Temporary capping material for oxide prevention in low temperature direct metal-metal bonding

TWI945139BActive Publication Date: 2026-11-11LAM RES CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
TW110133746
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-10
Filing Date
2021-09-10
Publication Date
2026-11-11
Estimated Expiration
2041-09-09

AI Technical Summary

Technical Problem

High-quality metal-to-metal bonding in semiconductor fabrication is hindered by the formation of metal oxides, which can degrade chip performance, and existing methods risk damaging critical components with high forces and temperatures.

Method used

The use of stimuli-responsive polymers (SRPs) as temporary capping materials to protect metal surfaces during bonding, which can be removed under mild conditions to prevent oxide formation and facilitate residue-free metal-to-metal bonding.

Benefits of technology

SRPs enable high-quality metal-to-metal bonding at lower temperatures, preventing oxide formation and minimizing damage to sensitive components, thereby enhancing the integrity and performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001919884_001
    Figure TWG2TB001919884_001
  • Figure TWG2TB001919884_002
    Figure TWG2TB001919884_002
  • Figure TWG2TB001919884_003
    Figure TWG2TB001919884_003
Patent Text Reader

Abstract

This disclosure relates to the use of stimulus-responsive polymers (SRPs) as capping materials during direct metal-to-metal bonding. The processing and layering of SRPs are described herein.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the use of stimulus-responsive polymers (SRPs) as capping materials during metal-to-metal bonding. The process and layers using SRPs are described herein. Prior Technology

[0002] During semiconductor manufacturing, thermal compression can be used to form direct metal-to-metal bonds, in which two clean metal features come into contact with each other. High-quality bonding typically requires high forces and temperatures, which can damage critical components on next-generation chips and heterogeneous integrated devices. Furthermore, some metals (e.g., copper) readily react with oxygen to form metal oxides at the bonding interface, which can degrade bonding quality and compromise chip performance.

[0003] The prior art description provided herein is for the purpose of generally presenting the background of this disclosure. The work of the inventors listed in this case, the scope of the prior art paragraphs herein, and the embodiments that may not have been qualified as prior art at the time of application are not intended or implied as prior art against the content of this disclosure. Summary of the Invention

[0004] This disclosure relates to a temporary capping material for protecting surfaces prior to bonding. In a particular embodiment, the capping material comprises a stimulus-responsive polymer (SRP) that can be deposited on a sensitive surface to prevent oxide formation. Sensitive surfaces include substrates and metal features exposed during semiconductor processing (e.g., integrated circuit (IC) and 3DIC manufacturing). The capping material can be removed under mild conditions to provide a residue-free interface for optimal metal-to-metal bonding formation prior to further processing. In some embodiments, SRP removal and metal-to-metal bonding are performed under cryogenic conditions and optionally within the same tool or apparatus.

[0005] Therefore, in the first embodiment, this disclosure includes a method comprising: aligning a first capped feature and a second capped feature, wherein each of the first and second capped features independently includes a stimulus-responsive polymer (SRP) layer disposed on the surface of a metal feature; and bonding the first and second capped features in an environment by removing the SRP and forming a metal-metal bond between the metal features. In some embodiments, the SRP layer prevents oxidation of the metal feature. In other embodiments, the SRP layer has a thickness of about 10 nm to 10 µm.

[0006] In some embodiments, the joining process includes: exposing the first capped feature and the second capped feature to a removal temperature for removing the SRP, thereby providing a plurality of exposed metal features; and contacting the exposed metal features to form the metal-metal bond. In some embodiments, the removal temperature is from about 50°C to about 250°C.

[0007] In other embodiments, the exposure includes the use of acidic vapors, heat, ultraviolet or vacuum ultraviolet light, plasma, metastable neutrals from inert gas plasma, or combinations thereof.

[0008] In some embodiments, the bonding process includes a bonding temperature from about 25°C to about 250°C. In other embodiments, the bonding process includes using an inert atmosphere, a vacuum environment, a reducing gas, or ambient air.

[0009] In a further embodiment, the method includes (e.g., prior to the alignment): (i) depositing a first SRP layer on the surface of a first metal feature to provide the first capped feature; and (ii) depositing a second SRP layer on the surface of a second metal feature to provide the second capped feature. In some embodiments, the first SRP layer is further deposited on the surface of a gap-filling layer surrounding the first metal feature. In other embodiments, the second SRP layer is further deposited on the surface of a gap-filling layer surrounding the second metal feature. In other embodiments, the method includes (e.g., prior to the deposition in (i) and / or (ii): pretreating the surfaces of the first and second metal features to clean the surfaces and / or remove oxide layers. In yet another embodiment, the deposition in (i) and / or (ii) includes vapor-based or solvent-based deposition of the SRP.

[0010] In a second embodiment, this disclosure includes a method comprising: depositing SRP on the surface of a first metallic feature to form an SRP layer thereby providing a first capped feature, wherein the first metallic feature includes an electrical contact. In some embodiments, the method further includes (e.g., after the deposition): removing the SRP layer to provide a first exposed metallic feature; and contacting the first exposed metallic feature with a second exposed metallic feature to form a metal-metal bond between the exposed metallic features.

[0011] In some embodiments, the deposition includes vapor-based or solvent-based deposition of the SRP. In other embodiments, the removal includes exposing the SRP layer to heat, ultraviolet or vacuum ultraviolet light, metastable neutrals from inert gas plasma, acidic vapors, or alkaline vapors.

[0012] In a further embodiment, the method includes: depositing SRP on the surface of the second metal feature to form an SRP layer, thereby providing a second capped feature; and removing the SRP layer from the second capped feature to provide a second exposed metal feature. In yet another embodiment, the method further includes: removing the SRP layer from the second capped feature to provide an exposed metal feature; and joining the exposed first metal feature and the second metal feature to form a metal-metal bond.

[0013] In the third state sample, this disclosure includes a method comprising: depositing SRP on the surfaces of a first metal feature and a second metal feature to form an SRP layer thereby providing a first capped feature and a second capped feature; aligning the first capped feature and the second capped feature; removing the SRP layer to provide a plurality of exposed metal features; and contacting the metal features thereby forming a metal-metal bond between the metal features.

[0014] In any embodiment herein, the SRP includes an upper limit temperature of less than about 300°C. In some embodiments, the upper limit temperature is less than about 60°C, less than about 50°C, less than about 40°C, less than about 30°C, or lower.

[0015] In any embodiment herein, the SRP further comprises an acid catalyst, an organic acid, a photoacid generator, or a thermal acid generator.

[0016] In any embodiment herein, the SRP further includes a metal bonding portion. Non-limiting metal bonding portions include optionally substituted heterocyclic groups (e.g., azoles), optionally substituted heterocyclic hydroxyl groups, optionally substituted heterocyclic acetyl groups, thiols, optionally substituted amino groups, optionally substituted aminoalkyl groups, carboxyl groups, optionally substituted carboxylalkyl groups, hydroxyl groups, and / or optionally substituted hydroxyalkyl groups, as well as others described herein.

[0017] In any embodiment herein, the SRP comprises a structure of one of the chemical formulas (I)-(XII), (Ia), (Ib), or salts thereof as described herein.

[0018] In any embodiment herein, the SRP layer prevents the first metal feature from oxidizing.

[0019] In any of the embodiments herein, the SRP layer has a thickness of approximately 10 nm to 10 µm.

[0020] In any embodiment herein, the metal feature includes an electrical contact, a protruding metal pillar, a bonding pad, a bump, a microbump, a metal contact surrounded by a dielectric, or an internal connector.

[0021] In any embodiment herein, the metallic feature (e.g., a first metallic feature and / or a second metallic feature) comprises copper (Cu), tin (Sn), silver (Ag), gold (Au), aluminum (Al), or alloys thereof. Additional embodiments are described herein. [definition] []

[0022] "Alkenyl" refers to an optionally substituted C2-24 alkyl group having one or more double bonds. The alkenyl group can be cyclic (e.g., C3-24 cycloalkenyl) or acyclic. The alkenyl group can also be substituted or unsubstituted. For example, one or more substituents described herein for alkyl groups can be used to substitute the alkenyl group.

[0023] "Alkoxy" refers to -OR, where R is an optionally substituted alkyl group as described herein. Exemplary alkoxy groups include methoxy, ethoxy, butoxy, trihaloalkoxy (e.g., trifluoromethoxy), etc. Alkoxy groups may be substituted or unsubstituted. For example, one or more substituents described herein for alkyl groups may be used to substitute the alkoxy group. Exemplary unsubstituted alkoxy groups include C1-3, C1-6, C1-12, C1-16, C1-18, C1-20, or C1-24 alkoxy groups.

[0024] "Alkyl" and the prefix "alk" refer to branched or unbranched saturated hydrocarbon groups with 1 to 24 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, dibutyl, tert-butyl, n-pentyl, isopentyl, dipentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, icosyl, icosyl, etc. Alkyl groups can be cyclic (e.g., C3-24 cycloalkyl) or acyclic. Alkyl groups can be branched or unbranched. Alkyl groups can also be substituted or unsubstituted. For example, an alkyl group may be substituted with a mono, di, or trisubstituent, or with a tetrasubstituent in the case of an alkyl group with two or more carbon atoms, wherein the substituent is independently selected from the group consisting of: (1) C1-6 alkoxy (e.g., -O-Ak, wherein Ak is a optionally substituted C1-6 alkyl); (2) alkylsulfinyl (e.g., -S(O)-Ak, wherein Ak is an optionally substituted C1-6 alkyl); (3) alkylsulfinyl (e.g., -SO2-Ak, wherein Ak is an optionally substituted C1-6 alkyl); (4) amino (e.g., -NRN1RN2, wherein each RN1 and RN2 is H or an optionally substituted alkyl group, or RN1 and RN2 are H or H respectively). (5) aryl; (6) arylalkoxy (e.g., -OL-Ar, where L is a divalent substituted alkyl group and Ar is an substituted aromatic group); (7) aryl (e.g., C(O)-Ar, where Ar is an substituted aryl group); (8) azide (e.g., -N3); (9) cyano (e.g., -CN); (10) aldehyde (e.g., -C(O)H); (11) C3-8 cycloalkyl (e.g., monovalent saturated or unsaturated non-aromatic cyclic C (12) Halogen (e.g., F, Cl, Br or I); (13) Heterocyclic group (e.g., unless otherwise specified, a 5, 6, or 7-membered ring containing one, two, three, or four non-carbon heteroatoms such as nitrogen, oxygen, phosphorus, sulfur, or halogen); (14) Heterocyclic oxygen group (e.g., -O-Het, where Het is the heterocyclic group described herein); (15) Heterocyclic acetyl group (e.g., -C(O)-Het, where Het is the heterocyclic group described herein); (16) Hydroxyl group (e.g., -OH); (17) N-protected amino group; (18) Nitro group (e.g., -NO 2); (19) Side oxygen group (e.g., =O); (20) C 3-8 spirocyclic group (e.g., alkyl or heteroalkyl diradical, the two ends of which are bonded to the same carbon atom of the parent group); (21) C 1-6 thioalkoxy groups (e.g., -S-Ak, where Ak is an optionally substituted C1-6 alkyl group); (22) thiols (e.g., -SH);(23-CO 2RA, wherein RA is selected from the group consisting of (a) hydrogen, (b) C1-6 alkyl, (c) C4-18 aryl, and (d) (C4-18 aryl) C1-6 alkyl (e.g., -L-Ar, wherein L is a divalent substituted alkyl group and Ar is an substituted aryl group); (24) -C(O)NR BR C, wherein each RB and RC is selected from the group consisting of (a) hydrogen, (b) C1-6 alkyl, (c) C4-18 aryl, and (d) (C4-18 aryl) C1-6 alkyl (e.g., -L-Ar, wherein L is a divalent substituted alkyl group and Ar is an substituted aryl group); (25) -SO 2RD, wherein RD is selected from the group consisting of (a) C1-6 alkyl, (b) C4-18 aryl, and (c) (C4-18 aryl) C1-6 alkyl (e.g., -L-Ar, wherein L is a divalent substituted alkyl group and Ar is an substituted aryl group); 1-6 alkyl (e.g., -L-Ar, where L is an optional substituted alkyl group in divalent form and Ar is an optional substituted aryl group); (26) -SO 2NR ER F, wherein each RE and RF group is selected from the group consisting of (a) hydrogen, (b) C 1-6 alkyl, (c) C 4-18 aryl, and (d) (C 4-18 aryl) C 1-6 alkyl (e.g., -L-Ar, where L is an optional substituted alkyl group in divalent form and Ar is an optional substituted aryl group); and (27) -NR GR H, wherein each RG and RH group is selected from the group consisting of (a) hydrogen, (b) N-protected amino, (c) C 1-6 alkyl, (d) C 2-6 alkenyl (e.g., an optional substituted alkyl group having one or more double bonds), (e) C 2-6 ynyl (e.g., an optional substituted alkyl group having one or more double bonds), (f) C 4-18 aryl, (g) (C The group consisting of (4-18 aryl)C1-6 alkyl (e.g., -L-Ar, where L is a divalent, optionally substituted alkyl group and Ar is an optionally substituted aryl group), (h)C3-8 cycloalkyl, and (i)(C3-8 cycloalkyl)C1-6 alkyl (e.g., -L-Cy, where L is a divalent, optionally substituted alkyl group as described herein and Cy is an optionally substituted cycloalkyl group), wherein in one embodiment, no two groups are bonded to the nitrogen atom via a carbonyl or sulfonylurea group. The alkyl group may be a primary, secondary, or tertiary alkyl group substituted with one or more substituents (e.g., one or more halogens or alkoxy groups). In some embodiments, the unsubstituted alkyl group is a C1-3, C1-6, C1-12, C1-16, C1-18, C1-20, or C1-24 alkyl group.

