular, if pulverization and cooling are performed simultaneously to obtain amorphous metal powder, the molten steel solidifies in the state it was in when pulverized, so the apparent density becomes less than 3.5 g / cm³.

[0022] On the other hand, the gas atomization method requires the use of a large amount of inert gas, and its ability to atomize molten steel is inferior to that of the water atomization method. However, metal powder produced by the gas atomization method has a longer time from atomization to cooling compared to the water atomization method, and since it cools after becoming spherical due to the surface tension of the molten steel until solidification, its shape is closer to a sphere than that of water-atomized metal powder, and thus tends to have a higher apparent density.

[0023] In the technology described in Patent Document 1, spheroidization and amorphization of metal powder are achieved simultaneously by adjusting the water jet angle (incident angle) through cooling after gas atomization. However, as described above, the gas atomization method has low productivity and high manufacturing costs due to the use of a large amount of high-pressure inert gas. Furthermore, since the fragmentation energy during gas atomization is smaller for metal powder produced by the gas atomization method compared to water atomization, the average particle size (D) is generally50 ) tends to grow larger than 50 µm.

[0024] In this regard, Patent Document 2 discloses a method in which spray nozzles are crossed in a V-shape in a tilted downward direction, molten steel is dropped onto the central part of the intersection, and the molten steel is atomized and spherical. The technology described in Patent Document 2 employs a water atomization method, in which spray nozzles are crossed in a V-shape and molten steel is dropped toward the intersection to obtain fine metal powder. Although this is a good method for obtaining fine metal powder, since water is dispersed, some of the water does not contribute at all to the fragmentation or cooling of the molten steel. Therefore, this method is not suitable for increasing cooling capacity. Consequently, there is a problem that it is difficult to achieve amorphization.

[0025] The present invention was made to solve the above problem, and its purpose is to provide a method for producing a water atomized metal powder that can be produced by the water atomization method, even if the Fe-based concentration (total content of iron-based components) is 76.0 at% or higher, has an average particle size of less than 50 μm, has a high amorphization rate, high apparent density, and high roundness.

[0026] Also, here, the Fe-based concentration refers to the total content of Fe, Ni, and Co.

[0027] In addition, high amorphous rate refers to an amorphous rate of 90% or more, high apparent density refers to an apparent density of 3.5 g / cm³ or more, and high roundness refers to a roundness of 0.90 or more. means of solving the problem

[0028] The inventors have conducted extensive research to solve the above problem.

[0029] Typically, in the water atomization method, the nozzle tip is positioned with a mounting angle (β) in a circumferential and downward direction so that the cooling water is concentrated at the same location where the molten steel falls vertically. The angle between the vertically falling molten steel and the direction of the cooling water sprayed from the nozzle tip is called the water convergence angle (α), and the thickness or expansion of the spray is ignored. The water convergence angle is half the mounting angle (α = β / 2). The nozzle tip is mounted on the nozzle header. Typically, a nozzle tip that sprays water in a straight line is used as the nozzle tip, but the inventors have found that it is effective to use a flat spray nozzle in which the sprayed water spreads out in a fan shape, as shown in FIG. 3. In particular, they have found that it is effective to use a spray nozzle in which the water sprayed from the discharge port spreads out at an angle of 5 to 30°.

[0030] In addition, in such a spray nozzle, the discharge port is positioned on the circumference and also in a downward direction, and the convergence angle is set to 5 to 10°.

[0031] In addition, it was found that the above problem can be solved by making the ratio of cooling water to molten steel : water / molten steel ratio 50 or higher.

[0032] Specifically, the present invention provides the following [1] method.

[0033] [1] A method for manufacturing water atomized metal powder by spraying cooling water that collides with molten metal falling vertically and breaking the molten metal into metal powder,

[0034] The process includes spraying the cooling water from each of three or more cooling water discharge ports spaced apart from the falling molten metal at a spreading angle in the range of 5 to 30° with a spray pressure of 10 MPa or more.

