Ion conducting polymer and separator including the same

An ion-conducting polymer with quaternary ammonium and ether groups addresses the limitations of existing ion exchange membranes by improving ion conductivity and mechanical strength, enabling superior performance in energy and water treatment applications.

KR103047230B1Active Publication Date: 2026-11-10SK INNOVATION CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020240086408
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2026-11-10
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

Existing ion exchange membranes lack enhanced ion conductivity, mechanical strength, and chemical stability, limiting their long-term performance in applications such as water treatment and energy systems.

Method used

Development of an ion-conducting polymer with a repeating unit represented by Chemical Formula 1, incorporating quaternary ammonium and ether groups, synthesized under mild acid conditions to improve ion conductivity and mechanical strength.

Benefits of technology

The ion-conducting polymer exhibits excellent ion conductivity of 40 mS/cm to 80 mS/cm, enhancing the performance of separators in devices like water electrolysis, CO2 electrolysis, fuel cells, and electrolytic cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024071300393-PAT00001
    Figure 112024071300393-PAT00001
  • Figure 112024071300393-PAT00002
    Figure 112024071300393-PAT00002
  • Figure 112024071300393-PAT00003
    Figure 112024071300393-PAT00003
Patent Text Reader

Abstract

The present disclosure relates to an ion-conducting polymer comprising a repeating unit comprising a quaternary ammonium and at least one ether group.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to an ion-conducting polymer and a separator containing the same. Background Technology

[0003] A membrane is generally a barrier that exists between two different substances and can selectively allow specific substances to pass through. Membranes can be classified into various types depending on their properties, materials, and forms. Ion exchange membranes include nonporous membranes, symmetric membranes, monolayer membranes, homogeneous membranes, hydrophilic membranes, charged membranes, and liquid separation membranes.

[0004] An ion exchange membrane is a type of high-efficiency separation membrane that possesses the function of exchanging ions for specific ions. When an ion exchange membrane is introduced into an electrolyte solution and an electric current is passed through it, functional groups with positive or negative charges on the pore walls attract only specific ions with opposite charges into the pores, causing the membrane to become electrically neutral. The specific ions bound to the functional groups continuously bind to and dissociate from the groups to pass through the membrane.

[0005] Ion exchange membranes can be classified into cation exchange membranes (CEM), anion exchange membranes (AEM), and bipolar exchange membranes (BEM) based on their characteristics. A cation exchange membrane is a membrane that allows only cations to pass through as anions have a fixed charge. An anion exchange membrane is a membrane that allows only anions to pass through as cations have a fixed charge. A bipolar exchange membrane is a structure in which cation and anion exchange membranes are combined on both sides, allowing for the selective permeation of both cations and anions.

[0006] Ion exchange membranes can be used in various fields such as water treatment, chemistry, and energy. Since ion exchange membranes must be able to selectively transmit different specific charges, they must have low electrical resistance and high ionic conductivity. In addition, they must have excellent mechanical strength and chemical stability to enable continuous long-term use. Prior art literature

[0008] Korean Published Patent No. 2018-0100079 The problem to be solved

[0009] One objective of the present disclosure is to provide an ion-conducting polymer having enhanced ion conductivity.

[0010] One objective of the present disclosure is to provide a separation membrane having improved ion conductivity. means of solving the problem

[0012] An ion-conducting polymer according to exemplary embodiments of the present disclosure comprises a repeating unit represented by the following chemical formula 1.

[0013] [Chemical Formula 1]

[0014]

[0015] In Chemical Formula 1, A + is quaternary ammonium, B - is an anion, a is an integer between 1 and 3, R 1 R is an organic group having 1 to 10 carbon atoms. 2 is H or an organic group having 1 to 10 carbon atoms, R 3 is an organic group having 1 to 20 carbon atoms comprising at least one of an alkylene group or an arylene group, and Ar is a benzene ring.

[0016] In exemplary embodiments, the B - It can be a monovalent or divalent anion.

[0017] In exemplary embodiments, the B - It can be a halogen anion.

[0018] In exemplary embodiments, the B - is a bromide anion (Br - It can be.

[0019] In exemplary embodiments, the R 1 It can be a methyl group (-CH3).

[0020] In exemplary embodiments, the R 2 It may be an organic group having 1 to 8 carbon atoms.

