Structural steel materials used in corrosive environments, especially near the coast or at sea, face challenges with corrosion resistance and lamellar tear resistance, leading to increased maintenance costs and safety concerns due to frequent repainting and potential lamellar tear issues in large and complex structures like bridges.
A structural steel material composition with specific element ratios and distribution, including C, Mn, P, S, Al, Sn, Cu, Ni, W, Sb, and Si, optimized to reduce Sn segregation and control Sn content, combined with a controlled coating system, enhances both corrosion resistance and lamellar tear resistance.
The steel material extends the repainting cycle, reduces maintenance costs, and ensures high safety by providing excellent corrosion resistance and lamellar tear resistance, even in severe corrosive environments, thereby reducing the risk of lamellar tear and maintaining structural integrity.
Abstract
Description
Structural Steel and Structures
[0001] The present invention relates to a steel material that is applied to structures such as bridges that are used in outdoor, on-land, atmospherically corrosive environments, particularly in severe corrosive environments such as at sea or on the coast where there is a large amount of airborne salt.
[0002] Steel structures used outdoors, such as bridges, are usually subjected to some kind of corrosion prevention treatment. For example, weathering steel is often used in environments with low levels of airborne salt.
[0003] Weathering steel is a steel material whose surface is covered with a highly protective rust layer containing concentrated alloying elements such as Cu, P, Cr, and Ni when used in an atmospheric exposure environment, thereby significantly reducing the corrosion rate. Bridges made of such weathering steel are known to be able to withstand decades of service without painting in environments with low levels of airborne salt.
[0004] On the other hand, in environments with high levels of airborne salt, such as at sea or near the coast, it is difficult for weathering steel to form a protective rust layer, making it difficult to use weathering steel without painting. For this reason, in environments with high levels of airborne salt, such as at sea or near the coast, steel that has been treated with anti-corrosion coatings, such as painting, is usually used.
[0005] However, painted steel materials require periodic repairs such as repainting due to deterioration of the paint film over time, the occurrence of rust, and swelling of the paint film. The painting work required for repainting often requires work at high altitudes, making the work itself difficult and requiring labor costs. Therefore, the use of painted steel materials increases the maintenance costs of structures, which in turn increases the life cycle costs.
[0006] Furthermore, in order to prevent corrosion while steel materials are stored until the construction of the structure, they are generally subjected to a rust prevention treatment (primary rust prevention treatment) such as zinc-rich primer. However, if the steel materials are stored for a long period of time or if the steel materials are stored near the sea and there is a large amount of airborne salt, corrosion may progress even if the above rust prevention treatment is performed.
[0007] In light of the above, there is a need for the development of steel materials with excellent corrosion resistance, particularly structural steel materials with excellent paint corrosion resistance, which can extend the repainting cycle, i.e., reduce the frequency of painting, thereby reducing the maintenance costs of structures and also improve primary rust prevention properties.
[0008] As a technology relating to steel materials with excellent corrosion resistance, for example, Patent Document 1 discloses the following: "A steel material with excellent coastal weathering resistance, characterized in that it contains, in mass %, C: 0.001 to 0.15%, Si: 2.5% or less, Mn: more than 0.5% and 2.5% or less, P: less than 0.03%, S: 0.005% or less, Cu: 0.05 to 1.0%, Ni: 0.01 to 0.5%, Cr: 0.01 to 3.0%, Al: 0.003 to 2.5%, and N: 0.001 to 0.1%, and further Sn and / or Sb: 0.03 to 0.50%, the balance being Fe and impurities, and having a Ni / Cu mass ratio of 0.5 or less." Patent Document 2 discloses "a method for manufacturing a steel material having excellent corrosion resistance and Z-direction toughness, comprising heating the surface temperature of a slab having a composition containing, by mass%, C: 0.001 to 0.15%, Si: 2.5% or less, Mn: more than 0.5% and 2.5% or less, P: less than 0.03%, S: 0.005% or less, Cu: less than 0.05%, Ni: less than 0.05%, Cr: 0.01 to 3.0%, Al: 0.003 to 0.1%, N: 0.001 to 0.1%, and Sn: 0.03 to 0.50%, with the balance being Fe and impurities, and having a Cu / Sn ratio of 1 or less, to a temperature of 1050 to 1200°C, followed by rolling to a temperature range of 900°C or higher by 70% or more of the total reduction, and then completing the rolling in a temperature range of 800°C or higher, followed by cooling." Patent Document 3 discloses "a steel material having excellent corrosion resistance, characterized in that it contains, by mass%, C: 0.01 to 0.2%, Si: 0.01 to 1.0%, Mn: 0.05 to 3.0%, P: 0.05% or less, S: 0.01% or less, Sn: 0.01 to 0.5%, Cr: more than 1.0% and 13.0% or less, Al: 0.1% or less, the balance being Fe and impurities, and the proportion of solute Sn in the Sn being 95.0% or more." Patent Document 4 discloses "a steel material with excellent corrosion resistance, characterized in that it contains, by mass%, C: 0.01 to 0.2%, Si: 0.01 to 1.0%, Mn: 0.05 to 3.0%, P: 0.05% or less, S: 0.01% or less, Sn: 0.01 to 0.5%, Al: 0.1% or less, the balance being Fe and impurities, and the proportion of dissolved Sn in the Sn being 95.0% or more."Patent Document 5 states, "The chemical composition is, in mass %, C: 0.01 to 0.20%, Si: 0.01 to 1.00%, Mn: 0.05 to 3.00%, Sn: 0.01 to 0.50%, O: 0.0001 to 0.0100%, Cu: 0 to less than 0.10%, Cr: 0 to less than 0.10%, Mo: 0 to less than 0.050%, W: 0 to less than 0.050%, Cu + Cr: 0 to less than 0.10%, Mo + W: 0 to less than 0.050%, Sb: 0 to less than 0.05%, Ni: 0 to 0.05%, Nb: 0 to 0.050%, V: 0 to 0.050%, Ti: 0 to 0.020%, Al: 0 to 0.100%, "A steel material comprising: Ca: 0 to less than 0.0100%, Mg: 0 to 0.0100%, REM: 0 to 0.0100%, P: 0.05% or less, S: 0.01% or less, the balance: Fe and impurities; having a soft structure which is ferrite and a hard structure which is pearlite, bainite, and martensite; and an Sn concentration ratio which is the ratio of the Sn concentration in the hard structure to the Sn concentration in the soft structure, of 1.2 or more and less than 6.0."
