System and method for evaluation of caking property of coal
By measuring the thickness of the liquid softening layer formed during coal heating using an iron rod and pressure-sensitive sensors, the system accurately evaluates coal caking properties, addressing inaccuracies in existing methods and improving coke quality prediction.
Patent Information
- Application Number
- KR1020220150378
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-11-11
AI Technical Summary
Existing methods for evaluating the coking properties of coal are inadequate, leading to inaccuracies in predicting the quality of coke produced, as coal is a heterogeneous material and cannot be perfectly evaluated solely by fluidity and total expansion coking indices.
A system and method that involves a carbonization furnace, a reaction tube, an iron rod, a load cell, and a position sensor to measure the thickness of the liquid softening layer formed during coal heating by detecting changes in pressure applied to the iron rod, using a Linear Variable Displacement Transducer (LVDT) to accurately determine the softening layer thickness.
This approach allows for more precise evaluation of coal caking properties, enabling better prediction of coke quality and improving the blending of coal for coke production, thereby enhancing coke quality and reducing variations.
Smart Images

Figure 112022120144303-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a system and method for evaluating the caking properties of coal, and more specifically, to a system and method for evaluating the caking properties of coal by measuring the thickness of a liquid softening layer generated when coal is heated. Background Technology
[0002] In a blast furnace, sintered ore produced by calcining fine ore and coke produced in lump form by carbonizing fine coal are charged from the top, and high-temperature hot air is supplied from the bottom to produce molten iron.
[0003] Coke, which is charged into the blast furnace along with ore, is produced by mixing various types of caking coal, loading it into a coke oven, and heating it in an inert atmosphere to form lumps. The coke charged into the blast furnace acts as a reducing agent to reduce the ore, while simultaneously reacting with the air supplied to the furnace to provide heat and serve as a passageway for the flow of gases, molten iron, and slag within the furnace.
[0004] Coal used in the production of such coke has the characteristic of softening, melting, and solidifying as the temperature increases when heated in an inert atmosphere; coal possessing such characteristics is called coking coal. Coking coal consists of coking components that soften, melt, and solidify upon heating, and fibrous components that remain unchanged as inert substances. Coking coal is broadly classified into strong coking coal and weak coking coal based on the degree of coking. When manufacturing coking coal, the coking components and fibrous components of the coal are ensured to be in an appropriate ratio; typically, the blending ratio of strong coking coal to weak coking coal is 50:50, although this ratio may vary slightly depending on coke quality, supply and demand, and costs.
[0005] The coking ability of coal for coke is typically measured by coking indices such as fluidity, total expansion, free swelling index, and furnace index, and coal is classified based on the coking indices.
[0006] Fluidity is measured by placing a small amount of coal into a stirrer and heating it at a constant speed in an inert atmosphere while applying a constant torque to the stirrer, thereby determining the degree of rotation. As the coal is heated and the temperature increases, a large amount of softened molten material is produced, causing the degree of rotation of the stirrer to increase. When the temperature exceeds a certain level, the coal solidifies and the stirrer stops; fluidity is then measured at the maximum degree of rotation of the stirrer. Therefore, fluidity evaluates the extent of the softened molten material formed during the heating of coal.
[0007] Total expansion is measured by forming a coal sample into a rod shape, placing it in a reaction tube, and heating it at a constant rate, thereby determining the extent of its contraction and expansion. Therefore, total expansion evaluates the degree of contraction and expansion of coal particles upon heating. The free swelling index is measured by placing a coal sample in a crucible and heating it at a constant temperature to determine the degree of expansion. The crucible index is measured by mixing a coal sample with an inert substance and heating it at a constant temperature to determine the extent to which it forms a lump.
[0008] In the production of coal for coke, fluidity and total expansion coking indices are generally used, and these indices can be used to predict the quality of the produced coke. However, as coal is a heterogeneous material, its coking properties cannot be perfectly evaluated solely by fluidity and total expansion coking indices, leading to significant errors in predicting the quality of the produced coke. The problem to be solved
[0009] One embodiment of the present invention aims to provide a system and method for evaluating the coking properties of coal that can more easily and accurately measure the coking properties of coal and more accurately predict the quality of coke. means of solving the problem
[0010] A system for evaluating the caking properties of coal according to one embodiment of the present invention comprises: a carbonization furnace for heating coal; a reaction tube installed inside the carbonization furnace and heated by the carbonization furnace; a tube installed inside the reaction tube and penetrating the coal; an iron rod inserted into a liquid softening layer generated from the coal charged into the reaction tube and heated; a load cell connected to the iron rod and measuring a change in pressure applied to one end of the iron rod; and a position sensor connected to the iron rod and the load cell and measuring the thickness of the softening layer using the change in pressure, wherein the iron rod is inserted into the tube and contacts the softening layer.
