Resin composition, molded article, and cosmetic container
A resin composition with a copolymer of aromatic vinyl and cyano monomers, enhanced with specific antioxidants, addresses color degradation and transparency issues, providing high transparency and chemical resistance for high-design-quality applications.
Patent Information
- Application Number
- KR1020237010106
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-28
- Filing Date
- 2021-08-20
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-08-20
AI Technical Summary
Thermoplastic copolymers with cyano monomers suffer from color degradation and low transparency during molding, making them unsuitable for high-design-quality applications like cosmetic containers.
A resin composition containing a copolymer of an aromatic vinyl monomer and a cyano monomer, combined with an antioxidant having three or more phenolic groups and a phosphorus-based antioxidant, within specific content ratios, to enhance transparency and color tone.
The resin composition achieves high transparency and chemical resistance, suitable for high-design-quality applications such as cosmetic containers.
Smart Images

Figure 112023033113662-PCT00001 
Figure 112023033113662-PCT00002 
Figure 112023033113662-PCT00003
Abstract
Description
Technology Field
[0001] The present invention relates to a resin composition containing a copolymer of an aromatic vinyl monomer and a cyano monomer, a molded article thereof, and a cosmetic container. Background Technology
[0002] Copolymers containing aromatic vinyl monomers and cyano monomers are used in a wide range of fields because they possess various properties such as excellent chemical resistance, rigidity, and moldability. However, thermoplastic copolymers with cyano monomers as a single component are prone to color degradation due to high temperatures during molding processing. Consequently, there was a problem in that the actual molded body had low clarity and became dull.
[0003] To solve these problems, methods have been proposed such as using an initiator with low hydrogen pulling ability during polymerization (Patent Document 1), adding an antioxidant having two phenolic groups in the molecule at a polymerization stage of 60% or more (Patent Document 2), and using t-amylperoxyesters that do not contain an aromatic ring when copolymerizing an acrylonitrile monomer and a styrene-based monomer (Patent Document 3). Prior art literature
[0004] Japanese Patent Publication No. Hei 4-146908 Japanese Patent Publication No. Hei 4-146907 Japanese Patent Publication No. Hei 8-301913 The problem to be solved
[0005] However, it cannot be said that color can be sufficiently improved with this method, and it is difficult to say that a resin meeting the required level in terms of transparency or color tone is obtained, especially for raw materials such as cosmetic containers where high design quality is required.
[0006] The present invention aims to provide a resin containing a copolymer of an aromatic vinyl monomer and a cyano monomer, which, as a raw material for cosmetic containers or the like that require particularly high design quality, can have chemical resistance and high transparency or high color tone after molding processing. means of solving the problem
[0007] As a result of repeated diligent research to solve the above problem, the inventors have discovered that the following embodiments are effective.
[0008] (1) In one embodiment, the resin composition according to the present invention is a resin (A) containing a copolymer of an aromatic vinyl monomer and a cyano monomer, an antioxidant (B) having a total of three or more phenolic groups in the molecule, and a phosphorus-based antioxidant (C).
[0009] (2) In another embodiment of the resin composition according to the present invention, the total content of antioxidant (B) and antioxidant (C) is 0.01 to 0.5 parts by mass per 100 parts by mass of resin (A).
[0010] (3) In another embodiment of the resin composition according to the present invention, the copolymer of the aromatic vinyl monomer and the cyano monomer contains 40 to 95 mass% of the aromatic vinyl monomer unit and 5 to 60 mass% of the cyano monomer unit when the total of the aromatic vinyl monomer and the cyano monomer is 100 mass%.
[0011] (4) In another embodiment, the molded body according to the present invention is characterized by being formed by molding with a resin composition described in any one of (1) to (3).
[0012] (5) In another embodiment, the cosmetic container according to the present invention is characterized by being formed by molding a resin composition described in any one of (1) to (3). Effects of the invention
[0013] According to the present invention, a resin having chemical resistance and also having high transparency or high color tone is provided. The resin composition can be used in cosmetic containers and the like that require high design quality. Specific details for implementing the invention
[0014] The resin composition of the present invention comprises a resin (A) containing a copolymer of an aromatic vinyl monomer and a cyano monomer, an antioxidant (B) having a total of three or more phenolic groups in the molecule, and a phosphorus-based antioxidant (C).