[0009] JP 2006-118011 A JP 2010-7109 A JP 2013-166992 A JP 2012-255184 A Japanese Patent No. 5839151 A
[0010] WES3008-1999
[0011] However, when a large amount of a component that improves corrosion resistance, such as Cr, is contained, performance other than corrosion resistance may be deteriorated. For example, in the techniques of Patent Documents 1 to 3, increasing the Cr content increases the alloy cost and deteriorates the toughness of the steel material.
[0012] In recent years, the risk of lamellar tearing has been pointed out in structures such as bridges. Here, lamellar tearing is a phenomenon in which cracks propagate parallel to the steel plate surface due to tensile stress in welded joints that are subjected to tensile stress in the plate thickness direction, such as cross joints, T-joints, and corner joints, causing cracks.
[0013] Regarding the occurrence of such lamellar tearing, for example, Non-Patent Document 1 shows the relationship between the reduction of area in the thickness direction and the amount of S in steel, and discloses that reducing the amount of S in steel improves the reduction of area in the thickness direction, and thus improves lamellar tearing resistance. However, with the recent increase in the size and complexity of structures, the constituent members of such large and complex structures are often subjected to greater tensile stress in the thickness direction due to welded joints with strict constraint conditions.
[0014] In such cases, it cannot be said that sufficient lamellar tearing resistance can be obtained simply by reducing the amount of S in the steel. Furthermore, the effects on lamellar tearing resistance of the various elements added for the purpose of improving corrosion resistance, as disclosed in Patent Documents 1 to 5, have not been clarified. For this reason, when steel materials with improved corrosion resistance, as disclosed in Patent Documents 1 to 5, are applied to large, complex structures such as those described above, there is a concern that lamellar tearing may occur.
[0015] The present invention has been developed in view of the above-mentioned current situation, and aims to provide a structural steel material that can be applied less frequently even when used in an atmospheric corrosive environment, particularly in a severe corrosive environment such as at sea or near a coast where there is a high amount of airborne salt, and that has excellent coating corrosion resistance with good primary rust prevention properties, and excellent lamellar tear resistance when used in large, complex structures such as bridges. Another aim of the present invention is to provide a structure made using the structural steel material.
[0016] The inventors have conducted extensive research to solve the above problems and have discovered the following: (1) To improve corrosion resistance, particularly corrosion resistance of coating, it is effective to add one or more elements selected from Cu, Ni, W, Sb, and Si in combination with Sn. (2) On the other hand, from the viewpoint of lamellar tear resistance, it is effective to reduce the amount of S in the steel and also reduce the amount of Sn.
[0017] (3) As described above, although adding Sn is effective from the viewpoint of improving the corrosion resistance of the coating, reducing the amount of Sn is effective from the viewpoint of lamellar tear resistance. Based on the above findings, the inventors have conducted extensive research to achieve both corrosion resistance and lamellar tear resistance.
[0018] As a result, the inventors discovered that: (4) by suppressing the centerline segregation of Sn and diffusing Sn throughout the steel material as much as possible, excellent lamellar tear resistance can be obtained even with a specified amount of Sn. In other words, by appropriately adjusting the Sn content from the perspective of improving paint corrosion resistance, suppressing the centerline segregation of Sn and diffusing Sn throughout the steel material, it is possible to achieve both paint corrosion resistance and lamellar tear resistance. (5) Furthermore, by minimizing the thickness of the Sn segregated area where the concentration in the thickness direction is above a predetermined level, lamellar tear resistance can be further improved. (6) Furthermore, by strictly controlling the Sn content according to the S content, lamellar tear resistance can be further improved. The present invention was completed based on the above findings and through further investigation.
[0019] That is, the gist and configuration of the present invention are as follows: 1. and one or more selected from Cu: 0.010% to 0.50%, Ni: 0.010% to 0.50%, W: 0.005% to 1.000%, Sb: 0.005% to 0.200%, and Si: 0.05% to 1.00% inclusive, with the balance being Fe and unavoidable impurities. A structural steel material having a Sn segregation degree of 20 or less. Here, the Sn segregation degree is defined by the following formula (1): [Sn segregation degree] = [Sn concentration in Sn segregated area] / [average Sn concentration] (1)
[0020] 2. The structural steel material according to 1 above, wherein the thickness of the Sn segregated portion in the plate thickness direction is 50 μm or less.
[0021] 3. The structural steel material according to 1 or 2 above, having an ST value of 1.50 or less, as defined by the following formula (2): ST = 10000 × [% S] × [% Sn] 2 --- (2) Here, [%S] and [%Sn] are the contents (mass%) of S and Sn in the above-mentioned composition, respectively.