[0035] The diameter of the droplets of the cooling water discharged toward the molten metal is 100 μm or less as a sutter average, and

[0036] The water convergence angle formed by the trajectory of the cooling water discharged toward the molten metal and the trajectory of the molten metal is in the range of 5 to 10°, and

[0037] The water / molten steel ratio (F / M) of the amount of cooling water F (kg / min) discharged toward the molten metals and the amount of molten metals falling M (kg / min) is 50 or more, and

[0038] The above metal powder is,

[0039] The total content of Fe, Ni, and Co is 76.0 at% or more and 86.0 at% or less in terms of atomic fraction, and

[0040] A method for manufacturing water atomized metal powder having an average particle size of less than 50 μm, an apparent density of 3.5 g / cm³ or more, a roundness of 0.90 or more, and a degree of amorphization of 90% or more. Effects of the invention

[0041] According to the present invention, even if the total content of Fe, Ni, and Co is 76.0 at% or more, it is possible to produce a metal powder having an average particle size of less than 50 μm, an amorphous rate of 90% or more, an apparent density of 3.5 g / cm³ or more, and a roundness of 0.90 or more.

[0042] In addition, if appropriate heat treatment is performed on the water atomized metal powder obtained in the present invention after molding, nano-sized crystals are precipitated.

[0043] In particular, if the water atomized metal powder has a high content of iron-based elements, it is possible to achieve both low loss and high magnetic flux density by performing appropriate heat treatment after molding the metal powder.

[0044] In addition, recently, hetero-amorphous materials with high magnetic flux density and nanocrystalline materials have been developed, as shown in Materia Japan Vol.41 No.6 P.392, Journal of Applied Physics 105, 013922 (2009), Japanese Patent Publication No. 4288687, Japanese Patent Publication No. 4310480, Japanese Patent Publication No. 4815014, WO2010 / 084900, Japanese Published Patent Publication No. 2008-231534, Japanese Published Patent Publication No. 2008-231533, Japanese Patent Publication No. 2710938, etc. The present invention is highly advantageously suitable when manufacturing metal powders containing a high content of iron-based elements using the water atomization method. In particular, when the concentration of Fe-based components in at% is 76.0% or higher, it was very difficult to increase the amorphization rate in conventional technology.

[0045] However, when the manufacturing method of the present invention is applied, the average particle size is less than 50 μm, the apparent density is 3.5 g / cm³ or more, and the roundness (C 50 A metal powder can be obtained in which ) is 0.90 or higher and the degree of amorphization is 90% or higher. Brief explanation of the drawing

[0046] FIG. 1 is a schematic diagram showing a manufacturing apparatus for water atomized metal powder used in the manufacture of the present embodiment. FIG. 2 is a schematic diagram showing an atomizing device used in the manufacture of the present embodiment. Figure 3 is a drawing showing the spraying state of a flat spray nozzle that spreads in a fan shape. Figure 4 is a drawing showing the spraying state of a flat spray nozzle viewed from the side with respect to Figure 3. Figure 5 is a diagram illustrating an example of a method for measuring the spreading angle (θ). Figure 6 is a drawing showing the spraying state of a flat spray nozzle viewed from the top surface with respect to Figure 2. Specific details for implementing the invention

[0047] Embodiments of the present invention are described below. Furthermore, the present invention is not limited to the following embodiments.

[0048] The method for manufacturing water atomized metal powder according to the present embodiment is a method for manufacturing water atomized metal powder by spraying cooling water that collides with molten metal falling in a vertical direction and splitting the molten metal into metal powder, comprising a process of spraying cooling water from each of three or more cooling water discharge ports spaced apart from the falling molten metal at a spreading angle in the range of 5 to 30° with a spray pressure of 10 MPa or more, wherein the droplet diameter of the cooling water discharged toward the molten metal is 100 μm or less in terms of Souter average, the convergence angle formed by the trajectory of the cooling water discharged toward the molten metal and the trajectory of the molten metal is in the range of 5 to 10°, and the water / molten steel ratio (F / M) of the amount of cooling water discharged toward the molten metal F (kg / min) and the amount of molten metal falling M (kg / min) is 50 or more.

[0049] And, the obtained metal powder has a total content of Fe, Ni, and Co of 76.0 at% or more and 86.0 at% or less in terms of atomic fraction, an average particle size of less than 50 μm, an apparent density of 3.5 g / cm³ or more, a roundness of 0.90 or more, and a degree of amorphousness of 90% or more.

[0050] In this embodiment, a method for manufacturing water-atomized metal powder is described while describing a preferred apparatus for manufacturing water-atomized metal powder.

