Flattening annealing method of grain-oriented electrical steel sheet

The controlled flattening annealing method with specific cooling temperature ranges and laser irradiation addresses stress management in grain-oriented electrical steel sheets, resulting in improved magnetic properties and reduced iron loss for enhanced equipment efficiency.

KR103046844B1Active Publication Date: 2026-11-10POHANG IRON & STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020210182097
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-17
Publication Date
2026-11-10
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

Existing methods for manufacturing grain-oriented electrical steel sheets fail to effectively remove residual stress generated during high-temperature annealing and control the occurrence of new stress during flattening annealing, which affects the magnetic properties and efficiency of the steel sheets.

Method used

A flattening annealing method involving controlled slow and rapid cooling sections with specific temperature ranges and optionally laser irradiation to manage stress and improve magnetic properties, using temperatures that satisfy the equation 100 ≤ ((T r1 -T r2 ) - (T s1 -T s2 ) ≤ 400 and employing gases like hydrogen or nitrogen to prevent oxidation.

Benefits of technology

The method produces electrical steel sheets with excellent magnetic properties and reduced iron loss, enhancing the efficiency of electrical equipment by effectively managing stress and maintaining magnetic domain refinement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112021146822550-PAT00001_ABST
    Figure 112021146822550-PAT00001_ABST
Patent Text Reader

Abstract

A flattening annealing method for a oriented electrical steel sheet according to one embodiment of the present invention, wherein the flattening annealing method for a oriented electrical steel sheet is performed after high-temperature annealing, the flattening annealing comprises a step of cooling to a slow cooling section including a slow cooling start temperature (Ts1) and a slow cooling end temperature (Ts2), and a step of cooling to a rapid cooling section including a rapid cooling start temperature (Tr1) and a rapid cooling end temperature (Tr2) after the slow cooling section, and the temperature difference in the rapid cooling section and the temperature difference in the slow cooling section may satisfy the following Equation 1.100 ≤ ((Tr1-Tr2) - (Ts1-Ts2)) ≤ 400
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to electrical steel sheets, and more specifically, to a flattening annealing method for oriented electrical steel sheets. Background Technology

[0002] Grain-oriented electrical steel is a soft magnetic material used as an iron core for electronic devices requiring excellent unidirectional magnetic properties, such as transformers, by forming a Goss texture throughout the steel sheet using an abnormal grain growth phenomenon called secondary recrystallization, which has excellent magnetic properties in the rolling direction. The above magnetic properties can be expressed in terms of magnetic flux density and iron loss.

[0003] The higher the magnetic flux density, the more the orientation of the crystal grains {110} <001> It is possible to obtain oriented electrical steel sheets that are accurately aligned in orientation, and by lowering hysteresis loss, it is possible to simultaneously achieve miniaturization and high efficiency of electrical equipment. The iron loss is power loss consumed as thermal energy when an arbitrary alternating magnetic field is applied to the steel sheet, and it varies significantly depending on factors such as the magnetic flux density and thickness of the steel sheet, the amount of impurities in the steel sheet, resistivity, and the size of secondary recrystallized grains. The higher the magnetic flux density and resistivity, the thinner the thickness of the steel sheet, and the lower the amount of impurities in the steel sheet, the lower the iron loss becomes, and the efficiency of the electrical equipment increases.

[0004] The secondary recrystallization of the above-mentioned grain-oriented electrical steel sheet occurs when normal grain growth is inhibited by precipitates, inclusions, or elements that are dissolved or segregated at the grain boundaries, unlike conventional grain growth. In addition, in order to grow grains with a high degree of accumulation in the Goss orientation, complex processes such as composition control during steelmaking, slab reheating during hot rolling, control of hot rolling process factors, hot-rolled sheet annealing heat treatment, primary recrystallization annealing, and secondary recrystallization annealing are required, and these processes must be managed very precisely and strictly.

[0005] As such, substances such as precipitates or inclusions that inhibit grain growth are referred to as grain growth inhibitors or inhibitors. In the technology for manufacturing oriented electrical steel sheets by secondary recrystallization of the aforementioned Goss orientation, research is actively being conducted on a technology that secures excellent magnetic properties by using a strong grain growth inhibitor to form secondary recrystallization with a high degree of integration for the aforementioned Goss orientation.

