Prediction method of dimensional stability of the resin for piping
A method using capillary and rotational rheometers to assess PE-RT resin stability addresses the challenge of predicting dimensional stability, ensuring uniform pipe thickness by satisfying specific conditions, enhancing manufacturing precision.
Patent Information
- Application Number
- KR1020210129842
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-09-30
AI Technical Summary
Existing methods struggle to predict and evaluate the dimensional stability of PE-RT resin, particularly for large-diameter pipes, leading to non-uniformity in pipe thickness during manufacturing.
A method involving two conditions: (1) a height deviation of 1 μm or less at a shear rate of 70/s using a capillary rheometer and (2) a △Tanδ value of less than 1.3 measured by a rotational rheometer, to assess resin stability and predict thickness uniformity without full-scale pipe production.
Enables simple evaluation and prediction of dimensional stability, ensuring stable extrusion and reduced thickness non-uniformity in large-diameter pipes by using a small sample, thereby improving manufacturing efficiency.
Smart Images

Figure 112021112589711-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The present application relates to a method for evaluating the dimensional stability of a resin for pipes. Specifically, the present application relates to a method for evaluating the dimensional stability of a resin for pipes, a method for manufacturing a pipe using a resin having excellent dimensional stability, and a pipe manufactured therefrom. Background Technology
[0002] PE-RT (Polyethylene Raised Temperature) resin refers to polyethylene-based resins used for fluid transport pipes, such as heating pipes or water supply pipes. These PE-RT resins are designed to have high pressure resistance at high temperatures and can be used in a cross-linked or non-cross-linked state depending on the specific application.
[0003] PE-RT resin can be used to manufacture pipes of various diameters. For example, pipes ranging from a relatively small diameter of 20 mm to a relatively large diameter of 250 mm can be manufactured using PE-RT resin. However, unlike the manufacturing process for small diameters, the extrusion speed of the PE-RT resin is slowed down during the manufacturing process for large diameters. For example, if the extrusion speed of the resin during small diameter manufacturing is 20 to 50 m / min, the extrusion speed of the resin during large diameter manufacturing is reduced to 40 m / hr. As a result of this reduced extrusion speed, non-uniformity in the thickness of the extruded pipe may occur.
[0004] To evaluate dimensional stability, such as thickness non-uniformity in PE-RT resins, it is necessary to verify the degree of thickness non-uniformity while extruding the resin with an actual extruder. However, since extruding large-diameter pipes requires a large volume of samples and large-scale extrusion facilities, a method to predict this in advance is required. The problem to be solved
[0005] One objective of the present application is to provide a method for evaluating or predicting the dimensional stability of a piping resin relatively simply.
[0006] Another objective of the present application is to provide a method for comparing and evaluating the dimensional stability of a plurality of piping resins.
[0007] Another objective of the present application is to provide a pipe with excellent dimensional stability.
[0008] The above-mentioned purpose of the present application and other other purposes can all be resolved by the present application described in detail below. means of solving the problem
[0009] In one example relating to the present application, the present application relates to a method for predicting or evaluating the dimensional stability of a resin for piping.
[0010] The inventor of the present application experimentally confirmed that when a resin simultaneously satisfies the predetermined conditions described below, it exhibits excellent dimensional stability, such as thickness uniformity, during pipe manufacturing, and completed the invention of the present application.
[0011] According to a specific embodiment of the present application, the method is a method for evaluating the dimensional stability of a resin for piping, comprising the step of checking whether the resin satisfies both of the following conditions 1 and 2.
[0012] [Condition 1]
[0013] When extruding a resin strand at a shear rate of 70 / s or less using a capillary rheometer, the height deviation of the surface of the extruded strand shall be 1 μm or less.
[0014] [Condition 2]
[0015] The △Tanδ value of the resin measured using a rotational rheometer shall be less than 1.3.
[0016] According to the present application, which uses the above conditions 1 and 2 to evaluate or predict the dimensional stability of a resin sample, the thickness uniformity of the resin can be simply predicted or evaluated using a small amount of sample without performing operations such as manufacturing an actual pipe.
[0017] In this specification, the sample subject to prediction or evaluation may be a resin or a resin composition containing components other than resin. Additionally, in this application, the term "pipe resin or resin composition" may refer to a resin or resin composition used in a pipe that forms a path for the movement of fluids, etc., and may mainly refer to a resin or resin composition for heating pipes.