[0025] "Phenylalkyl" refers to the polyvalent (e.g., divalent) form of the alkyl group described herein. Exemplary alkyl groups include methylene, ethylalkyl, propylalkyl, butylalkyl, etc. In some embodiments, the alkyl group is a C1-3, C1-6, C1-12, C1-16, C1-18, C1-20, C1-24, C2-3, C2-6, C2-12, C2-16, C2-18, C2-20, or C2-24 alkyl group. The alkyl group may be branched or unbranched. The alkyl group may also be substituted or unsubstituted. For example, one or more substituents described herein for alkyl groups may be used to substitute the alkyl group.

[0026] "Alynyl" refers to an optionally substituted C2-24 alkyl group having one or more substituted bonds. The alkynyl group can be cyclic or acyclic, and is, for example, ethynyl, 1-propynyl, etc. The alkynyl group can also be substituted or unsubstituted. For example, one or more substituents described herein as alkyl can be used to substitute the alkynyl group.

[0027] "Amino group" refers to -NR N1RN2, where each RN1 and RN2 is H or an optional substituted alkyl group, or an optional substituted aromatic group, or RN1 and RN2 together with their respective attached nitrogen atoms form a heterocyclic group.

[0028] "Aminoalkyl" refers to an alkyl group as defined herein that has been replaced by an amino group as defined herein.

[0029] "Aryl" means aryl as defined herein, which is attached to the parent molecular group via an alkyl group as defined herein. In some embodiments, the aryl group is -Ak-Ar, where Ak is an optional substituted alkyl group as defined herein, and Ar is an optional substituted aryl group as defined herein. The aryl group may be substituted or unsubstituted. For example, one or more substituents described herein for aryl and / or alkyl groups may be used to substitute the aryl group. Exemplary unsubstituted aryl groups are those with 7 to 16 carbons (C 7-16 aryl groups) and aryl groups having 4 to 18 carbons and 1 to 6 carbons (i.e., (C 4-18 aryl)C 1-6 alkyl groups).

[0030] "Aromatic group" refers to any group based on carbon aromatics, including but not limited to phenyl, benzyl, anthraquinyl, benzocyclobutenyl, benzocyclooctenyl, biphenyl, etc. The aromatic group includes chrysenyl, dihydroindenyl, propylene[di]enyl, dicyclopentadienylphenyl, indanyl, naphthyl, phenanthrene, phenoxybenzyl, lavyl, pyrene, terphenyl, etc., including fused benzo[c]C4-8 cycloalkane radicals (e.g., as defined herein), such as dihydroindanyl, tetrahydronaphthyl, genyl, etc. The term "aromatic group" also includes heteroaryl, wherein heteroaryl is defined as a group comprising an aromatic group having at least one heteroatom within the aromatic ring. Examples of heteroatoms include, but are not limited to, nitrogen, oxygen, sulfur, and phosphorus. Similarly, the term "non-heteroaryl," also included in the term "aromatic group," is defined as a group comprising an aromatic group that does not contain a heteroatom. Aromatic groups can be substituted or unsubstituted. The aryl group can be substituted using one, two, three, four, or five substituents described herein for alkyl groups. In certain embodiments, the unsubstituted aryl group is a C4-18, C4-14, C4-12, C4-10, C6-18, C6-14, C6-12, or C6-10 aryl group.

[0031] "Aryl" refers to the polyvalent (e.g., divalent) form of the aromatic group described herein. Exemplary aryl groups include arylphenyl, arylnaphthyl, biphenyl diphenyl, biphenyl triphenyl, diphenyl ether, aryldihydroacenaphthyl, arylanthrayl, or arphenanthryl. In some embodiments, the aryl group is a C4-18, C4-14, C4-12, C4-10, C6-18, C6-14, C6-12, or C6-10 aryl group. The aryl group may be branched or unbranched. The aryl group may also be substituted or unsubstituted. For example, one or more substituents described herein as alkyl or aromatic groups may be used to substitute the aryl group.

[0032] "Aryl(alkyl)" refers to a divalent form of the aryl group described herein, wherein the aryl group is attached to the alkyl or heteroalkyl group described herein. In some embodiments, the aryl(alkyl) group is -L-Ar-, or -L-Ar-L-, or -Ar-L-, wherein the Ar group is the aryl group and each L group is an optionally substituted alkyl group or an optionally substituted heteroalkyl group.

[0033] "Azide group" refers to -N 3 group.

[0034] "Azide alkyl" refers to an azide group attached to the parent molecule group through the alkyl group defined herein.

[0035] "Aldehyde group" refers to the -C(O)H group.

[0036] "Carboxyalkyl" means alkyl as defined herein, which is substituted by one or more carboxyl groups as defined herein.

[0037] "Carboxyl group" refers to the -CO 2H group.

[0038] "Cyano" refers to the -CN group.

[0039] "Cycloalkenyl" refers to a non-aromatic carbonyl ring consisting of 3 to 10 carbon atoms and containing at least one double bond (i.e., C=C). Exemplary cycloalkenyl groups include, but are not limited to, cyclopropenyl, cyclobutenyl, cyclopentenyl, cyclopentadienyl, cyclohexenyl, and cyclohexadienyl.

[0040] Unless otherwise specified, "cycloalkyl" means a monovalent saturated or unsaturated non-aromatic cyclic hydrocarbon group of 3 to 8 carbons, and examples include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, bicyclic [2.2.1.]heptyl, etc. Cycloalkyl groups can also be substituted or unsubstituted. For example, one or more groups can be used to substitute for a cycloalkyl group, including those groups described herein as alkyl.

[0041] "Cycloalkyl" refers to the polyvalent (e.g., divalent) form of the cycloalkyl group described herein. Exemplary cycloalkyl groups include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cyclohexenyl, cyclohexadienyl, etc. In some embodiments, the cycloalkyl group is a C3-6, C3-12, C3-16, C3-18, C3-20, or C3-24 cycloalkyl group. The cycloalkyl group may be branched or unbranched. The cycloalkyl group may also be substituted or unsubstituted. For example, one or more substituents described herein as alkyl groups may be used to substitute the cycloalkyl group.

[0042] "Fluoroacid" refers to A1CO2H, where A1 is an optional substituted alkyl or optional substituted aryl group substituted with one or more fluorine (F).

[0043] As used herein, "ester" refers to -OC(O)A1 or -C(O)OA1, where A1 can be any of the alkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl, or heterocycloalkenyl groups described herein.

[0044] As used herein, "ether" refers to A1OA2, where A1 and A2 can be independently alkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl or heterocycloalkenyl as described herein.

[0045] "Halogen" refers to F, Cl, Br or I.

[0046] "Halogenated alkyl" refers to an alkyl group as defined herein, which is replaced by one or more halogens.

[0047] "Heteroalkyl" means alkyl as defined herein, which contains 1, 2, 3 or 4 non-carbon heteroatoms (e.g., independently selected from the group consisting of nitrogen, oxygen, phosphorus, sulfur, selenium or halogen).

[0048] "Heteroalkylene" refers to the divalent form of an alkylene group as defined herein, wherein the alkylene group comprises 1, 2, 3, or 4 non-carbon heteroatoms (e.g., independently selected from the group consisting of nitrogen, oxygen, phosphorus, sulfur, selenium, or halogen). In some embodiments, the heteroalkylene group is -Ak-X-, -X-Ak-, -(Ak-X)h1-Ak-, or -X-(Ak-X)h1-, wherein Ak is an optionally substituted alkylene group as defined herein, X is or includes non-carbon heteroatoms (e.g., -O-, -S-, or -NR N1-, where RN1 is H, an optionally substituted alkylene group, or an optionally substituted aryl group), and h1 is an integer from 1 to 5. The heteroalkylene group may be substituted or unsubstituted. For example, one or more substituents described herein for alkylene groups may be used to substitute the heteroalkylene group. The heteroalkylene group may be linear or cyclic, for example, the divalent form of a heterocyclic group formed by removing a hydrogen atom from a heterocyclic group described herein. Exemplary heteroalkyl groups include piperdylidene, quinolinediyl, etc.

[0049] The term "heterocyclic alkenyl" is one type of cycloalkenyl as defined herein, wherein at least one carbon atom of the ring is substituted with O, S, N, or NH. Cycloalkenyl and heterocyclic alkenyl groups may be substituted or unsubstituted. Cycloalkenyl and heterocyclic alkenyl groups may be substituted with one or more groups, including but not limited to alkyl, alkoxy, alkenyl, alkynyl, aryl, heteroaryl, formaldehyde, amino, carboxyl, sulfonic acid, sulfinic acid, fluoroacid, phosphonic acid, ester, ether, halogen, hydroxyl, ketone, nitro, cyano, azide, silica, sulfonylurea, sulfinyl, or thiol.

[0050] The term "heterocyclic alkyl" refers to one type of cycloalkyl group as defined herein, wherein at least one carbon atom and its attached hydrogen atom (if present) are substituted with O, S, N, or NH. Heterocyclic alkyl and heterocyclic alkenyl groups may be substituted or unsubstituted. Cycloalkyl and heterocyclic alkyl groups may be substituted with one or more groups, including but not limited to alkyl, alkoxy, alkenyl, alkynyl, aryl, heteroaryl, formaldehyde, amino, carboxyl, sulfonic acid, sulfinic acid, fluoroacid, phosphonic acid, ester, ether, halogen, hydroxyl, ketone, nitro, cyano, azide, silica, sulfonylurea, sulfinyl, or thiol.

[0051] Unless otherwise specified, "heterocyclyl" means a 3, 4, 5, 6, or 7-membered ring (e.g., 5, 6, or 7-membered ring) comprising one, two, three, or four non-carbon heteroatoms (e.g., independently selected from a group consisting of nitrogen, oxygen, phosphorus, sulfur, selenium, or halogens). 3-membered rings have zero to one double bond, 4- and 5-membered rings have zero to two double bonds, and 6- and 7-membered rings have zero to three double bonds. The term "heterocyclyl" also includes bicyclic, tricyclic, and tetracyclyl, wherein any of the heterocyclic rings are combined with one, two, or three rings independently selected from the groups constituted below: an aromatic ring, a cyclohexane ring, a cyclohexene ring, a cyclopentane ring, a cyclopentene ring, and a heterocyclic ring of another single ring, such as indolyl, quinolyl, isophenyl, benzohydrophenyl, benzohydrophenyl, benzohydrophenyl, etc. Heterocyclic groups include acridyl, adenine, larzyl, acridine, acribenzimidazolyl, acridbicyclononyl, acryl heptyl, acryl cyclooctyl, acridinononyl, acridine xanthine group, acridazolidinyl, and acridine Dolyl, Acridyl, Acridyl, Acridyl, Acridyl, Acridyl, Acridyl, Acridyl, Acridyl, Acridyl, Acridyl, Benzimidazolyl, Benzoisothiazolyl, Benzoisozazolyl, Benzo Acridine benzoyl, benzoacridyl, benzodihydrofuranyl, benzodihydrofuranyl, benzodihydrogenyl, benzodihydroalkyl, benzodihydryl, benzodihydryl, benzodiathio-acyl, benzodiathyroxyl, Benzodihydryl, benzofuranyl, benzophine 𠯤yl, benzopyranone group, benzopiperanyl, benzopyrene, benzopiperanyl, benzoquinolyl, benzoquinolyl, benzothiadiacridyl, benzothione Diazoyl, benzothiacridyl, benzothiacridyl, benzothiazolyl, benzothiophene, benzothio, benzothiacridone, benzothiacridyl, benzothiacridyl, benzothiacridyl, benzothiopiperanyl , benzotriacridyl, benzotriacridyl, benzotriacridyl, benzotriazolyl, benzotriacidyl, benzotriacidyl, benzotriacridyl, benzotriacridyl, benzothiacidyl, Benzothiacryl, benzothiacryl, benzoacridyl, benzoacridyl, benzozolinone group, benzozolinyl, benzosulfonactyl, benzylsu ltamyl), benzylsulfinolactamyl (benzylsultimyl), bipyridyl, bipyridinyl, carbazolyl (e.g., 4H-carbazolyl), carbaline (e.g.,β-Carboline), succinyl, succinyl, succinyl, succinyl, coumarinyl, cytdinyl, cytosine, decahydroisoquinolinyl, decahydroquinolinyl, diacylbis(octyl), diacyl, diacylthionyl, diacylone, diacyl, diacyl, diacyl, dibenzoisoquinolinyl, dibenzoacrylyl, dibenzocarbazolyl, dibenzofuranyl, dibenzophenone α-yl, dibenzopiperanone, dibenzopiperanone (oxanthrone), dibenzoquinoline, dibenzothiazoline, dibenzothiazoline, dibenzophenylthio, dibenzopiperanone, dihydroazoline, dihydroazoline, dihydrofuranyl (dihydrofuranyl / dihydrofuryl), dihydroisoquinoline, dihydropiperanyl, dihydropyridinyl (di) hydropyridinyl / dihydroypyridyl), dihydroquinolinyl, dihydrothiophenyl, dihydroindolyl, dialkyl, diazonyl, diindolone, diazonyl, dioxenyl, diazonyl, dioxenyl, dioxobenzofuranyl, diazonyl, dioxtetrahydrofuranyl, dioxothiopyrinyl, dithiazolyl Dithiazolyl, dithienyl, dithiazolyl, furanyl, furazolidyl, furanyl, guanine, sepiazolyl, sepiazolinyl, hypoxanthine, hydantoinyl, imidazolidinyl, imidazolinyl, imidazolyl, indazole (e.g., 1H-indazole), indolenyl, indolinyl, indoleyl, in... Indoleyl (e.g., 1H-indoleyl or 3H-indoleyl), isatyl (isatinyl, isatyl), isobenzofuranyl, isobenzoyl, isobenzoenyl, isoindazoyl, isoindolinyl, isoindolinyl, isopyrazolyl, isopyrazolyl, isoazolyl, isoquinolinyl, isoquinolinyl, isothiazolyl, isothiazolyl, pirinyl, naphthinazoleyl Naphthiridinyl, naphthiridyl, naphthiazolyl, naphthothioxolyl, naphthriazolyl, naphthiridone, naphthyridinyl, octahydroisoquinolinyl, bis(heptyl), uracilyl, diazolyl, azoxy, azoxy, azoxinone, azoxolinyl, azoxolinyl Azolinone, ethazolyl, ethazolyl, ethazolyl, ethazolyl, ethazolyl, oxtenayl, ethindolyl, ethazolyl, ethazolyl, ethazolyl, ethazolyl, ethazolyl, ethazolyl, ethazolyl, ethazolyl, ethazolyl (benzothiofuranyl), ethazolyl, ethazolyl, ethazolyl α-yl, β-yl, β-ylone, phthalyl, benzylylamine, piperyl, piperidinyl, piperidinone (e.g., 4-piperidinone), pteridinyl, purine, piperanyl, pyridine, pyrazolidine, pyrazolinyl, pyrazolpyrimidinyl, pyrazolyl, pyridinyl, pyridinyl, pyrimidinyl, pyrimidinyl, pyrimidinyl / pyrimidyl, piperyl, pyrrolidinyl, pyrrolone (e.g., 2-pyrrolone), pyrrololinyl, pyrroleyl pyrrolyl, pyrrole (e.g., 2-pyrrole), n-pyrylium, quinazolinyl, quinolinyl, quin Benzyl (e.g., 4-quinoline) group), quinolyl, 𪡓yl, selenium, selenazolyl, benzene (selenophenyl), succinimidyl, cyclobutanyl, tetrahydrofuranyl (tetrahydrofuranyl / tetrahydrofuryl), tetrahydroisoquinolinyl (tetrahydroisoquinolinyl / tetrahydroisoquinolyl), tetrahydropyridyl (tetrahydropyridyl / tetrahydropyridyl) (piperidinyl), tetrahydropiperanyl, tetrahydropiperanyl, tetrahydroquinolyl (tetrahydroquinolinyl / tetrahydroquinolyl), tetrahydrothiophene, tetrahydrophenylthio, tetrahydrophenyl, tetrazolyl, thiadithioyl (e.g., 6H-1,2,5-thiadilysyl, or 2H,6H-1,5,2-dithiosyl ), thiazolyl, thiafyl, thiazyl, thianaphthenyl, thiacridyl, thiacridyl, thiazolidinedionyl, thiazolidinedionyl, Thiazolidinyl, thi azolyl, thiophene, thiophyl, thiazyl, thiazyl, thialancyl, thiophanyl, thioglynyl, thioglycoside, thiopyrayl, thiodiazoyl, thiodiazoyl, thiodiazoyl, thioindophenol, thiopiperanyl, thiopiperanyl, thiotriazolyl, thioureazolyl, thiosyl, thiosyl, thymidyl, thymidinyl, triacridyl, triazolyl, trithiazyl, ureaconyl, ureaconyl, uretidinyl / uretinyl), urea group (uricyl), urea glycoside group, 𠮿 group, xanthine group, 𠮿thione group, etc., and their reformed forms (e.g., including one or more side oxygen groups and / or amine groups), and salts thereof. Heterocyclic groups may be substituted or unsubstituted. For example, one or more substituents described herein for aryl groups may be utilized for substitution of heterocyclic groups.