[0051] FIG. 1 is a schematic diagram showing a manufacturing apparatus for water-atomized metal powder used in the manufacture of the present embodiment. FIG. 2 is a schematic diagram showing an atomizing apparatus used in the manufacture of the present embodiment. FIG. 3 and FIG. 4 are diagrams showing the spraying state of a flat spray nozzle that spreads in a fan shape.

[0052] The device for manufacturing water atomized metal powder shown in FIG. 1 consists of an atomizing device (14), a high-pressure pump for cooling water (17), and a cooling water tank (15). Regarding the cooling water, the temperature in the cooling water tank (15) is adjusted using a temperature controller (16) for cooling water, and is sent to the high-pressure pump (17) for cooling water, and then sent from the high-pressure pump (17) to the atomizing device (14) through a cooling water pipe (a water supply pipe from the high-pressure pump) (18). In addition, in the atomizing device (14), cooling water (7) is sprayed from a cooling water nozzle (spray nozzle) (5) against molten metal (6) falling in a vertical direction, and the molten metal (6) is divided into metal powder, and the metal powder is cooled to manufacture metal powder. The high-pressure pump (17) for the cooling water is shown as one unit in the drawing, but two or more units may be formed for each cooling water.

[0053] The atomizing device (14) shown in FIG. 2 has a tundish (1), a molten steel nozzle (3), a nozzle header (4), a cooling water nozzle (spray nozzle) (5A, 5B), a water supply pipe (18) from a high-pressure pump, and a chamber (19).

[0054] A tundish (1) is a vessel-like member into which molten steel (2) melted in a melting furnace is poured. A commonly known tundish (1) can be used. As shown in FIG. 1, an opening is formed in the bottom of the tundish (1) to connect a molten steel nozzle (3).

[0055] By adjusting the composition of the molten steel (2), the composition of the water atomized metal powder produced can be adjusted. The manufacturing method of this embodiment is suitable for producing atomized metal powder in which the total content of Fe, Ni, and Co is 76.0 at% or more and 86.0 at% or less in terms of atomic fraction, and the average particle size is less than 50 μm. In addition, it is preferable that the above atomized metal powder contains at least one type selected from Si, P, and B, or additionally contains Cu. Therefore, in order to produce a water atomized metal powder of the above composition, the composition of the molten steel (2) can be adjusted to the above range.

[0056] The molten steel nozzle (3) is a conventional body connected to the opening at the bottom of the tundish (1). Molten steel (2) passes through the interior of the molten steel nozzle (3). If the length of the molten steel nozzle (3) is long, the temperature of the molten steel (2) decreases while passing through it. Therefore, the melting temperature in the melting furnace needs to be determined by predicting the temperature decrease in the molten steel nozzle (3). The length of the molten steel nozzle (3) depends on the thickness of the nozzle header (4). Since it is necessary to make the nozzle header thicker due to internal pressure when the injection pressure increases, the length of the molten steel nozzle (3) also needs to be changed. The amount of molten steel falling per unit time (the amount of molten metal falling M (kg / min)) can be adjusted by the diameter of the injection hole of the molten steel nozzle (3).

[0057] The spray nozzle (5A, 5B) is a preferred nozzle for discharging cooling water (7) that collides with molten metal (6), and the ratio of the amount of cooling water (7) F discharged from the discharge port of the spray nozzle (5A, 5B) to the amount of molten steel M is the water / molten steel ratio (F / M). In this embodiment, this water / molten steel ratio (F / M) is adjusted to be 50 or more.

[0058] If the water / molten steel ratio (F / M) is less than 50, the cooling rate is slow and some or all of the powder is prone to crystallization, so there is a possibility that the desired degree of amorphization may not be obtained. Also, the water / molten steel ratio (F / M) is preferably 80 or higher, and more preferably 100 or higher.

[0059] The spray nozzles (5A, 5B) collide with the molten metal (6) falling vertically through the molten metal nozzle (3) by spraying cooling water (7). As a result, the molten metal (6) is broken up and metal powder is obtained.