[0018] Satisfying the above condition 1 means that the fluidity of the resin is stable at a relatively low shear rate. In other words, when the resin satisfies condition 1, stable extrusion is possible during the extrusion process for manufacturing actual pipes, especially large-diameter pipes, due to the resin having stable fluidity, and as a result, it is thought that the possibility of non-uniformity in pipe thickness is reduced.
[0019] In addition, satisfying the above condition 2 means that the change in elasticity of the polymer according to the shear rate is controlled to a relatively small level, that is, that a stable flow profile is formed. In other words, when the resin satisfies condition 2, stable extrusion is possible during the extrusion process for manufacturing actual pipes, especially large-diameter pipes, due to the resin having a small degree of change in elasticity, and as a result, it is thought that the possibility of non-uniformity in the thickness of the pipe is reduced.
[0020] In relation to the verification of Condition 1, the height deviation refers to the absolute value of the arithmetic mean obtained by establishing an arbitrary reference line parallel to the horizontal plane between the highest peak and the lowest valley observed on the surface of the extruded strand, and measuring the distances of each of the multiple peaks and valleys forming the surface from said reference line. At this time, the distances measured to calculate the arithmetic mean value may be measured for at least 10 peaks and valleys.
[0021] In a specific embodiment of the present application, the peaks and valleys used for measuring the height deviation may be selected from among the peaks and valleys forming the surface of the strand, within a baseline range whose length is within 3000 μm.
[0022] In relation to the verification of Condition 1, the types of capillary rheometers available are not specifically limited, and any known capillary rheometer device may be used.
[0023] In one example, regarding the verification of Condition 1, the resin extrusion in the capillary rheometer may be performed through a die with a diameter of 2.0 mm or less. Although not specifically limited, the die diameter of the capillary rheometer through which the resin is extruded may be 1.9 mm or less, 1.8 mm or less, 1.7 mm or less, 1.6 mm or less, or 1.5 mm or less. In addition, the lower limit of the die diameter may be, for example, 1.0 mm or more, 1.1 mm or more, 1.2 mm or more, 1.3 mm or more, 1.4 mm or more, or 1.5 mm or more.
[0024] In one example, regarding the verification of condition 1, the resin extruded through the die may be a resin melted at a temperature above its melting point. Although the melting temperature may vary depending on the type of resin, considering the melting point of commonly used piping resins, the melting point that can be set for the extrusion may be 170°C or higher, 180°C or higher, 190°C or higher, or 200°C or higher.
[0025] In relation to the verification of Condition 2, the type of rotary rheometer available is not particularly limited, and any known rotary rheometer may be used.
[0026] According to a specific example of the present application, with respect to Condition 2 above, △Tanδ is the difference between Tanδ2 measured at 10 rad / s and Tanδ1 measured at 0.1 rad / s. Each of these rad / s is a value set considering the extrusion speed at which the resin is extruded during pipe manufacturing, particularly the extrusion speed in which the shear rate is in the range of 5 / s to 10 / s when extruding large-diameter pipes. In this case, Tanδ1 and Tanδ2 may be the ratio (G” / G’) between the loss modulus G” and the storage modulus G’ at each angular frequency in which they are measured. Additionally, △Tanδ may be treated as an absolute value.
[0027] In one example, in relation to the verification of condition 2, the loss modulus G” and storage modulus G’ using the rotational rheometer may be measured at angular frequencies of 0.01 to 500 rad / s and under 0.1% strain conditions.
[0028] In one example, regarding the verification of condition 2, the resin in which the loss modulus G” and storage modulus G’ are measured may be a resin melted at a temperature above its melting point. Although the melting temperature may vary depending on the type of resin, considering the melting point of commonly used piping resins, the melting point that can be set for the extrusion may be 170°C or higher, 180°C or higher, 190°C or higher, or 200°C or higher.
[0029] If it can be used for the manufacture of piping or pipes, the type of resin subject to dimensional stability prediction or evaluation is not particularly limited.
[0030] For example, the resin may be a homopolymer formed from one type of monomer component, or a copolymer formed from multiple different monomer components. Additionally, the resin may include two or more types of different homopolymers and / or copolymers.