[0006] The above-mentioned oriented electrical steel sheet undergoes high-temperature annealing in a coil state for a long period of time for secondary recrystallization, and during this process, shape defects occur due to residual stress and the self-weight of the coil. To eliminate these, flattening annealing is performed after high-temperature annealing. The flattening annealing requires cooling technology that not only removes residual stress generated during high-temperature annealing but also controls the cooling to prevent new stress from occurring during the cooling of the flattening annealing. Therefore, to manufacture oriented electrical steel sheets with excellent magnetic properties, it is necessary to control the temperature pattern of the cooling section during flattening annealing. The problem to be solved

[0007] The technical problem that the present invention aims to solve is to provide a method for manufacturing a grain-oriented electrical steel sheet that not only removes residual stress generated during high-temperature annealing of the grain-oriented electrical steel sheet but also controls the occurrence of new stress during flattening annealing. means of solving the problem

[0008] A flattening annealing method for a oriented electrical steel sheet according to one embodiment of the present invention, wherein flattening annealing is performed after high-temperature annealing, the flattening annealing is performed at a slow cooling start temperature (T s1 ) and slow cooling end temperature (T s2 A step of cooling to a slow cooling section including ), and after the slow cooling section, a rapid cooling start temperature (T r1 ) and quenching end temperature (T r2The method includes a step of cooling to a rapid cooling section including ), and the temperature difference in the rapid cooling section and the temperature difference in the slow cooling section may satisfy the following Equation 1.

[0009] <Equation 1>

[0010] 100 ≤ ((T r1 -T r2 ) - (T s1 -T s2 )) ≤ 400

[0011] In one embodiment, the temperature difference (T) in the slow cooling section s1 -T s2 ) may be 10 ℃ or higher. In one embodiment, the temperature difference (T) in the slow cooling section. s1 -T s2 ) can be 10 to 50 ℃.

[0012] In one embodiment, the slow cooling start temperature (T s1 ) may be 750 to 900 ℃. In one embodiment, the slow cooling end temperature (T s2 ) can be 700 to 850 ℃.

[0013] In one embodiment, the temperature difference (T) in the rapid cooling section r1 -T r2 ) may be 130 to 430 ℃. In one embodiment, the quenching start temperature (T r1 ) can be 700 to 850 ℃.

[0014] In one embodiment, the rapid cooling end temperature (T r2 ) may be 270 to 700 ℃. In one embodiment, the iron loss of the oriented electrical steel sheet may be 0.76 W / kg or less.

[0015] In one embodiment, after the step of cooling to the rapid cooling section, the method may further include the step of irradiating the surface of the oriented electrical steel sheet with a laser beam. In one embodiment, the flattening annealing method of the oriented electrical steel sheet may be performed under a gas atmosphere of at least one of hydrogen, nitrogen, an inert gas, and combinations thereof. In one embodiment, the proportion of hydrogen may be 5 vol% or less. Effects of the invention

[0016] A method for manufacturing a oriented electrical steel sheet according to one embodiment of the present invention can provide a oriented electrical steel sheet with excellent magnetic properties by controlling the slow cooling section and the rapid cooling section during flattening annealing, thereby not only removing residual stress generated during high-temperature annealing but also controlling to prevent new stress from occurring during flattening annealing. Brief explanation of the drawing

[0017] FIGS. 1a and 1b are flowcharts of a flattening annealing method for oriented electrical steel sheets according to one embodiment of the present invention. Specific details for implementing the invention

[0018] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.

[0019] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of “comprising” specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.

[0020] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.

[0021] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0022] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0023] FIGS. 1a and 1b are flowcharts of a flattening annealing method for oriented electrical steel sheets according to one embodiment of the present invention.

[0024] Referring to FIG. 1a, a flattening annealing method for a oriented electrical steel sheet according to one embodiment of the present invention involves a slow cooling start temperature (Ts1 ) and slow cooling end temperature (T s2 A step (S100) of cooling to a slow cooling section including ) and, after the slow cooling section, a rapid cooling start temperature (T r1 ) and quenching end temperature (T r2 It may include a step (S200) of cooling to a rapid cooling section including ). The flattening annealing of the oriented electrical steel sheet may be performed after high-temperature annealing for secondary recrystallization of the oriented electrical steel sheet.

[0025] In the flattening annealing method for the above-mentioned oriented electrical steel sheet, performing flattening annealing after the high-temperature annealing is performed to remove residual stress generated during the high-temperature annealing. The flattening annealing method for the above-mentioned oriented electrical steel sheet may be for controlling the temperature pattern of the cooling section.

[0026] Slow cooling start temperature (T s1 ) and slow cooling end temperature (T s2 The step of cooling into a slow cooling section (S100) including ) is a step of slowly cooling the oriented electrical steel sheet after high-temperature annealing is completed. The step of cooling into a slow cooling section (S100) may be a step for removing residual stress formed in the oriented electrical steel sheet after high-temperature annealing is completed and for shape correction.