[0022] 4. The structural steel material according to any one of 1 to 3 above, wherein the chemical composition further contains, in mass%, one or two elements selected from Mo: 0.500% or less and Co: 1.00% or less.
[0023] 5. The structural steel material according to any one of 1 to 4 above, wherein the chemical composition further contains, in mass%, one or more selected from Ti: 0.050% or less, V: 0.200% or less, Nb: 0.200% or less, and Zr: 0.100% or less.
[0024] 6. The structural steel material according to any one of 1 to 5 above, wherein the chemical composition further contains, in mass%, B: 0.0050% or less.
[0025] 7. The structural steel material according to any one of 1 to 6, wherein the chemical composition further contains, in mass%, one or two elements selected from: Ca: 0.0100% or less; and Mg: 0.0100% or less.
[0026] 8. The structural steel material according to any one of 1 to 7 above, which has a coating film on the surface.
[0027] 9. The structural steel material according to 8 above, wherein the coating film has a corrosion-resistant base layer, a primer layer, an intermediate coat layer, and a top coat layer, the corrosion-resistant base layer being made of inorganic zinc-rich paint, the primer layer being made of epoxy resin paint, the intermediate coat layer being made of intermediate paint for a fluororesin top coat, and the top coat layer being made of a fluororesin top coat.
[0028] 10. The structural steel material according to any one of 1 to 7 above, which has a zinc-rich primer layer on its surface.
[0029] 11. A structure formed using the structural steel material according to any one of 1 to 10 above.
[0030] 12. The structure according to 11 above, which is a bridge.
[0031] According to the present invention, a structural steel material can be obtained that can extend the repainting cycle and reduce the frequency of painting, even when used in an atmospheric corrosive environment, particularly in a severe corrosive environment such as at sea or near a coast where there is a high amount of airborne salt, and that also has excellent lamellar tear resistance.The use of the structural steel material of the present invention in structures such as bridges that are used in outdoor atmospheric corrosive environments, particularly in a severe corrosive environment such as at sea or near a coast where there is a high amount of airborne salt, makes it possible to reduce the maintenance costs and therefore the life cycle costs of such structures, and further makes it possible to effectively prevent the occurrence of lamellar tearing and ensure high safety even for large, complex structures.
[0032] The present invention will be described in detail below. First, the chemical composition of one embodiment of the structural steel material of the present invention will be described. Note that the unit of the content of elements in the chemical composition is always "mass%", but hereinafter, unless otherwise specified, it will be simply expressed as "%".
[0033] C: 0.020% or more, 0.200% or less C is an element that increases the strength of steel. Therefore, in order to ensure the specified strength as structural steel, C must be contained in an amount of 0.020% or more. On the other hand, if the C content exceeds 0.200%, weldability and toughness deteriorate. Therefore, the C content is set to 0.020% or more, 0.200% or less. Preferably, it is 0.040% or more. Also, it is preferably 0.180% or less.
[0034] Mn: 0.20% or more, 2.00% or less Mn is an element that increases the strength of steel. Therefore, in order to ensure the required strength as structural steel, Mn needs to be contained in an amount of 0.20% or more. On the other hand, if the Mn content exceeds 2.00%, toughness and weldability deteriorate. Therefore, the Mn content is set to 0.20% or more, 2.00% or less, preferably 0.75% or more, and more preferably 1.80% or less.
[0035] P: 0.003% or more, 0.030% or less P is an element that contributes to improving the coating corrosion resistance of steel materials. From the viewpoint of obtaining this effect, P needs to be contained in an amount of 0.003% or more. On the other hand, if the P content exceeds 0.030%, weldability deteriorates. Therefore, the P content is set to 0.003% or more, 0.030% or less.
[0036] S: 0.0001% or more, 0.0100% or less S is an important element involved in lamellar tear resistance. In other words, when the S content increases, coarse MnS is formed, which becomes the starting point for lamellar tearing. For this reason, the S content must be 0.0100% or less. However, if the S content is reduced to less than 0.0001%, the production cost increases. Therefore, the S content is set to 0.0001% or more, 0.0100% or less. Preferably, it is 0.0080% or less, more preferably 0.0060% or less.
[0037] Al: 0.001% or more, 0.100% or less Al is an element necessary for deoxidation during steelmaking. To obtain this effect, the Al content must be 0.001% or more. On the other hand, if the Al content exceeds 0.100%, it will have an adverse effect on weldability. Therefore, the Al content is set to 0.001% or more, 0.100% or less. It is preferably 0.005% or more, more preferably 0.010% or more. It is also preferably less than 0.050%, more preferably less than 0.030%.
[0038] Sn: 0.005% or more, 0.200% or less. Sn not only improves the durability of the coating film but also plays an important role in lamellar tear resistance. In other words, it improves the corrosion resistance of the coating while reducing lamellar tear resistance. Specifically, Sn is present in the rust layer near the surface of the steel substrate, refining the rust particles and preventing chloride ions, a corrosion-accelerating factor, from penetrating the rust layer and reaching the steel substrate. Sn also inhibits anodic reactions at the steel surface. To fully achieve these effects, the Sn content must be 0.005% or more. It is preferably 0.010% or more, and more preferably 0.020% or more. However, Sn tends to segregate in the center of the steel plate thickness. In these Sn-segregated areas, a highly hard and embrittled structure is formed. This structure acts as a fracture initiation point, deteriorating lamellar tear resistance. Therefore, to ensure lamellar tear resistance, the Sn content is set to 0.200% or less. The content is preferably 0.100% or less, and more preferably less than 0.050%.
