Ruthenium carbide for dram capacitor mold patterning

TWI944214BActive Publication Date: 2026-11-01APPLIED MATERIALS INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
TW112120108
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-06
Filing Date
2023-05-30
Publication Date
2026-11-01
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

The semiconductor industry faces challenges in reliably forming high aspect ratio features with precise positioning for submicron and smaller structures, requiring improved etch selectivity in hard mask materials for next-generation NAND and DRAM components, as boron-doped silicon is nearing its limit in selectivity.

Method used

The use of ruthenium carbide as a hard mask material with specific atomic compositions and thicknesses, combined with a hard mask oxide and anti-reflective coatings, to enhance etch selectivity during patterning processes.

Benefits of technology

Ruthenium carbide hard masks provide improved selectivity and reliability in patterning operations, enabling precise formation of capacitor molds with higher integration density and uniformity on larger substrate areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001918468_001
    Figure TWG2TB001918468_001
  • Figure TWG2TB001918468_002
    Figure TWG2TB001918468_002
  • Figure TWG2TB001918468_003
    Figure TWG2TB001918468_003
Patent Text Reader

Abstract

A method for forming electronic components and film stacks includes depositing a ruthenium carbide hard mask on a capacitor mold formed on a substrate. A hard mask oxide and a patterned photoresist are formed, and the pattern of the patterned photoresist is transferred into the ruthenium carbide hard mask. Film stacks containing the ruthenium carbide hard mask on the capacitor mold are also described.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of priority to U.S. Provisional Application No. 63 / 349,355, filed on June 6, 2022, the entire text of which is incorporated by reference into this application.

[0002] Embodiments of the present disclosure generally relate to the fabrication of integrated circuits. More particularly, embodiments of the present disclosure relate to film stacks and methods of forming film stacks for electronic devices using a ruthenium carbide hard mask. Prior Art

[0003] Reliable fabrication of submicron and smaller features is a key requirement for very large scale integration (VLSI) and ultra-large scale integration (ULSI) of semiconductor devices. However, as circuit technology continues to miniaturize, the size and pitch of circuit features (such as interconnects) place additional demands on processing capabilities. Various semiconductor components (such as interconnects, vias, capacitors, and transistors) require precise positioning of high-aspect-ratio features. Reliable formation of these features is crucial to further increasing device density.

[0004] Furthermore, the electronics and semiconductor industries are constantly striving for higher production yields while improving the uniformity of deposited layers on increasingly larger substrates. These same factors, combined with new materials, are also enabling higher circuit integration per unit area on substrates.

[0005] During the formation of many electronic components, a hard mask is used to protect portions of the substrate from being removed. Hard masks are typically used during patterning operations. Once patterning is complete, the hard mask is often removed, leaving the protected portions of the substrate. Removal of the hard mask material can be performed independently or in conjunction with other etching processes. The ability to remove the hard mask material without affecting other surface features (also known as etch selectivity) is a useful characteristic.

[0006] Developing hard mask materials with high etch selectivity is crucial for patterning next-generation NAND and DRAM devices. For each device technology node, a capacitor mold hard mask with 30% higher selectivity than the previous node is required. Currently, boron-doped silicon is used for patterning DRAM capacitor molds for N to N+2 nodes.

[0007] Since the N+2 node has been proposed, the dopant concentration is dominated by boron. Therefore, increasing the boron dopant concentration is unlikely to continue to sufficiently improve the selectivity of the hard mask.

[0008] Therefore, there is a continuing need in the art for capacitor mold hardmasks with improved selectivity. Summary of the Invention

[0009] One or more embodiments of the present disclosure are directed to methods comprising depositing a ruthenium carbide hard mask on a capacitor mold formed on a substrate, forming a hard mask oxide on the ruthenium carbide layer, forming a patterned photoresist on the hard mask oxide, and transferring the pattern of the patterned photoresist to the ruthenium carbide hard mask to form a patterned ruthenium carbide hard mask.