[0011] It may further include a driving motor that is connected to one end of the iron rod and adjusts the position of the one end of the iron rod inserted into the softening layer.
[0012] The above-mentioned carbonization furnace may include a carbonization furnace body and a heater installed at the bottom of the carbonization furnace body to heat the reaction tube.
[0013] It may further include a temperature measuring unit for measuring the temperature of the coal in the reaction tube.
[0014] The above position sensor may include a Linear Variable Displacement Transducer (LVDT).
[0015] In addition, a method for evaluating the caking properties of coal according to one embodiment of the present invention comprises the steps of: installing a tube inside a reaction tube and charging coal into the reaction tube; installing the reaction tube inside a carbonization furnace and heating the coal to form a softening layer; inserting an iron rod through the tube into the softening layer; and measuring the change in pressure applied to the iron rod to measure the thickness of the softening layer.
[0016] The step of measuring the thickness of the softening layer may include measuring a change in pressure applied to one end of the iron rod using a load cell connected to the iron rod, and measuring the thickness of the softening layer by detecting the positions of the upper and lower surfaces of the softening layer measured by the change in pressure using a position sensor connected to the load cell. Effects of the invention
[0017] A system and method for evaluating the caking properties of coal according to one embodiment of the present invention can more accurately evaluate the caking properties of coal by inserting an iron rod into a softened layer generated from heated coal and measuring the thickness of the softened layer by detecting a change in pressure applied to the inserted iron rod. Accordingly, the quality of coke can be predicted more accurately.
[0018] In addition, the coking properties of coal for coke can be newly evaluated and utilized in the blending of coal for coke to improve the quality of coke and reduce variations. Brief explanation of the drawing
[0019] FIG. 1 is a schematic diagram of a system for evaluating the caking properties of coal according to one embodiment of the present invention. FIG. 2 is a flowchart of a method for evaluating the caking properties of coal according to one embodiment of the present invention. FIG. 3 is a graph illustrating a method for measuring the thickness of a softened layer formed in coal A (low volatile matter coal) using a method for evaluating the coagulation properties of coal according to one embodiment of the present invention. FIG. 4 is a graph illustrating a method for measuring the thickness of a softened layer formed in coal B (mixed coal for coke) using a method for evaluating the coking properties of coal according to one embodiment of the present invention. Specific details for implementing the invention
[0020] Hereinafter, various embodiments of the present invention will be described in detail with reference to the attached drawings so that those skilled in the art can easily implement the present invention. The present invention may be embodied in various different forms and is not limited to the embodiments described herein.
[0021] To clearly explain the present invention, parts unrelated to the explanation have been omitted, and the same reference numerals are used for identical or similar components throughout the specification.
[0022] Then, a system for evaluating the coking properties of coal according to one embodiment of the present invention will be described in detail with reference to the drawings.
[0023] FIG. 1 is a schematic diagram of a system for evaluating the caking properties of coal according to one embodiment of the present invention.
[0024] As illustrated in FIG. 1, a coal caking evaluation system according to one embodiment of the present invention includes a carbonization furnace (100), a reaction tube (200), a tube (300), a steel rod (400), a load cell (500), a position sensor (600), a driving motor (700), a temperature measuring unit (800), and a coal gas outlet (900).
[0025] The carbonization furnace (100) can heat coal (10). The coal (10) may be anaerobic coal having a particle size of about 1.5 mm or less, and the coal (10) may contain about 6 to 9% moisture.
[0026] The carbonization furnace (100) may include a carbonization furnace body (110) and a heater (120). The carbonization furnace body (110) may have a cylindrical shape having an internal space. The heater (120) may be installed at the bottom of the carbonization furnace body (110) to heat the reaction tube (200). Since the heater (120) is installed at the bottom of the carbonization furnace body (110), it can gradually heat the coal (10) inside the reaction tube (200) from the bottom to the top. Therefore, the direction of formation of the softened layer (20) formed by heating the coal (10) can be made vertical, so the caking properties of the coal (10) can be accurately evaluated using the thickness of the softened layer (20). Such a carbonization furnace (100) may be a unidirectional carbonization furnace.