[0021] In exemplary embodiments, the R 3 It can be an organic group having 4 to 16 carbon atoms.

[0022] In exemplary embodiments, the repeating unit represented by Formula 1 may include at least one of the repeating units represented by Formulas 1-1 to 1-5 below.

[0023] [Chemical Formula 1-1]

[0024]

[0025] [Chemical Formula 1-2]

[0026]

[0027] [Chemical Formula 1-3]

[0028]

[0029] [Chemical Formula 1-4]

[0030]

[0031] [Chemical Formula 1-5]

[0032]

[0033] In exemplary embodiments, the OH ion conductivity of the ion-conducting polymer may be 40 mS / cm to 80 mS / cm.

[0034] In a method for preparing an ion-conducting polymer comprising a repeating unit represented by Chemical Formula 1 according to exemplary embodiments, a monomer comprising an alkoxy group is synthesized. An intermediate comprising the monomer can be synthesized. An ion-conducting polymer can be synthesized by introducing a quaternary ammonium group into the intermediate.

[0035] In a method for preparing an ion-conducting polymer according to exemplary embodiments of the present disclosure, a monomer having a benzene ring substituted with at least one alkoxy group is prepared. The monomer is reacted with an aldehyde under mild acid conditions to obtain a precursor polymer. A quaternary ammonium group is introduced into the precursor polymer to synthesize an ion-conducting polymer comprising a repeating unit represented by the following chemical formula 1.

[0036] [Chemical Formula 1]

[0037]

[0038] In Chemical Formula 1, A + is quaternary ammonium, B - is an anion, a is an integer between 1 and 3, R 1 R is an organic group having 1 to 10 carbon atoms. 2 is H or an organic group having 1 to 10 carbon atoms, R 3 is an organic group having 1 to 20 carbon atoms comprising at least one of an alkylene group or an arylene group, and Ar is a benzene ring.

[0039] The separator according to exemplary embodiments comprises an ion-conducting polymer comprising repeating units represented by the above chemical formula 1.

[0040] An apparatus according to exemplary embodiments comprises an anode, a cathode opposite to the anode, and a separator.

[0041] In exemplary embodiments, the device may include a water electrolysis device, a CO2 electrolysis device, a fuel cell, an electrolytic cell, a vanadium flow cell, etc. Effects of the invention

[0043] The ion-conducting polymer according to the exemplary embodiments of the present disclosure can exhibit excellent ion conductivity.

[0044] A separator according to exemplary embodiments of the present disclosure can exhibit excellent ionic conductivity by including the ionic conductive polymer.

[0045] The ion-conducting polymer and separator of the present disclosure can be widely applied in green technology fields such as electric vehicles, battery charging stations, and other battery-utilizing solar power generation and wind power generation.

[0046] In addition, the ion-conducting polymer and separator of the present disclosure can be used in eco-friendly electric vehicles, hybrid vehicles, etc., to prevent climate change by suppressing air pollution and greenhouse gas emissions. Specific details for implementing the invention

[0048] According to embodiments of the present disclosure, an ion-conducting polymer comprising a repeating unit including a quaternary ammonium and at least one ether group is provided.

[0049] As the above ion-conducting polymer contains quaternary ammonium, stability and ion conductivity can be improved.

[0050] As the above ion-conducting polymer contains ether groups, the synthesis of the polymer can proceed under mild acid conditions.

[0051] As the above ion-conducting polymer includes a main chain composed of carbon-carbon bonds (CC bonds), physicochemical durability can be improved.

[0052] The present disclosure will be described in detail below. However, this is merely illustrative and the present disclosure is not limited to the specific embodiments described illustratively.

[0053] An ion-conducting polymer according to exemplary embodiments of the present disclosure comprises a repeating unit represented by the following chemical formula 1.

[0054] [Chemical Formula 1]

[0055]

[0056] In exemplary embodiments, A + may be a quaternary ammonium. In exemplary embodiments, A + may be a substituent containing at least one methyl group. For example, A + It can be a quaternary ammonium.

[0057] In the present disclosure, the ammonium may also include two different substituents bonded to the nitrogen atom that are connected to form a ring structure. For example, A + It may be trimethylammonium, triethylammonium, tripropylammonium, tributylammonium, imidazolium, piperidinium, quinuclidinium, etc.