[0060] It is preferable that spray nozzles (5A, 5B) be arranged at equal intervals (equal angles) on the circumference to maintain the symmetry of the atomizer. In this embodiment, cooling water (7) is discharged from each of three or more cooling water discharge ports spaced apart from the falling molten metal (6). To correspond to the number of cooling water discharge ports, it is preferable to form three or more spray nozzles (5A, 5B) on the lower part of the nozzle header (4). Also, while it is preferable to have a large number of spray nozzles (5A, 5B) to suppress the occurrence of coarseness (areas with a small amount of water sprayed and areas with a large amount of water sprayed) in the water film formed by the cooling water (7) sprayed from the nozzles, it is preferable to have 36 or fewer, taking into account that there is a limit to the number that can be mounted on the circumference and processed. Also, it is more preferable that the number of spray nozzles (5A, 5B) be 8 or more. Also, it is more preferable that the number of spray nozzles (5A, 5B) be 18 or fewer. Also, the number of spray nozzles (5A, 5B) may be odd or even.

[0061] Here, the configuration of the spray nozzles (5A, 5B) is not particularly limited, but it is preferable to use flat spray nozzles. As shown in FIG. 3, in the flat spray nozzle, water is sprayed onto the molten metal (6) so that water droplets spread out in a fan shape from the cooling water discharge port (5X) toward the molten metal (6) when viewed from the direction of descent of the molten metal (6), that is, in a cross-section perpendicular to the direction of descent of the molten metal (6) (see FIG. 6 described later).

[0062] As shown in FIG. 3, the spreading angle (θ) refers to the angle formed by the trajectory of water droplets at both ends (outermost) with the cooling water discharge port (5X) as the center of the circle in the fan shape.

[0063] FIG. 5 is a drawing for explaining an example of a method for measuring a specific spreading angle (θ). As shown in FIG. 5, a transparent acrylic mesh having a predetermined size (e.g., height 300 mm, length (depth) 150 mm, width 700 mm) and divided into a predetermined pitch (e.g., 10 mm pitch) is prepared, and spray nozzles (5A, 5B) are installed at a predetermined position from the top of the mesh (e.g., a position 1 m from the top of the transparent acrylic mesh), and cooling water (7) is sprayed so as not to spill out of the mesh in a vertical downward direction. Then, when the cooling water (7) reaches the top of the mesh (100%), the spraying is stopped, and at that time, the angle formed by the two end positions and the center of the circle in the range where the cooling water (7) is accumulated in the mesh at a predetermined ratio (it may be 80% or more, 75% or more, or 70% or more) may be the spreading angle (θ).

[0064] Meanwhile, as shown in FIG. 4, when viewed from the side of the spreading surface of FIG. 3 (the straight YZ plane when the spreading surface of the water droplet is the XZ plane, also referred to as the cross-section), if a flat spray nozzle is used, the water droplet is sprayed without spreading. At this time, in the direction shown in FIG. 4, the spreading angle (φ) in the thickness direction (cross-section direction) is preferably 2° or less, and more preferably 1.5° or less. Also, it is preferable that it be 1° or more.

[0065] Regarding this, the spreading angle (θ) of the droplet shown in Fig. 3 is set to 5 to 30°.

[0066] If θ is less than 5°, the density of the aforementioned cooling water (7) is likely to occur. That is, in the molten metal (6), large particles are likely to occur in the sparse parts that do not come into contact with the sprayed cooling water (7), while in the dense parts that come into contact with a lot of the sprayed cooling water (7), the cooling action is strong, so the apparent density of the particles obtained is lower. Therefore, there are cases where the desired apparent density and roundness are not obtained. On the other hand, if θ is greater than 30°, the cooling energy sprayed at high pressure is lost as adjacent cooling water (7) spread out in a fan shape interferes with each other. Therefore, there are cases where the desired average particle size and degree of amorphousness are not obtained, as large particles are likely to occur and crystallization becomes easier due to the reduced cooling capacity. Accordingly, the spreading angle (θ) of the water droplets is set to 5 to 30°. Also, more preferably, θ is 8° or more, and even more preferably 10° or more. Also, more preferably, θ is 20° or less, and even more preferably 15° or less.

[0067] FIG. 6 is a drawing showing the spraying state of a flat spray nozzle viewed from the top surface with respect to FIG. 2. When multiple flat spray nozzles having the configuration described above are used, as shown in FIG. 6, when viewed from the top of the device (14) in the direction (vertical direction) where the molten metal (6) shown in FIG. 2 falls, the cooling water (7) is sprayed so as to spread toward the center (towards the molten metal (6)). Also, FIG. 2 is a drawing of cross-section A in FIG. 6 viewed from the vertical direction of cross-section A.