[0027] The above slow cooling start temperature (T s1 ) may refer to the temperature immediately after the above high-temperature annealing is completed. The above slow cooling end temperature (T s2 ) gradually cools the oriented electrical steel sheet from the temperature immediately after the high-temperature annealing is completed, and the rapid cooling section (T described later) r1 It may refer to the temperature just before the start of the ) or the start temperature of the rapid cooling section.

[0028] In one embodiment, the slow cooling start temperature (T s1The temperature range may be 750 to 900 ℃. If the upper limit of the above temperature range is exceeded, there is a high possibility of residual stress occurring during cooling and difficulty in further inhibiting oxidation, and if the lower limit of the above temperature range is exceeded, there is a problem that the strength of the steel plate is high and shape correction is difficult.

[0029] In one embodiment, the slow cooling end temperature (T s2 The temperature range may be 700 to 850°C. If the upper limit of the above temperature range is exceeded, there is a problem in that the temperature at which rapid cooling begins is high and the temperature difference during rapid cooling increases, making it highly likely that residual stress will occur due to thermal stress. If the lower limit of the above temperature range is exceeded, in order to control the temperature difference in the slow cooling section, the temperature of the flattening annealing cracking section becomes excessively low, resulting in a problem in that the strength of the steel plate is high and shape correction is difficult.

[0030] In one embodiment, the temperature difference (T) in the slow cooling section s1 -T s2 ) may be 10 ℃ or higher. Specifically, the temperature difference in the slow cooling section may be in the range of 10 to 80 ℃. More specifically, the temperature difference in the slow cooling section may be in the range of 10 to 50 ℃.

[0031] Temperature difference (T) of the above slow cooling section s1 -T s2 ) refers to the difference between the starting temperature of the slow cooling and the ending temperature of the slow cooling. If the temperature difference of the slow cooling section exceeds the upper limit of the above range, there is a problem that the length of the annealing furnace increases excessively in order to apply the same cooling rate, and if it exceeds the lower limit of the above temperature range, there is a problem that the temperature at which rapid cooling begins increases, and there is a high possibility that residual stress will occur.

[0032] After the above slow cooling section, the rapid cooling start temperature (T r1 ) and quenching end temperature (T r2The step of cooling in a rapid cooling section (S200) including ) rapidly cools the oriented electrical steel sheet that has passed through the slow cooling section. The step of cooling in the rapid cooling section (S200) forms a pattern of flattening annealing together with the slow cooling section, thereby serving not only to remove residual stress formed during the high-temperature annealing process but also to remove residual stress formed in the oriented electrical steel sheet during the flattening annealing process. If residual stress is formed during the flattening annealing process, there is a problem that the magnetic properties deteriorate even after magnetic domain refinement treatment.

[0033] The above rapid cooling start temperature (T r1 ) is the above slow cooling end temperature (T s2 It can mean the temperature immediately after ). Therefore, the above rapid cooling start temperature (T r1 ) may be the same as or lower than the second slow cooling temperature above. The rapid cooling termination temperature (T r2 ) is the above rapid cooling start temperature (T r1 The temperature may be the temperature at which the above-mentioned oriented electrical steel sheet is rapidly cooled from ) to the room temperature range.

[0034] In one embodiment, the rapid cooling start temperature may be in the temperature range of 700 to 850°C. If the upper limit of the temperature range is exceeded, there is a problem in that the temperature at which rapid cooling starts is high and the temperature difference during rapid cooling increases, making it highly likely that residual stress will occur due to thermal stress. If the lower limit of the temperature range is exceeded, in order to control the temperature difference in the slow cooling section, the temperature of the flattening annealing cracking section becomes excessively low, resulting in a problem in that the strength of the steel plate is high and shape correction is difficult.

[0035] In one embodiment, the second rapid cooling temperature may be in a temperature range of 270 to 700°C. If the upper limit of the temperature range is exceeded, there is a problem in that the temperature difference in the rapid cooling section after the rapid cooling section to a temperature close to room temperature increases, making it highly likely that residual stress due to thermal stress will occur. If the lower limit of the temperature range is exceeded, there is a problem in that the temperature difference in the rapid cooling section increases, making it highly likely that residual stress due to thermal stress will occur. After the second rapid cooling temperature, rapid cooling may be performed, for example, to a temperature close to room temperature.