[0058] In exemplary embodiments, B - may be an anion. In exemplary embodiments, B - can be a monovalent or divalent anion. For example, B - In the case where ga is a divalent anion, there are two A's located on different chains. + A is 1 B - It can be combined with to form a cross-linked structure.

[0059] In exemplary embodiments, B - can be a halogen anion. For example, the above B - is a chloride anion (Cl - ), bromide anion (Br - ), iodide anion (I - ), hydroxide ion (OH - ), sulfate anion (SO4 2- ), carbonate anion (CO3 2- ), bicarbonate anion (HCO3 - ), carboxylate anion (RCO2 - It can be.

[0060] In exemplary embodiments, a may be an integer between 1 and 3. For example, a may be 1 or 3.

[0061] In exemplary embodiments, the R 1 It can be an organic group having 1 to 10 carbon atoms.

[0062] In exemplary embodiments, the organic group may be a substituent comprising only carbon and hydrogen, or one or more atoms other than carbon and hydrogen. For example, the atoms other than carbon and hydrogen may be nitrogen (N), oxygen (O), phosphorus (P), sulfur (S), etc.

[0063] In exemplary embodiments, the R 1 can be an organic group having 1 to 6 carbon atoms. For example, the above R 1 It can be a methyl group (-CH3).

[0064] In exemplary embodiments, the ion-conducting polymer comprising the repeating unit represented by Formula 1 may include an ether bond in the benzene ring. When an ether bond is included in the benzene ring, the benzene ring is placed in an electron-rich state. Accordingly, the synthesis of the ion-conducting polymer can be carried out under relatively mild acid conditions rather than under superacid conditions such as triflic acid.

[0065] According to exemplary embodiments, the pKa of the mild acid may be -7 or higher.

[0066] For example, the above mild acid may be methanesulfonic acid, trifluoroacetic acid, nitric acid, sulfuric acid, hydrochloric acid, etc.

[0067] In exemplary embodiments, the R 2 can be H or an organic group having 1 to 10 carbon atoms.

[0068] In exemplary embodiments, the organic group may be a hydrocarbon group or a hydrocarbon group containing one or more heteroatoms. The heteroatoms may be, for example, nitrogen (N), oxygen (O), phosphorus (P), and sulfur (S).

[0069] For example, the above R 2 may be an organic group having 1 to 8 carbon atoms. Or the above R 2 It may be an organic group having 1 to 6 carbon atoms.

[0070] In exemplary embodiments, the R 2It can be further substituted with an electron withdrawing group (EWG). The electron withdrawing group can be, for example, a nitro group, a trifluoromethyl group, a cyano group, a fluoro group, an acyl group, etc. Accordingly, the synthesis of ion-conducting polymers can be made easier.

[0071] In exemplary embodiments, the R 3 It may be an organic group having 1 to 20 carbon atoms comprising at least one of an alkylene group or an arylene group. For example, the R 3 Silver may be an organic group having 4 to 16 carbon atoms. Or, the above R 3 Silver may be an organic group having 6 to 14 carbon atoms. Or, the above R 3 It can be an organic group having 8 to 12 carbon atoms.

[0072] When the quaternary ammonium ion is directly connected to the benzene ring, bimolecular nucleophilic substitution (S N The ammonium functional group can be decomposed by reaction 2) or Hofmann elimination. S N 2. When the reaction occurs, the ammonium functional group is OH - It can react with to decompose into an alcohol functional group and a tertiary amine. In the event of the Hofmann elimination reaction, the beta hydrogen atom of the ammonium functional group becomes OH - It may form a double bond upon attack, and the decomposition of the ammonium functional group may occur. If the decomposition of the ammonium functional group occurs, the mechanical strength and ionic conductivity of the ion-conducting polymer may be significantly reduced.

[0073] In the present disclosure, the quaternary ammonium ion is R 3Since it is connected to the benzene ring through, the electron withdrawing inductive effect and resonance effect caused by the benzene ring are reduced, resulting in OH - Attack by [it] can be reduced. Accordingly, the decomposition of the ammonium functional group can be prevented.

[0074] In exemplary embodiments, the R 3 Aromatic and aliphatic chains may be mixed. Accordingly, the mechanical strength of the ion-conducting polymer can be further improved.

[0075] In exemplary embodiments, the Ar may be a benzene ring.