[0010] Other embodiments of the present disclosure are directed to methods that include forming a capacitor mold on a substrate. The capacitor mold includes a silicon oxide (SiO) layer and a silicon carbonitride (SiCN) layer or a silicon nitride (SiN) layer on the silicon oxide layer. The thickness of the silicon oxide (SiO) layer ranges from 1 micron to 3 microns, while the thickness of the SiCN or SiN layer is up to 1000 angstroms. Optionally, one or more of an amorphous silicon film or a carbon film is deposited directly on the capacitor mold. A ruthenium carbide hard mask is deposited on the capacitor mold or on the optional amorphous silicon film or carbon film (if present). The ruthenium carbide hard mask contains ruthenium in a range of 20 to 45 atomic percent and hydrogen in a range of 5 to 15 atomic percent. The combined thickness of the optional amorphous silicon film or carbon film and the ruthenium carbide hard mask ranges from 2500 to 3500 angstroms. A hard mask oxide is formed on the ruthenium carbide layer. An antireflective coating comprising one or more of a dielectric antireflective coating (DARC) or a bottom antireflective coating (BARC) is formed on the hard mask oxide. A patterned photoresist is formed on the antireflective coating. The pattern of the photoresist is transferred to the antireflective coating, the hard mask oxide, and the ruthenium carbide hard mask by exposing the substrate to an etchant plasma containing an oxygen content, a chlorine content, and a carbonyl sulfide content to form a patterned hard mask oxide, a patterned ruthenium carbide hard mask, and the antireflective coating is removed. The chlorine content is in the range of 5% to 15% of the oxygen content on a molar basis, and the carbonyl sulfide content is in the range of 5% to 10% of the oxygen content on a molar basis. The remaining photoresist and antireflective coating are removed, leaving the patterned hard mask oxide and the patterned ruthenium carbide hard mask. The patterns of the patterned hard mask oxide and the patterned ruthenium carbide hard mask are optionally transferred to an optional amorphous silicon film or carbon film.

[0011] Other embodiments of the present disclosure are directed to a film stack comprising: a capacitor die; a ruthenium carbide hard mask on the capacitor die; a hard mask oxide on the ruthenium carbide hard mask; and a patterned photoresist on the hard mask oxide. Simple diagram description

[0012] Thus, a more detailed understanding of the aforementioned features of the present disclosure can be obtained by reference to the embodiments, a more particular description of the present disclosure, briefly summarized above, can be obtained by reference to the embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings illustrate only typical embodiments of the present disclosure and, therefore, should not be considered limiting of the scope of the present disclosure, as the disclosure may admit to other equally effective embodiments.

[0013] FIG. 1 illustrates a plasma processing chamber for use with embodiments of the present disclosure; and

[0014] 2A-2D illustrate a process flow of a method according to one or more embodiments of the present disclosure.

[0015] To facilitate understanding, identical reference numerals have been used, where possible, to denote identical elements common to the figures. The figures are not drawn to scale and may be simplified for clarity. Elements and features of one embodiment may be beneficially incorporated into other embodiments without further recitation. Implementation Method

[0016] Before describing several exemplary embodiments of the present disclosure, it should be understood that the present disclosure is not limited to the details of construction or process steps described in the following description. The present disclosure is capable of other embodiments and can be practiced or carried out in various ways.

[0017] As used in this specification and the appended claims, the term "substrate" refers to a surface, or portion of a surface, upon which a process operates. Those skilled in the art will also understand that, unless the context clearly indicates otherwise, references to a substrate may also refer to only a portion of a substrate. Furthermore, references to depositing on a substrate may refer to both a bare substrate and a substrate having one or more films or features deposited or formed thereon.

[0018] As used herein, "substrate" refers to any substrate or material surface formed on a substrate on which film processing is performed during a manufacturing process. For example, depending on the application, substrate surfaces on which processing may be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), carbon-doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials. Substrates include, but are not limited to, semiconductor wafers. Substrates may be exposed to pretreatment processes to grind, etch, reduce, oxidize, hydroxylate, anneal, UV cure, electron beam cure, and / or bake the substrate surface. In addition to performing film processing directly on the surface of the substrate itself, in the present disclosure, any of the disclosed film processing steps may also be performed on an underlying layer formed on the substrate (as described in more detail below), and the term "substrate surface" is intended to include such an underlying layer, as indicated by the context.

[0019] The term "on" indicates that there is direct contact between elements. The term "directly disposed on" indicates that there is no intermediate element between the elements and that there is direct contact.

[0020] As used in this specification and the appended claims, the terms "precursor," "reactant," "reactive gas," and similar terms are used interchangeably to refer to any gaseous species that can react with the substrate surface.

[0021] Some embodiments of the present disclosure advantageously provide novel hard mask materials with improved selectivity relative to boron-doped silicon. In some embodiments, ruthenium carbide films are used as hard masks that are selective relative to adjacent hard mask oxides and / or capacitor mold components. Some embodiments provide ruthenium carbide hard masks that can be ashed or etched from substrate surfaces.