[0027] At this time, the carbonization furnace (100) can heat the coal (10) at a heating rate of 2°C / min to 4°C / min. This is to simulate the heating rate carried out in a blast furnace.
[0028] The reaction tube (200) is installed inside the carbonization furnace (100) and can be heated by the carbonization furnace (100). Coal (10) can be loaded into the reaction tube (200).
[0029] The coal (10) loaded into the reaction tube (200) is heated by a heater to create a liquid softening layer (20) at the bottom of the coal (10), and a solid semi-coke layer (30) can be created below the softening layer (20).
[0030] The tube (300) is installed inside the reaction tube (200) and can penetrate the coal (10) loaded inside the reaction tube (200). Therefore, there is no coal (10) inside the tube (300). Since this tube (300) is made of a combustible material such as paper, it can be carbonized and destroyed during a subsequent heating process. The diameter of this tube (300) is approximately 2 to 3 mm, and the diameter of the tube (300) can be about 60 mm. The tube (300) can be maintained in a vertical state using a vertical guide (not shown).
[0031] The iron rod (400) is installed within the reaction tube (200) and can be inserted into the tube (300). Thus, the iron rod (400) does not come into contact with the coal (10) but comes into contact with the liquid softening layer (20) formed at the bottom of the coal (10), and one end (400a) of the iron rod (400) can be inserted into the softening layer (20) as it descends downward. The tube (300) can guide the iron rod (400) to move in a vertical direction.
[0032] The load cell (500) is connected to the iron rod (400) and can measure changes in pressure applied to one end (400a) of the iron rod (400). When the one end (400a) of the iron rod (400) is located inside the tube (300), there is almost no resistance to the one end (400a) of the iron rod (400), so the pressure becomes relatively small. However, when the one end (400a) of the iron rod (400) descends downward and comes into contact with the liquid softening layer (20) and is inserted into the softening layer (20), the magnitude of the pressure applied to the one end (400a) of the iron rod (400) increases. The upper surface of the softening layer (20) can be detected using this change in pressure. And, when one end (400a) of the iron rod (400) penetrates the liquid softening layer (20) and comes into contact with the solid semi-coke layer (30) formed below the softening layer (20), the one end (400a) of the iron rod (400) is unable to penetrate the solid semi-coke layer (30), so the magnitude of the pressure exerted on the one end (400a) of the iron rod (400) is reduced. By utilizing this change in pressure, the lower surface of the softening layer (20) can be detected.
[0033] A position sensor (600) is connected to a steel bar (400) and a load cell (500), and can measure the thickness of the softening layer (20) by utilizing the change in pressure applied to one end (400a) of the steel bar (400). That is, the thickness of the softening layer (20) can be measured by using the position sensor (600) to measure the positions of the upper and lower surfaces of the softening layer (20) detected by the load cell (500). Such a position sensor (600) may include a Linear Variable Displacement Transducer (LVDT).
[0034] The drive motor (700) is connected to the other end (400b) of the iron rod (400) and can adjust the position of the one end (400a) of the iron rod (400) that is inserted into the softening layer (20).
[0035] The temperature measuring unit (800) can measure the temperature of the coal (10) inside the reaction tube (200) as high, medium, or low. The measured temperature of the coal (10) can be fed back to the heater (120) to adjust the heating speed, etc. The temperature measuring unit (800) can maintain a vertical state using a vertical guide (not shown). This temperature measuring unit (800) may include a thermocouple, but is not necessarily limited thereto, and a temperature measuring device of various structures is possible.
[0036] A coal gas outlet (900) can be installed at the top of the carbonization furnace (100). Coke oven gas (COG) generated during the carbonization process of coal (10) is discharged through the coal gas outlet (900), and the discharged coke oven gas (COG) is burned in a burner and discharged to the outside.
[0037] In this way, the evaluation system for the coking properties of coal according to one embodiment of the present invention can evaluate the coking properties of coal (10) by inserting an iron rod (400) into a softened layer (20) generated from heated coal (10) and detecting a change in pressure applied to the inserted iron rod (400) to measure the thickness of the softened layer (20). That is, since the thickness of the softened layer (20) affects the bonding between coal particles, gas generation, and coke tissue density during the process of mixing various types of coal and coking, the coking properties of the coal can be evaluated by measuring the thickness of the softened layer (20).