[0031] In one example, the resin may include a polyolefin. The type of polyolefin is not particularly limited.
[0032] For example, the polyolefin may be a polymer formed from at least ethylene, butylene, propylene, and / or α-olefin monomers. The types of α-olefin monomers are not particularly limited. For example, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, or 1-eicocene may be used, but are not particularly limited thereto.
[0033] In one example, the above method may be a method for evaluating the dimensional stability of a resin used for manufacturing large diameters among resins for piping. In this case, a large diameter may be a pipe with a diameter of at least 110 mm.
[0034] In one example, the above method may be a method of measuring condition 1 and condition 2 for a plurality of resins and comparing and evaluating the dimensional stability of each resin.
[0036] In another example relating to the present application, the present application relates to a method for manufacturing a pipe. Specifically, the method comprises the step of manufacturing a pipe by extruding a resin that satisfies both Condition 1 and Condition 2.
[0037] Conditions 1 and 2, the type of resin, and piping characteristics are as described above.
[0039] In another example relating to the present application, the present application relates to a pipe. Specifically, the pipe comprises a resin satisfying both Condition 1 and Condition 2 below, specifically manufactured by extruding the resin.
[0040] Conditions 1 and 2, the type of resin, and piping characteristics are as described above. Effects of the invention
[0042] According to a specific embodiment of the present application, a method for predicting or evaluating the dimensional stability of a piping resin by a relatively simple method may be provided. Furthermore, the present application has the effect of an invention that provides a piping resin with improved dimensional stability. Brief explanation of the drawing
[0044] Figure 1 is a schematic diagram illustrating a method for calculating the height deviation of condition 1. Among the 10 consecutive peaks and valleys forming the strand surface, it is confirmed that the distance between each peak and valley is measured with respect to a reference line parallel to the horizontal plane drawn between the highest first peak on the left and the lowest second valley on the right. FIG. 2 is a schematic diagram illustrating the calculation process of Condition 2 in the Examples and Comparative Examples. A to E correspond, respectively, to the resins of Preparation Examples 1 to 5 used in Example 1, Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3. Figure 3 is a graph illustrating the relationship between satisfying conditions 1 and 2 and the occurrence of dimensional non-uniformity during the actual manufacturing of large-diameter pipes. Specific details for implementing the invention
[0045] The operation and effects of the invention will be explained in more detail below through specific embodiments. However, these are presented as examples of the invention and do not limit the scope of the invention in any way.
[0047] Preparation Example
[0048] The polyethylene resin to be evaluated for dimensional stability was prepared as follows.
[0049] Preparation Example 1 (Resin A): XRT-70, an ethylene-1-hexene copolymer prepared with a Ziegler-Natta catalyst from Total (density 0.947 g / cm³ 2 , number average molecular weight (Mn) 13942 g / mol)
[0050] Preparation Example 2 (Resin B): Ethylene-1-butene copolymer prepared with a metallocene catalyst (density 0.9473 g / cm³ 2 , number average molecular weight (Mn) 17988 g / mol)
[0051] Preparation Example 3 (Resin C): Ethylene-1-butene copolymer prepared with a metallocene catalyst (density 0.9479 g / cm³ 2 , number average molecular weight (Mn) 14670 g / mol)
[0052] Preparation Example 4 (Resin D): Ethylene-1-butene copolymer prepared with a metallocene catalyst (density 0.9442 g / cm³ 2 , number average molecular weight (Mn) 13157 g / mol)
[0053] Preparation Example 5 (Resin E): Ethylene-1-butene copolymer prepared with a metallocene catalyst (density 0.9467 g / cm³ 2 , number average molecular weight (Mn) 17448 g / mol)
[0055] Reference Example: Checking for Thickness Non-uniformity in Large-Diameter Pipes
[0056] Each resin prepared in the manufacturing examples was extruded under the same temperature conditions within the range of 180 to 220 ℃ to manufacture pipes of the same diameter (diameter 110 mm or more), and it was checked whether thickness non-uniformity occurred. Specifically, pipes extruded to a length of several m were divided into five or more sections, and the circumference of each section was measured. Then, if the difference in length between the largest and smallest circumferences exceeded 7%, the dimensional stability was evaluated as poor, and if it was within 7%, the dimensional stability was evaluated as good. As a result, thickness non-uniformity was confirmed in the large-diameter pipes manufactured from Manufacturing Examples 3 to 5.