[0015] The resin (A) in the present invention is a resin having a copolymer of an aromatic vinyl monomer and a cyano monomer as its main component. The content of the copolymer of the aromatic vinyl monomer and the cyano monomer in 100 mass% of the resin (A) is, for example, 50 mass% or more. In one embodiment, the content of the copolymer in the resin (A) is preferably 80 mass% or more, and more preferably, the resin (A) is substantially composed only of a copolymer of an aromatic vinyl monomer and a cyano monomer.
[0016] Aromatic vinyl monomers are not particularly limited, but examples include styrene, α-methylstyrene, p-methylstyrene, 3,5-dimethylstyrene, 4-methoxystyrene, 2-hydroxystyrene, substituted styrenes having substituents, α-bromstyrene, 2,4-dichlorostyrene, 1-vinylnaphthalene, etc.
[0017] Cyano-based monomers are not particularly limited, but examples include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-ethylacrylonitrile, etc.
[0018] It is important that the antioxidant (B) of the present invention has a total of three or more phenolic groups within the basic framework of the molecule. If there are two or fewer, the antioxidant ability is insufficient, and the resin deteriorates during molding, and the color deteriorates.
[0019] The antioxidant (B) that can be used in the present invention specifically includes trisphenols such as 1,3,5,tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5,triazine-2,4,6(1H,3H,5H)-trione, 4,4',4''-(1-methylpropanyl-3-iridene)tris(6-tert-butyl-m-cresol), 1,3,5,tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene, tetraphenols such as pentaerythritol-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], and may be used alone or in combination of two or more types.
[0020] The phosphorus-based antioxidant (C) of the present invention is, for example, trisnonylphenylphosphite, triphenylphosphite, tris(2,4-di-t-butylphenyl)phosphite, cyclic neopentanetetraylbis(2,4-di-t-butylphenylphosphite), cyclic neopentanetetraylbis(octadecylphosphite), cyclic neopentanetetraylbis(nonylphenylphosphite), tris(mixed, mono and dinonylphenyl)phosphite, 4,4'-isopropylidenediphenolalkyl(C12~C15)phosphite, diphenylisooctylphosphite, diphenylisodecylphosphite, phenyldiisodecylphosphite, trisisodecylphosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, Examples include 2,2-methylenebis(4,6-di-t-butylphenyl)octylphosphite, and can be used alone or in combination of two or more types.
[0021] The total content of the antioxidant (B) and the phosphorus-based antioxidant (C) of the present embodiment is preferably 0.01 to 0.50 parts by mass per 100 parts by mass of the resin (A), more preferably 0.05 to 0.40 parts by mass, and even more preferably 0.10 to 0.30 parts by mass. Specifically, for example, it is 0.01, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, or 0.50 parts by mass, and may be within the range between any two of the values exemplified herein. If the total content of the antioxidant (B) and the phosphorus-based antioxidant (C) exceeds 0.50 parts by mass, the heat resistance of the resulting resin composition may decrease. In addition, if the total content of the antioxidant (B) and the phosphorus-based antioxidant (C) is less than 0.01 parts by mass, the deterioration of the color of the resulting molded product cannot be suppressed.
[0022] In addition, the mixing ratio of the antioxidant (B) and the phosphorus-based antioxidant (C) is not particularly limited. The mass ratio of the antioxidant (B) and the phosphorus-based antioxidant (C) is preferably 5 / 1 to 1 / 5, more preferably 4 / 1 to 1 / 4. Specifically, for example, it is 5 / 1, 4 / 1, 3 / 1, 2 / 1, 1 / 1, 1 / 2, 1 / 3, 1 / 4, or 1 / 5, and may be within the range between any two of the values exemplified herein. By setting the mixing ratio of the antioxidant (B) and the phosphorus-based antioxidant (C) to a mass ratio of 5 / 1 to 1 / 5, the deterioration of the color of the resulting molded article can be effectively suppressed.