[0038] Hereinafter, a method for evaluating the caking properties of coal using a coal caking property evaluation system according to one embodiment of the present invention illustrated in FIG. 1 will be described in detail with reference to the drawings.
[0039] FIG. 2 is a flowchart of a method for evaluating the caking properties of coal according to one embodiment of the present invention.
[0040] As illustrated in FIGS. 1 and 2, a method for evaluating the coking properties of coal according to one embodiment of the present invention first installs a tube (300) inside a reaction tube (200) and charges coal (10) into the reaction tube (200) (S100). The tube (300) may be installed vertically inside the reaction tube (200). The coal (10) charged into the reaction tube (200) may be leveled using a leveling device (not shown).
[0041] Next, a reaction tube (200) is installed inside the carbonization furnace (100), and coal (10) is heated to form a softened layer (20) (S200). At this time, a temperature measuring unit (800) may be inserted inside the reaction tube (200). For example, using a heater (120), the coal (10) is heated at a heating rate of about 8°C / min until its temperature reaches 250°C, and after the temperature of the coal (10) reaches 250°C, it is heated at a heating rate of about 3°C / min, and when the surface temperature of the coal (10) charged into the reaction tube (200) reaches 650°C, the measurement of the thickness of the softened layer (20) is terminated.
[0042] Next, the iron rod (400) is lowered to penetrate the tube (300), and then the iron rod (400) is periodically inserted into the softening layer (20) at regular time intervals (S300).
[0043] Next, the thickness (t) of the softening layer (20) is measured by measuring the change in pressure applied to the iron rod (400) (S400). At this time, the iron rod (400) can be inserted into the softening layer (20) periodically in a vertical direction by penetrating the tube (300).
[0044] Below, the step of measuring the thickness of the softening layer (20) is described in detail.
[0045] First, a load cell (500) connected to the iron bar (400) is used to measure the change in pressure applied to one end (400a) of the iron bar (400).
[0046] And, the position of the upper and lower surfaces of the softening layer (20) is detected through the change in pressure measured by the load cell (500). That is, the load cell (500) detects the position of the upper surface of the softening layer (20) by detecting the resistance caused by the liquid softening layer (20), and detects the position of the lower surface of the softening layer (20) by detecting the resistance caused by the solid semi-coke layer (30).
[0047] Then, the thickness (t) of the softening layer (20) is measured using a position sensor connected to the load cell (500).
[0048] Then, when the upper layer of the coal (10) loaded into the reaction tube (200) is semi-coked, the measurement of the thickness of the softened layer (20) is terminated. For example, when the surface temperature of the coal (10) reaches 600°C, the insertion of the iron rod (400) is stopped, and when the surface temperature of the coal (10) reaches 650°C, the measurement of the thickness of the softened layer (20) is terminated.
[0049] Hereinafter, a method for evaluating the caking properties of coal by measuring the thickness of the softening layer formed in coal A (low volatile matter coal) and coal B (mixed coal for coke) respectively using a method for evaluating the caking properties of coal according to one embodiment of the present invention will be described in detail.
[0050] FIG. 3 is a graph illustrating a method for measuring the thickness of a softened layer generated in coal A (low volatile matter coal) using a method for evaluating the coking properties of coal according to one embodiment of the present invention, and FIG. 4 is a graph illustrating a method for measuring the thickness of a softened layer generated in coal B (mixed coal for coke) using a method for evaluating the coking properties of coal according to one embodiment of the present invention.
[0051] The physical properties of the coal used in the method for evaluating the caking properties of coal according to one embodiment of the present invention are shown in Table 1 below.
[0052] division Industrial Analysis (db, wt%) fluidity (LMF) Total expansion (%) Degree of coalification (Rm, %) Types of coal ASH VM FC Coal A 11.59 19.11 69.30 1.98 57 1.37 Coal B 9.32 25.23 65.45 2.41 72 1.10
[0053] In Table 1, Coal A is a low-volatile coal with a high vitrinite reflectance, and although its fluidity (LMF) and total expansion are relatively low, it is classified as a strongly coking coal. Also, in Table 1, Coal B is a blended coal made by mixing various types of coal used in the production of blast furnace coke.
[0054] As shown in FIG. 3, the temperature of the coal at the bottom of the reaction tube (200) reaches 630°C, and as the iron rod (400) located at the top of the reaction tube (200) descends vertically through the inside of the tube (300), the change in pressure measured by the load cell (500) connected to the iron rod (400) can be confirmed.