[0022] FIG1 is a schematic representation of an exemplary substrate processing system 132 according to an embodiment of the present disclosure, which can be used for ruthenium carbide deposition or other processes. Examples of suitable process chambers and tools include, but are not limited to, CENTURA® systems, which can utilize DxZ™ process chambers, PRECISION 5000® systems, and PRODUCER™ systems, such as the PRODUCER SE™ process chamber and the PRODUCER GT™ process chamber, all of which are available from Applied Materials, Inc., Santa Clara, California. It is contemplated that the processes described herein can be performed on other substrate processing systems, including systems from other manufacturers.

[0023] As shown in FIG. 1 , substrate processing system 132 includes a process chamber 100 coupled to a gas distribution plate 130 and a controller 110. Process chamber 100 generally includes a top 124, side walls 101, and a bottom wall 122, defining an internal processing volume 126. A support pedestal 150 is positioned within the internal processing volume 126 of chamber 100. Pedestal 150 is supported by pillars 160 or pedestal supports and is typically made of aluminum, ceramic, or other suitable materials. Pedestal 150 can be moved vertically within chamber 100 using a translation mechanism (not shown) or rotated about the central axis of pillars 160 using a suitable rotation mechanism (not shown).

[0024] As shown, the susceptor 150 includes an embedded heating element 170 suitable for controlling the temperature of a substrate 190 supported on a surface 192 of the susceptor 150. The susceptor 150 can be resistively heated by applying an electric current from a power supply 106 to the heater element 170. The heater element 170 can be made of nickel-chromium wire encapsulated in a nickel-iron-chromium alloy (e.g., INCOLOY®) sheath tube. The current provided by the power supply 106 is regulated by the controller 110 to control the heat generated by the heater element 170, thereby maintaining the substrate 190 and the susceptor 150 at a substantially constant temperature during film deposition. The supplied electric current can be adjusted to selectively control the temperature of the susceptor 150 between approximately 100°C and approximately 700°C.

[0025] A temperature sensor 172 (e.g., a thermocouple) may be embedded in the support pedestal 150 to monitor the temperature of the pedestal 150 in a conventional manner. The controller 110 uses the measured temperature to control the power supplied to the heating element 170 to maintain the substrate at a desired temperature.

[0026] A vacuum pump 102 is coupled to a port formed in the bottom of the chamber 100. The vacuum pump 102 is used to maintain a desired gas pressure in the process chamber 100. The vacuum pump 102 also exhausts post-processing gases and process byproducts from the chamber 100.

[0027] The processing system 132 may also include additional equipment to control chamber pressure, such as valves (eg, throttle valves and isolation valves) located between the process chamber 100 and the vacuum pump 102 to control chamber pressure.

[0028] A showerhead 120 having a plurality of holes 128 is located at the top of the process chamber 100, above the substrate support pedestal 150. The holes 128 of the showerhead 120 are used to introduce process gases into the chamber 100. The holes 128 can have different sizes, numbers, distributions, shapes, designs, and diameters to facilitate the flow of various process gases according to different process requirements. The showerhead 120 is connected to a gas distribution plate 130, which allows the supply of various gases to the internal processing volume 126 during the process. The process gas mixture discharged from the showerhead 120 forms a plasma, which enhances the pyrolysis of the process gases, thereby depositing material on the surface 191 of the substrate 190.

[0029] The gas distribution tray 130 can also be used to control and supply various vaporized liquid precursors. Although not shown, the liquid precursors from the liquid precursor supply can be evaporated, for example, by a liquid injection evaporator, and delivered to the process chamber 100 in the presence of a carrier gas. The carrier gas is typically an inert gas, such as nitrogen, or a noble gas, such as argon or helium. Alternatively, the liquid precursors can be evaporated from ampoules using a heat- and / or vacuum-enhanced evaporation process.

[0030] The showerhead 120 and the substrate support pedestal 150 can form a pair of spaced electrodes within the internal processing volume 126. One or more RF power supplies 140 provide a bias potential to the showerhead 120 via a matching network 138 to promote plasma generation between the showerhead 120 and the pedestal 150. Alternatively, the RF power supply 140 and the matching network 138 can be coupled to the showerhead 120, the substrate pedestal 150, or both, or to an antenna (not shown) positioned external to the chamber 100. In one embodiment, the RF power supply 140 can provide a power between approximately 50 watts and approximately 10,000 watts at a frequency between approximately 50 kHz and approximately 100 MHz. In another embodiment, the RF power supply 140 can provide a power between approximately 500 watts and approximately 1,800 watts at a frequency between approximately 50 kHz and approximately 13.6 MHz.