[0023] As for the method of adding the antioxidant (B) and the phosphorus-based antioxidant (C), methods such as adding and mixing during the polymerization process, degassing process, or granulation process of the resin (A), or adding and mixing using an extruder or injection molding machine during molding processing, are not particularly limited.
[0024] The content ratio of aromatic vinyl monomers and cyano monomers in resin (A) can be arbitrarily selected, but the amount of aromatic vinyl monomers contained in 100 mass% of the copolymer is preferably 40 mass% to 95 mass%, more preferably 50 mass% to 85 mass%, and even more preferably 70 mass% to 85 mass%. Specifically, for example, it is 40, 50, 60, 65, 70, 75, 80, 85, 90, or 95 mass%, and may be within the range between any two of the values exemplified herein. The amount of cyano monomers contained in 100 mass% of the copolymer is preferably 5 mass% to 60 mass%, more preferably 15 mass% to 50 mass%, and even more preferably 15 mass% to 70 mass%. Specifically, for example, 5, 10, 15, 20, 35, 40, 50, or 60 mass%, and may be within the range between any two of the values exemplified herein. If each monomer is outside the above compositional range, it is difficult to achieve the appearance, chemical resistance, transparency, mechanical properties, etc. of the molded article that is the object of the present invention.
[0025] As a method for manufacturing a resin (A) containing a copolymer of an aromatic vinyl monomer and a cyano monomer in the present invention, a suspension polymerization method, a solution polymerization method, a bulk polymerization method, etc., may be used, but a solution polymerization method or a bulk polymerization method is suitably used for the purpose of preventing incorporation of dispersants, etc. into the resin.
[0026] In the resin (A), copolymerizable monomers other than cyano-based monomers and aromatic vinyl monomers may be copolymerized to a extent that does not impede the effects of the present invention. Examples of other vinyl compounds copolymerizable with cyano-based monomers and aromatic vinyl monomers include acrylic acid esters such as methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, and butyl acrylate; unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid, or their anhydrides; and maleimide compounds such as N-phenylmaleimide and N-cyclohexylmaleimide. In particular, ethyl acrylate and butyl acrylate are preferred, and two or more of these may be used in combination.
[0027] The content of these monomers can be 0% to 20%, preferably 0% to 10%, when the total of the cyano monomer, aromatic vinyl monomer, and monomer copolymerizable with them is 100% by mass.
[0028] In the manufacture of resin (A), for example, t-dodecyl mercaptan, n-dodecyl mercaptan, unsaturated dimer of α-methylstyrene, terpinolene, octyl thioglycolate, etc. can be used as a molecular weight regulator.
[0029] The resin composition of the present invention may contain mineral oil to the extent that it does not impede the effects of the present invention. In addition, it may include additives such as internal lubricants such as stearic acid and ethylenebisstearylamide, sulfur-based antioxidants, lactone-based antioxidants, ultraviolet absorbers, hindered amine-based stabilizers, antistatic agents, and external lubricants.
[0030] UV absorbers are those that have the function of suppressing deterioration or discoloration caused by ultraviolet rays, and examples include benzophenone-based, benzotriazole-based, triazine-based, benzoate-based, salicylate-based, cyanoacrylate-based, boric acid anilide-based, malonic acid ester-based, and formamidine-based UV absorbers. These may be used individually or in combination of two or more types, and light stabilizers such as hindered amines may also be used in combination.
[0031] The resin composition of the present invention may contain various dyes within a range that does not impede the effects of the present invention in order to express various design properties. Examples include coumarin-based fluorescent dyes, benzopyran-based fluorescent dyes, perylene-based fluorescent dyes, anthraquinone-based fluorescent dyes, thioindigo-based fluorescent dyes, xanthene-based fluorescent dyes, xanthone-based fluorescent dyes, thioxanthene-based fluorescent dyes, thioxanthene-based fluorescent dyes, thiazine-based fluorescent dyes, and diaminostilbene-based fluorescent dyes. The content of the above dye pigments is preferably 0.00001 to 1 mass based on 100 mass parts of the total of the resin (A), antioxidant (B), and antioxidant (C), and is more preferably 0.00003 to 0.3 mass parts.