[0039] Furthermore, from the viewpoint of improving the corrosion resistance of steel materials to paint coatings, it is necessary to add, in combination with Sn, one or more elements selected from Cu, Ni, W, Sb, and Si. That is, as described above, Sn improves the corrosion resistance of steel materials to paint coatings, but from the viewpoint of lamellar tear resistance, Sn cannot be added in large amounts. Therefore, from the viewpoint of improving the corrosion resistance of steel materials to paint coatings while maintaining good lamellar tear resistance, it is necessary to add, in combination with Sn, one or more elements selected from Cu, Ni, W, Sb, and Si.
[0040] Cu: 0.010% or more, 0.50% or less Cu refines the rust grains in the rust layer, forming a dense rust layer and suppressing the penetration of oxygen and chloride ions, which are corrosion-accelerating factors, into the base steel. This effect is achieved when the Cu content is 0.010% or more. On the other hand, a Cu content exceeding 0.50% increases the alloy cost. Therefore, the content required to obtain the effect of Cu addition is 0.010% or more, and 0.50% or less. Preferably, the Cu content is 0.030% or more, more preferably 0.040% or more, and even more preferably 0.050% or more. Also, the Cu content is preferably 0.40% or less, more preferably 0.30% or less, and even more preferably 0.25% or less.
[0041] Ni: 0.010% or more, 0.50% or less Ni refines the rust grains in the rust layer, forming a dense rust layer and suppressing the penetration of oxygen and chloride ions, which are corrosion-accelerating factors, into the base steel. This effect is achieved when the Ni content is 0.010% or more. On the other hand, a Ni content exceeding 0.50% increases the alloy cost. Therefore, the Ni content required to obtain the effect of Ni addition is 0.010% or more and 0.50% or less. Preferably, the Ni content is 0.030% or more, more preferably 0.040% or more, and even more preferably 0.050% or more. Furthermore, the Ni content is preferably less than 0.40%, more preferably 0.30% or less, and even more preferably 0.15% or less.
[0042] W: 0.005% or more, 1.000% or less W is dissolved in association with the anodic reaction of the steel material and forms WO in the rust layer. 4 2-By distributing W as a W-containing compound, chloride ions, which are corrosion-accelerating factors, are electrostatically prevented from penetrating the rust layer and reaching the base steel. Furthermore, W-containing compounds are precipitated on the steel surface, suppressing the anodic reaction of the steel. This effect is achieved when the W content is 0.005% or more. On the other hand, a W content exceeding 1.000% increases the alloy cost. Therefore, the content required to obtain the effect of W addition is 0.005% or more and 1.000% or less. Preferably, it is 0.010% or more, more preferably 0.030% or more, and even more preferably 0.050% or more. Furthermore, it is preferably 0.700% or less, more preferably 0.500% or less, and even more preferably 0.300% or less.
[0043] Sb: 0.005% or more, 0.200% or less Sb is present in the rust layer near the surface of the base steel, and by refining the rust particles, it prevents chloride ions, a corrosion-accelerating factor, from penetrating the rust layer and reaching the base steel. Sb also suppresses anodic reactions at the steel surface. This effect is achieved when the Sb content is 0.005% or more. On the other hand, an Sb content exceeding 0.200% leads to deterioration in the ductility and toughness of the steel. Therefore, the content required to obtain the effect of Sb addition is 0.005% or more, and 0.200% or less. Preferably, it is 0.010% or more, more preferably 0.020% or more. Also, it is preferably 0.150% or less, more preferably 0.100% or less.
[0044] Si: 0.05% or more, 1.00% or less Si refines the rust grains throughout the rust layer to form a dense rust layer, thereby improving the paint corrosion resistance of the steel material. Si is also an element necessary for deoxidation during steelmaking. This effect is achieved when the Si content is 0.05% or more. On the other hand, if the Si content exceeds 1.00%, toughness and weldability deteriorate significantly. Therefore, the content required to obtain the effect of Si addition is 0.05% or more, but 1.00% or less. It is preferably 0.15% or more. It is also preferably 0.80% or less. Furthermore, from the viewpoint of further improving the paint corrosion resistance of the steel material, it is more preferable that the Si content be 0.40% or more, but 0.60% or less.
[0045] The basic components have been described above, but the following elements may be added as needed: Mo: 0.500% or less Mo dissolves during the anodic reaction of the steel material and forms MoO in the rust layer. 4 2- The distribution of Mo inhibits chloride ions, a corrosion-accelerating factor, from penetrating the rust layer and reaching the base steel. Furthermore, the precipitation of Mo-containing compounds on the steel surface inhibits the anodic reaction of the steel. However, if the Mo content exceeds 0.500%, the alloy cost increases. Therefore, if Mo is contained, the Mo content is set to 0.500% or less. To obtain the above effects, the Mo content is preferably 0.005% or more.
[0046] Co: 1.00% or less Co is distributed throughout the rust layer and refines the rust grains, forming a dense rust layer and thereby improving the weather resistance of the steel. However, a Co content exceeding 1.00% increases the alloy cost. Therefore, when Co is contained, the Co content is set to 1.00% or less. Preferably, it is 0.50% or less, and more preferably, it is 0.35% or less. To achieve the above effect, the Co content is preferably 0.01% or more, more preferably, 0.03% or more, and even more preferably, it is 0.10% or more.