[0055] When one end (400a) of the iron rod (400) is located at the top of the tube (300), the one end (400a) of the iron rod (400) does not come into contact with the softening layer (20), so no pressure is applied to the iron rod (400). Then, when the one end (400a) of the iron rod (400) reaches a point located 22 mm from the top of the tube (300), the pressure applied to the iron rod (400) begins to increase. Here, the position where the pressure applied to the iron rod (400) begins to increase corresponds to the upper surface of the softening layer (20). Then, when the one end (400a) of the iron rod (400) reaches a point located 34.5 mm from the top of the tube (300), the pressure reaches its maximum, so the insertion of the iron rod is stopped and the iron rod (400) is raised vertically. Here, the position where the pressure applied to the iron bar (400) is maximum corresponds to the lower surface of the softening layer (20).
[0056] At a point 22 mm from the top of the tube (300), the coal (10) is softened and melted to form a liquid softening layer (20), and the softening layer (20) provides resistance to the descending iron rod (400), causing the pressure to rise, and from a point 34.5 mm from the top of the tube (300), the coal (10) solidifies to form a semi-coke layer, so the iron rod (400) cannot be inserted further and rises vertically and retracts.
[0057] Accordingly, it can be seen that the section from the top of the tube (300) to a point 22 mm to a point 34.5 mm away corresponds to the softening layer (20), and the thickness (t) of this softening layer (20) is approximately 12.5 mm.
[0058] After 15 minutes, in the second measurement, the temperature of the coal bottom in the reaction tube (200) reaches 688℃, and when the iron rod (400) located at the top of the reaction tube (200) is lowered vertically through the inside of the tube (300) in the same way, a softening layer (20) is formed in the section from the top of the tube (300) to the point 19.7mm to the point 26.8mm away from the top of the iron rod (400), and it can be seen that the thickness (t) of the softening layer (20) is about 7.1mm.
[0059] And, at the third measurement after 15 minutes, the temperature of the coal bottom in the reaction tube (200) reaches 744℃, and when the iron rod (400) located at the top of the reaction tube (200) is lowered vertically through the inside of the tube (300) in the same way, a softening layer (20) is formed in the section from the top of the tube (300) to the point 14.4mm to the point 20.9mm away from the top of the iron rod (400), and it can be seen that the thickness (t) of the softening layer (20) is about 6.5mm.
[0060] In this way, coal A has a high degree of carbonization and has the characteristic of softening, melting, and solidifying at high temperatures, and as coal A solidifies at the bottom of the unidirectional carbonization furnace (100) and moves to the top, the thickness of the softened layer (20) decreases as it is measured repeatedly.
[0061] Meanwhile, as shown in FIG. 4, the temperature of the coal at the bottom of the reaction tube (200) reaches 553℃, and as the iron rod (400) located at the top of the reaction tube (200) descends vertically through the inside of the tube (300), the change in pressure measured by the load cell (500) connected to the iron rod (400) can be confirmed.
[0062] When the end portion (400a) of the iron rod (400) is located at the top of the tube (300), the end portion (400a) of the iron rod (400) does not come into contact with the softening layer (20), so no pressure is applied to the iron rod (400). Then, when the end portion (400a) of the iron rod (400) reaches a point located 31.5 mm from the top of the tube (300), the pressure applied to the iron rod (400) begins to increase. Then, when the end portion (400a) of the iron rod (400) reaches a point located 59 mm from the top of the tube (300), the pressure reaches its maximum, so the insertion of the iron rod is stopped, and the iron rod (400) is vertically raised and retracted.
[0063] At a point 31.5 mm from the top of the tube (300), the coal (10) is softened and melted to form a liquid softening layer (20), and the softening layer (20) provides resistance to the descending iron rod (400), causing the pressure to rise, and from a point 59 mm from the top of the tube (300), the coal (10) is solidified to form a semi-coke layer (30), so the iron rod (400) cannot be inserted further and rises vertically and retracts.
[0064] Accordingly, it can be seen that the section from the top of the tube (300) to a point 31.5 mm to a point 59 mm away corresponds to the softening layer (20), and the thickness (t) of this softening layer (20) is approximately 27.5 mm.