[0068] In addition, the injection pressure is set to 10 MPa or higher. If the injection pressure is less than 10 MPa, the power as an atomizing agent becomes insufficient, and the resulting atomized metal powder cannot obtain the desired average particle size. In addition, there are cases where the desired degree of amorphization cannot be obtained. Therefore, the injection pressure is set to 10 MPa or higher. In addition, the injection pressure is preferably set to 12 MPa or higher, and more preferably to 15 MPa or higher. In addition, the injection pressure is preferably set to 100 MPa or lower, and more preferably to 50 MPa or lower.

[0069] In this way, in the method for manufacturing water atomized metal powder of the present embodiment, cooling water is sprayed from each of three or more cooling water discharge ports spaced apart from the falling molten metal flow at a spreading angle in the range of 5 to 30° with a spray pressure of 10 MPa or more.

[0070] In addition, the spray pressure is the pressure of water in the nozzle header (4) and the pressure of the cooling water discharged from the cooling water discharge port (5X), which is preset by the design of the spray nozzles (5A, 5B).

[0071] Also, the distance (LJ) (see FIG. 2) from the cooling water discharge port (5X) of each spray nozzle (5A, 5B) to the contact position of the molten metal (6) is not particularly limited, but it is preferable to have a distance of 50 mm or more. Also, it is preferable that the distance (LJ) be 200 mm or less.

[0072] If the distance (LJ) is excessively long, the energy of the sprayed cooling water (7) is lost, making it easy for the particles to become coarse, whereas if the distance (LJ) is excessively short, it is easy for the sprayed cooling water (7) to become dense. Therefore, it is preferable that the distance (LJ) be 50 mm or more, and more preferable that it be 80 mm or more. Also, it is preferable that the distance (LJ) be 200 mm or less, and more preferably 150 mm or less.

[0073] Also, the droplet diameter of the cooling water (7) discharged toward the molten metal (6) is the Souter average (D 32 ) is 100 μm or less. If the droplet diameter is greater than 100 μm as a sutter average, the amount of molten metal (6) in contact with the droplet increases when the molten metal (6) is divided, and the desired average particle size cannot be obtained.

[0074] In addition, as the average particle size increases, the amount of cooling water required per powder particle increases, and in some cases, it becomes difficult to amorphize. Therefore, the droplet diameter is set to 100 μm or less as a sutter average. Also, the droplet diameter is preferably set to 80 μm or less, and more preferably to 50 μm or less.

[0075] In addition, the droplet diameter is measured offline by the PDA method, and if the injection pressure is high and measurement by the PDA method is difficult, it is obtained by image analysis using a high-speed camera with a speed of 1 million frames / second or more.

[0076] Also, as indicated by the symbol α in FIG. 2, the angle of convergence formed by the trajectory of the cooling water (7) discharged toward the molten metal (6) from each of the three or more cooling water discharge ports (5X) spaced apart from the falling molten metal (6) and the trajectory of the molten metal is 5 to 10°. Here, the above trajectory refers to a linear trajectory formed by connecting the center position of the area where the cooling water (7) and the molten metal (6) come into contact with the cooling water discharge port (5X).

[0077] If α is less than 5°, the energy for splitting the molten metal (6) becomes smaller, so the desired degree of amorphization may not be obtained. On the other hand, if α is greater than 10°, the impact force for splitting the molten metal (6) becomes stronger, and the cooling action becomes stronger, so the desired degree of circularity may not be obtained. Therefore, the convergence angle (α) is set to 5 to 10°. Also, preferably, the convergence angle (α) is 7.5° or more. Also, in FIG. 2, β represents the angle (mounting angle) formed by the trajectory of one cooling water (7) and the trajectory of the other cooling water (7) in a pair of cooling waters (7) discharged toward molten metal when two cooling discharge ports (5X) face each other, and since α is 5 to 10°, β is 10 to 20°.