[0047] Ti: 0.050% or less Ti is an element that increases strength. However, if the Ti content exceeds 0.050%, it may cause a deterioration in toughness. Therefore, when Ti is contained, the Ti content is set to 0.050% or less, and more preferably 0.030% or less. In order to obtain the above effects, the Ti content is preferably 0.001% or more, and more preferably 0.005% or more.
[0048] V: 0.200% or less V is an element that increases strength. However, when the V content exceeds 0.200%, this effect saturates. Therefore, when V is contained, the V content is set to 0.200% or less. In order to obtain the above effect, the V content is preferably 0.005% or more.
[0049] Nb: 0.200% or less Nb is an element that increases strength. However, if the Nb content exceeds 0.200%, it may cause a deterioration in toughness. Therefore, when Nb is contained, the Nb content is set to 0.200% or less. In order to obtain the above effects, the Nb content is preferably 0.005% or more.
[0050] Zr: 0.100% or less Zr is an element that increases strength. However, if the Zr content exceeds 0.100%, this effect saturates. Therefore, when Zr is contained, the Zr content is set to 0.100% or less. In order to obtain the above-mentioned effect, the Zr content is preferably 0.005% or more.
[0051] B: 0.0050% or less B is an element that increases strength. However, if the B content exceeds 0.0050%, there is a risk of deterioration in toughness. Therefore, when B is contained, the B content is set to 0.0050% or less. In order to obtain the above effects, the B content is preferably 0.0001% or more.
[0052] Ca: 0.0100% or less Ca is an element that fixes S in steel and improves the toughness of the weld heat affected zone. However, if the Ca content exceeds 0.0100%, the amount of inclusions in the steel increases, which actually leads to a deterioration in toughness. Therefore, if Ca is contained, the Ca content is set to 0.0100% or less. In order to obtain the above effect, the Ca content is preferably 0.0001% or more.
[0053] Mg: 0.0100% or less Mg is an element that fixes S in steel and improves the toughness of the weld heat affected zone. However, if the Mg content exceeds 0.0100%, the amount of inclusions in the steel increases, which actually leads to a deterioration in toughness. Therefore, if Mg is contained, the Mg content is set to 0.0100% or less. In order to obtain the above effect, the Mg content is preferably 0.0001% or more.
[0054] The other components are Fe and unavoidable impurities, such as N and O (oxygen), and N: 0.010% or less and O: 0.010% or less are permissible.
[0055] Furthermore, in the structural steel material of the present invention, it is extremely important to control the Sn segregation degree as follows: Sn segregation degree: 20 or less As described above, Sn tends to segregate in the center of the plate thickness. In such Sn-segregated areas (hereinafter also referred to as Sn-segregated areas), a hard and brittle structure is formed, which becomes the origin of fracture, resulting in a decrease in the lamellar tear resistance of the steel plate. Therefore, in order to ensure excellent lamellar tear resistance, it is important to suppress the center segregation of Sn, in other words, to reduce the Sn segregation degree defined by the following formula (1). For this reason, the Sn segregation degree is set to 20 or less, preferably 18 or less, more preferably 15 or less, and even more preferably 12 or less. Since a smaller amount of Sn segregation is preferable, the lower limit is not particularly limited, but is preferably 1, and more preferably 5. [Sn segregation degree] = [Sn concentration in Sn-segregated areas] / [average Sn concentration] --- (1)
[0056] Here, more specifically, the Sn segregation degree is the ratio of the maximum Sn concentration in the Sn-segregated area to the average Sn concentration obtained by line analysis with an electron probe microanalyzer (hereinafter referred to as EPMA) in a cross section cut parallel to the rolling direction of the steel (a cross section perpendicular to the steel surface). That is, assuming that the thickness of the steel is t (mm) and the width (direction perpendicular to the rolling direction and thickness direction of the steel) is W (mm), first, an EPMA area analysis of Sn is performed on a surface area of the cross section cut parallel to the rolling direction of the steel (a cross section perpendicular to the steel surface) with a thickness direction of (0.5±0.1)×t and a rolling direction of 15 mm (i.e., a surface area including the center position in the thickness direction of the steel) under the conditions of a beam diameter of 20 μm and a pitch of 20 μm. The EPMA area analysis of Sn is performed in three cross-sectional fields of view: 1 / 4×W, 1 / 2×W, and 3 / 4×W. Next, the position with the highest Sn concentration in each cross-sectional field of view is selected from the above EPMA surface analysis, and EPMA line analysis of Sn is performed at each of these positions in the thickness direction of the steel material under conditions of a beam diameter of 5 μm and a pitch of 5 μm. Note that when performing the EPMA line analysis, regions up to 25 μm from the front and back surfaces of the steel material are excluded. Next, the maximum Sn concentration (mass concentration) is determined for each measurement line, and these average values are taken as the Sn concentration (mass concentration) in the Sn segregation area. The Sn concentration in this Sn segregation area is then divided by the average Sn concentration (mass concentration), which is the arithmetic average of all the measured values in the measurement line, and this value is taken as the Sn segregation degree.
[0057] Thickness of the Sn segregated portion in the sheet thickness direction: 50 μm or less. Furthermore, by minimizing the thickness of the Sn segregated portion in the sheet thickness direction, the lamellar tear resistance is further improved. Therefore, the thickness of the Sn segregated portion is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less. The lower limit is not particularly limited and may be 0 μm.