[0076] In exemplary embodiments, the repeating unit represented by Formula 1 may include at least one of the repeating units represented by Formulas 1-1 to 1-5 below.

[0077] [Chemical Formula 1-1]

[0078]

[0079] [Chemical Formula 1-2]

[0080]

[0081] [Chemical Formula 1-3]

[0082]

[0083] [Chemical Formula 1-4]

[0084]

[0085] [Chemical Formula 1-5]

[0086]

[0087] In exemplary embodiments, the OH ion conductivity of the ion-conducting polymer may be 40 mS / cm to 80 mS / cm. For example, the OH ion conductivity of the ion-conducting polymer may be 43 mS / cm to 70 mS / cm, or 45 mS / cm to 65 mS / cm, or 46 mS / cm to 63 mS / cm, or 47 mS / cm to 60 mS / cm.

[0088] In one embodiment according to the present disclosure, a method for manufacturing an ion-conducting polymer is provided.

[0089] First, prepare a monomer having a benzene ring substituted with at least one alkoxy group.

[0090] The above alkoxy group is -(OR in Chemical Formula 1) 1 ) a a can be an integer between 1 and 3.

[0091] The benzene ring is R, whose terminals are substituted with a halogen. 3 This could be a combined thing.

[0092] Next, the above monomer is reacted with an aldehyde under mild acid conditions to obtain a precursor polymer.

[0093] When the above monomer is reacted with an aldehyde under mild acid conditions (primary polymerization), a precursor polymer containing the above benzene ring in the main chain can be obtained.

[0094] The primary polymerization can be carried out in the presence of a mild acid. The mild acid may be any of the aforementioned mild acids. For example, an acid with a pKa of -7 or higher may be used.

[0095] As mentioned above, when an ether bond (alkoxy group) is included in the benzene ring, the benzene ring is placed in an electron-rich state. Accordingly, the synthesis of ion-conducting polymers can be carried out under relatively mild acid conditions rather than under superacid conditions such as triflic acid.

[0096] The above aldehyde is R 2 It can have -CHO, and after primary polymerization R 2 It has a structure connected to the main chain of the precursor polymer.

[0097] In some embodiments, R 2 The electron-withdrawing group can be further substituted, and in this case, the reactivity of the aldehyde can be increased, making it easier to produce the precursor polymer.

[0098] Next, a quaternary ammonium group is introduced into the above precursor polymer to synthesize an ion-conducting polymer containing a repeating unit represented by Chemical Formula 1.

[0099] A quaternary ammonium group can be introduced into the side chain of a benzene ring to exhibit ionic conductivity.

[0100] According to embodiments of the present disclosure, a separator comprising the ion-conducting polymer is provided.

[0101] In exemplary embodiments, the separator may be manufactured by laminating an ion-conducting polymer membrane comprising repeating units represented by Chemical Formula 1.

[0102] According to embodiments of the present disclosure, an apparatus comprising the separator is provided. The apparatus may include an anode, a cathode opposite to the anode, and the separator. An apparatus according to exemplary embodiments may include a water electrolysis apparatus, a CO2 electrolysis apparatus, a fuel cell, an electrolytic cell, a vanadium flow cell, etc.

[0103] The following embodiments are provided to aid in understanding the present disclosure; however, these embodiments are merely illustrative of the present disclosure and are not intended to limit the appended claims. It is obvious to those skilled in the art that various changes and modifications to the embodiments are possible within the scope and spirit of the present disclosure, and that such variations and modifications fall within the scope of the appended claims.

[0104] Preparation Example 1: Preparation of monomer

[0105] (1) Preparation of monomer 1 (A-1)

[0106] A mixed solution was prepared by adding 50 mL of dichloromethane, anisole (5 g, 46 mmol), and aluminum chloride (6.78 g, 51 mmol) to a 100 mL two-necked round-bottom flask and stirring in an ice bath.

[0107] 6-bromohexanoyl chloride (10.4 g, 49 mmol) was added to the prepared mixed solution via a syringe pump over a period of 2 hours, followed by the addition of 85 mL of a 1 M aqueous hydrochloric acid solution. After the reaction was complete, the aqueous layer was removed using a separatory funnel and washed with a 1 M aqueous sodium hydroxide solution. After washing, the aqueous layer was removed, and the organic solvent layer was dried with anhydrous magnesium sulfate. The organic solvent was then removed using a vacuum concentrator to obtain the solid.