[0036] In one embodiment, the temperature difference (T) in the rapid cooling section r1 -T r2 ) may be in the range of 130 to 430 ℃. The temperature difference (T) in the rapid cooling section above. r1 -T r2 ) refers to the difference between the above-mentioned rapid cooling start temperature and the above-mentioned rapid cooling end temperature.

[0037] If the temperature difference in the above rapid cooling section exceeds the upper limit of the temperature range, there is a problem in that the thermal stress generated during cooling increases, leading to the excessive formation of residual stress; and if it exceeds the lower limit of the temperature range, there is a problem in that the temperature difference in the section where rapid cooling to a temperature close to room temperature after the above rapid cooling section increases, making it highly likely that residual stress will occur due to thermal stress.

[0038] In one embodiment, the temperature difference in the rapid cooling section and the temperature difference in the slow cooling section may satisfy the following Equation 1.

[0039] <Equation 1>

[0040] 100 ≤ ((T r1 -T r2 ) - (T s1 -T s2 )) ≤ 400

[0041] Equation 1 above represents the difference value between the temperature difference in the rapid cooling section and the temperature difference in the slow cooling section. The difference value between the temperature difference in the rapid cooling section and the temperature difference in the slow cooling section may be 100 to 400.

[0042] If the above difference value exceeds the upper limit of the above difference value, there is a problem in that excessive thermal stress occurs in the rapid cooling section, causing magnetic domain iron loss to deteriorate. If the above difference value exceeds the lower limit of the above difference value, there is a problem in that the length of the equipment in the cooling section becomes excessively long and cooling does not proceed sufficiently. Accordingly, by satisfying the above range for the above difference value, it is possible to manufacture oriented electrical steel sheets with excellent magnetic properties.

[0043] In one embodiment, the iron loss of the grain-oriented electrical steel sheet may be in the range of 0.76 W / kg or less. In one embodiment, the iron loss may be in the range of 0.76, specifically 0.73 W / kg or less. By satisfying the above range for the iron loss of the grain-oriented electrical steel sheet, the efficiency of the electrical equipment may be increased. If the iron loss of the grain-oriented electrical steel sheet is greater than the above range, there is a problem that the efficiency of the electrical equipment decreases.

[0044] Referring to FIG. 1b, a flattening annealing method according to another embodiment of the present invention has a slow cooling start temperature (T s1 ), slow cooling end temperature (T s2 A step (S100) of cooling to a slow cooling section including ) and, after the slow cooling section, a rapid cooling start temperature (T r1 ) and quenching end temperature (T r2 The method may include a step of cooling to a rapid cooling section (S200) including ), and a step of irradiating a laser beam onto the surface of the oriented electrical steel sheet after the step of cooling to the rapid cooling section (S300). The detailed description of the slow cooling step (S100) and the rapid cooling step (S200) is identical to that of FIG. 1 described above to the extent that it does not contradict FIG. 1.

[0045] The laser beam may be irradiated onto the surface of the oriented electrical steel sheet for temporary magnetic domain refinement of the oriented electrical steel sheet. In one embodiment, the laser beam may be, for example, a CO2 laser beam. The laser beam may be irradiated in the width direction of the oriented electrical steel sheet.

[0046] In one embodiment, the flattening annealing method may include a cracking step prior to the slow cooling step. The cracking step is at the aforementioned slow cooling start temperature (T s1 It may be the same range as ). In one embodiment, the flattening annealing method may be performed in a gas atmosphere. The gas atmosphere may be at least one gas atmosphere selected from hydrogen, nitrogen, inert gas, and combinations thereof. Specifically, the gas atmosphere may be, for example, dry hydrogen and nitrogen.

[0047] In one embodiment, the proportion of hydrogen in the gas atmosphere may be 5 vol% or less. By satisfying the proportion of hydrogen to be 5 vol% or less, there is an advantage of preventing further oxidation.

[0048] Specific embodiments of the present invention are described below. However, the following embodiments are merely specific examples of the present invention, and the present invention is not limited to the following embodiments.

[0050] Examples and Comparative Examples

[0051] After high-temperature annealing of the grain-oriented electrical steel sheet, a 0.23 mm thick grain-oriented electrical steel sheet from which unreacted MgO had been removed was insulated, and then flattening annealing was performed at 850 ℃. The temperature difference between the slow cooling section and the rapid cooling section immediately after the flattening annealing cracking section was controlled as shown in Table 1 below.

[0052] The loading time, which is the time from charging to extraction in the above slow cooling section, was 4 seconds, and the loading time in the above rapid cooling section was 6 seconds. After the flattening annealing was completed, a continuous mode CO2 laser (TEM) was used for temporary magnetic domain refinement on the surface of the oriented electrical steel sheet. 00 ) irradiated the beam.