[0058] The Sn segregated portion referred to here is a region where the ratio of the Sn concentration (mass concentration) to the average Sn concentration (mass concentration) obtained by the above-mentioned EPMA line analysis is equal to or greater than 5. The thickness of the Sn segregated portion is determined by averaging the thickness in the sheet thickness direction in the above-mentioned region obtained for each of the above-mentioned measurement lines.
[0059] ST value: 1.50 or less. Furthermore, by setting the ST value defined by the following formula (2) to 1.50 or less, lamellar tear resistance can be further improved. It is more preferably 1.20 or less. There is no particular lower limit, but it is about 0.0000005. ST = 10000 x [% S] x [% Sn] 2 --- (2) Here, [%S] and [%Sn] are the contents (mass%) of S and Sn in the above-mentioned composition, respectively.
[0060] In addition, a structural steel material according to one embodiment of the present invention is used with its surface painted. The coating film on the steel surface is not particularly limited, but examples include a coating film having a corrosion-resistant base layer, a primer layer, an intermediate coat layer, and a top coat layer in this order. It is preferable that the corrosion-resistant base layer be formed using an inorganic zinc-rich paint (e.g., SD Zinc 1500), the primer layer be formed using an epoxy resin paint (e.g., Epomarine HB(K)), the intermediate coat layer be formed using an intermediate coat paint for a fluororesin top coat paint (e.g., Ceratect F intermediate coat), and the top coat layer be formed using a fluororesin top coat paint (e.g., Ceratect F(K) top coat).
[0061] Furthermore, before shipping the product, it is preferable to form a zinc-rich primer layer on the surface of the steel material for the purpose of primary rust prevention. The zinc-rich primer layer is a primer layer formed using a zinc-rich primer specified in JIS K 5552 (2002).
[0062] Next, a manufacturing method according to one embodiment of the structural steel material described above will be described. Specifically, steel prepared to have the above-described chemical composition is melted using a known refining process, such as a converter, electric furnace, or vacuum degassing, and then formed into a steel material (slab) by a continuous casting method or an ingot casting-blooming rolling method. This steel material is then reheated as necessary and hot rolled to form a steel plate, shaped steel, or the like. The thickness of the steel material is not particularly limited, but is preferably 2 to 100 mm. It is more preferably 3 mm or more, and even more preferably 4 mm or more. It is also more preferably 80 mm or less, and even more preferably 60 mm or less.
[0063] However, as described above, in order to obtain excellent lamellar tear resistance, it is extremely important to suppress the center segregation of Sn, specifically, to control the Sn segregation degree to 20 or less. Here, even if the component composition is the same, the Sn segregation degree varies greatly depending on the manufacturing conditions. Therefore, in order to suppress the center segregation of Sn, it is important to appropriately control the manufacturing conditions, in particular the casting conditions and hot rolling conditions.
[0064] That is, in the case of continuous casting, a soft reduction method is preferably used, in which a slab having a wet layer at the final stage of solidification is gradually reduced by a group of reduction rolls at a total reduction amount and reduction rate equivalent to the sum of the solidification shrinkage and thermal shrinkage. In this case, the casting speed (drawing speed) is preferably 0.50 to 2.80 m / min. A casting speed of less than 0.50 m / min results in poor operational efficiency. Furthermore, solidification of the slab is completed before it reaches the soft reduction zone, and sufficient reduction in the wet layer is not achieved. This prevents sufficient suppression of Sn segregation by the soft reduction method, and promotes center segregation of Sn. A casting speed of 0.70 m / min or more is more preferable, and 0.80 m / min or more is even more preferable. On the other hand, a casting speed exceeding 2.80 m / min results in uneven surface temperature and insufficient supply of molten steel to the interior of the slab, promoting center segregation of Sn. Furthermore, the position where solidification is completely completed is beyond the soft reduction zone, so the effect of suppressing Sn segregation by the soft reduction method is not sufficiently obtained, and center segregation of Sn is promoted. The speed is more preferably 2.50 m / min or less, and even more preferably 1.20 m / min or less.
[0065] Furthermore, when the above-mentioned steel material is hot-rolled to the desired dimensions and shape, it is preferable to heat it to a temperature of 1000°C to 1350°C. That is, a higher heating temperature promotes the diffusion of Sn in the center segregation region, which is advantageous from the viewpoint of ensuring lamellar tear resistance. From this viewpoint, the heating temperature is preferably 1000°C or higher. However, if the heating temperature exceeds 1350°C, surface marks may occur, and scale loss and fuel consumption may increase. Therefore, the upper limit of the heating temperature is preferably 1350°C.
[0066] Furthermore, it is preferable to soak the steel material (slab) at the above heating temperature so that the temperature difference between the surface layer and the center is 50°C or less. This sufficiently promotes the diffusion of Sn in the center segregation region. Therefore, it is preferable to set the soaking time at the above heating temperature to 30 minutes or more, more preferably 60 minutes or more, and even more preferably 90 minutes or more. There is no particular upper limit, but it is preferably 1000 minutes.
[0067] If the temperature of the steel material is originally in the range of 1000 to 1350°C and has been maintained in that temperature range for 30 minutes or more, the steel may be subjected to hot rolling as is without heating. Alternatively, the hot-rolled sheet obtained after hot rolling may be subjected to reheating, pickling, and cold rolling to form a cold-rolled sheet having a predetermined thickness.