[0108] Triethylsilane (16.1 g, 139 mmol), trifluoroacetic acid (5.3 g, 46 mmol), and the solid were added to a 100 mL round-bottom flask. A reflux condenser was installed in the round-bottom flask, and the mixture was stirred at 85 °C for 24 hours. After stirring, the mixture was cooled in an ice bath, and 53 mL of a 1 M aqueous sodium hydroxide solution was added. After the reaction was complete, the aqueous layer was removed using a separatory funnel, the organic solvent layer was dried with anhydrous magnesium sulfate, and purified by column chromatography to prepare 11.1 g of monomer 1 (A-1) represented by the following chemical formula 2-1.

[0109] [Chemical Formula 2-1]

[0110]

[0111] (2) Preparation of monomer 2 (A-2)

[0112] A mixed solution was prepared by adding 30 mL of dichloromethane, 1,3,5-trimethoxybenzene (3 g, 18 mmol), and aluminum chloride (2.85 g, 21 mmol) to a 100 mL two-necked round-bottom flask and stirring in an ice bath.

[0113] 6-bromohexanoyl chloride (4.57 g, 21 mmol) was added to the prepared mixed solution via a syringe pump over a period of 2 hours, followed by the addition of 45 mL of 1 M aqueous hydrochloric acid solution. After the reaction was complete, the aqueous layer was removed using a separatory funnel and washed with 1 M aqueous sodium hydroxide solution. After washing, the aqueous layer was removed, and the organic solvent layer was dried with anhydrous magnesium sulfate. The organic solvent was then removed using a vacuum concentrator to obtain the solid.

[0114] Triethylsilane (6.1 g, 52 mmol), trifluoroacetic acid (1.98 g, 17 mmol), and the solid were added to a 100 mL round-bottom flask. A reflux condenser was installed in the round-bottom flask, and the mixture was stirred at 85 °C for 24 hours. After stirring, the mixture was cooled in an ice bath, and 53 mL of a 1 M aqueous sodium hydroxide solution was added. After the reaction was complete, the aqueous layer was removed using a separatory funnel, the organic solvent layer was dried with anhydrous magnesium sulfate, and purified by column chromatography to prepare 3.65 g of monomer 2 (A-2) represented by the following chemical formula 2-2.

[0115] [Chemical Formula 2-2]

[0116]

[0117] (3) Preparation of monomer 3 (A-3)

[0118] A mixed solution was prepared by adding 75 mL of dichloromethane, 4-methoxybiphenyl (5 g, 27 mmol), and aluminum chloride (3.98 g, 30 mmol) to a 100 mL two-necked round-bottom flask and stirring in an ice bath.

[0119] 6-bromohexanoyl chloride (6.08 g, 28 mmol) was added to the prepared mixed solution via a syringe pump over a period of 2 hours, followed by the addition of 50 mL of 1 M aqueous hydrochloric acid solution. After the reaction was complete, the aqueous layer was removed using a separatory funnel and washed with 1 M aqueous sodium hydroxide solution. After washing, the aqueous layer was removed, the organic solvent layer was dried with anhydrous magnesium sulfate, and the organic solvent was removed using a vacuum concentrator to obtain a solid.

[0120] Triethylsilane (12.6 g, 109 mmol), trifluoroacetic acid (6.2 g, 54 mmol), and the solid were added to a 100 mL round-bottom flask. A reflux condenser was installed in the round-bottom flask, and the mixture was stirred at 85 °C for 24 hours. After stirring, the mixture was cooled in an ice bath, and 60 mL of a 1 M aqueous sodium hydroxide solution was added. After the reaction was complete, the aqueous layer was removed through a separatory funnel, the organic solvent layer was dried with anhydrous magnesium sulfate, and purified by column chromatography to prepare 6.20 g of monomer 3 (A-3) represented by the following chemical formula 2-3.