[0032] Regarding the method of obtaining a molded article from a resin composition, known molding processing techniques may be used, such as injection molding, extrusion molding, sheet molding, press molding, etc.
[0033] A molded article obtained by molding the resin composition according to the present invention can be processed into a cosmetic container in which particularly high design quality is required. In addition, the resin composition according to the present invention is suitably used alone or as a mixed resin blended with other resins such as ABS resin or PC resin.
[0034] [Example]
[0035] The following detailed description will be explained using examples, but the present invention is not limited to the following examples.
[0036] <Preparation Example of Resin (A-1)>
[0037] A feed solution supplied to a 50L reaction vessel was prepared to contain 70 parts by mass of styrene, 15 parts by mass of acrylonitrile, 15 parts by mass of ethylbenzene, 0.02 parts by mass of t-butylperoxyisopropylcarbonate as a polymerization initiator, and 0.01 parts by mass of n-dodecyl mercaptan as a chain transfer agent. After bubbling this feed solution with nitrogen gas, it was continuously supplied to the reaction vessel at a rate of 10.8L / hour, maintaining a polymerization temperature of 145°C and a reaction solution filling rate of 70 vol% within the reaction vessel, and an amount of reaction solution equal to the amount of feed solution was continuously withdrawn. The withdrawn reaction solution was introduced into a volatile component removal device maintained at 250°C and a high vacuum of 10 mmHg, where unreacted monomers and organic solvents were degassed and recovered, and the copolymer was recovered as pellets.
[0038] <Preparation Example of Resin (A-2)>
[0039] A feed solution supplied to a 50L reaction vessel was prepared to contain 58 parts by mass of styrene, 22 parts by mass of acrylonitrile, 20 parts by mass of ethylbenzene, 0.02 parts by mass of t-butylperoxyisopropylcarbonate as a polymerization initiator, and 0.04 parts by mass of n-dodecyl mercaptan as a chain transfer agent. After bubbling this feed solution with nitrogen gas, it was continuously supplied to the reaction vessel at a rate of 8L / hour, maintaining a polymerization temperature of 145°C and a reaction solution filling rate of 60 vol% within the reaction vessel, and an amount of reaction solution equal to the amount of feed solution was continuously withdrawn. The withdrawn reaction solution was introduced into a volatile component removal device maintained at 250°C and a high vacuum of 10 mmHg, where unreacted monomers and organic solvents were degassed and recovered, and the copolymer was recovered as pellets.
[0040] <Preparation Example of Resin (A-3)>
[0041] A feed solution supplied to a 50L reaction vessel was prepared to contain 49 parts by mass of styrene, 29 parts by mass of acrylonitrile, 23 parts by mass of ethylbenzene, 0.02 parts by mass of t-butylperoxyisopropylcarbonate as a polymerization initiator, and 0.12 parts by mass of n-dodecyl mercaptan as a chain transfer agent. After bubbling this feed solution with nitrogen gas, it was continuously supplied to the reaction vessel at a rate of 9.8L / hour, maintaining a polymerization temperature of 145°C and a reaction solution filling rate of 80 vol% within the reaction vessel, and an amount of reaction solution equal to the amount of feed solution was continuously withdrawn. The withdrawn reaction solution was introduced into a volatile component removal device maintained at 250°C and a high vacuum of 10 mmHg, where unreacted monomers and organic solvents were degassed and recovered, and the copolymer was recovered as pellets.