[0068] In addition, in hot rolling, the reduction ratio is preferably 3.0 or more. By setting the reduction ratio to 3.0 or more, the thickness of the Sn segregated portion in the sheet thickness direction becomes thin. It is more preferably 3.2 or more, and even more preferably 4.0 or more. The upper limit of the reduction ratio is preferably about 60. In addition, the finish rolling end temperature is preferably 650°C or more. If the finish rolling end temperature is less than 650°C, the rolling load increases due to an increase in deformation resistance, making it difficult to carry out rolling. The upper limit of the finish rolling end temperature is preferably 950°C.
[0069] Cooling after hot rolling can be performed by either air cooling or accelerated cooling, but accelerated cooling is preferable if higher strength is desired. When accelerated cooling is performed, the cooling rate is preferably 2 to 100°C / s and the cooling stop temperature is preferably 700 to 400°C. That is, if the cooling rate is less than 2°C / s and / or the cooling stop temperature is greater than 700°C, the effect of accelerated cooling is small, and sufficient strength may not be achieved. From the viewpoint of equipment capacity, the cooling rate is preferably 100°C / s or less. Furthermore, if the cooling stop temperature is less than 400°C, the toughness of the steel may decrease or distortion may occur in the shape of the steel. If the cooling stop temperature is less than 400°C, it is preferable to perform a tempering heat treatment in a temperature range of 400°C to 700°C in a subsequent process.
[0070] Steels having the chemical compositions shown in Table 1 (the balance being Fe and unavoidable impurities) were melted and subjected to continuous casting under the conditions shown in Table 2 to produce steel slabs. The continuous casting was carried out by a soft reduction method. These steel slabs were then reheated, soaked, and hot rolled under the conditions shown in Table 2 to obtain various steel sheets. The cooling after hot rolling was carried out by air cooling to room temperature. The Sn segregation degree and the thickness of the Sn segregated portion were then determined for the steel sheets obtained by the above-mentioned method. The results are also shown in Table 2. When the Sn segregation degree was less than 5, the columns for the Sn segregation degree and the thickness of the Sn segregated portion in Table 2 are both marked with "-".
[0071] (1) Evaluation of Paint Corrosion Resistance The steel plates obtained as described above were evaluated for paint corrosion resistance in the following manner. Specifically, test pieces measuring 70 mm x 50 mm x 5 mm were taken from the steel plates obtained as described above. The surfaces of these test pieces were shot blasted to a rust removal degree Sa of 2.5 as specified in JIS Z 0313 (2004), then ultrasonically degreased in acetone for 5 minutes, and air-dried. Next, one side of the test piece was treated as the painted surface, and an inorganic zinc-rich paint (SD Zinc 1500A, manufactured by Kansai Paint Co., Ltd., thickness: 75 μm) was applied as a corrosion-resistant base coat, followed by an epoxy resin paint (Epomarine for primer mist coat, manufactured by Kansai Paint Co., Ltd.) as a mist coat, followed by an epoxy resin paint (Epomarine HB (K), manufactured by Kansai Paint Co., Ltd., thickness: 120 μm) as a primer coat, followed by an intermediate coat paint for a fluororesin top coat paint (Ceratect F intermediate coat paint, manufactured by Kansai Paint Co., Ltd., thickness: 30 μm) as an intermediate coat, and then a fluororesin paint top coat paint (Ceratect F top coat paint, manufactured by Kansai Paint Co., Ltd., thickness: 25 μm) as a top coat, to form a coating film consisting of a corrosion-resistant base layer, an undercoat layer (including the coating film formed by the mist coat), an intermediate coat layer, and a top coat layer. The other side and end face of the test piece were sealed with a solvent-based epoxy resin paint and further coated with a silicone-based sealant.
[0072] After painting, a straight cut of 1 mm in width and 40 mm in length was made in the center of the coating film formed on the test piece so as to reach the steel substrate, creating an initial defect. Then, a corrosion test was carried out in accordance with ISO 16539 2013 under the following conditions. That is, the amount of artificial sea salt attached to the surface of the test piece was 6.0 g / m 2 A solution of artificial sea salt diluted with pure water to a predetermined concentration was sprayed onto the test piece to adhere the artificial sea salt. Then, using this test piece, a corrosion test was conducted under the following conditions: (Condition 1: Temperature: 60°C, Relative Humidity: 35%, Holding Time: 3 hours) (Condition 2: Temperature: 40°C, Relative Humidity: 95%, Holding Time: 3 hours). Each transition time from Condition 1 to Condition 2 and from Condition 2 to Condition 1 was 1 hour, with a total of 8 hours per cycle. This cycle was repeated 1,200 times. The artificial sea salt was applied once a week. After the corrosion test, the blister width from the initial defect in the paint (hereinafter referred to as the paint blister width) was measured to evaluate the corrosion resistance of the paint. Here, the paint blister width is the average value of the widthwise paint blister width of the initial defect (total blister width on both sides). Specifically, the widthwise paint blister width (total blister width on both sides) was measured at 10 positions equally spaced along the length of the initial defect and averaged. If the paint blister width was 12.0 mm or less, it was determined that the paint corrosion resistance was excellent.