[0052] "Heterocyclic diyl" refers to the bivalent form of a heterocyclic group as described herein. In one instance, heterocyclic digroups are formed by recourse to removal of hydrogen from heterocyclic groups. Exemplary heterocyclic digroups include sphenidilyl, quinoline diyl, and the like. Heterocyclic digroups may also be substituted or unsubstituted. For example, one or more substituents described herein for heterocyclic groups may be utilized for substitution of heterocyclic digroups.

[0053] “Heteroepoxy” refers to a heterocyclic group, as defined herein, which is attached to a parent molecular group via an oxygen atom.

[0054] "Heterocyclic acetyl" refers to the heterocyclic group defined in this article, which is attached to the parent molecular group via a carbonyl group.

[0055] "Hydroxy" refers to -OH.

[0056] "Hydroxyalkyl" refers to an alkyl group as defined herein that is replaced by one to three hydroxyl groups, with the additional condition that a single carbon atom of the alkyl group may not be attached to more than one hydroxyl group, such as hydroxymethyl, dihydroxypropyl, etc.

[0057] "Ketone" refers to A1C(O)A2, where A1 and A2 can be independently alkyl, haloalkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl or heterocycloalkenyl groups as described herein.

[0058] "Nitro" refers to -NO2 group.

[0059] "Oxygen group" refers to the -O- group.

[0060] "Phosonic acid" refers to -P(O)(OH)2.

[0061] "Silicone" refers to -SiA1A2A3, where A1, A2 and A3 can each be an alkyl, haloalkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl or heterocycloalkenyl group as described herein.

[0062] "Sulinate" refers to -S(O)OH.

[0063] "Sulphinyl" refers to -S(O)A1, where A1 can be hydrogen, alkyl, haloalkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl or heterocycloalkenyl groups as described herein.

[0064] "Sulfonic acid" refers to -S(O) 2OH.

[0065] "Sulfoyl" refers to -S(O)2A1, where A1 can be hydrogen, alkyl, haloalkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl or heterocycloalkenyl groups as described herein.

[0066] "Thio-" refers to the -S- group.

[0067] "Thiol group" refers to the -SH group.

[0068] The term "about" as used herein means + / - 10% of any value presented. This term, as used herein, refers to the endpoints of any value, range of values, or one or more ranges presented.

[0069] The terms “top,” “bottom,” “upper,” “lower,” “above,” and “below” used herein are used to provide relative relationships between plural structures. The use of these terms does not imply or require that a particular structure be located in a specific position within the apparatus.

[0070] This document refers in detail to specific embodiments of the present disclosure. Examples of these specific embodiments are illustrated in the accompanying drawings. Although the present disclosure will be described in conjunction with these specific embodiments, it should be understood that it is not intended to limit the present disclosure to these specific embodiments. Rather, it is intended to cover alternatives, modifications, and equivalents that may be included within the spirit and scope of this disclosure. In the following description, numerous specific details are set forth to provide a thorough understanding of the present disclosure. The present disclosure may be practiced without some or all of these specific details. In other instances, conventional processing operations have not been described in detail so as not to unnecessarily obscure the present disclosure.

[0071] Other features and advantages of the present invention will become apparent from the following description of the embodiments and the claims. Simple Explanation of the Diagram

[0072] Figures 1A-1B show multiple flowcharts illustrating certain operations in a semiconductor manufacturing process example using stimulus-responsive polymers (SRPs). Provided is (A) method 100, which uses SRP layers 118, 128 to form a bonded assembly 130; and (B) a bonding operation, which includes removing the SRP and exposing feature contacts to form the bonded assembly 130.

[0073] Figures 2A-2B show complex flowcharts with certain other operations. Provided are (A) a method using thin SRP layers 218, 228, and (B) a method using thick SRP layers 248, 258.

[0074] Figure 3 shows a flowchart with some other operations. What is provided is a method using a metal feature 314 surrounded by a gap-filling material 315.

[0075] Figures 4A-4D show process flow diagrams of a non-limiting method using SRP during the formation of a metal-to-metal bond.

[0076] Figure 5 shows a process flow diagram of another non-limiting method using SRP during the process of forming a metal-metal bond.

[0077] Figure 6 shows a process flow diagram of another non-limiting method using SRP during the process of forming a metal-to-metal bond.

[0078] Figure 7 is a functional block diagram of an example electroplating tank according to the present disclosure.

[0079] Figure 8 is a functional block diagram of an example electrodeposition apparatus according to the present disclosure.

[0080] Figure 9 is a functional block diagram of another example of an electrodeposition apparatus according to this disclosure.

[0081] Figure 10 is a functional block diagram of an example of electroplating equipment according to this disclosure.

[0082] Figure 11 is a functional block diagram of an example of a substrate processing system according to the present disclosure, wherein the substrate processing system includes a plurality of substrate processing tools and a storage temporary area.

[0083] Figure 12 illustrates a cross-sectional schematic diagram of an example dry deposition apparatus for depositing SRP according to this disclosure.

[0084] Figure 13 shows a detailed side cross-sectional view and a plan view of the top plate, base plate and edge ring of the part.

[0085] Figure 14 is a plan view of an example wet deposition apparatus for SRP deposition according to the present disclosure.

[0086] Figure 15 is a cross-sectional view along line III-III in Figure 14.

[0087] Figure 16 is an enlarged view of detail IV in Figure 15.

[0088] Figure 17 shows a plan view of the heating assembly of an example wet deposition apparatus.

[0089] Figure 18 shows another example of a wet deposition apparatus for depositing SRP according to this disclosure.

[0090] Figure 19 shows the embodiment of Figure 18 in the loading and unloading position. Implementation

[0091] Stimulus-responsive polymers (SRPs) can be used in semiconductor manufacturing processes as temporary or sacrificial layers that can be subsequently removed. Low-temperature SRPs can spontaneously remove themselves upon exposure to stimuli such as mild heating or acidic vapors, avoiding the use of aggressive wet or dry removal chemicals that could damage the substrate surface. Other processes for removing SRPs are described herein. In certain embodiments, this SRP can be removed without residue, providing a clean surface suitable for forming metal-to-metal bonds.

[0092] This document describes a capping process in which SRP is deposited on metallic features (e.g., plated metallic features) as a protective layer. This temporary layer prevents oxide formation on the features during wafer stacking and transfer to a thermocompression bonding tool. Upon entering the chamber of the thermocompression bonding tool, the temperature is gradually increased to a removal temperature (e.g., below 250°C) to cause the capping material to evaporate or bake off. The plurality of metallic features are then aligned and brought into contact for high-quality bonding. Therefore, a bonding process is also described herein, in which the SRP is removed to form a metal-to-metal bond.

[0093] In use, sacrificial films can provide extended standby time. In one example, the SRP film can be a thin or thick sacrificial polymer configured to protect sensitive metal features for an extended period, such as during substrate transfer or feature alignment, or before thermocompression bonding. This sacrificial surface protection layer can ultimately be removed by triggering its spontaneous depolymerization and vaporization above the upper limit temperature of the protection layer using a suitable stimulus (e.g., acid, heat, and / or electromagnetic field), thereby minimizing the impact on the sensitive surface. Such surfaces may include surfaces sensitive to environmental standby time effects, or surfaces also affected by undesirable oxidation, corrosion, and / or halogenation. Examples of such surfaces include, but are not limited to, copper (Cu), tin (Sn), tin-silver (SnAg), silver (Ag), gold (Au), aluminum (Al), silicon (Si), silicon / germanium (Si / Ge), tungsten (W), cobalt (Co), ruthenium (Ru), molybdenum (Mo), and titanium nitride (TiN).

[0094] Please refer to Figure 1A, which shows an example of a method 100 for protecting a metal feature. First, a substrate 116 including a metal feature 114 is provided. This feature may be an electrical contact, such as a pillar (e.g., a protruding metal pillar), a bonding pad, a bump, a microbump, a metal contact surrounded by a dielectric, or an interconnect. In a next operation 101, SRP is deposited on the surface of the metal feature 114 to form an SRP layer 118. The SRP may be deposited in a vapor phase (e.g., using a carrier gas) or in a liquid phase (e.g., using a solvent or as a formulation). When solvent-based deposition is used, the SRP may optionally be dried or solidified by removing the liquid portion to form a layer or film.

[0095] SRPs can be polymers with a low upper temperature limit (Tc) (e.g., homopolymers or copolymers) that are thermodynamically unstable at room temperature. Tc is the temperature at which the polymer and its monomers exist in equilibrium. Below Tc, it is a polymer, and above Tc, it is a monomer. Because polymers have excellent storage life at temperatures much above Tc, these low-Tc polymer systems can be kinetically captured. For example, poly(phenylene phthalaldehyde) (PPHA) has a Tc of -40°C but is stable at room temperature for 2.5 years. This stability is achieved by kinetically suppressing the depolymerization mechanism. Additional SRPs and their formulations are described herein.

[0096] The SRP can be deposited using any practical method. Low-Tc volatile polymer capping layers can be formulated using only spin-coating solvents, which can be dry-deposited from the vapor phase, or formulated using spin-coating solvents and weak acids to lower degradation temperatures. For example, equipment such as a spin coater (scalpel) can be used to coat thick (e.g., greater than 1 µm) films, with some modifications to the formulation.

[0097] For wet deposition, the choice of solvent for spin coating formulations can affect the amount of residual solvent remaining in the polymer layer or film. Residual solvent may plasticize the polymer, lowering its glass transition temperature. By plasticizing the polymer, feature filling can be achieved at temperatures below the polymer's degradation temperature, and stress from the spin coating process can be reduced. Such features may include high-density features (e.g., with a pitch of less than about 20 µm between multiple features), high aspect ratio features (e.g., having an aspect ratio (AR) of, for example, at least 8, 10, 20, 30, 40, or 80), and / or thick features (e.g., with a thickness of about 30 µm to 50 µm).

[0098] Furthermore, SRP can be formulated using acid catalysts (e.g., weak organic acids (e.g., pKa ≥ 1)). These weak organic acids can catalyze the degradation of SRP without compromising membrane stability. By catalyzing the degradation of the polymer, the initiation temperature of degradation can be lowered and the degradation rate increased.

[0099] SRP can be deposited as a uniform or non-uniform layer on the feature. Furthermore, the thickness of the SRP layer can range from approximately 10 nm to 10 µm. Depending on the size of the feature, the SRP layer can provide conformal or non-conformal stepped or planar coverage. If vias or openings exist, the SRP layer can be used to fill such openings.