[0031] Controller 110 includes a central processing unit (CPU) 112, memory 116, and support circuitry 114 for controlling the programming sequence and regulating the flow of gas from gas distribution panel 130. CPU 112 can be any general-purpose computer processor suitable for use in an industrial environment. Software routines can be stored in memory 116, such as random access memory (RAM), read-only memory (ROM), a floppy or hard drive, or other forms of digital storage. Support circuitry 114 is conventionally coupled to CPU 112 and may include cache memory, clock circuitry, input / output systems, a power supply, and the like. Bidirectional communication between controller 110 and various components of processing system 132 is carried out via a plurality of signal cables, referred to as signal buses 118, as shown in FIG. 1 .

[0032] 2A through 2D, an example process for forming an electronic component is described using schematic cross-sectional representations of the electronic component. The shading shown in the figures is used to illustrate different components and should not be construed as representing any particular material of construction unless otherwise specified.

[0033] FIG2A illustrates an electronic component 200 having a capacitor die 210 formed on a substrate 205. In some embodiments, the capacitor die 210 comprises one or more of silicon oxide (SiO), silicon carbide (SiC), or silicon carbonitride (SiCN). As used in this specification and the appended claims, unless otherwise specified, chemical formulas represent only the elemental identity of the film and do not imply stoichiometry. For example, a SiO film comprises silicon and oxygen atoms. A typical silicon oxide film primarily comprises silicon dioxide (SiO2), implying a specific stoichiometric relationship. In some embodiments, the elemental formula of a layer means that the layer contains greater than or equal to approximately 95%, 98%, 99%, or 99.5% of the element on an atomic basis. Those skilled in the art will recognize that interlayer diffusion of atoms may occur unintentionally, thereby affecting the overall composition of the layer. Thus, for example, in a silicon oxide (SiO) layer, the sum of silicon and oxygen atoms constitutes greater than or equal to 95%, 98%, 99%, or 99.5% of the total atoms in the layer, allowing for small amounts of contamination and interlayer diffusion. In other words, the layer is "consisting essentially of the stated element," where "consisting essentially of" means that the stated element constitutes greater than or equal to 95%, 98%, 99%, or 99.5% of the atoms. The term "consisting essentially of" can apply to any individual layer described herein and is not limited to the example of silicon oxide.

[0034] In some embodiments, the capacitor mold 210 includes a silicon oxide (SiO) layer 212 and a second layer 214, wherein the second layer 214 includes one or more of a silicon carbonitride (SiCN) layer or a silicon nitride (SiN) layer. In some embodiments, the thickness of the silicon oxide layer 212 is in the range of 0.5 microns to 5 microns, or in the range of 1 micron to 3 microns. In some embodiments, the thickness of the silicon oxide layer 212 is at most 3.5 microns.

[0035] In some embodiments, second layer 214 comprises a silicon carbonitride (SiCN) layer. In some embodiments, second layer 214 comprises a silicon nitride (SiN) layer. Second layer 214, either a SiCN layer or a SiN layer, has a thickness of at most 10,000 Å, or 5,000 Å or 1,000 Å. In some embodiments, second layer 214 has a thickness in the range of 100 Å to 1,000 Å, or in the range of 500 Å to 900 Å.

[0036] The silicon oxide layer 212 and the second layer 214 may be formed using any suitable technique known to those skilled in the art. For example, these layers may be formed by chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), plasma-enhanced atomic layer deposition (PEALD), or physical vapor deposition (PVD).

[0037] In some embodiments, substrate 205 and / or capacitor die 210 have a substantially flat surface. Alternatively, in some embodiments, substrate 205 and / or capacitor die 210 have a patterned structure, with trenches, holes, or vias formed in the surface. Although substrate 205 is depicted as a single body, those skilled in the art will appreciate that it may comprise one or more material layers used in forming semiconductor devices such as metal contacts, trench isolation, gates, bit lines, or any other interconnect features. Substrate 205 may include one or more metal layers, one or more dielectric materials, semiconductor materials, and other combinations thereof used to fabricate semiconductor devices. For example, substrate 205 may include oxide materials, nitride materials, polysilicon materials, and the like, depending on the application. In one embodiment requiring a memory application, substrate 205 may include silicon substrate material, oxide materials, and nitride materials, with or without polysilicon interposed therebetween.