[0121] [Chemical Formula 2-3]

[0122]

[0123] Preparation Example 2: Preparation of a polymer

[0124] (1) Preparation of Polymer 1 (B-1)

[0125] 14.8 mL of chloroform, 1.8 mL of methanesulfonic acid, paraformaldehyde (0.24 g, equivalent to 8 mmol of formaldehyde), and the above A-1 (2 g, 7 mmol) were added to a 25 mL round-bottom flask. A reflux condenser was installed in the round-bottom flask, and the mixture was refluxed at 85 °C for 2 hours. After reflux, the mixture was cooled to room temperature (25 °C), and 200 mL of methanol was added to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and dried in an oven to prepare 1.9 g of polymer 1 (B-1) represented by the following chemical formula 3-1.

[0126] [Chemical Formula 3-1]

[0127]

[0128] (2) Preparation of Polymer 2 (B-2)

[0129] 12.0 mL of chloroform, 1.5 mL of methanesulfonic acid, paraformaldehyde (0.20 g, equivalent to 7 mmol of formaldehyde), and the above A-2 (2 g, 6 mmol) were added to a 25 mL round-bottom flask. A reflux condenser was installed in the round-bottom flask, and the mixture was refluxed at 85 °C for 2 hours. After reflux, the mixture was cooled to room temperature (25 °C) and added to 200 mL of methanol to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and dried in an oven to prepare 1.6 g of polymer 2 (B-2) represented by the following chemical formula 3-2.

[0130] [Chemical Formula 3-2]

[0131]

[0132] (3) Preparation of Polymer 3 (B-3)

[0133] 14.8 mL of chloroform, 1.8 mL of methanesulfonic acid, 0.77 g of benzaldehyde (7 mmol), and the above A-1 (2 g, 7 mmol) were added to a 25 mL round-bottom flask. A reflux condenser was installed in the round-bottom flask, and the mixture was refluxed at 85 °C for 2 hours. After reflux, the mixture was cooled to room temperature (25 °C) and added to 200 mL of methanol to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and dried in an oven to prepare 2.3 g of polymer 3 (B-3) represented by the following chemical formula 3-3.

[0134] [Chemical Formula 3-3]

[0135]

[0136] (4) Preparation of Polymer 4 (B-4)

[0137] 14.8 mL of chloroform, 1.8 mL of methanesulfonic acid, 4-nitrobenzaldehyde (1.09 g, 7 mmol), and the above A-1 (2 g, 7 mmol) were added to a 25 mL round-bottom flask. A reflux condenser was installed in the round-bottom flask, and the mixture was refluxed at 85 °C for 2 hours. After reflux, the mixture was cooled to room temperature (25 °C) and added to 200 mL of methanol to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and dried in an oven to prepare 3.0 g of polymer 4 (B-4) represented by the following chemical formula 3-4.

[0138] [Chemical Formula 3-4]

[0139]

[0140] (5) Preparation of polymer 5 (B-5)

[0141] 11.5 mL of chloroform, 1.44 mL of methanesulfonic acid, paraformaldehyde (0.61 g, equivalent to 20 mmol of formaldehyde), and the above A-3 (2 g, 6 mmol) were added to a 25 mL round-bottom flask. A reflux condenser was installed in the round-bottom flask, and the mixture was refluxed at 85 °C for 2 hours. After reflux, the mixture was cooled to room temperature (25 °C) and added to 200 mL of methanol to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and dried in an oven to prepare 1.7 g of polymer 5 (B-5) represented by the following chemical formula 3-5.

[0142] [Chemical Formula 3-5]

[0143]

[0144] Preparation Example 3: Preparation of a separator

[0145] Example 1

[0146] 1.45 mL of N-methylpyrrolidone and 0.25 g of B-1 were added to a 20 mL glass vial and stirred at room temperature (25 ℃). After B-1 was completely dissolved, 0.17 g of N,N-dimethylcyclohexylamine was added and stirred at 80 ℃ for 24 hours. After stirring, the solution was cooled to room temperature (25 ℃), poured into a Petri dish, and dried in an 80 ℃ oven for 24 hours to prepare a separation membrane (C-1) formed from a polymer containing repeating units represented by Chemical Formula 1-1.

[0147] Regarding the above C-1 1 H-nuclear magnetic resonance spectroscopy analysis ( 1 H-Nuclear Magnetic Resonance, 1 The results of the H-NMR analysis are as follows.