[0100] Referring again to Figure 1A, a capped feature 110 is formed after SRP deposition. The capped feature may include an SRP layer 118 disposed on any exposed surface of the metallic feature 114. In some instances, the metallic feature may be surrounded by another material (e.g., a dielectric material or interstitial material), with the SRP layer disposed on the exposed top surface of the feature. In other instances, the metallic feature may be a pillar with exposed top and side surfaces, with the SRP layer disposed on these surfaces or portions thereof. The capped feature may be used immediately, or stored or stored prior to further processing.

[0101] Further processing may include aligning the first capped feature 110 and the second capped feature 120 102, and thus may include an SRP layer 128 disposed on the surface of the second metal feature 124 on the substrate 126. The second capped feature may be formed by using any SRP deposition process described herein. Alignment may include vertically and / or horizontally aligning the top surfaces of the first and second metal features. In FIG1A, the top surface of the first feature 114 is away from the substrate 116, and the top surface of the second feature 124 is away from the substrate 126.

[0102] In operation 103, features 114, 124 may be metal-to-metal bonded to form a metal structure 134 within the bonded assembly 130. In some non-limiting embodiments, the bonded assembly does not include solder. In other embodiments, the bonded assembly includes direct metal-to-metal bonding. In yet another embodiment, the metal structure provides a reduction in internal interconnect line length, which can enhance performance and reduce power consumption. This bonded assembly can be present in any practical stack, device, substrate, vertically integrated architecture, multilayer integrated architecture, or high pitch density circuitry. For example, direct metal-to-metal bonding allows for closer pitch (e.g., denser stacking in the xy direction, where the axes are parallel to the plane of the substrate) and / or shorter interconnect height or length (e.g., in the z direction, where the axes are orthogonal to the plane of the substrate).

[0103] Bonding may include removing SRP layers 118, 128 to provide exposed features; and contacting the exposed features to form a metal-to-metal bond. Conditions for SRP removal may include exposure to a removal temperature, where the degraded SRP is volatile, and bonding conditions may include exposure to a bonding temperature, where the metal-to-metal bond is formed. When the removal and bonding temperatures are similar, a continuous operation can be performed under these temperature conditions to remove the SRP and form a metal-to-metal bond. Alternatively, removal and bonding may be performed as a dispersion operation. Non-limiting removal temperatures include about 50°C to about 250°C, for example, about 50°C to 150°C; and non-limiting bonding temperatures include about 25°C to about 250°C, for example, about 100°C to 250°C.

[0104] As further shown in Figure 1B, operation 103a includes removing SRP from the first capped feature 110 and the second capped feature 120 to provide a first exposed metal feature 114 and a second exposed metal feature 124. The capped features may be exposed to a stimulus that degrades all or only part of the SRP. Volatile monomers or fragments from the degraded polymer may be removed (e.g., by purging the chamber). The stimulus may be any stimulus that breaks the bonds of the SRP, causing it to degrade.

[0105] Controlled SRP degradation may include depolymerization, which can be catalyzed in the presence of an acid. This catalysis can be promoted by formulating SRP with an acid (e.g., a weak organic acid, a photoacid generator, or a thermal acid generator). In other embodiments, SRP removal may be carried out in the presence of acidic vapors (e.g., formic acid, acetic acid, citric acid, or others described herein) to catalyze the decomposition reaction. The use of acids can promote degradation at lower temperatures (e.g., below 100°C) and incidentally remove metal oxides formed on the metallic features. Other removal methods include the use of heat, ultraviolet (UV) light, or vacuum UV, which may be combined with the acidic vapors described herein. In other embodiments, SRP removal may include the use of heat with another stimulus, such as UV exposure or acid vapor exposure.

[0106] Referring again to Figure 1B, operation 103b includes contacting the exposed features to provide a bonded metal structure 134 within assembly 130. In certain embodiments, this bonding process enables high-integrity metal-to-metal direct bonding at low temperatures (e.g., below 250°C) and uses low-Tc volatile SRP to prevent oxide formation. In some embodiments, a temporary capping layer cleanly evaporates from the surface at low temperatures (e.g., between about 50°C and 250°C) to resolve oxide formation and enable metal-to-metal bonding at low temperatures (e.g., below 250°C). This contact may include thermocompression bonding, where heat and pressure are applied to the metal features to allow atomic interdiffusion and grain growth at the metal-to-metal interface.

[0107] SRP removal and thermal compression can be performed in any conventional thermal compression tool or chamber with an inert atmosphere (e.g., oxygen-free), vacuum, reducing gas, or ambient air (e.g., including oxygen). Depending on the conditions, dwell time can be controlled and minimized to prevent oxide formation. For example, if the ambient air contains oxygen, the capping layer can be volatilized immediately after bonding. Otherwise, oxides may eventually form on the feature surface.

[0108] The processing described herein includes any practical combination of operations for forming features, depositing SRP layers, and bonding exposed features. As shown in FIG2A, a non-limiting processing may include coating a device having metallized features with a temporary capping layer. Initially, the stack may include a substrate 216, a seed layer or barrier layer 211 disposed on the surface of the substrate, and a patterned photoresist 212 having an opening 213 defined therein and disposed on the surface of the seed / barrier layer. In operation 201, metallized pillars 213a are formed within the openings 213. Next, in operation 202, the photoresist is stripped to provide released metal pillars 213b. Operation 203 includes etching to remove the seed / barrier layer to provide freestanding or isolated metal features 214. Optionally, operation 204 may be performed to clean the surface of the metal features using a wet cleaning process or a plasma treatment. This cleaning step may be performed immediately before depositing the SRP layer, ensuring a clean and oxide-free surface before capping.

[0109] In operation 205, an SRP layer 218 is deposited on an exposed surface, said exposed surface may include the top surface and / or sidewalls of the metal feature 214, and optionally the surface of the substrate 216. A first capped feature 210 is thus formed. A second capped feature 220 is formed in a similar manner. Although the first and second capped features are shown in FIG. 2A as having similar geometries, the features may be the same or different. In a non-limiting example, the first capped feature may be a pillar, while the second capped feature may be a contact pad. In other embodiments, both the first and second capped features may be pillars having similar or different dimensions.

[0110] In operation 206, a first capped feature 210 and a second capped feature 220, the second capped feature 220 including a substrate 226, a second metal feature 224, and an SRP layer 228, are aligned. Next, in operation 207, the first and second features are joined together to form a metal structure 234 within the joined assembly 230. As described herein, this joining may include continuous or discrete operations for removing the SRP layers 218, 228 and joining the exposed features 214, 224 to form a metal-to-metal bond. Furthermore, complete removal or evaporation of the capping material is not required, only a sufficient amount needs to be removed from the joining surfaces of the features to allow for cryogenic bonding. In some instances, the capping material may be retained within the stack or assembly after the feature joining is performed.

[0111] The capping material does not need to be uniformly coated onto the surface of the feature and / or substrate. As shown in FIG2B, the first capped feature 240 may include a non-uniform SRP layer 248, wherein the SRP layer 248 has a variable thickness near the metal feature 214. This non-uniformity may originate from the dimensions, aspect ratio, pitch density, surface chemicals, or material composition of the deposited surface. This disclosure includes capped features having uniform or non-uniform SRP layers.

[0112] Referring again to Figure 2B, in operation 206, the first capped feature 240 can be aligned with the second capped feature 250 having a non-uniform SRP layer 258, a metal feature 254, and a substrate 256. As shown in operation 207, a metal structure 264 is provided within the bonding assembly 260.

[0113] Metal-to-metal bonding can be formed between multiple features provided in any practical device. In some instances, the device includes individual or isolated metal features, such as pillars. In other instances, such features can be embedded within multiple layers, with only the bonding surface accessible to the surface of the device.

[0114] As shown in Figure 3, a non-limiting process may include applying a temporary capping layer to a device having a gap-filling material, wherein the filler material surrounds the metallized feature. Initially, the stack may include a substrate 316, a seed layer or barrier layer 311, and a patterned photoresist 312 having an opening 313 defined therein. In operation 301, a metallized pillar 313a is formed within the opening 313. Next, in operation 302, the photoresist is stripped to provide a released metal pillar 313b. Operation 303 includes etching to remove the seed / barrier layer to provide a separate or isolated metallized feature 314.

[0115] Operation 304 includes depositing a gap-filling material around the metal feature 314, which may result in incidental deposition on the metal surface. Therefore, operation 305 includes etch-back cleaning of the stack, which results in a portion of the gap-filling layer being etched away and the metal surface being cleaned before capping. This etch-back cleaning may include the use of reducing chemicals, such as ammonia, or a combination of nitrogen (N₂) and hydrogen (H₂) gases. Next, in operation 306, an SRP layer 318 is deposited on an exposed surface, which may include the surface of the metal feature 314 and the surface of the gap-filling layer 315. The first capped feature 310 is thus formed. A second capped feature 320 having a second SRP layer 328, a second metal feature 324, a gap-filling layer 325, and a second substrate 326 can be formed in a similar manner.

[0116] In operation 307, the first capped feature 310 and the second capped feature 320 are aligned. Alignment may include configuring the top surfaces of each capped feature such that vertical compression will provide contact between the multiple surfaces and create a metal-to-metal bond. Next, in operation 308, the first and second features are joined together to form a metal structure 334 within the joined assembly 330. As described herein, this joining may include sequential or discrete operations for removing SRP layers 318, 328 and for bringing exposed features 314, 324 into contact, thereby forming a metal-to-metal bond. In some instances, SRP removal includes exposing only the surfaces of the metal features and removing only a portion of the SRP layer.

[0117] This disclosure generally includes the use of SRP with metallic features (e.g., electrical contacts). A non-limiting method may include forming an SRP layer on a first metallic feature to provide a first capped feature. As shown in FIG4A, an example of method 400 includes operation 401, providing a substrate including one or more metallic features (e.g., electrical contacts); and operation 405, depositing SRP on the surface of the metallic feature to form an SRP layer, thereby providing a capped feature. This method may optionally include operation 403, pretreating the surface of the metallic feature prior to SRP deposition, wherein such pretreating may include a wet cleaning process or a plasma process (e.g., a non-thermal plasma process). The methods herein may include one or more pre-bonding operations (e.g., prior to SRP deposition), such as cleaning the metallic feature, isolating the metallic feature by depositing a dielectric or gap-filling material, and recessing one or more non-metallization layers.

[0118] Another non-limiting method may include aligning a plurality of capped features having an SRP layer. As shown in FIG4B, method 420 example includes operation 407, aligning first and second capped features, wherein each capped feature includes an SRP layer disposed on a surface of a metal feature; and operation 409, bonding the first and second capped features in an environment in which the SRP is removed and a metal-to-metal bond is formed between the metal features. This environment may have any of the removal or bonding temperatures described herein. Furthermore, the exposed features may be contacted using a contact pressure that facilitates the formation of the metal-to-metal bond, wherein the contact pressure is, for example, a pressure of about 0.2 MPa to about 1 MPa or about 0.7 MPa (about 100 psi). The methods herein may include one or more post-bonding operations, such as annealing, wafer thinning, or other back-side processing of the metal structure within the bonding assembly.

[0119] Other methods may include SRP deposition, alignment of capped features, and bonding. As shown in FIG4C, an example of method 440 includes operation 401, providing a substrate including one or more metal features; optionally operation 403, pretreating the surface of the metal features to provide a clean surface and / or an oxide-free surface; operation 405, depositing SRP on the surface of the metal features to provide a first capped feature; operation 407, aligning the first capped feature with a second capped feature having an SRP layer disposed on the surface of the metal features; and operation 409, bonding the first and second capped features in an environment in which SRP is removed and a metal-metal bond is formed between the metal features.

[0120] If necessary, bonding may include a dispersion step. As shown in FIG4D, method 460 may include bonding operation 409, wherein bonding operation 409 includes operation 409a, such as exposing to a removal temperature to volatilize the SRP and / or exposing to acidic vapors to catalyze SRP removal, thereby removing the SRP; and operation 409b, contacting the exposed features to provide a metal-metal bond. This contact may be performed at any bonding temperature and / or contact pressure described herein.

[0121] The processing described herein may include further operations such as forming a stack prior to SRP deposition. As shown in FIG5, an example of method 500 may include operation 501, forming one or more openings in a photoresist layer, which may optionally be disposed on a seed layer or a barrier layer; operation 502, electroplating or depositing metal within the openings to provide one or more metallic features; operation 503, stripping the photoresist layer to release the metallic features; operation 504, etching the seed / barrier layer to provide isolated or electrically isolated metallic features; operation 505, depositing SRP on the surface of the metallic features to provide a first capped feature; operation 507, aligning the first capped feature with a second capped feature having an SRP layer disposed on the surface of the metallic feature; and operation 509, bonding the first and second capped features in an environment in which SRP is removed and a metal-metal bond is formed between the metallic features.

[0122] The stack may include further material for use on the metallic features, and the methods herein may include operations for depositing such material. As shown in FIG6, an example of method 600 may include operation 601, providing a substrate including one or more metallic features; operation 603, depositing a gap-filling material around the metallic features to electrically isolate these features; operation 604, etching back the surface of the gap-filling material and the surface of the metallic features; operation 605, depositing SRP on the cleaned surface of the metallic features to provide a first capped feature; operation 607, aligning the first capped feature with a second capped feature having an SRP layer disposed on the surface of the metallic features; and operation 609, bonding the first and second capped features in an environment in which the SRP is removed and a metal-metal bond is formed between the metallic features. [Metallic Feature Parts and Substrate] []

[0123] The SRP and methods described herein can be applied to metallic features and related structures. These metallic features may form oxides during exposure to air, and such interfacial oxide layers should be avoided when forming metal-to-metal bonds. Therefore, in one state, the SRP described herein can be used to reduce oxidation of such metallic features.