[0065] After 15 minutes, in the second measurement, the temperature of the coal bottom in the reaction tube (200) reaches 601℃, and when the iron rod (400) located at the top of the reaction tube (200) is lowered vertically through the inside of the tube (300) in the same way, a softening layer (20) is formed in the section from the top of the tube (300) to the point 29.9mm to the point 58.1mm away from the top of the iron rod (400), and it can be seen that the thickness (t) of the softening layer (20) is about 28.2mm.
[0066] And, at the third measurement after 15 minutes, the temperature of the coal bottom in the reaction tube (200) reaches 651℃, and when the iron rod (400) located at the top of the reaction tube (200) is lowered vertically through the inside of the tube (300) in the same way, a softening layer (20) is formed in the section from the top of the tube (300) to the point 24.4mm to the point 56.3mm away from the top of the iron rod (400), and it can be seen that the thickness (t) of the softening layer (20) is about 31.9mm.
[0067] In this way, coal B is a blended coal made by mixing various types of coal, and since coal with a high volatile content softens and melts at a low temperature and coal with a low volatile content softens and melts at a high temperature, the thickness of the softened layer (20) can be greater than that of coal A.
[0068] Therefore, it can be confirmed that the thickness of the softening layer (20) varies depending on the difference in the coagulation of the coal (10).
[0069] Accordingly, the system and method for evaluating the coking properties of coal according to one embodiment of the present invention can more accurately evaluate the coking properties of coal by inserting an iron rod into the softening layer generated from heated coal and measuring the thickness of the softening layer by detecting a change in pressure applied to the inserted iron rod. Consequently, the quality of coke can be predicted more accurately.
[0070] In addition, the coking properties of coal for coke can be newly evaluated and utilized in the blending of coal for coke to improve the quality of coke and reduce variations.
[0071] Although the present invention has been described through preferred embodiments as described above, those skilled in the art will readily understand that the invention is not limited thereto and that various modifications and variations are possible without departing from the concept and scope of the claims set forth below. Explanation of the symbols
[0072] 10: Coal 20: Softened layer 30: Semi-coke layer 100: Carbonization furnace 200: Reaction tube 300: Tube 400: Pull-up bar 500: Load cell 600: Position sensor 700: Drive motor 800: Temperature measuring unit 900: Coal gas outlet
Claims
Claim 1 A system for evaluating the cohesiveness of coal, comprising: a carbonization furnace for heating coal; a reaction tube installed inside the carbonization furnace and heated by the carbonization furnace; a tube installed inside the reaction tube and penetrating the coal; an iron rod inserted into a liquid softening layer generated from the coal that is charged into the reaction tube and heated; a load cell connected to the iron rod and measuring a change in pressure applied to one end of the iron rod; and a position sensor connected to the iron rod and the load cell and measuring the thickness of the softening layer using the change in pressure, wherein the iron rod is inserted into the tube and contacts the softening layer, and the iron rod does not contact the coal. Claim 2 A coal caking evaluation system according to claim 1, further comprising a driving motor connected to one end of the iron rod and adjusting the position of the one end of the iron rod inserted into the softening layer. Claim 3 In claim 1, the above-mentioned carbonization furnace comprises a carbonization furnace body and a heater installed at the bottom of the carbonization furnace body to heat the reaction tube, a system for evaluating the caking properties of coal. Claim 4 A coal caking evaluation system according to claim 1, further comprising a temperature measuring unit for measuring the temperature of the coal in the reaction tube. Claim 5 In claim 1, the position sensor is a coal caking evaluation system comprising a Linear Variable Displacement Transducer (LVDT). Claim 6 A method for evaluating the coagulation properties of coal, comprising the steps of: installing a tube inside a reaction tube and charging coal into the reaction tube; installing the reaction tube inside a carbonization furnace and heating the coal to form a softening layer; inserting an iron rod through the tube into the softening layer; and measuring the change in pressure applied to the iron rod to measure the thickness of the softening layer, wherein the iron rod is inserted into the tube and contacts the softening layer, and the iron rod does not contact the coal. Claim 7 A method for evaluating the coagulation properties of coal according to claim 6, wherein the step of measuring the thickness of the softening layer comprises: a step of measuring a change in pressure applied to one end of the iron rod using a load cell connected to the iron rod; and a step of measuring the thickness of the softening layer by detecting the positions of the upper and lower surfaces of the softening layer measured by the change in pressure using a position sensor connected to the load cell.
Citation Information
Patent Citations
Detergent additive and detergent composition containing same
JP1983023896A