[0148] 1 H-NMR (DMSO-d6, ppm): 7.3 (br, 2H), 4.0 (br, 2H) 3.8 (br, 3H), 3.6 - 3.2 (br, 9H), 2.6 - 2.5 (br, 2H), 2.0 - 1.0 (br, 18H)

[0149] Example 2

[0150] 2.12 mL of N-methylpyrrolidone and 0.25 g of B-2 were added to a 20 mL glass vial and stirred at room temperature (25 °C). After B-2 was completely dissolved, 0.28 g of 28 wt% trimethylamine was added and stirred at 80 °C for 24 hours. After stirring, the solution was cooled to room temperature (25 °C), poured into a Petri dish, and dried in an 80 °C oven for 24 hours to prepare a separation membrane (C-2) formed from a polymer containing repeating units represented by Chemical Formula 1-2.

[0151] Regarding the above C-21 The results of the H-nuclear magnetic resonance spectroscopy analysis are as follows.

[0152] 1 H-NMR (DMSO-d6, ppm): 3.9 (br, 2H) 3.8 (br, 9H), 3.3~3.2(br, 11H), 2.7~2.6(br, 2H), 2.0~1.0(br, 8H)

[0153] Example 3

[0154] 1.38 mL of N-methylpyrrolidone and 0.25 g of B-3 were added to a 20 mL glass vial and stirred at room temperature (25 °C). After B-3 was completely dissolved, 0.10 g of 1-methylimidazole was added and stirred at 80 °C for 24 hours. After stirring, the solution was cooled to room temperature (25 °C), poured into a Petri dish, and dried in an 80 °C oven for 24 hours to prepare a separation membrane (C-3) formed from a polymer containing repeating units represented by Chemical Formula 1-3.

[0155] Regarding the above C-3 1 The results of the H-nuclear magnetic resonance spectroscopy analysis are as follows.

[0156] 1 H-NMR (DMSO-d6, ppm): 8.92(br, 1H), 7.9~7.0(br, 9H), 5.48(br, 1H) 5.01(br, 2H), 3.9~3.7(br, 6H), 2.64(br, 2H), 2.1~1.2(br, 8H)

[0157] Example 4

[0158] 1.83 mL of N-methylpyrrolidone and 0.25 g of B-4 were added to a 20 mL glass vial and stirred at room temperature (25 °C). After B-4 was completely dissolved, 0.21 g of 28 wt% trimethylamine was added and stirred at 80 °C for 24 hours. After stirring, the solution was cooled to room temperature (25 °C), poured into a Petri dish, and dried in an 80 °C oven for 24 hours to prepare a separation membrane (C-4) formed from a polymer containing repeating units represented by Chemical Formula 1-4.

[0159] Regarding the above C-4 1 The results of the H-nuclear magnetic resonance spectroscopy analysis are as follows.

[0160] 1 H-NMR (DMSO-d6, ppm): 8.16(br, 2H), 7.5~7.0(br, 4H), 5.50(br, 1H), 3.78(br, 3H), 3.5~3.0(br, 11H), 2.66(br, 2H), 1.8~1.2(br, 8H)

[0161] Example 5

[0162] 1.44 mL of N-methylpyrrolidone, 1.44 g of dimethyl sulfoxide, and 0.25 g of B-5 were added to a 20 mL glass vial and stirred at room temperature (25 °C). After B-5 was completely dissolved, 0.1 g of N-methylpiperidine was added and stirred at 80 °C for 24 hours. After stirring, the solution was cooled to room temperature (25 °C), poured into a Petri dish, and dried in an 80 °C oven for 24 hours to prepare a separation membrane (C-5) formed from a polymer containing repeating units represented by the chemical formula 1-5.

[0163] Regarding the above C-5 1 The results of the H-nuclear magnetic resonance spectroscopy analysis are as follows.

[0164] 1 H-NMR (DMSO-d6, ppm): 7.8~7.0(br, 6H), 4.0~3.8(br, 5H), 3.4~3.0(br, 9H), 2.63(br, 2H), 2.0~1.0(br, 14H)

[0165] Comparative Example 1

[0166] We used Sustainion® X37-50 Grade RT product from Dioxide Materials.

[0167] Comparative Example 2

[0168] We used Sustainion® X37-50 Grade T product from Dioxide Materials.

[0169] Experimental Example: Evaluation of Ionic Conductivity of Separator

[0170] The membrane samples of Examples 1 to 5 and Comparative Examples 1 to 2 were cut to a size of 1 cm × 3 cm and fixed between the Pt electrodes of a Conductivity Clamp (BT-110, Scribner).