[0038] In some embodiments, substrate 205 includes a plurality of alternating oxide and nitride materials (i.e., oxide-nitride-oxide (ONO)) deposited on a surface of the substrate. In various embodiments, substrate 205 may include a plurality of alternating oxide and nitride materials, one or more oxide or nitride materials, polycrystalline silicon or amorphous silicon materials, oxide alternating with amorphous silicon, oxide alternating with polycrystalline silicon, undoped silicon alternating with doped silicon, undoped polycrystalline silicon alternating with doped polycrystalline silicon, or undoped amorphous silicon alternating with doped amorphous silicon. Substrate 205 may be any substrate or material surface on which film processing is performed. For example, substrate 205 may be a material such as crystalline silicon, silicon oxide, silicon oxynitride, silicon nitride, strained silicon, silicon germanium, tungsten, titanium nitride, doped or undoped polysilicon, doped or undoped silicon wafers and patterned or unpatterned wafers, silicon on insulator (SOI), carbon-doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire, low-k dielectrics, and combinations thereof.

[0039] FIG2B illustrates electronic component 220 after forming an optional hard mask bottom layer 222 on capacitor mold 210. In some embodiments, hard mask bottom layer 222 comprises one or more of an amorphous silicon (a-Si) film or a carbon (C) film. In some embodiments, hard mask bottom layer 222 comprises an amorphous silicon film. In some embodiments, hard mask bottom layer 222 comprises a carbon film. In some embodiments, hard mask bottom layer 222 is formed directly on capacitor mold 210 without an intervening layer.

[0040] As shown, an optional seed layer 224 is formed on the hard mask bottom layer 222. In some embodiments, the optional seed layer 224 is formed directly on the hard mask bottom layer 222. In some embodiments, the optional seed layer 224 is formed directly on the capacitor mold 210, and the hard mask bottom layer 222 is omitted. In one or more embodiments, the optional seed layer 224 comprises boron. In some embodiments, the thickness of the optional seed layer 224 is up to 100 Å, or is in the range of 10 Å to 100 Å, or is in the range of 20 Å to 60 Å.

[0041] A ruthenium carbide hard mask 226 is formed on the capacitor mold 210. In the embodiment shown, the ruthenium carbide hard mask 226 is formed directly on the optional seed layer 224 on the hard mask bottom layer 222. In some embodiments, the optional hard mask bottom layer 222 and the optional seed layer 224 are omitted, and the ruthenium carbide hard mask 226 is formed directly on the capacitor mold 210. In some embodiments, the hard mask bottom layer 222 is omitted, and the ruthenium carbide hard mask 226 is formed directly on the optional seed layer 224, which is formed on the capacitor mold 210.

[0042] The ruthenium carbide hard mask 226 can be an amorphous, semi-crystalline, or crystalline material. This hard mask can also be referred to as a ruthenium-doped carbon film. However, those skilled in the art will understand that ruthenium-doped carbon film and ruthenium carbide film can be used interchangeably and may depend on the degree of crystallinity of the material.

[0043] In some embodiments, the ruthenium carbide hard mask 226 has a ruthenium composition in the range of 20 to 45 atomic % ruthenium. In some embodiments, the composition of the ruthenium carbide hard mask 226 includes a range of greater than 0 to 50 atomic % ruthenium, 5 to 50 atomic % ruthenium, 10 to 45 atomic % ruthenium, 20 to 45 atomic % ruthenium, or a range of 25 to 40 atomic % ruthenium, or a range of 30 to 35 atomic % ruthenium.

[0044] In some embodiments, the ruthenium carbide hard mask 226 has a hydrogen composition in the range of 2 to 20 atomic % hydrogen. In some embodiments, the composition of the ruthenium carbide hard mask 226 includes a range of 5 to 15 atomic % hydrogen, or a range of 8 to 12 atomic % hydrogen. In some embodiments, the composition of the ruthenium carbide hard mask 226 includes less than or equal to 15 atomic % hydrogen, less than or equal to 10 atomic % hydrogen, or less than or equal to 5 atomic % hydrogen.

[0045] In some embodiments, the ruthenium carbide hard mask 226 comprises ruthenium in a range of greater than 0 to 50 atomic percent and less than or equal to 15 atomic percent hydrogen, with the remainder being carbon. In some embodiments, the ruthenium carbide hard mask 226 comprises ruthenium in a range of 10 to 45 atomic percent and less than or equal to 10 atomic percent hydrogen, with the remainder being carbon. In some embodiments, the ruthenium carbide hard mask 226 comprises ruthenium in a range of 20 to 45 atomic percent and 5 to 15 atomic percent hydrogen, with the remainder being carbon. In some embodiments, the ruthenium carbide hard mask 226 comprises ruthenium in a range of 20 to 45 atomic percent and less than or equal to 15, 10, or 5 atomic percent hydrogen, with the remainder being carbon.