[0124] SRPs can be disposed on any practical feature, substrate, or surface. The surface can be a flat surface or include one or more electrical contacts, pillars, pads, bumps, microbumps, interconnects, through-holes, holes, gaps, and trenches. Other surfaces may include surfaces located on devices, such as electronic components, printed circuit boards, packages, etc. Examples of substrate surfaces include silicon, silicon-germanium, and germanium structures; metallic surfaces include, but are not limited to, copper, cobalt, titanium, titanium nitride, tungsten, ruthenium, or molybdenum; and / or other structures and materials. In particular, metallic features may include conductive metals, transition metals, and their alloys or doped forms. [Sedimentation] [SRP]

[0125] In many embodiments, SRP is a polymer with a low upper temperature limit (Tc). Tc is the equilibrium temperature between the polymer and its monomers. As used herein, the term "low Tc" means a Tc value below the removal temperature. In some embodiments, the Tc is below room temperature, making the polymer thermodynamically unstable at room temperature. Alternatively, low Tc polymers are kinetically trapped, allowing for extended storage at room temperature. In some examples, the stable storage period is several months or years. Low Tc polymers will rapidly depolymerize into their monomer components if the terminal groups or main chain bonds break. Therefore, the polymer system depolymerizes in response to stimulation such as acidic catalysts, basic catalysts, ultraviolet (UV) light, heat, thermal catalysts, and / or photocatalysts. The monomer products are volatile and leave the surface and chamber, or can be easily removed from the surface and chamber.

[0126] While in some embodiments Tc is below room temperature, in the context of semiconductor processing, a low Tc can also represent an upper limit temperature above room temperature. For example, a removal temperature up to 300 °C can be used, representing an upper limit temperature below 300 °C.

[0127] In some embodiments, the SRP may include one or more metal bonding portions. These metal bonding portions facilitate bonding or adhesion of the SRP layer to metal features. Furthermore, such portions may be present in a specific amount or percentage of the polymer monomers. In other embodiments, the SRP may be a copolymer, and one of the monomers in the copolymer may include at least one metal bonding portion.

[0128] The non-limiting metal bonding portion may include one or more of the following: optionally substituted heterocyclic group, optionally substituted heterocyclic oxy group, optionally substituted heterocyclic acetyl group, thiol (-SH), optionally substituted amino group (e.g., -NH 2 or -NR N1R N2), optionally substituted aminoalkyl group (e.g., -Ak-NH 2 or -Ak-NR N1R N2), carboxyl group (-CO 2H), optionally substituted carboxylalkyl group (e.g., -Ak-CO 2H), hydroxyl group (-OH), and / or optionally substituted hydroxyalkyl group (e.g., -Ak-OH), wherein Ak is an optionally substituted alkyl group, and wherein each of RN1 and RN2 is independently H, optionally substituted alkyl or optionally substituted aryl, or RN1 and RN2 together with their respective attached nitrogen atoms form a heterocyclic group as defined herein. In certain embodiments, the optionally substituted heterocyclic group includes optionally substituted azole groups, such as optionally substituted imidazolyl, isozolyl, isothiazolyl, acediazolyl (e.g., 1,2,3-acediazolyl, 1,2,4-acediazolyl, 1,2,5-acediazolyl or 1,3,4-acediazolyl), acezolyl, pyrazolyl, tetrazolyl, thiadiazolyl (e.g., 1,2,3-thiadiazolyl, 1,2,4-thiadiazolyl, 1,2,5-thiadiazolyl or 1,3,4-thiadiazolyl), thiazolyl, triazolyl (e.g., 1,2,3-triazolyl or 1,2,4-triazolyl), or any of those described herein.

[0129] In other embodiments, the metal bonding portion is a multidentate (e.g., didentate, tetradentate, or octate) ligand. Non-limiting multidentate ligands include R1-L1-R2, wherein L1 is an optionally substituted alkyl group, optionally substituted heteroalkyl group, optionally substituted aryl group, or optionally substituted heterocyclic diene; and each of R1 and R2 independently comprises a thiol, optionally substituted amino group, carboxyl group, or hydroxyl group. In some embodiments, each of R1 and R2 is independently -L2-R3; L2 is a covalent bond, optionally substituted alkyl group, or optionally substituted heteroalkyl group; and each of R3 is independently a thiol, optionally substituted amino group, carboxyl group, or hydroxyl group.

[0130] Another non-limiting polydentate ligand includes R1-L1-R2, wherein L1 is an optionally substituted alkyl group; and each of R1 and R2 independently includes an optionally substituted heterocyclic group (e.g., an optionally substituted azole). In yet another embodiment, the metal-binding moiety is a Schiff base ligand. Other metal-binding moieties include imidazolyl, pyrazolyl, triazolyl, thiol, nitrile, 3,4-dihydroxyphenylalanine (DOPA), histidine, ethylenediamine, 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid (DOTA), and derivatives thereof.

[0131] Examples of SRPs are provided below. However, the methods described herein can be used for any SRP. In some embodiments, the SRP comprises an isomeric or copolymeric polymer of polyaldehyde. In a particular embodiment, the isomeric or copolymeric polymer may be a self-immolative polymer as described in U.S. Patent Publication No. 2018 / 0155483, published June 7, 2018, the entire contents of which are incorporated herein by reference.

[0132] SRPs can be any suitable polymer in linear or cyclic form (e.g., homopolymers or copolymers). Non-limiting SRPs include poly(phthalaldehyde), poly(aldehyde), poly(benzyl carbamate), poly(benzyl ether), poly(α-methylstyrene), poly(carbonate), poly(norbornene), poly(olefinic ether), poly(glyoxylate), poly(acetoxymethylamine), poly(ester), or poly(methyl methacrylate), and derivatives thereof. These derivatives may include substitutions with optional substituted heteroalkyl groups substituted with oxygen (-O-) as defined herein, and with one or more substituents described herein as alkyl.

[0133] Other SRPs may include those with a structure of one of the chemical formulas (I)-(XIV), (Ia), (Ib), or (Ic). This SRP may be a linear polymer or a cyclic polymer. If linear, the polymer may include any useful terminal group that terminates the molecule. This terminal group may depend on the reactive terminal group present on the monomer used to synthesize the polymer. In a particular embodiment, the terminal group may include fragments formed using an anionic initiator (e.g., fragments of alkyl anions present in n-BuLi, s-BuLi, etc.), fragments formed using acetylation or alkylation agents (e.g., fragments of acetylation or optionally substituted alkyl groups, such as methyl, acetylation, benzoyl, methyl, ethyl, etc.), fragments formed using conjugated alkyl monomers (e.g., quinone methylated monomers), or fragments formed using an alcohol terminator (e.g., fragments of optionally substituted alkoxy groups). The terminal group may include any useful joining or reactive group (e.g., groups including optionally substituted trialkylsiloxy, optionally substituted alkenyl, optionally substituted aryl, etc.).

[0134] SRP may comprise poly(phenylene phthalaldehyde) or its derivatives, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or comprises a structure of formula (I): or its salts, of which R1 can be H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halogen; R2' and R2'' are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; Z1 and Z2 are each independently -O-, -S-, or optionally substituted heteroalkyl groups; r1 is an integer from 1 to 4; and The number of n ranges from approximately 2 to approximately 100,000.

[0135] In certain embodiments (e.g., of formula (I)), R2' and R2'' are each independently H or optionally substituted alkyl. In some embodiments, Z1 and Z2 are each -O-. In other embodiments, at least one of R1, R2', or R2'' includes a metallic bonding portion (e.g., any of those described herein).

[0136] SRP may comprise polyaldehyde or a derivative thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or comprises a structure of formula (II): or its salts, of which R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; Z 1 is -O-, -S-, or optionally substituted heteroalkyl; and The number n ranges from approximately 2 to approximately 100,000. In some embodiments, at least one of R2 or R3 includes a metal bonding portion (e.g., any of those described herein).

[0137] SRP may comprise poly(benzyl aminocarbamate) or a derivative thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or comprises a structure of formula (III): or its salts, of which R1 can be H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halogen; R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; R4 is H or an optionally substituted alkyl group; Z1 is -O-, -S-, or optionally substituted heteroalkyl; r1 is an integer from 1 to 4; and The number n ranges from approximately 2 to approximately 100,000.

[0138] In certain embodiments (e.g., of formula (III)), R1 is an optionally substituted alkoxy group. In other embodiments, the n-series ranges from about 2 to about 100 (e.g., from about 2 to 10, 2 to 15, 2 to 20, 2 to 25, 2 to 30, 2 to 40, 2 to 50, 2 to 75, 4 to 10, 4 to 15, 4 to 20, 4 to 25, 4 to 30, 4 to 40, 4 to 50, 4 to 75, and 4 to 100). In other embodiments, at least one of R1, R2, R3, or R4 comprises a metallic bonding portion (e.g., any of those described herein).

[0139] SRP may comprise poly(benzyl ether) or a derivative thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or comprises a structure of formula (IV): R1 can be H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halogen; R2 is H, an optional substituted alkyl, an optional substituted heteroalkyl, or an optional substituted aryl; Ar is an optional substituted aryl, optional substituted alkyl, or optional substituted aralkyl; Z1 is -O-, -S-, or optionally substituted heteroalkyl; r1 is an integer from 1 to 4; and The number n ranges from approximately 2 to approximately 100,000.

[0140] In certain embodiments (e.g., of formula (IV)), R1 is an optionally substituted alkyl group. In other embodiments, Ar is an optionally substituted phenyl group. In other embodiments, the n-series ranges from about 2 to about 5000. In other embodiments, at least one of R1, R2, or Ar includes a metal-bonded portion (e.g., any of those described herein).

[0141] SRP may comprise poly(benzyl diaminoformate) or a derivative thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or comprises a structure of formula (V): or its salts, wherein: R1 can be H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halogen; R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; R 4' and R 4'' are each independently H or optionally substituted alkyl; L1 is an optional substituted alkyl group, an optional substituted heteroalkyl group, an optional substituted aryl group, or an optional substituted cycloalkyl group; Z1 and Z2 are each independently -O-, -S-, or optionally substituted heteroalkyl groups; r1 is an integer from 1 to 4; and The number n ranges from approximately 2 to approximately 100,000.

[0142] In certain embodiments (e.g., of formula (V)), R1 is an optionally substituted alkyl group. In other embodiments, Ar is an optionally substituted phenyl group. In other embodiments, n ranges from about 2 to about 5000. In other embodiments (e.g., of formula (V)), R4' and R4'' are each independently an optionally substituted alkyl group. In some embodiments, L1 is an optionally substituted alkyl group. In other embodiments, Z1 and Z2 are -O-. In other embodiments, at least one of R1, R2, R3, R4', or R4'' includes a metal bonding portion (e.g., any of those described herein).

[0143] SRP may comprise poly(diaminocarbamate) or derivatives thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or comprises a structure of formula (VI): or its salts, wherein: R 4' and R 4'' are each independently H or optionally substituted alkyl; L1 and L2 are each independently a substituted alkyl group, a substituted heteroalkyl group, a substituted aryl group, or a substituted cycloalkyl group, wherein L2 may optionally be covalently bonded; Z1 and Z2 are each independently -O-, -S-, or optionally substituted heteroalkyl groups; and The number n ranges from approximately 2 to approximately 100,000.

[0144] In certain embodiments (e.g., of formula (VI)), R 4' and R 4'' are each independently an optionally substituted alkyl group. In other embodiments, L 1 and L 2 are each independently an optionally substituted alkyl group. In other embodiments, Z 1 and Z 2 are each independently -O- or -S-. In still other embodiments, Z 1 and Z 2 are -O-. In other embodiments, at least one of L 1, L 2, R 4', or R 4'' includes a metallic bonding portion (e.g., any of those described herein).

[0145] SRP may include poly(α-methylstyrene) or derivatives thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or includes a structure of formula (VII): or its salts, wherein: R2', R2'', and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; Ar is an optionally substituted aryl, optionally substituted alkyl, or optionally substituted aralkyl; and The number n ranges from approximately 2 to approximately 100,000. In other embodiments, at least one of Ar, R 2', R 2'', or R 3 includes a metallic bonding portion (e.g., any of those described herein).

[0146] SRPs may include poly(carbonate) or derivatives thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or includes the structure of formula (VIII): or its salts, wherein: L 1 is optionally substituted alkyl, optionally substituted heteroalkyl, optionally substituted aryl, or optionally substituted cycloalkyl; and The number n ranges from approximately 2 to approximately 100,000.

[0147] In certain embodiments (e.g., of formula (VIII)), L1 is an optionally substituted alkyl group, an optionally substituted heteroalkyl group, or an optionally substituted cycloalkyl group. In some embodiments, the optionally substituted heteroalkyl group is -X-Ak-X-, where X is an oxygen group and Ak is an optionally substituted alkyl group. In other embodiments, L1 includes a metal-bonded portion (e.g., any of those described herein). Non-limiting SRPs may include poly(vinyl carbonate), poly(propylene carbonate) (PPC), poly(butene carbonate) (PBC), poly(cyclohexene carbonate) (PCHC), poly(norbornene carbonate) (PNC), and poly(cyclohexene propylene carbonate) (PCPC).

[0148] The SRP may comprise poly(norbornene) or a derivative thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or comprises a structure of formula (IX): or its salts, wherein: R3 is H, an optional substituted alkyl, an optional substituted heteroalkyl, or an optional substituted aryl; and The number n ranges from approximately 2 to approximately 100,000. In other embodiments, R3 includes a metal bonding portion (e.g., any of those described herein).

[0149] SRPs may include poly(olefin) or derivatives thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or includes a structure of chemical formula (X): or its salts, wherein: R3 is H, an optional substituted alkyl, an optional substituted heteroalkyl, or an optional substituted aryl; and The number n ranges from approximately 2 to approximately 100,000.

[0150] In certain embodiments (e.g., of formula (X)), R3 is an optionally substituted heteroalkyl group, such as -OC(O)-RO1, -NRN1-C(O)-RO1, -OC(O)NRN1RN2, -(Ak-O)h1RO1, or -Ak-NRN1RN2, where Ak is an optionally substituted alkyl group, h1 is from 1 to 5, and RO1, RN1, and RN2 are each independently H or an optionally substituted alkyl group (e.g., hydroxyalkyl, carboxylalkyl, aminoalkyl, or azidealkyl). In other embodiments, R3 includes a metal-bonded portion (e.g., any of those described herein).