[0058] Examples and Comparative Examples
[0059] Example 1
[0060] For the sample prepared in Preparation Example 1, it was checked whether Condition 1 and Condition 2 were satisfied. The results are as shown in Table 1.
[0061] Example 2 and Comparative Examples 1 to 3
[0062] As shown in Table 1, conditions 1 and 2 were checked in the same way as in Example 1, except that the type of resin used was different from Example 1.
[0064] The verification process for specific conditions 1 and 2 is as follows.
[0066] Capillary Rheometer (Rheograph75 by Goettfert) Verification of Condition 1 using
[0067] 1. Mount a die (length approximately 20 mm, diameter approximately 1 mm) on the capillary rheometer.
[0068] 2. Set the internal barrel temperature to an extrusion temperature of approximately 190°C.
[0069] 3. After introducing the resin into the measuring barrel, melt it sufficiently for about 5 minutes.
[0070] 4. Remove air bubbles remaining in the resin using upper geometry.
[0071] 5. Wait until the stress of the upper geometry stabilizes.
[0072] 6. Sample resins were extruded into strands at a predetermined shear rate. At this time, each sample resin was extruded at shear rates of 5, 10, 20, 40, 60, 80, 100, 200, and 400 / s, respectively. For the strands extruded at each shear rate, the ends were cut to 20 cm, and the surfaces of the strands were compared using an optical microscope. Then, the lowest shear rate at which the surface characteristics could be classified as "excellent" according to the following classification criteria—that is, the shear rate at which the surface characteristics began to be classified as excellent—was identified.
[0073] Excellent: Ten points are randomly selected on the strand boundary surface, and the arithmetic mean of the protrusions observed at the 10 points shows a length within 1 μm.
[0074] Poor: Ten points are randomly selected on the strand boundary surface, and the arithmetic mean of the protrusions observed at the 10 points shows a length exceeding 1 μm.
[0076] Rotational Rheometer (DHR2) Verification of Condition 2 using
[0077] 1. After fixing the 25 mm parallel plate, set the extrusion temperature to approximately 190 ℃.
[0078] 2. Load an appropriate amount of each sample resin onto a plate, then close the oven and melt it sufficiently.
[0079] 3. Adjust the trim gap to approximately 1.05 mm and trim the resin that has escaped the trim gap.
[0080] 4. Adjust the measurement gap to 1 mm and measure dynamic shear characteristics in Oscillation Frequency sweep mode (Ang. Frequency 0.01~500 rad / s, Strain 0.1%)
[0081] 5. After the measurement is completed, plot the Tanδ graph according to Ang. Frequency.
[0082] 6. Calculate △ Tanδ according to the following formula.
[0083] △ Tanδ = Tanδ2(@Ang.Frequency 0.1rad / s) - Tanδ1(@Ang.Frequency 10rad / s)
[0085] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Resin used Preparation Example 1 (Resin A) Preparation Example 2 (Resin B) Preparation Example 3 (Resin C) Preparation Example 4 (Resin D) Preparation Example 5 (Resin E) Condition 1 40 / s 20 / s 80 / s 200 / s 40 / s Condition 2 1.09 1.04 1.46 2.26 1.52
[0086] Figure 3 summarizes the results from the reference example and Table 1. Specifically, it is confirmed that for a sample satisfying both Condition 1 and Condition 2, the dimensional uniformity is high when manufacturing large-diameter pipes. In other words, the dimensional stability evaluation or prediction method of the present application can simply evaluate the dimensional stability of a piping resin without the cumbersome process of manufacturing pipes.