[0046] In some embodiments, the thickness of the ruthenium carbide hard mask 226 is in a range of 500 Å to 4000 Å, or in a range of 1000 Å to 4000 Å, or in a range of 1500 Å to 3500 Å. In some embodiments, the thickness of the ruthenium carbide hard mask is in a range of 2500 Å to 3500 Å. In some embodiments, the thickness of the optional hard mask bottom layer 222 is in a range of 100 Å to 500 Å, and the thickness of the ruthenium carbide hard mask 226 is in a range of 2500 Å to 3400 Å. In some embodiments, the combined thickness of the optional hard mask bottom layer 222 and the ruthenium carbide hard mask 226 is in a range of 2500 Å to 3500 Å. In some embodiments, the combined thickness of the optional hard mask bottom layer 222, the optional seed layer 224, and the ruthenium carbide hard mask 226 is in a range of 500 Å to 4000 Å.

[0047] In the embodiment shown, a hard mask oxide 228 is formed on a ruthenium carbide hard mask 226. The hard mask oxide 228 can be any suitable material known to those skilled in the art that has an etch selectivity relative to the ruthenium carbide hard mask 226. In some embodiments, the hard mask oxide 228 has a thickness in a range of 500 Å to 1500 Å.

[0048] In the illustrated embodiment, an advanced patterning film (APF) 230 is formed on the hard mask oxide 228. In some embodiments, the advanced patterning film 230 comprises carbon or a diamond-like carbon film. In some embodiments, the thickness of the advanced patterning film 230 ranges from 500 Å to 1500 Å. In some embodiments, the thickness of the advanced patterning film 230 is greater than 0 Å and less than or equal to 1500 Å, or 1000 Å.

[0049] A dielectric antireflective coating (DARC) 232 is formed on the advanced patterned film 230. The DARC 232 can be formed using any suitable technique known to those skilled in the art. In some embodiments, the DARC 232 comprises silicon oxynitride (SiON). In some embodiments, the thickness of the DARC 232 ranges from 250 Å to 500 Å. In some embodiments, the thickness of the DARC 232 is greater than 0 Å and less than or equal to 500 Å.

[0050] A bottom antireflective coating (BARC) 234 is formed on the DARC 232. The BARC 234 can be formed using any suitable technique known to those skilled in the art. In some embodiments, the thickness of the BARC 234 is in a range of 100 Å to 500 Å. In some embodiments, the thickness of the BARC 234 is greater than 0 Å and less than or equal to 500 Å.

[0051] A photoresist 236 is formed over the BARC 234. The photoresist 236 can be deposited using any suitable technique known to those skilled in the art. The photoresist 236 is patterned using any suitable technique (e.g., lithography) to form a patterned photoresist and expose the top surface 235 of the BARC 234. In some embodiments, the photoresist 236 is an energy-sensitive resist material that can be patterned by exposing the energy-sensitive resist material to UV radiation through a patterning device, such as a mask (not shown), and then developing the energy-sensitive resist material in a suitable developer. After the energy-sensitive resist material is developed, through-openings 237 defining a pattern exist in the photoresist 236.

[0052] FIG. 2C illustrates electronic component 220 after the pattern of photoresist 236 has been transferred to antireflective coatings 232, 234, advanced patterning film 230, hard mask oxide layer 228, and ruthenium carbide hard mask 226. In some embodiments, transferring the pattern of photoresist 236 removes photoresist 236, BARC 234, DARC 232, and advanced patterning film 230, leaving behind patterned hard mask oxide 248 and patterned ruthenium carbide hard mask 246. In the illustrated embodiment, the pattern transfer also forms patterned hard mask bottom layer 242 and patterned seed layer 244. In some embodiments, optional hard mask bottom layer 222 and optional seed layer 224 are present and are not patterned along with ruthenium carbide hard mask 226.

[0053] In some embodiments, pattern transfer occurs by exposing the substrate to an etchant plasma using the photoresist 236 as a mask. The etchant plasma in some embodiments includes an oxygen (O2) content and a chlorine (Cl2) content. In some embodiments, the chlorine content of the etchant plasma is in a range of 5% to 15% of the oxygen content on a molar basis. In some embodiments, the chlorine content of the etchant plasma is less than or equal to 15%, 10%, or 5% of the oxygen content on a molar basis.

[0054] In some embodiments, the etchant plasma contains carbonyl sulfide (COS) content. The COS content of some embodiments is in the range of 1% to 10% of the oxygen content on a molar basis.