[0151] SRPs may include poly(glyoxylate) or derivatives thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or includes the structure of formula (XI): or its salts, wherein: R3 is H, an optional substituted alkyl, an optional substituted heteroalkyl, or an optional substituted aryl; and The number n ranges from approximately 2 to approximately 100,000.

[0152] In certain embodiments (e.g., of formula (XI)), R3 is an optionally substituted alkyl or optionally substituted heteroalkyl, such as -(Ak-O)h1RO1 or -Ak-NRN1RN2, where Ak is an optionally substituted alkyl group, h1 is from 1 to 5, and RO1, RN1, and RN2 are each independently H or optionally substituted alkyl. In other embodiments, R3 includes a metal-bonded portion (e.g., any of those described herein).

[0153] SRP may comprise poly(methyl methacrylate) or a derivative thereof, wherein the SRP may be a linear or cyclic polymer. In one embodiment, the SRP has or comprises a structure of formula (XII): or its salts, wherein: R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; and The number n ranges from approximately 2 to approximately 100,000.

[0154] In certain embodiments (e.g., of formula (XII)), R2 is an optionally substituted alkyl group. In other embodiments (e.g., of formula (XII)), R3 is an optionally substituted alkyl group or an optionally substituted heteroalkyl group, such as -(Ak-O)h1RO1 or -Ak-NRN1RN2, where Ak is an optionally substituted alkyl group, h1 is from 1 to 5, and RO1, RN1, and RN2 are each independently H or an optionally substituted alkyl group. In other embodiments, at least one of R2 or R3 includes a metal-bonded portion (e.g., any of those described herein).

[0155] As can be seen from chemical formulas (I) and (II), the SRP can be a polyaldehyde, including poly(phthalaldehyde), or a general polyaldehyde, including poly(formaldehyde), having a backbone composed of alternating carbon and oxygen atoms. The SRP can be a linear or cyclic polymer. The SRP can be poly(phthalaldehyde) or its derivatives, such as polymers comprising the structure of chemical formula (Ia): Or its salts, wherein R1, R2', R2'', r1, and n are any of those described herein. In some instances, n is an integer from 4 to 100,000. In other embodiments, at least one of R1, R2', or R2'' includes a metallic bonding portion (e.g., any of those described herein).

[0156] In other embodiments, the poly(phenylene phthalaldehyde) is cyclic. In some instances, the polymer has a structure with chemical formula (Ib) or (Ic): Or its salts, or any of the following described herein: R1, R5, R6, R2', R2'', R3', R3'', R4', R4'', Z1, Z2, Z3, Z4, Z5, Z6, r1, r5, r6, and n1. In some instances, n1 is an integer from 1 to 100. In other embodiments, at least one of R1, R5, R6, R2', R2'', R3', R3'', R4', or R4'' includes a metallic bonding portion (e.g., any described herein).

[0157] In any of the embodiments described herein (e.g., chemical formulas (I)-(VI) and (Ib)), Z1 to Z6, L1 and L2 (if present) are each independently selected from -CR2R3O-, -OCR2R3-, -OCR2R3O-, -(CR2R3S)h1CR2R3-, -S(CR2R3S)h1-, -CR2R3S-, -SCR2R3-, -SCR2R3S-, -(CR2R3S)h1CR2R3- and -S(CR2R3S)h1-, wherein R2 and R3 are each independently H, an optionally substituted alkyl or an optionally substituted aryl, and h1 is an integer from 1 to 5. In other embodiments, Z1 to Z6, L1 and L2 (if present) are each independently -O- or optionally substituted heteroalkyl.

[0158] In any of the embodiments described herein (e.g., chemical formulas (I)-(V), (VII) and (XII)), R2, R2' and R2'' (if present) are each independently H or optionally substituted alkyl (e.g., C1-6 alkyl).

[0159] In any of the embodiments described herein (e.g., chemical formulas (II), (III), (V), (VII), (IX), (X), (XI), and (XII)), R3 is an optional substituted aryl group.

[0160] In any of the embodiments described herein (e.g., chemical formulas (II), (III), (V), (VII), (IX), (X), (XI), and (XII)), R3 is an optional substituted heteroalkyl group, such as -OC(O)-RO1, -NR N1-C(O)-RO1, -OC(O)NR N1RN2, -(Ak-O)h1RO1, or -Ak-NR N1RN2, where Ak is an optional substituted alkyl group, h1 is from 1 to 5, and RO1, RN1, and RN2 are each independently H or an optional substituted alkyl group (e.g., hydroxyalkyl, carboxylalkyl, aminoalkyl, or azidealkyl).

[0161] In any embodiment herein, the polymer is a homopolymer or copolymer. The polymer may have a practical number of monomers, for example, n-series from about 2 to about 100,000 (e.g., about 2 to 50, 2 to 100, 2 to 200, 2 to 300, 2 to 400, 2 to 500, 2 to 1,000, 2 to 2000, 2 to 5,000, 2 to 10,000, 2 to 20,000, 2 to 50,000, 2 to 100,000, 3 to 50, 3 to 100, 3 to 200, 3 to 300, 3 to 400, 3 to 500, 3 to 1,000, 3 to 2,000, 3...). 3 to 5,000, 3 to 10,000, 3 to 20,000, 3 to 50,000, 3 to 100,000, 4 to 50, 4 to 100, 4 to 200, 4 to 300, 4 to 400, 4 to 500, 4 to 1,000, 4 to 2,000, 4 to 5,000, 4 to 10,000, 4 to 20,000, 4 to 50,000, 4 to 100,000, 5 to 50, 5 to 100, 5 to 200, 5 to 300, 5 to 400, 5 to 500, 5 to 1,000, 5 to 2,000, 5 to 5,000, 5 to 10,000, 5 to 20,000, 5 to 50,000, 5 to 100,000, 10 to 50, 10 to 100, 10 to 200, 10 to 300, 10 to 400, 10 to 500, 10 to 1,000, 10 to 2,000, 10 to 5,000, 10 to 10,000, 10 to 20,000, 10 to 50,000, 10 to 100,000, 50 to 100, 50 to 200, 50 to 300, 50 to 400, 10 to 500, 10 to 1,000, 50 to 100, 50 to 200, 50 to 300, 50 to 400, 10 to 500, 10 to 10 ... 50 to 200, 50 to 300, 50 to 400, 10 to 500, 10 to 200, 10 to 200, 10 to 500, 10 to 100,000, 50 to 100, 50 00, 50 to 500, 50 to 1,000, 50 to 2,000, 50 to 5,000, 50 to 10,000, 50 to 20,000, 50 to 50,000, 50 to 100,000, 100 to 200, 100 to 300, 100 to 400, 100 to 500, 100 to 1,000, 100 to 2,000, 100 to 5,000, 10 to 10,000, 100 to 20,000, 100 to 50,000, and 100 to 100,000). In other embodiments, the polymer system is cyclic, wherein n ranges from about 3 to about 100. In other embodiments, the cyclic polymer comprises any practical monomer number n1+2, for example, n1 ranges from about 1 to about 100.

[0162] In certain embodiments, the SRP may also be any suitable linear or cyclic copolymer, wherein the copolymer includes isomeric polymers of pure phthalaldehyde, isomeric polymers of poly(phthalaldehyde) derivatives (e.g., poly(4,5-dichlorophthalaldehyde)), or isomeric polymers of poly(aldehyde) derivatives. The SRP may include a copolymer having a structure comprising one of the chemical formulas (I)-(XII), (Ia), (Ib), (Ic) or their salts, and any copolymer described herein (e.g., one of the chemical formulas (XIII) or (XIV).

[0163] Further examples of SRP are provided below. In some embodiments, SRP comprises a copolymer of polyaldehyde. In particular embodiments, the copolymer may be a self-consuming polymer described in U.S. Patent Publication No. 2018 / 0155483, published June 7, 2018, the entire contents of which are incorporated herein by reference. Examples of copolymers in that document include copolymers having the chemical formula (XIII): (XIII) Wherein R is a substituted or unsubstituted C1-C20 alkyl, C1-C20 alkoxy, C2-C20 alkenyl, C2-C20 alkynyl, C6-C10 heteroaryl, C3-C10 cycloalkyl, C3-C10 cycloalkenyl, C3-C10 heterocycloalkyl, or C3-C10 heterocycloalkenyl; and when substituted, R is a C1-C20 alkyl, C1-C20 alkoxy, C2-C20 alkenyl, C2-C20 alkynyl, C6-C10 aryl, C6-C The 10 R groups are substituted with heteroaryl, formaldehyde, amino, sulfonic acid, sulfinic acid, fluoroacid, phosphonic acid, ether, halogen, hydroxyl, ketone, nitrogen, cyano, azide, silicon, sulfonylurea, sulfinyl, or thiol. In other embodiments, at least one R includes a metal bonding portion (e.g., any of those described herein).

[0164] In certain embodiments, SRP is a cyclic copolymer of a phthalaldehyde monomer with a second aldehyde (e.g., acetaldehyde, propionaldehyde, or butyraldehyde). Examples of such copolymers are given in U.S. Patent Publication No. 2018 / 015548 as chemical formula (XIV): (XIV) Where n is an integer from 1 to 100,000, and R can be any of those described herein (e.g., those described by chemical formula (XIII)). In other embodiments, at least one R includes a metallic bonding portion (e.g., any of those described herein).

[0165] Specific examples in U.S. Patent Publication No. 2018 / 015548 include copolymers of phthalaldehyde with one or more of the following: acetaldehyde, propionaldehyde, butyraldehyde, pentanaldehyde, hexanal, heptanaldehyde, octanaldehyde, nonanaldehyde, decanaldehyde, undecenaldehyde, acrolein, butenaldehyde, pentanaldehyde, hexenaldehyde, heptanaldehyde, octenaldehyde, nonanaldehyde, decenaldehyde, undecenaldehyde, and any combination thereof.

[0166] SRP can also be any suitable linear or cyclic copolymer, including pure phthalaldehyde isomeric polymers. SRP can also be isomeric polymers of polyphthalaldehyde derivatives, such as poly(4,5-dichlorophthalaldehyde).

[0167] In any embodiment herein, the SRP comprises a monomer having or having any of the following structures: (I)-(XIV), (Ia), or a salt thereof, wherein n is 1, and wherein the monomer system is then linked to another monomer via a linker. Non-limiting linkers include optionally substituted alkyl groups, optionally substituted heteroalkyl groups, optionally substituted alkyl(aryl)(alkyl), optionally substituted aryl, optionally substituted cycloalkyl, oxy, or thio groups. In other embodiments, the linker may be -Ak-, -Ak-X-, -X-Ak-, -(Ak-X)h1-Ak-, -X-(Ak-X)h1-, -Ak-Ar-, -Ak-Ar-Ak-, -Ar-Ak-, -(Ak-X)h1-Ar-(Ak-X)h1-, -Ar-(Ak-X)h1-, -X-(Ak-X)h1-Ar-, -X-(Ak-X)h1-Ar-X-(Ak-X)h1- and -Ar-X-(Ak-X)h1-, wherein Ak is an optionally substituted alkyl group, Ar is an optionally substituted aryl group, and X is or includes a non-carbon heteroatom (e.g., -O-, -S- or -NR N1-, wherein R N1 is H, optionally alkyl or optionally substituted aryl), and h1 is an integer from 1 to 5.

[0168] In any of the embodiments herein, the SRP may be an amorphous polymer that remains soluble in a solvent.

[0169] The SRP can be synthesized using any suitable monomer. For example, the monomer can be a structure having any of the chemical formulas (I)-(XIV), (Ia), or salts thereof, where n is 1. The monomer can have any useful terminal groups disposed at either end of the structure. In other embodiments, the monomer can be volatile and have a melting point below 20°C.

[0170] In a particular embodiment, the SRP is formed without any unwanted byproducts. Under this method, residue-free polymer vaporization can be achieved because no byproducts need to be removed. For removal, breaking one (or more) of the chemical bonds within the SRP would result in complete and rapid polymer depolymerization. Since all bonds are identical (without unintended impurities), minimal or no residue is expected.

[0171] The SRP or its formulation can be deposited by any practical method. For example, the SRP can be spin-coated or vapor-deposited. [Formulation, including solvents and additives] []

[0172] The SRP can be provided as a formulation having a solvent or a combination of solvents. In one embodiment, the formulation comprises about 0.1% to about 50% by weight of one or more SRPs (e.g., about 5% to 20% by weight), with the remainder being a solvent. Exemplary solvents include dimethyl ether diglyceride, tetrahydrofuran, N-methylpyrrolidone, dimethylformamide, propylene carbonate, cyclopentanone, anisole, dichlorobenzene, and propylene glycol methyl ether acetate.

[0173] The formulation may include one or more further additives selected from organic acids with a pKa greater than or equal to 1, photocatalysts (e.g., photoacid generators or photoalkali generators), thermal catalysts (e.g., thermal acid generators or thermal alkali generators), plasticizers, and / or dyes. The amount of additives may include a single additive from about 0.001% by weight to about 25% by weight, and a combination of additives from about 0.001% by weight to about 25% by weight.

[0174] In some embodiments, the SRP and the additive (e.g., any of those herein) may be formulated and stored as separate solutions, but may be mixed together during or relatively early deposition on the wafer. In some embodiments, the SRP and the additive may be provided as powders mixed in a solvent prior to spin coating. The SRP and the additive (alone or together) may be provided in a relative weight percentage of at least 5:1, or at least 10:1 or 20:1 SRP:additive.

[0175] Low-Tc polymers can be formulated with weak acids to produce films that are stable in their surrounding environment and exhibit accelerated degradation characteristics compared to pure, unformed polymers in solvents. Examples of specific acids exhibiting this behavior include weak organic acids (e.g., pKa greater than or equal to 1). Other acids include tartaric acid, oxalic acid, and acetic acid.