[0171] The ionic conductivity (σ) of the anion exchange membrane is OH under the conditions of room temperature (25 ℃) and triple distilled water. - It was evaluated by shape. The membrane resistance (R) was measured using an impedance analyzer (VSP-3e, Biologics) in the frequency range of 0.1 kHz to 1 MHz using the 4-point probe method. The thickness (T) of the membrane sample was measured with a micrometer.

[0172] The ionic conductivity (σ) was calculated using Equation 1 below, and the results are shown in Table 1 below.

[0173] [Equation 1]

[0174]

[0175] In Equation 1, R is the film resistance (Ω), and A is the cross-sectional area of ​​the film sample (cm²). 2), L is the distance between electrodes (cm), W is the width of the membrane sample (cm), and T is the thickness of the membrane sample (cm).

[0176] OH ion conductivity (mS / cm) Example 1 50.6 Example 2 47.1 Example 3 43.3 Example 4 46.7 Example 5 45.5 Comparative Example 1 38.0 Comparative Example 2 32.7

[0177] Referring to Table 1, it can be seen that the OH ion conductivity of Examples 1 to 5 is superior to the OH ion conductivity of Comparative Examples 1 to 2.

Claims

Claim 1 Ionic conductive polymer comprising a benzene ring substituted with an alkoxy group and a quaternary ammonium group, and comprising a repeating unit represented by the following chemical formula 1: [Chemical Formula 1] (In Chemical Formula 1, A + is quaternary ammonium, B - is an anion, a is an integer between 1 and 3, R 1 R is an organic group having 1 to 10 carbon atoms. 2 Each independently consists of H or an organic group having 1 to 10 carbon atoms, R 3 is an organic group having 1 to 20 carbon atoms comprising at least one of an alkylene group or an arylene group, and Ar is a benzene ring). Claim 2 In claim 1, the B - is an ion-conducting polymer that is a monovalent or divalent anion. Claim 3 In claim 1, the B - is an ion-conducting polymer that is a halogen anion. Claim 4 In claim 3, the B - is a bromide anion (Br - )Ionic conductive polymer. Claim 5 In claim 1, the R 1 Ionic conductive polymer, which is a methyl group (-CH3). Claim 6 In claim 1, the R 2 is an ion-conducting polymer that is an organic group having 1 to 8 carbon atoms. Claim 7 In claim 1, the R 3 An ion-conducting polymer that is an organic group having 4 to 16 carbon atoms. Claim 8 An ion-conducting polymer according to claim 1, wherein the repeating unit represented by Chemical Formula 1 comprises at least one of the repeating units represented by Chemical Formulas 1-1 to 1-5 below. [Chemical Formula 1-1] [Chemical Formula 1-2] [Chemical Formula 1-3] [Chemical Formula 1-4] [Chemical Formula 1-5] Claim 9 An ion-conducting polymer according to claim 1, wherein the OH ion conductivity of the ion-conducting polymer at 25°C is 40 mS / cm to 80 mS / cm. Claim 10 A method for preparing an ion-conducting polymer comprising: a step of preparing a monomer having a benzene ring substituted with at least one alkoxy group; a step of reacting the monomer with an aldehyde under mild acid conditions of pKa -7 or higher to obtain a precursor polymer; and a step of introducing a quaternary ammonium group into the precursor polymer to synthesize an ion-conducting polymer comprising a repeating unit represented by the following chemical formula 1: [Chemical Formula 1] (In Chemical Formula 1, A + is quaternary ammonium, B - is an anion, a is an integer between 1 and 3, R 1 R is an organic group having 1 to 10 carbon atoms. 2 is H or an organic group having 1 to 10 carbon atoms, R 3 is an organic group having 1 to 20 carbon atoms comprising at least one of an alkylene group or an arylene group, and Ar is a benzene ring). Claim 11 A separator comprising the ion-conducting polymer of claim 1. Claim 12 An apparatus comprising: an anode; a cathode facing the anode; and a separator of claim 11. Claim 13 The device of claim 12, wherein the device comprises a water electrolysis device, a CO2 electrolysis device, a fuel cell, an electrolytic cell, and a vanadium flow cell.

Citation Information

Patent Citations

  • Spiro polymer electrolyte material and preparation method and application thereof

    CN115093523A