[0078] The chamber (19) forms a space for manufacturing metal powder below the nozzle header (4). Metal powder manufactured by water atomization is collected in the chamber (19) along with water, dehydrated, and dried at a temperature of 200°C or lower to obtain metal powder that does not contain moisture.

[0079] Next, the average particle size, apparent density, circularity, and degree of amorphization are measured for the obtained metal powder.

[0080] Apparent density is measured in accordance with JIS Z 2504:2012.

[0081] The circular shape is obtained by using a powder image analysis device (G3SE) manufactured by Morphologic Co., Ltd., capturing approximately 5,000 projected images of powder particles dispersed on a slide, and performing image analysis by binarizing each powder data of the projected images to obtain a volume average value (C 50 Calculate the value of ).

[0082] The degree of amorphization is calculated by removing dust other than the metal powder from the obtained metal powder, measuring the halo peaks from the amorphous phase and the diffraction peaks from the crystal by X-ray diffraction, and calculating the WPPD method. The term "WPPD method" here is an abbreviation for Whole-powder-pattern decomposition method, and is explained in detail in Hideo Toraya: Journal of the Japan Crystallographic Society, vol.30 (1988), No.4, pages 253–258.

[0083] In addition, the particle size is the average particle size (D) by the integration method. 50 It calculates ). It is also possible to use laser diffraction / scattering particle size distribution measurement.

[0084] In this way, the metal powder obtained has a total content of Fe, Ni, and Co of 76.0 at% or more and 86.0 at% or less in terms of atomic fraction, an average particle size of less than 50 μm, an apparent density of 3.5 g / cm³ or more, a roundness of 0.90 or more, and a degree of amorphousness of 90% or more.

[0085] Examples

[0086] The examples and comparative examples were carried out by applying and using the same equipment as the manufacturing equipment shown in FIGS. 1 and FIGS. 2.

[0087] In the atomizing device, 12, 4, or 2 spray nozzles are installed at equal intervals in a circumferential manner on a plane perpendicular to the direction of descent of the molten metal, and the convergence angle (α) formed by the trajectory of the cooling water discharged toward the molten metal and the trajectory of the molten metal is set to 2.5 to 15°. That is, the spray nozzles are installed circumferentially on a plane perpendicular to the direction of descent of the molten metal, and the mounting angle (β) of the two opposing spray nozzles is set to 5 to 30°. Here, "opposing" means that the spray nozzles are installed within a range of 180° ± 10° with the direction of descent of the molten metal as the central axis. In addition, the spreading angle (θ) of the flat spray nozzles shown in FIGS. 3 and 4 used in the example is set to 3 to 40°. The amount of cooling water F was adjusted to 120 to 500 kg / min, and the spray pressure was set to a range of 5 to 30 MPa. The spray nozzle was modified to achieve the desired amount and spray pressure for each purpose.

[0088] In carrying out the manufacturing methods of the examples and comparative examples, soft magnetic materials with the following compositions were prepared. Also, “%” means “at%”. (i) to (v) are Fe-based soft magnetic raw materials, (vi) is Fe + Co-based soft magnetic material, and (vii) is Fe + Co + Ni-based soft magnetic material.

[0089] (i) Fe 76.0% - Si 9.0% - B 10.0% - P 5.0%

[0090] (ii) Fe 78.0% - Si 9.0% - B 9.0% - P 4.0%

[0091] (iii) Fe 80.0% - Si 8.0% - B 8.0% - P 4.0%

[0092] (iv) Fe 82.8% - B 11.0% - P 5.0% - Cu 1.2%

[0093] (v) Fe 84.8% - Si 4.0% - B 10.0% - Cu 1.2%

[0094] (vi) Fe 69.8% - Co 15.0% - B 10.0% - P 4.0% - Cu 1.2%

[0095] (vii) Fe 69.8% - Ni 1.2% - Co 15.0% - B 9.4% - P 3.4% - Cu 1.2%

[0096] Tables 1 and 2 show the raw material conditions, atomization conditions, and powder evaluation of the examples and comparative examples.