[0055] In some embodiments, the etchant plasma comprises oxygen, chlorine, and carbonyl sulfide. The etchant plasma of some embodiments has a composition of 1-10% COS and 5-15% Cl2 based on the amount of O2 on a molar basis.

[0056] In some embodiments, the photoresist 236, the anti-reflective coatings 232, 234, and the advanced patterned film 230 are removed simultaneously with the pattern transfer. In some embodiments, one or more of the photoresist 236, the anti-reflective coatings 232, 234, or the advanced patterned film 230 remain after the pattern transfer and are removed in another independent process.

[0057] 2D illustrates an embodiment of an electronic component 240 after transferring a pattern to a capacitor mold 210 to form an electronic component 260 having a patterned capacitor mold 262. In the embodiment shown, the patterned capacitor mold 262 includes a patterned silicon oxide layer 264 and a patterned second layer 266.

[0058] FIG2D illustrates the electronic component 240 after removing the patterned hard mask oxide 248, the patterned ruthenium carbide hard mask 246, the patterned optional seed layer 244, and the patterned optional hard mask bottom layer 242. The patterned hard mask oxide 248, the patterned ruthenium carbide hard mask 246, the patterned optional seed layer 244, and the patterned optional hard mask bottom layer 242 can be removed simultaneously with the pattern transfer to the capacitor mold 210 or in one or more separate processes. In some embodiments, a plasma containing oxygen and chlorine content is used to remove the patterned ruthenium carbide hard mask 246, the patterned optional seed layer 244, and the patterned optional hard mask bottom layer 242.

[0059] References throughout this specification to "one embodiment," "certain embodiments," "one or more embodiments," or "an embodiment" mean that a particular feature, structure, material, or characteristic described in connection with the embodiment is included in at least one embodiment of the present disclosure. Thus, phrases such as "in one or more embodiments," "certain embodiments," "in one embodiment," or "in an embodiment" appearing in various places throughout this specification are not necessarily referring to the same embodiment of the present disclosure. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0060] Although the disclosure herein has been described with reference to specific embodiments, those skilled in the art will appreciate that the described embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the methods and apparatuses of the disclosure without departing from the spirit and scope of the disclosure. Therefore, the disclosure is intended to encompass modifications and variations within the scope of the appended claims and their equivalents.

[0061] 100: Process chamber 101: Side 102: Vacuum pump 106: Power Supply 110: Controller 112: Central Processing Unit 114: Support circuit 116: Memory 118:Signal bus 120: Nozzle 122: Bottom wall 124: Top 126: Internal processing volume 128: Hole 130: Gas distribution plate 132:Processing System 138: Matching Network 140: RF power supply 150: Base / substrate base 160: Pillar 170: Built-in heating element / heater element 172: Temperature sensor 190:Substrate 191:Substrate surface 192: Base surface 200: Electronic components 205:Substrate 210:Capacitor mold 212: Silicon oxide layer 220: Electronic components 222: Hard mask bottom layer 224: Seed layer 226: Ruthenium Carbide Hard Mask 228:Hard Mask Oxide 230: Advanced Patterned Film 232: Anti-reflective coating 234: Anti-reflective coating 235: Top surface 236: Photoresist 237:Through opening 240: Electronic components 242: Hard mask bottom layer 244: Seed layer 246: Ruthenium carbide hard mask 248: Patterned Hard Mask Oxide 260: Electronic components 262: Patterned capacitor mold 264: Patterned silicon oxide layer 266: Second floor

[0062] Domestic storage information (please note the order of storage institution, date, and number) none Overseas deposit information (please note the order of deposit country, institution, date, and number) none

Claims

1. A method for forming a film stack, comprising: depositing a ruthenium carbide hard mask on a capacitor mold formed on a substrate, wherein the ruthenium carbide hard mask comprises 20 to 45 atomic% ruthenium and less than or equal to 15 atomic% hydrogen, with the remainder being carbon; forming a hard mask oxide on the ruthenium carbide hard mask; forming a patterned photoresist on the hard mask oxide; and transferring the pattern of the patterned photoresist onto the ruthenium carbide hard mask to form a patterned ruthenium carbide hard mask.

2. The method as described in claim 1 further comprises transferring a pattern of the patterned ruthenium carbide hard mask into the capacitor mold.

3. The method as described in claim 2 further comprises etching the patterned ruthenium carbide hard mask from the capacitor mold.

4. The method as claimed in claim 1, wherein the step of transferring the pattern of the patterned photoresist to the ruthenium carbide hard mask comprises: exposing the substrate to an etchant plasma containing an oxygen content and a chlorine content.