[0176] Other examples include linear alkyl carboxylic acids, CXH2XO2, where X is an integer, and corresponding dicarboxylic acid variants. Specific examples include formic acid (X=1) and acetic acid (X=2). Specific examples of dicarboxylic acids include oxalic acid and malonic acid. Organic weak acids may also be variants of any of these examples with additional alcohol substitution and / or unsaturated bonds. For example, oxoacetic acid, 2-hydroxyacetic acid, 2-propionic acid, 2-propynic acid, 2-hydroxymalonic acid, oxomalonic acid, 2,2-dihydroxymalonic acid, 2-oxopropionic acid, 2-hydroxypropionic acid, 3-hydroxypropionic acid, 2,3-dihydroxypropionic acid, etc., may be used.

[0177] Other organic acids can exhibit similar properties. Low-Tc polymers can be pre-formulated with suitable acids before tooling and then spin-coated onto a substrate for sacrificial support or surface protection applications. Alternatively, the low-Tc polymer and acid can be mixed at the point of use, during spin-coating. This method can be used to extend the shelf life of polymer formulations because, although the polymer formulation is stable in film form (solid state), it may be unstable in solution after contact with an acid. In some embodiments, the formulation provides approximately 5–20% by weight of SRP and <1% by weight of a weak organic acid, with the remainder being solvent.

[0178] The formulation (and the resulting membrane) may include a photoacid generator (PAG), wherein the SRP is exposed to electromagnetic radiation to generate acid. In this manner, high-energy light (e.g., UV, IR, or X-ray) exposure generates acid that promotes in-situ degradation of the membrane. Non-limiting photoacid generators include onium salts, such as monium and strontium salts having perfluorinated anions (e.g., diarylmonium and triarylstrontium salts), disulfonyldiazomethane compounds, N-sulfonyloxydicarboxylated amide compounds, and O-arylsulfonyloxime compounds. The photoacid generator may optionally include a photosensitizer (e.g., having a modified polyarylene hydrocarbon or a fused aromatic ring).

[0179] Other acid-generating agents can be used, such as thermal acid-generating agents that release acidic groups upon exposure to heat. In this manner, the depolymerization of the SRP may include both thermal and acidic treatment. Non-limiting thermal acid-generating agents include ammonium salts, sulfonyl esters, and acid amplifiers.

[0180] Plasticizers can be used to enhance the plasticity or flexibility of films. Non-limiting plasticizers may include adipates, alkyl dibenzoates, dialkyl phthalates, trialkyl trimellitate, tertiary amines, quaternary ammonium compounds, azelaate, citrate, ether-esters, polyethers, glutarate, diols, isobutyrate, maleic acid esters, phosphates, phosphonium compounds, organophosphates, sebacate, sulfonamides, strontium compounds, as well as ionic liquids, surfactants and acid enhancers, or combinations thereof. [SRP] [Removal] []

[0181] Several methods have been developed to achieve residue-free SRP removal without modifying the sensitive substrate. One method for depolymerizing the material involves exposing the polymer to elevated temperatures under vacuum conditions. This method allows the polymer to evaporate rapidly; however, it often leaves angstrom-level residues on the surface, consisting of carbon and residual monomers.

[0182] SRP can be removed using less aggressive triggers (e.g., light or mild temperatures). These sacrificial polymers allow for the protection of sensitive surfaces and subsequent removal of the barrier film without exposing those surfaces to aggressive plasma or wet chemical solutions. For some challenging applications, there may be limitations related to the temperature of the exposed substrate, extreme contamination, or production volume requirements. SRP and its films can be designed to meet these applications.

[0183] Non-limiting removal conditions also include exposure to acidic or basic vapors. These vapors may be provided by reactants, such as acids (e.g., pKa less than 7, and in some embodiments less than 4 or less than 2) or bases (e.g., pKb less than 7, and in some embodiments less than 4 or less than 2). Non-limiting reactants include sulfurous acid, formic acid, nitric acid, carbonic acid, or ammonium hydroxide.

[0184] Other unrestricted acid / base catalysts include hydrogen bromide (HBr), hydrogen chloride (HCl), hydrogen fluoride (HF), hydrogen iodide (HI), nitric acid (HNO₃), formic acid (CH₂O₂), acetic acid (CH₃COOH), formonitrile (HCN), sulfurous acid (H₂SO₃), carbonic acid (H₂CO₃), nitrous acid (HNO₂), or ammonia (NH₃), and methyl or ethylamine gas or vapor may be used. In some examples, when using HBr vapor, the substrate is maintained at a pressure ranging from 5 mTorr to 5000 mTorr and a temperature ranging from 0°C to 100°C. In some examples, the substrate is maintained at a pressure ranging from 750 mTorr to 1500 mTorr and a temperature ranging from 35°C to 70°C. In some examples, the substrate is maintained at a pressure of 1000 mTorr and a temperature of 60°C. The amount of acid vapor or vapor of other compounds is controlled to limit diffusion. Exposure time may depend on the strength of the acid or base, as well as the membrane thickness and the exposure temperature (e.g., from about 20°C to about 125°C, or from about 100°C to about 125°C). Unrestricted exposure times may include less than about 60 seconds, or in minutes.

[0185] In other embodiments, removal may include exposure to a two-reactant mixture, wherein the two-reactant mixture reacts to form an acid or base that can trigger the degradation of the SRP. This exposure is performed sequentially to provide more precise top-down control. In some embodiments, the method involves diffusing the compound or reactant that forms the compound only to the top portion of the SRP. The top portion is then degraded and removed, leaving undamaged remaining SRP. This exposure and removal cycle may be repeated. Optionally, a purging operation may follow the exposure operation to remove the compound or reactant from the chamber.

[0186] Non-limiting reactants (e.g., to form acids or bases) may include water vapor accompanied by ammonia (NH₃) or a gaseous oxide that reacts with water vapor to become an acidic or basic species. For example, NH₃ reacts with water to form ammonium hydroxide (NH₄OH). Examples of gaseous oxides include nitrogen dioxide (NO₂, which reacts with water to form nitric acid, HNO₃), sulfur dioxide (SO₂, which reacts with water to form sulfurous acid, H₂SO₃), and carbon dioxide (CO₂, which reacts with water to form carbonic acid, H₂CO₃). Other oxides may react with water or another reactant to form acids or bases.

[0187] Alternative polymer removal processes can provide lower levels of contamination. In one process, the polymer is exposed to long-lived metastable species from an inert gas plasma at elevated temperatures under vacuum. In another process, the polymer is exposed to infrared (IR) or ultraviolet (UV) radiation at elevated temperatures under vacuum. Other processes include a limited-time high-temperature exposure (e.g., from about 50°C to about 250°C) under vacuum conditions (e.g., <760°T). Another process may include simultaneous high-temperature exposure under vacuum and radiation exposure by either UV or IR. Yet another process may include simultaneous high-temperature exposure under vacuum and exposure to an inert gas metastable species. In certain embodiments, these removal processes also exhibit low contamination without increasing surface modification of the sensitive substrate.

[0188] Within the chamber, the substrate can be exposed to heat for SRP removal. Heat can be provided as a constant temperature hold. Alternatively, heat can be provided as a ramped temperature, where increasing or decreasing temperature rises and falls can be used between temperature holds. By providing heat at a temperature above Tc, this thermal energy provides sufficient energy to depolymerize the SRP. For SRP with Tc below 250°C, this condition may include exposure to temperatures up to 250°C, where the SRP kinetics are trapped below this Tc. In other embodiments, thermal exposure may include temperatures from about 50°C to about 250°C (e.g., about 50°C to 150°C, 50°C to 250°C, 150°C to 200°C, 150°C to 250°C, or 200°C to 250°C, etc.). In other embodiments, thermal exposure includes exposure to elevated temperatures with rapid rise and fall rates and short durations (e.g., up to 800°C). When using an additive (e.g., photoacid generator (PAG) or any of the additives described herein), the removal temperature may be between about 50°C and about 125°C, except for exposure to other stimuli that may help activate the additive (e.g., UV exposure to activate the PAG).

[0189] For basic thermal removal of surface protective films (e.g., providing the substrate on a heated plate), exposure times can range from about 20 seconds to about 400 seconds (e.g., about 30 to 300 seconds). Thicker films may require longer exposure times to heat to remove SRP compared to thinner films. The required film thickness will depend on the application. For example, some removal heat treatments (e.g., using a rapid thermal processor (RTP)) may involve very short periods of exposure at higher temperatures (e.g., above about 400°C) (e.g., 1 to 2 seconds for RTP systems and milliseconds for flash lamp-type treatments). For thermally budget-sensitive applications, RTP-type conditions may be used, while other treatments may use heated plates under vacuum.

[0190] Alternatively, the SRP can be removed under vacuum or non-vacuum conditions by exposure to radiation (e.g., UV or IR radiation). In some instances, treatment conditions include exposure to approximately 200°C under vacuum at a UV dose rate of approximately 2.5 W / cm². In other instances, treatment conditions (e.g., for SRPs used with photoacid generators) include exposure to approximately 110°C under vacuum at a UV dose rate of approximately 0.05 W / cm². In any of these treatment conditions, the exposure may range from approximately 100 seconds to approximately 400 seconds (e.g., approximately 300 seconds).

[0191] For radiation removal of surface protective films (e.g., pure SRP), exposure times can range from about 20 seconds to about 400 seconds (e.g., about 30 to 300 seconds). Thicker films may require longer exposure to radiation (e.g., UV) to remove SRP compared to thinner films. The required film thickness will depend on the application. For films containing acid-generating additives (e.g., PAG), exposure times can range from 2 minutes to 10 minutes. Exposure time can depend on many conditions, including additive loading, wafer temperature, UV dose rate, and film thickness. Therefore, these requirements will depend on the application (e.g., feature size, aspect ratio, pattern density, etc.).

[0192] For UV radiation, the dose can range, for example, from about 0.1 mW / cm² to about 15 W / cm². For collapse-sensitive applications where degradation rate control may be necessary, lower dose rates can be used, for example, from about 0.01 to about 0.07 mW / cm². For removing pure SRP film from a blanket-coated surface, higher dose rates can be used, for example, about 2.5 W / cm². Generally, higher dose rates result in cleaner removal. Of course, radiation exposure can also depend on the application, and excessive radiation can be avoided to reduce substrate damage.

[0193] During radiation exposure, the substrate can be maintained at elevated temperatures (e.g., from about 50°C to about 250°C, including about 200°C). When the formulation includes acid-generating additives (e.g., PAG), lower temperatures can be combined with UV exposure to provide a controlled degradation rate (e.g., a temperature range of about 50°C to about 125°C, or from about 100°C to about 110°C).

[0194] Metastable atoms can be used. These metastable atoms can be generated from an inert gas plasma to remove residues from the substrate; the inert gas is one or more of helium (He), neon (Ne), argon (Ar), krypton (Kr), and xenon (Xe). In some embodiments, the metastable species is non-chemically reactive and does not significantly affect the underlying surface. Metastable species from the inert gas plasma can effectively remove residues remaining after exposure to other stimuli, such as heat. In the methods described herein, removing SRP includes exposure to high-energy metastable species generated in an inert gas plasma at elevated temperatures. These metastable species have sufficient energy and lifetime to cleave bonds on the polymer or other residues. At temperatures above this upper limit, a strong thermodynamic driving force exists to revert to volatile monomers after bond cleavage. The metastable species is non-chemically reactive and does not significantly affect the underlying surface. The metastable species can effectively remove residues remaining after exposure to other stimuli, such as heat. This residue can be some SRP that has been polymerized or crosslinked and / or carbonized fragments, detectable by ellipsometry. While most SRP can be removed by the aforementioned stimuli, the residue may be difficult to remove completely by these methods. Not limited to any particular theory, the metastasizer can be removed by restarting the initiation process by severing chains that may have stopped prematurely due to byproduct formation, by disintegrating char that may have formed during depolymerization, and by assisting monomer desorption.

[0195] In some embodiments, most of the SRP is removed before exposing the substrate to metastable atoms. In some embodiments, the substrate is exposed to metastable atoms before most of the SRP is removed. In some embodiments, the plasma pressure is between about 10 mTorr and 10 Torr. In some embodiments, the plasma pressure is between about 100 mTorr and 1 Torr. In some embodiments, the SRP is provided as a protective coating on the substrate. In some embodiments, the plasma is generated in an inductively coupled plasma (ICP) source. In some of these embodiments, the ICP source is separated from the substrate by a spray head or other filter. In some embodiments, the plasma is generated in a capacitively coupled plasma (CCP) source. Any other type of plasma source can be used. In some embodiments, exposing the substrate to the stimulus and exposing the substrate to metastable atoms are performed in the same chamber.

[0196] The processing and plasma source chamber pressure can be used to control this plasma-based removal. Pressure is important for controlling the density of metastable atoms. If the pressure is too low, the density of metastable atoms may not be high enough to effectively clean the surface. If the pressure is too high, the metastable species may run rampant and cause collisions. Exemplary pressure ranges can be from 10 mTorr to 10 Torr, 100 mTorr to 1 Torr, 100 mTorr to 700 mTorr, 200 mTorr to 1 Torr, or 200 mTorr to 2 Torr.

[0197] Substrate temperature and plasma power can also be used to control removal. The temperature is sufficiently high, exceeding the upper limit temperature of the polymer. Higher temperatures facilitate removal at the maximum temperature limited by the thermal budget of the device or other materials on the substrate. Exemplary temperature ranges can be from 150°C to 1000°C or from 150°C to 250°C. Plasma power is sufficiently high to generate metastable atoms. Exemplary power ranges from 500 W to 5000 W or from 800 W to 5000 W, for example, 2500 W for a 300 mm wafer, and is linearly proportional to the substrate area. Exemplary exposure times range from 10 seconds to 300 seconds or from 10 seconds to 180 seconds.