[0053] The above laser beam is in the shape of an oval with a width of 0.1 mm and a length of 10 mm, respectively, and was irradiated such that the length direction of the oval aligns with the width direction of the steel plate, and the laser output / (irradiation interval × irradiation speed) is 3 Mj / mm 2 A laser was irradiated. The magnetic properties of the oriented electrical steel sheets according to each planarization annealing cooling condition are as shown in Table 1 below.

[0054] In Table 1 below, the iron loss was measured using the single sheet measurement method, and the iron loss W17 / 50 is the loss (W / kg) when a magnetic flux density of 1.7 Tesla is induced at a frequency of 50 Hz.

[0055] division Temperature difference in the slow cooling section (T s1 -T s2 )[℃] Temperature difference in the rapid cooling section (T r1 -T r2 )[℃] (T r1 -T r2 ) - (T s1 -T s2 )[℃] Iron loss [W / kg] Comparative Example 1 10 540 530 0.79 Comparative Example 2 10 440 430 0.77 Invention Example 1 10 340 330 0.73 Invention Example 2 10 140 130 0.73 Comparative Example 3 40 510 470 0.77 Invention Example 3 40 410 370 0.73 Invention Example 4 40 310 270 0.72 Invention Example 5 40 210 170 0.72

[0056] Looking at Table 1 above, the difference value between the temperature difference of the rapid cooling section and the temperature difference of the slow cooling section (T r1 -T r2 ) - (T s1 -T s2 When the cooling rate is controlled so that ) is between 100 and 400, the iron loss may be 0.76 W / kg or less. In Comparative Examples 1 to 3, where the difference value falls outside the above range, it can be confirmed that the iron loss value increases and the magnetic properties deteriorate.

[0058] The present invention is not limited to the above embodiments and / or examples but can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments and / or examples described above should be understood as illustrative in all respects and not restrictive.

Claims

Claim 1 In a flattening annealing method for oriented electrical steel sheets, wherein flattening annealing is performed after high-temperature annealing, the flattening annealing is performed at a slow cooling start temperature (T s1 ) and slow cooling end temperature (T s2 A step of cooling to a slow cooling section including ); and after the slow cooling section, a rapid cooling start temperature (T r1 ) and quenching end temperature (T r2 The step of cooling to a rapid cooling section including ) is included, wherein the temperature difference in the rapid cooling section and the temperature difference in the slow cooling section satisfy the following Equation 1, and the slow cooling start temperature (T s1 ) is 750 to 900 ℃, and the above slow cooling end temperature (T s2 ) is 700 to 850 ℃, and the rapid cooling start temperature (T r1 ) is 700 to 850 ℃, and the rapid cooling termination temperature (T r2 ) is a flattening annealing method for oriented electrical steel sheets at 270 to 700 ℃. <Equation 1> 100 ≤ ((T r1 -T r2 ) - (T s1 -T s2 )) ≤ 400 Claim 2 In claim 1, the temperature difference (T) in the slow cooling section above. s1 -T s2 ) is a flattening annealing method for oriented electrical steel sheets at 10 ℃ or higher. Claim 3 In claim 1, the temperature difference (T) in the slow cooling section above. s1 -T s2 ) is a flattening annealing method for oriented electrical steel sheets at 10 to 50 ℃. Claim 4 delete Claim 5 delete Claim 6 In claim 1, the temperature difference (T) in the rapid cooling section above. r1 -T r2 ) is a flattening annealing method for oriented electrical steel sheets at 130 to 430 ℃. Claim 7 delete Claim 8 delete Claim 9 A flattening annealing method for a oriented electrical steel sheet according to claim 1, wherein the iron loss of the oriented electrical steel sheet is 0.76 W / kg or less. Claim 10 A flattening annealing method for a oriented electrical steel sheet according to claim 1, further comprising the step of irradiating the surface of the oriented electrical steel sheet with a laser beam after the step of cooling to the rapid cooling section. Claim 11 In claim 1, the flattening annealing method of the oriented electrical steel sheet is performed under a gas atmosphere of at least one of hydrogen, nitrogen, inert gas, and a combination thereof. Claim 12 In claim 11, a flattening annealing method for a oriented electrical steel sheet in which the ratio of hydrogen is 5 vol% or less.

Citation Information

Patent Citations

  • Grain oriented silicon steel sheet having no forsterite film, and excellent in adhesion to insulation film, and production method therefor

    JP2004143532A

  • High permeability grain oriented electrical steel

    JP2013100602A