[0042] <Preparation Example of Resin (A-4)>
[0043] A mixture was prepared with 70 parts by mass of styrene, 9 parts by mass of acrylonitrile, 21 parts by mass of ethylbenzene, 0.02 parts by mass of t-butylperoxyisopropylcarbonate as a polymerization initiator, and 0.12 parts by mass of n-dodecyl mercaptan as a chain transfer agent. After bubbling this feed solution with nitrogen gas, it was continuously supplied to a reaction vessel at a rate of 9.8 L / hour, maintaining a polymerization temperature of 145°C and a reaction solution filling rate of 75 vol% within the reaction vessel, and continuously withdrawing an amount of reaction solution equal to the amount of feed solution. The withdrawn reaction solution was introduced into a volatile component removal device maintained at 250°C and a high vacuum of 10 mmHg, where unreacted monomers and organic solvents were degassed and recovered, and the copolymer was recovered as pellets.
[0044] <Example of preparation of resin (A-5)>
[0045] A feed solution supplied to a 50L reaction vessel was prepared to contain 84 parts by mass of styrene, 16 parts by mass of ethylbenzene, 0.02 parts by mass of t-butylperoxyisopropylcarbonate as a polymerization initiator, and 0.12 parts by mass of n-dodecyl mercaptan as a chain transfer agent. After bubbling this feed solution with nitrogen gas, it was continuously supplied to the reaction vessel at a rate of 9.8L / hour, maintaining a polymerization temperature of 145°C and a reaction solution filling rate of 80 vol% within the reaction vessel, and continuously withdrawing an amount of reaction solution equal to the amount of feed solution. The withdrawn reaction solution was introduced into a volatile component removal device maintained at 250°C and a high vacuum of 10 mmHg, where unreacted monomers and organic solvents were degassed and recovered, and the copolymer was recovered as pellets.
[0046] The composition analysis in the resin was measured in accordance with JIS K6451-2:2016. In addition, the sample amount was 0.2 g, the decomposition temperature was 400℃, and the standard titration solution used was a standard aqueous sulfuric acid solution.
[0047] <Antioxidant (B)>
[0048] The following was used as an antioxidant (B).
[0049] B-1: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate](Irganox1010 manufactured by BASF Japan Co., Ltd.)
[0050] B-2: 4,4',4''-(1-methylpropanyl-3-iridene)tris(6-tert-butyl-m-cresol) (ADKSTAB AO-30 manufactured by ADEKA Co., Ltd.)
[0051] B-3: 1,3,5,tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene (Irganox1330 manufactured by BASF Japan Co., Ltd.)
[0052] B-4: 4,6-bis(octylthiomethyl)-o-cresol (Irganox 1520 manufactured by BASF Japan Co., Ltd.)
[0053] B-5: 2,4-bis(octylthio)-6-(4-hydroxy-3,5-di-tert-butylanilino)-1,3,5-triazine (Irganox 565 manufactured by BASF Japan Co., Ltd.)
[0054] B-6: Ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-trile)propionate](Irganox 245 manufactured by BASF Japan Co., Ltd.)
[0055] B-7: 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylic acid (Sumilicizer GS manufactured by Sumitomo Chemical Co., Ltd.)
[0056] B-8: n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenyl)propionate (Irganox 1076 manufactured by BASF Japan Co., Ltd.)
[0057] <Phosphorus-based antioxidant (C)>
[0058] As a phosphorus-based antioxidant, the following was used.
[0059] C-1: Tris(2,4-di-tert-butylphenyl)phosphite (manufactured by ADEKA Co., Ltd. ADKSTAB 2112)
[0060] C-2: Tetra-C12-15-alkyl(propane-2,2-diylbis(4,1-phenylene))bis(phosphite)(ADKSTAB 1500 manufactured by ADEKA Co., Ltd.)
[0061] <Resin Composition>
[0062] Examples 1–14, Comparative Examples 1–8
[0063] Resins A-1 to A-5, antioxidant (B), and phosphorus-based antioxidant (C) were blended in the mixing ratios shown in Tables 1 to 3, and then extruded using a single-screw extruder (MS-40 manufactured by IKG Co., Ltd.) to form pellets. Test specimens were prepared using an injection molding machine with these pellets, and each physical property was measured. The results are shown in Tables 1 to 3.