5. The method as described in claim 4, wherein the chlorine content, expressed in moles, is less than or equal to 15% of the oxygen content.

6. The method as described in claim 5, wherein the etchant plasma further comprises a carbonyl sulfide content.

7. The method as described in claim 6, wherein the carbonyl sulfur content is less than or equal to 10% of the oxygen content in moles.

8. The method as described in claim 1, wherein the thickness of the ruthenium carbide hard mask is in the range of 500 Å to 400 Å.

9. The method as described in claim 1, further comprising: forming one or more carbon films or amorphous silicon films on the capacitor mold between the capacitor mold and the ruthenium carbide hard mask.

10. The method as described in claim 9, wherein the thickness of the combination of the carbon film, the amorphous silicon film, and the ruthenium carbide hard mask is in the range of 500 Å to 4000 Å.

11. The method as described in claim 1, wherein the capacitor mold comprises a silicon monoxide (SiO) layer.

12. The method as claimed in claim 11, wherein the capacitor mold further comprises a silicon carbonitride (SiCN) layer or a silicon nitride (SiN) layer on the silicon oxide layer.

13. The method as described in claim 12, wherein the thickness of the silicon oxide (SiO) layer is at most 3 µm and the thickness of the SiCN layer is at most 1000 Å.

14. A method for forming an electronic component, comprising: forming a capacitor mold on a substrate, the capacitor mold comprising a silicon oxide (SiO) layer and a silicon carbonitride (SiCN) layer or a silicon nitride (SiN) layer on the silicon oxide layer, wherein the thickness of the silicon oxide (SiO) layer is in the range of 1 µm to 3 µm, and the thickness of the SiCN layer or the SiN layer is at most 1000 Å; optionally depositing one or more of an amorphous silicon film or a carbon film directly on the capacitor mold; depositing a ruthenium carbide hard mask on the capacitor mold and the optional amorphous silicon film or carbon film (if present), the ruthenium carbide hard mask comprising 20 to 45 atomic% ruthenium and 5 to 15 atomic% hydrogen, the remainder being carbon, wherein the sum of the thicknesses of the optional amorphous silicon film or carbon film and the ruthenium carbide hard mask is in the range of 2500 to 3500 Å; A hard mask oxide is formed on the ruthenium carbide layer; an antireflective coating is formed on the hard mask oxide, the antireflective coating comprising one or more of a dielectric antireflective coating (DARC) or a bottom antireflective coating (BARC); a photoresist having a pattern is formed on the antireflective coating; the pattern of the photoresist is transferred to the antireflective coating, the hard mask oxide, and the ruthenium carbide hard mask by exposing the substrate to an etchant plasma containing an oxygen content, a chlorine content, and a carbonyl sulfide content, to form a patterned hard mask oxide and a patterned ruthenium carbide hard mask, and the antireflective coating is removed, wherein the chlorine content is in the range of 5% to 15% of the oxygen content in moles, and the carbonyl sulfide content is in the range of 5% to 10% of the oxygen content in moles; Remove the remaining photoresist and antireflective coating to leave a patterned hard mask oxide and a patterned ruthenium carbide hard mask; and optionally transfer the pattern of the patterned hard mask oxide and the patterned ruthenium carbide hard mask into the optional amorphous silicon film or carbon film.

15. A film stack for forming an electronic component, comprising: a capacitor mold; a ruthenium carbide hard mask on the capacitor mold, wherein the ruthenium carbide hard mask comprises 20 to 45 atomic% ruthenium and less than or equal to 15 atomic% hydrogen, with the remainder being carbon; a hard mask oxide on the ruthenium carbide hard mask; and a patterned photoresist on the hard mask oxide.

16. The film stack as described in claim 15, wherein the thickness of the ruthenium carbide hard mask is in the range of 500 Å to 4000 Å.

17. The film stack as described in claim 15 further includes one or more carbon films or amorphous silicon films between the capacitor mold and the ruthenium carbide hard mask, and the thickness of the combination of the carbon film, amorphous silicon film and ruthenium carbide hard mask is in the range of 500 Å to 4000 Å.

Citation Information

Patent Citations

  • Semiconductor device and method for fabricating the same

    TW201807832A

  • Method of manufacturing a semiconductor device using anti-reflective layer and self-aligned contact technique and semiconductor device manufactured thereby

    US20020042196A1

  • Method for fabricating semiconductor device

    US20100055922A1

  • ETCH profile control of interconnect structures

    US20180315648A1

  • Patterning material film stack comprising hard mask layer having high metal content interface to resist layer