Claims
Claim 1 A method for evaluating the dimensional stability of a piping resin comprising the step of verifying whether the resin satisfies both of the following Condition 1 and Condition 2: [Condition 1] When extruding a resin strand at a shear rate of 70 / s or less using a capillary rheometer, the height deviation of the surface of the extruded strand is 1 μm or less (provided that the height deviation refers to the absolute value of the arithmetic mean obtained by establishing an arbitrary reference line parallel to the horizontal plane between the highest peak and the lowest valley observed on the surface of the extruded strand, and measuring the respective distances of a plurality of peaks and valleys forming the surface from said reference line, wherein said distances may be measured for at least 10 peaks and valleys). [Condition 2] The △Tanδ value of the resin measured using a rotational rheometer is less than 1.3 (provided that, in Condition 2, △Tanδ is the Tanδ2 measured at 10 rad / s and It is the difference value of Tanδ1 measured at 0.1 rad / s, and Tanδ1 and Tanδ2 are the ratio G” / G’ between the loss modulus G” and the storage modulus G’ at each angular frequency in which they are measured, respectively. Claim 2 A method for evaluating the dimensional stability of a piping resin according to claim 1, wherein the resin extrusion in the capillary rheometer is performed through a die having a diameter of 2.0 mm or less. Claim 3 A method for evaluating the dimensional stability of a piping resin according to claim 2, wherein the resin is extruded through a die at a temperature above the melting point to verify condition 1. Claim 4 A method for evaluating the dimensional stability of a piping resin, wherein, in claim 1, the loss modulus G” and storage modulus G’ using the rotational rheometer are measured at an angular frequency of 0.01 to 500 rad / s and under conditions of 0.1% strain. Claim 5 A method for evaluating the dimensional stability of a piping resin according to claim 4, wherein the loss modulus G” and storage modulus G’ are measured for a resin melted at a temperature above its melting point. Claim 6 A method for evaluating the dimensional stability of a pipe resin according to claim 1, wherein the resin comprises a polyolefin resin. Claim 7 A method for evaluating the dimensional stability of a pipe resin according to claim 6, wherein the polyolefin resin comprises a polymer of one or more monomers selected from ethylene, butylene, propylene, and α-olefin monomers. Claim 8 A method for evaluating the dimensional stability of a piping resin, wherein the resin is used to manufacture a large-diameter pipe with a diameter of at least 110 mm. Claim 9 A method for manufacturing a pipe comprising the step of manufacturing a pipe by extruding a resin satisfying both Condition 1 and Condition 2 below: [Condition 1] When extruding a strand of resin at a shear rate of 70 / s or less using a capillary rheometer, the height deviation of the surface of the extruded strand is 1 μm or less (provided that the height deviation refers to the absolute value of the arithmetic mean obtained by establishing an arbitrary reference line parallel to the horizontal plane between the highest peak and the lowest valley observed on the surface of the extruded strand, and measuring the respective distances of a plurality of peaks and valleys forming the surface from said reference line, and said distances may be measured for at least 10 peaks and valleys). [Condition 2] The △Tanδ value of the resin measured using a rotational rheometer shall be less than 1.3 (provided that in Condition 2, △Tanδ is the difference between Tanδ2 measured at 10 rad / s and Tanδ1 measured at 0.1 rad / s, and Tanδ1 and Tanδ2 are the ratio G” / G’ between the loss modulus G” and the storage modulus G’ at each angular frequency in which they are measured). Claim 10 Piping containing a resin satisfying both Condition 1 and Condition 2 below: [Condition 1] When extruding a resin strand at a shear rate of 70 / s or less using a capillary rheometer, the height deviation of the extruded strand surface shall be 1 μm or less (provided that the height deviation refers to the absolute value of the arithmetic mean obtained by establishing an arbitrary reference line parallel to the horizontal plane between the highest peak and the lowest valley observed on the extruded strand surface, and measuring the respective distances of a plurality of peaks and valleys forming the surface from said reference line, and said distances may be measured for at least 10 peaks and valleys). [Condition 2] The △Tanδ value of the resin measured using a rotational rheometer shall be less than 1.3 (provided that in Condition 2, △Tanδ is the difference between Tanδ2 measured at 10 rad / s and Tanδ1 measured at 0.1 rad / s, and Tanδ1 and Tanδ2 are the ratio G” / G’ between the loss modulus G” and the storage modulus G’ at each angular frequency in which they are measured).
Citation Information
Patent Citations
Co-extrusion of rheologically mismatched polymers
KR1020160130973A
Ethylene / α-olefin / non-conjugated polyene copolymer composition and articles manufactured therefrom
KR1020190095479A
Polymerisation process
US20030120001A1
Ethylene / 1-butene copolymers with enhanced resin processability
US20160347891A1
Improving rheological properties of thermoplastic polyolefin compositions