[0064] (Color · Transmittance)
[0065] Using the obtained pellets, a plate-shaped molded article with a thickness of 127 x 127 x 3 mm was molded at a molding temperature of 230°C using an injection molding machine (J140AD-180H, manufactured by Nihon Seikosho Co., Ltd.). A test specimen with a thickness of 115 x 85 x 3 mm was cut from the plate-shaped molded article, and the cross-section was polished by buff polishing to produce a plate-shaped molded article having a mirror finish on the cross-section. For the plate-shaped molded article after polishing, the spectral transmittance from 350 nm to 800 nm was measured at an optical path length of 115 mm under incident light with a size of 20 x 1.6 mm and an angle of 0° using a UV-Vis spectrophotometer V-670 manufactured by Nihon Bunko Co., Ltd., and the YI value at a field of view of 2° under a wavelength C light source was calculated according to JIS K7105. In addition, the transmittance represents the total light transmittance in the range of 430 to 700 nm. The results are shown in Tables 1 to 3.
[0066] (Chemical resistance)
[0067] To exclude the influence of molding deformation, test specimens were prepared by press-forming each pellet to a thickness of 4 mm at 260°C and cutting them into 50 mm x 50 mm squares. After immersion in each chemical set at 40°C for 14 days, they were classified as follows based on changes in weight and appearance. The chemicals used were a 5% aqueous urea solution and salad oil.
[0068] ◎: The impact is hardly acknowledged.
[0069] ○: Slight cloudiness or discoloration is observed.
[0070] △: Slight cracking or crazing occurs
[0071] ×: Dissolution or significant impact
[0072]
[0073]
[0074]
[0075] Examples 1 to 14, which contain a resin (A) said to contain a copolymer of an aromatic vinyl monomer and a cyano-based monomer, an antioxidant (B) having a total of three or more phenolic groups in the molecule, and a phosphorus-based antioxidant (C), had chemical resistance and excellent transparency and YI values. On the other hand, Comparative Examples 1 to 5, which used an antioxidant having two or fewer phenolic groups in the molecule, Comparative Example 6, which did not use an antioxidant, and Comparative Example 7, which did not use a phosphorus-based antioxidant (C), resulted in low transmittance and high YI values, leading to a deterioration in color. Comparative Example 8, which used a resin not containing cyano-based monomer components, had excellent transparency and color, but its chemical resistance was significantly deteriorated. Industrial applicability
[0076] The resin composition and molded article of the present invention exhibit excellent chemical resistance, color, and transparency, making them suitable for applications requiring high design quality and chemical resistance. Specifically, examples include cosmetic containers, food containers, and miscellaneous goods such as lighters.
Claims
Claim 1 A resin composition comprising only a resin (A) comprising a binary copolymer of an aromatic vinyl monomer and a cyano monomer, an antioxidant (B) having a total of three or more phenolic groups in the molecule, and a phosphorus-based antioxidant (C), wherein the resin composition does not include any resin other than the resin (A), and the copolymer comprises 74 to 95 mass% of the aromatic vinyl monomer unit and 5 to 26 mass% of the cyano monomer unit when the total of the aromatic vinyl monomer unit and the cyano monomer unit is 100 mass%. Claim 2 A resin composition according to claim 1, wherein the total content of the antioxidant (B) and the antioxidant (C) is 0.01 to 0.5 parts by mass per 100 parts by mass of the resin (A). Claim 3 A resin composition according to claim 1, wherein the antioxidant (B) has a total of 4 or more phenolic groups within the molecule. Claim 4 A resin composition according to claim 3, wherein the total content of the antioxidant (B) and the antioxidant (C) is 0.10 to 0.50 parts by mass per 100 parts by mass of the resin (A). Claim 5 A molded body characterized by being formed by molding with a resin composition described in any one of claims 1 to 4. Claim 6 A cosmetic container characterized by being formed by molding from a resin composition described in any one of claims 1 to 4.
Citation Information
Patent Citations
Cosmetic resistant PC / ABS alloy material and preparation method thereof
CN104927334A
Heat-resistant ABS resin composition
JP1992139254A
Thermoplastic resin composition excellent in coloring property
JP1999116767A
Flame-retardant resin composition
JP2003226818A
Flame-retardant resin composition
JP2003226819A