[0073] The reason why a paint blister width of 12.0 mm or less was determined to be excellent in paint corrosion resistance is as follows. Specifically, when a C5-series paint, which is typically used for new bridges, is applied to ordinary steel, the paint's lifespan is estimated to be about 50 years in a mild corrosive environment (general atmospheric corrosive environment). On the other hand, in severe corrosive environments such as offshore or coastal areas, the paint's lifespan is estimated to be about 30 years. Here, in order to extend the paint's lifespan from 30 years to 50 years in severe corrosive environments such as offshore or coastal areas, it is necessary to suppress the progression of paint blistering due to steel corrosion caused by paint film defects. Here, assuming that (a) the paint blister area is expressed by a linear equation of the exposure period, and (b) the blister shape is a circle or rectangle originating from a pinhole or the like, and that the paint blister area is proportional to the square of the paint blister width, if the paint blister area after exposure for a certain period of time in a specified environment is 60% or less of the paint blister area when ordinary steel is exposed under similar conditions (in terms of paint blister width, this is approximately 77.5% or less), or more conservatively, 56.25% or less (in terms of paint blister width, this is approximately 75% or less), then the paint life can be considered to be extended from 30 to 50 years. Here, when ordinary steel was applied with a C5-series paint and subjected to the above corrosion test, the paint blister width was 16.0 mm, and a paint blister width of 12.0 mm, equivalent to 75% of that, was determined to be excellent in terms of paint corrosion resistance.
[0074] The primary rust prevention properties of each steel plate were evaluated in the following manner. That is, in accordance with the salt spray resistance test described in JIS K 5552 (2002): "Zinc-Rich Primer," a zinc-rich primer (SD Zinc 1000 manufactured by Kansai Paint Co., Ltd.) was applied to blast-treated test specimens to a dry film thickness of 20 μm, and after drying, a salt spray test was performed using these test specimens. The number of days until red rust was visually observed on the zinc-rich primer layer was then measured, and the primary rust prevention properties were evaluated according to the following evaluation criteria. In this evaluation, the test period was longer than the test period specified in JIS K 5552 (2002) in order to evaluate the primary rust prevention properties of the steel plate underlying the zinc-rich primer layer. A (pass, extremely excellent): Red rust is observed in 120 days or more. B (pass, particularly excellent): Red rust is observed in 90 days or more but less than 120 days. C (pass, excellent): Red rust is observed in 60 days or more but less than 90 days. D (pass): Red rust is observed in 30 days or more but less than 60 days. E (fail): Red rust is observed in less than 30 days.
[0075] Furthermore, the lamellar tear resistance was evaluated in the following manner. (2) Evaluation of Lamellar Tearing Resistance In accordance with JIS G 3199, a tensile test was carried out in the thickness direction (Z direction) of the steel plate obtained as described above, and the reduction of area was calculated. Then, based on the calculated reduction of area, the lamellar tear resistance was evaluated according to the following criteria: A (pass, extremely excellent): 85% or more B (pass, particularly excellent): 75% or more and less than 85% C (pass, excellent): 65% or more and less than 75% D (pass): 35% or more and less than 65% E (fail): less than 35%
[0076] The evaluation results of (1) and (2) are shown in Table 2.
[0077]
[0078]
[0079]
[0080]
[0081] As shown in Table 2, all of the inventive examples have excellent coating corrosion resistance and lamellar tear resistance. In contrast, the comparative examples do not exhibit sufficient properties in at least one of the coating corrosion resistance and lamellar tear resistance.
Claims
1. By mass percentage, C: 0.020% or more and 0.200% or less, Mn: 0.20% or more and 2.00% or less, P: 0.003% or more and 0.030% or less, S: 0.0001% or more and 0.0100% or less, Al: 0.001% or more and 0.100% or less, and Sn: 0.005% or more and 0.200% or less, and further contains one or more selected from Cu: 0.010% or more and 0.50% or less, Ni: 0.010% or more and 0.50% or less, W: 0.005% or more and 1.000% or less, Sb: 0.005% or more and 0.200% or less, and Si: 0.05% or more and 1.00% or less, with the balance being Fe and inevitable impurities, and having a segregation degree of Sn of 20 or less. Here, the segregation degree of Sn is defined by the following formula (1). [Segregation degree of Sn] = [Sn concentration in the Sn segregation part] / [Average Sn concentration] --- (1) 2. The structural steel material according to claim 1, wherein the thickness of the Sn segregation part in the plate thickness direction is 50 μm or less.
3. The structural steel material according to claim 1 or 2, wherein the ST value defined by the following formula (2) is 1.50 or less. ST = 10000 × [%S] × [%Sn] 2 --- (2) Here, [%S] and [%Sn] are the contents (mass %) of S and Sn in the component composition, respectively.
4. The structural steel material according to any one of claims 1 to 3, wherein the component composition further contains one or two selected from Mo: 0.500% or less and Co: 1.00% or less by mass percentage.
5. The structural steel material according to any one of claims 1 to 4, wherein the component composition further contains one or more selected from Ti: 0.050% or less, V: 0.200% or less, Nb: 0.200% or less, and Zr: 0.100% or less by mass percentage.
6. The structural steel material according to any one of claims 1 to 5, wherein the component composition further contains B: 0.0050% or less by mass percentage.
7. The structural steel according to any one of claims 1 to 6, wherein the component composition further contains one or two selected from the following in mass%: Ca: 0.0100% or less and Mg: 0.0100% or less.
8. The structural steel according to any one of claims 1 to 7, which has a coating film on the surface.
9. The coating film has an anticorrosive primer layer, an undercoat layer, a middle coat layer, and a top coat layer. The anticorrosive primer layer is an inorganic zinc-rich paint, the undercoat layer is an epoxy resin paint, the middle coat layer is a middle coat paint for a fluororesin top coat paint, and the top coat layer is a fluororesin top coat paint. The structural steel according to claim 8.
10. The structural steel according to any one of claims 1 to 7, which has a zinc-rich primer layer on the surface.
11. A structure comprising the structural steel according to any one of claims 1 to 10.
12. The structure according to claim 11, which is a bridge.