[0097]

[0098]

[0099] In the examples and comparative examples, for each component (i) to (vii), raw materials such as iron were placed in a high-frequency melting furnace and melted by applying high frequency. At that time, the melting temperature prior to atomization was set to a range of 1500 to 1650°C. Since the melting point increases with higher iron content, the melting temperature is increased. When the target melting temperature is reached, the high-frequency melting furnace is tilted and the molten steel is poured into a tundish. A molten steel nozzle with a predetermined hole diameter is installed at the bottom of the tundish, and the molten steel drop rate is adjusted to a range of 4 to 5 kg / min. The hole at the tip of the molten steel nozzle that drops the molten steel is adjusted to φ1.5 - 2.5 mm. As shown in Table 1, the water convergence angle, type and number of nozzles, injection pressure, and amount of cooling water were adjusted for each atomization condition. In addition, regarding the type of nozzle, for example, a fan-shaped 30° spray refers to the use of a flat spray nozzle with a spreading angle (θ) of 30°, and the same applies to other types.

[0100] Diameter at the souter average of the droplet ejected from the spray nozzle (hereinafter, souter average diameter (D 32Regarding )), it was measured separately offline using the PDA method. When the injection pressure is high, measurement using the PDA method is difficult, and in some cases, it was obtained by image analysis using a high-speed camera with a speed of 1 million frames / second or more.

[0101] In evaluating the powder, circularity (C 50 ), average particle size (D 50 ), apparent density, and degree of amorphousness were measured using the following methods.

[0102] Apparent density was measured in accordance with JIS Z 2504:2012.

[0103] The circular shape is obtained by using a powder image analysis device (G3SE) manufactured by Morphologic Co., Ltd. to take approximately 5,000 projected images of powder particles dispersed on a slide, and by binarizing each powder data of the projected images to perform image analysis and obtain a volume average value (C 50 The value of ) was calculated.

[0104] The degree of amorphization was calculated by removing dust other than the metal powder from the obtained metal powder, measuring the halo peak from the amorphous phase and the diffraction peak from the crystal by X-ray diffraction, and calculating it by the WPPD method.

[0105] The particle size is the average particle size (D) by the integration method. 50 ) was calculated. Laser diffraction / scattering particle size distribution measurement was used.

[0106] Average particle size (D 50 ) has a target value of less than 50 µm, and for apparent density, 3.5 g / cm³ or more, and roundness (C 50The goal was to have an apparent density of 0.90 or higher and a degree of amorphousness of 90% or higher. If the apparent density, roundness, average particle size, and degree of amorphousness all meet the target, it was considered a pass (○), and if any of the apparent density, roundness, average particle size, and degree of amorphousness do not meet the target, it was considered a fail (×).

[0107] In Example 1, the spreading angle of the fan-shaped flat spray nozzle was set to 30°, in Example 2 to 15°, and in Example 3 to 5°. In Examples 1 to 3, which are atomization conditions within the scope of the present invention, the evaluation of the powder was all acceptable. In addition, the average particle size tended to be smaller when the spreading angle of the fan-shaped flat spray nozzle was 5° rather than 30°.

[0108] Example 4 is an atomization condition within the scope of the present invention in which the convergence angle of the spray nozzle is 5.0° (mounting angle 10°), and compared to Example 2, the particle size is larger but the apparent density is higher.

[0109] Example 5 is an atomization condition within the scope of the present invention in which the convergence angle of the spray nozzle is 7.5° (mounting angle 15°), and compared to Example 4, the average particle size could be reduced.

[0110] Example 6 is an atomization condition within the scope of the present invention with 4 spray nozzles, and compared to Example 2 with 12 spray nozzles, the average particle size is larger and the apparent density is smaller.

[0111] Example 7 lowers the injection pressure and the droplet diameter at the Souter average of the droplet (hereinafter, Souter average diameter) (D 32 The atomization conditions within the range of the present invention are set to 89 μm, and compared to Example 2, the average particle size is larger.

[0112] In Example 8, the amount of cooling water F was adjusted to 400 kg / min based on the conditions of Example 4. The water / molten steel ratio (F / M) was 80-100 [-], which is a desirable water / molten steel ratio. Example 8 is an atomization condition within the scope of the present invention, and compared to Example 4, the degree of amorphization was improved in a composition with a high Fe-based concentration.

[0113] In Example 9, the amount of cooling water F was adjusted to 500 kg / min based on the conditions of Example 4. The water / molten steel ratio (F / M) became 100 - 125 [-], which is a more desirable water / molten steel ratio. Example 9 is an atomization condition within the scope of the present invention, and compared to Example 4, the degree of amorphization was further improved in a composition with a high Fe-based concentration.

[0114] In any of the conditions of Examples 1 to 9, the evaluation of the powder was acceptable.

[0115] Comparative Example 1 used a solid spray nozzle in which water is sprayed in a straight line to an atomized water spray nozzle, and the spreading angle was less than 5°, and a nozzle outside the scope of the present invention was used.

[0116] Comparative Example 2 used a flat spray nozzle with a spreading angle of 3° that spreads in a fan shape, and used a nozzle outside the scope of the present invention.

[0117] Comparative Examples 1 and 2 both had small average particle sizes, but were rejected because their apparent density did not meet the target. In addition, their circularity was also rejected.

[0118] Comparative Example 3 used a flat spray nozzle with a spreading angle of 40° that spreads in a fan shape, and thus used a nozzle outside the scope of the present invention. In this comparative example, the degree of amorphization did not reach the target and was rejected. In addition, the average particle size was rejected.

[0119] Comparative Example 4 has a spray pressure of 5 MPa and an average diameter of the droplet (D 32 The condition was outside the scope of the present invention, with ) set to 126 μm, and the average particle size and degree of amorphization did not reach the target, so it was rejected.

[0120] Comparative Example 5 and Comparative Example 6 were both outside the scope of the present invention, with the convergence angle of the spray nozzle set to 2.5° and 15°, respectively. In Comparative Example 5, the degree of amorphization did not reach the target, and in Comparative Example 6, the apparent density and roundness did not reach the target, so both were rejected.

[0121] Comparative Example 7 was under conditions outside the scope of the present invention, with a water / molten steel ratio of 24 to 30 [-], and was rejected because the degree of amorphization did not reach the target.

[0122] Comparative Example 8 was a condition outside the scope of the present invention in which the number of spray nozzles was set to two, and it was rejected because the average particle size and degree of amorphization did not reach the target. In addition, there were cases where the apparent density and roundness also did not reach the target.

[0123] As described above, the metal powders prepared in Examples 1 to 9, which are within the scope of the present invention, were all accepted, while the comparative examples 1 to 8, which are outside the scope of the present invention, were all rejected. Explanation of the symbols

[0124] 1 : Turnish 2 : Molten Steel 3: Molten steel nozzle 4: Nozzle Header 5, 5A, 5B: Coolant nozzle (spray nozzle) 5X: Coolant outlet 6 : Molten metals 7 : Coolant 9: Metal powder 14: Atomizer 15: Coolant tank 16 : Coolant temperature controller 17: High-pressure pump for cooling water 18: Cooling water piping (water supply pipe from high-pressure pump) 19: Chamber α: Convergence angle (contact angle between vertically falling molten steel and sprayed cooling water) β : Mounting angle (vertex angle) θ: Spread angle

Claims

Claim 1 A method for manufacturing water-atomized metal powder by spraying cooling water that collides with molten metal falling vertically, splitting the molten metal into metal powder, and cooling the metal powder, comprising a process of spraying the cooling water from each of three or more cooling water discharge ports spaced apart from the falling molten metal at a spreading angle in the range of 5 to 30° with a spray pressure of 10 MPa or more, wherein a water film is formed by the cooling water sprayed from each of the three or more cooling water discharge ports, wherein the droplet diameter of the cooling water discharged toward the molten metal is 100 μm or less as a souter average, and the convergence angle formed by the trajectory of the cooling water discharged toward the molten metal and the trajectory of the molten metal is in the range of 5 to 10°, and the amount of the cooling water F (kg / min) discharged toward the molten metal and the molten metal A method for producing a water atomized metal powder in which the water / molten steel ratio (F / M) of the drop rate M (kg / min) is 50 or higher, and the produced water atomized metal powder has a total content of Fe, Ni, and Co of 76.0 at% or higher and 86.0 at% or lower in atomic fraction, an average particle size of less than 50 μm, an apparent density of 3.5 g / cm³ or higher, a roundness of 0.90 or higher, and a degree of amorphization of 90% or higher.

Citation Information

Patent Citations

  • Method for producing metal powder by water atomizing process

    JP2016141817A

  • Production method of water atomization metal powder

    JP2017031461A

  • Method for producing atomized metal powder

    JP2020105593A