[0198] Removal can be performed in a single step or multiple steps. Non-limiting methods may include providing a substrate with an SRP film. Then, a stimulus to degrade the SRP is pulsed in a chamber. This stimulus may include exposure to a compound (e.g., acid, base, acid- or base-forming compound, plasma, metastable compound, etc.) or a reaction environment (e.g., UV radiation, IR radiation, heat, etc.). In some embodiments, removal includes exposure to heat and / or radiation, thereby eliminating the need for plasma and / or harsh wet chemicals that would modify the sensitive surface to be protected.

[0199] When using compounds, the partial pressure and / or pulse duration of the vapor can be controlled to control the overall exposure and diffusion depth of the vapor. The chamber can be purged. Purging may involve evacuating the chamber and / or passing an inert gas to be purged through it. For example, the gas can be continuously flowed into the chamber, or the gas can be pulsed into the chamber itself. The volatile monomer or SRP fragment can be aspirated or purged out of the chamber, and this process can be repeated until the SRP is removed. As described above, in some embodiments, the SRP is sequentially exposed to the reactants in each cycle. This provides additional control over the process and can be implemented in various ways.

[0200] According to various embodiments, the reaction can be catalytic or uncatalytic. In some embodiments, a catalyst (e.g., a thermally activated catalyst) may be provided in the SRP, wherein the catalyst may be delivered using the reactants or introduced as a separate pulse. However, in many embodiments, the reaction is uncatalytic to provide a catalyst-free SRP. This facilitates the removal of the SRP. In some embodiments, the reaction is byproduct-free.

[0201] Additional examples of SRP and methods using SRP are described in U.S. Patent Nos. 9,466,511, 9,666,427, 10,008,396 and 10,068,781, the entire contents of which are incorporated herein by reference. [equipment] []

[0202] The metal features described herein can be formed using the electroplating or electrodeposition processes and equipment. Such electroplating or electrodeposition equipment can be used in conjunction with one or more additional substrate processing tools, said substrate processing tools being used to process the substrate, including depositing SRP, removing SRP, aligning the metal features, bonding the metal features, and other upstream and downstream processes. In other embodiments, the electroplating or electrodeposition equipment can be adapted to deposit SRP within a processing chamber, thereby capping the metal features after deposition.

[0203] Figure 7 shows an example of an electroplating tank suitable for electroplating. Typically, electroplating equipment includes one or more electroplating tanks in which substrates (e.g., wafers) are processed. Only one electroplating tank is shown in Figure 7 for clarity. To optimize bottom-up electroplating, additives (e.g., accelerators, inhibitors, and / or homogenizers) are added to the electrolyte; however, electrolytes containing additives may react with the anode in undesirable ways. Therefore, sometimes a permeable membrane is used to separate the anode and cathode regions of the electroplating tank, where different electroplating solutions of different compositions can be used. The electroplating solution located in the cathode region is called the cathodic electrolyte, and the electroplating solution in the anode region is called the anodic electrolyte. Multiple engineering designs can be used to guide the anodic and cathodic electrolytes into the electroplating equipment.

[0204] Please refer to Figure 7, which shows a schematic cross-sectional view of an electroplating apparatus 701 according to an embodiment. An electroplating bath 703 contains an electroplating solution (having the composition as described above), wherein the electroplating solution is shown located at layer 705. The cathode electrolyte portion of this container is adapted for receiving a substrate in the cathode electrolyte. A wafer 707 is immersed in the electroplating solution and held by a "clamshell" substrate holder 709 mounted on a rotatable mandrel 711, wherein the rotatable mandrel 711 allows the clamshell substrate holder 709 to rotate together with the wafer 707. A general description of a clamshell-type electroplating apparatus having a configuration suitable for use with the present invention is given in U.S. Patent Nos. 6,156,167 to Patton et al. and 6,800,187 to Reid et al., the entire contents of which are incorporated herein by reference.

[0205] The anode 713 is positioned below the wafer within the plating bath 703 and separated from the wafer area by a permeable membrane 715 (preferably an ion-selective membrane). For example, a Nafion™ cation exchange membrane (CEM) can be used. The area beneath the anode membrane is typically referred to as the "anode chamber." The ion-selective anode membrane 715 allows ion communication between the anode and cathode areas of the plating bath and prevents particles generated at the anode from entering and contaminating the wafer. The anode membrane is also useful for redistributing current flow during the plating process, thereby improving plating uniformity. A detailed description of suitable anode membranes is provided in U.S. Patents 6,126,798 and 6,569,299 to Reid et al., the entire contents of which are incorporated herein by reference. Ion exchange membranes (e.g., cation exchange membranes) are particularly suitable for these applications. These membranes are typically made of ionomerically polymerizable materials, such as perfluorinated copolymers containing sulfonates (e.g., Nafion™), sulfonated polyimides, and other materials known to those skilled in the art suitable for cation exchange. Examples of suitable Nafion™ membranes include N324 and N424 membranes available from DuPont de Nemours Co.

[0206] During electroplating, ions from the plating solution are deposited on the substrate. Metal ions must diffuse through the diffusion boundary layer and enter through-silicon vias (TSVs), openings, or other features. A typical method to facilitate diffusion is to provide convection of the plating solution via a pump 717. Alternatively, vibration or acoustic disturbance elements, as well as wafer rotation, can be used. For example, a vibration transducer 708 can be attached to a clamshell substrate holder 709.

[0207] The electroplating solution is continuously supplied to the electroplating bath 703 via a pump 717. Generally, the electroplating solution flows upwards through the anode membrane 715 and diffuser plate 719 to the center of the wafer 707, and then flows radially outwards to cover all parts of the wafer 707. The electroplating solution can also be supplied from the side of the electroplating bath 703 to the anode region of the bath. The electroplating solution then overflows from the electroplating bath 703 and reaches the overflow tank 721. Next, the electroplating solution is filtered (not shown) and returned to the pump 717 to complete the recycling of the electroplating solution. In some configurations of the electroplating tank, a distinct electrolyte circulates through the portion of the electroplating tank containing the anode, and a micropermeable membrane or ion-selective membrane is used to prevent mixing with the main electroplating solution.

[0208] The reference electrode 731 is located on the outside of the electroplating bath 703, within the separation chamber 733, which is replenished by overflow from the electroplating bath 703. Alternatively, in some embodiments, the reference electrode is disposed as close as possible to the substrate surface, and the reference electrode chamber is connected to the side of the wafer substrate via a capillary or other method, or is located directly beneath the wafer substrate. In some preferred embodiments, the device further includes contact sensing leads connected to the wafer periphery, and the contact sensing leads are configured to sense the potential of the metal seed layer at the wafer periphery, but do not carry any current to the wafer.

[0209] When electroplating requires a controlled potential, a reference electrode 731 is typically used. The reference electrode 731 can be one of various commonly used types, such as mercury / mercury sulfate, silver chloride, saturated calomel, or copper metal. In addition to the reference electrode, in some embodiments, contact sensing leads that are in direct contact with the wafer 707 can be used for more precise potential measurements (not shown).

[0210] DC power supply 735 can be used to control the current flow to wafer 707. Power supply 735 has a negative output lead 739 electrically connected to wafer 707 through one or more slip rings, brushes, and contacts (not shown). Positive output lead 741 of power supply 735 is electrically connected to anode 713 located in plating bath 703. Power supply 735, reference electrode 731, and contact sensing lead (not shown) can be connected to system controller 747, which, among other functions, allows regulation of the current and potential supplied to the components in the plating bath. For example, the controller may allow plating to be performed in a potential-controlled state and / or a current-controlled state. The controller may include program instructions specifying the current and voltage levels that must be applied to various components in the plating bath, and the time at which these levels must be changed. When a forward current is applied, power supply 735 biases wafer 707 to have a negative potential relative to anode 713. This causes current to flow from the anode 713 to the wafer 707, and generates an electrochemical reduction reaction (e.g., Cu²⁺ + 2e⁻ = Cu₀) on the wafer surface (cathode), resulting in the deposition of a conductive layer (e.g., copper) on the wafer surface. An inert anode 714 can be mounted below the wafer 707, within the electroplating bath 703, and separated from the wafer area by a transparent membrane 715.

[0211] The apparatus may also include a heater 745 for maintaining the temperature of the electroplating solution at a specific level. The electroplating solution can be used to transfer heat to other components of the electroplating bath. For example, when a wafer 707 is fed into the electroplating bath, the heater 745 and pump 717 can be turned on to circulate the electroplating solution through the electroplating apparatus 701 until the temperature throughout the apparatus becomes substantially uniform. In one embodiment, the heater is connected to a system controller 747. The system controller 747 may be connected to a thermocouple to receive feedback on the temperature of the electroplating solution within the electroplating apparatus and determine the need for additional heating.

[0212] The controller typically includes one or more memory devices and one or more processors. The processor may include a CPU or computer, analog and / or digital input / output connections, a stepper motor controller board, etc. In some embodiments, the controller controls all activities of the electroplating equipment. A non-transient machine-readable medium containing instructions for controlling the processing operations according to this embodiment may be coupled to the system controller.

[0213] In some embodiments, a user interface will be present in relation to the controller 747. The user interface may include a display screen, a graphical software display of the device and / or processing status, and user input devices such as pointing devices, keyboards, display screens, microphones, etc. The computer program code for controlling the electroplating process can be written in any known computer-readable programming language: for example, assembly language, C, C++, Pascal, Fortran, etc. The compiled object code or script is executed by a processor to perform the tasks specified in the program. An example of an electroplating apparatus that may be used according to the embodiments herein is the Lam Research Sabre tool. Electrodeposition can be performed on a plurality of components, which form a larger electrodeposition apparatus.

[0214] Figure 8 shows a top schematic of an exemplary electrodeposition apparatus. The electrodeposition apparatus 800 may include three separate electroplating modules 802, 804, and 806. The electrodeposition apparatus 800 may also include three separate modules 812, 814, and 816 configured for various processing operations, including those described herein. For example, in some embodiments, one or more of modules 812, 814, and 816 may be a spin rinse-dry (SRD) module. In other embodiments, one or more of modules 812, 814, and 816 may be a post-filled electrodeposition module (PEM), each configured to perform functions such as substrate edge removal, back-side etching, and acid cleaning after processing via one of the electroplating modules 802, 804, and 806. In another embodiment, one or more of modules 812, 814 and 816 may be configured to deposit SRP on the surface of a substrate after being processed by one of electroplating modules 802, 804 and 806.

[0215] The electrodeposition apparatus 800 includes a central electrodeposition chamber 824. The central electrodeposition chamber 824 is a chamber containing a chemical solution used as the electroplating solution in electroplating modules 802, 804, and 806. The electrodeposition apparatus 800 also includes a conditioning system 826 that stores and delivers additives used in the electroplating solution. A chemical dilution module 822 stores and mixes chemicals used as etchants. A filtration and extraction unit 828 filters the electroplating solution in the central electrodeposition chamber 824 and extracts it to the electroplating modules 802, 804, and 806.

[0216] System controller 830 provides the electronic and interface control necessary for operating electrodeposition apparatus 800. System controller 830 (which may include one or more physical or logic controllers) controls some or all of the properties of electrodeposition apparatus 800. Controller 830 typically includes one or more memory devices and one or more processors. The processor may include a central processing unit (CPU) or computer, analog and / or digital input / output connections, stepper motor controller boards, and other similar components. Instructions for carrying out the appropriate control operations described herein may be executed on the processor. These instructions may be stored in memory devices associated with system controller 830 or may be made available via a network. In some embodiments, system controller 830 executes system control software.

[0217] The system control software in the electrodeposition apparatus 800 may include a plurality of instructions for controlling: time, mixing of electrolyte components, inlet pressure, plating tank pressure, plating tank temperature, substrate temperature, current and potential applied to the substrate and any other electrodes, substrate position, substrate rotation, and other parameters for specific processes performed by the electrodeposition apparatus 800. The system control logic can be configured in any suitable manner. For example, subroutines or control objects of various processing tool components can be written to control the operation of the processing tool components required to perform various processing operations. The system control software can be coded in any suitable computer-readable programming language. The logic can also be implemented as hardware in a programmable logic device (e.g., FPGA), ASIC, or other suitable carrier.

[0218] In some embodiments, the system control logic includes a sequence of input / output control (IOC) instructions for controlling the various parameters described above. For example, each stage of the electroplating process may include one or more instructions executed by the system controller 830. Instructions for setting the processing conditions for the immersion process may be included in the corresponding immersion formulation stage. In some embodiments, the electroplating formulation stages may be arranged sequentially such that all instructions for the electroplating process stage are executed simultaneously with that process stage.

[0219] In some embodiments, control logic can be divided into various assemblies, such as programs or program segments. Examples of logic assemblies for this purpose include a substrate positioning assembly, an electrolyte composition control assembly, a pressure control assembly, a heater control assembly, and a potential / current power supply control program.

[0220] In some embodiments, a user interface may exist associated with the system controller 830. The user interface may include a display screen, an image software display of the device and / or processing conditions, and user input devices such as pointing devices, keyboards, touch screens, microphones, etc.

[0221] In some embodiments, the parameters adjusted by the system controller 830 may be related to processing conditions. Non-limiting examples include bath conditions (temperature, composition, and flow rate) at various stages, substrate position (rotation speed, linear (vertical) speed, angle from the horizontal), etc. These parameters are provided to the user in the form of a recipe, which can be input using a user interface.

[0222] Multiple signals for monitoring processing can be provided from various processing tool sensors via analog and / or digital input connectors of the system controller 830. These signals for controlling the processing can be output to the analog and digital output connectors of the processing tool. Non-limiting examples of processing tool sensors that can be monitored include mass flow controllers, pressure sensors (e.g., pressure gauges), thermocouples, optical position sensors, etc. Appropriately programmed feedback and control algorithms can be used with data from these sensors to maintain processing conditions.

[0223] An automated hand-off tool 840 selects a substrate from a substrate cassette (e.g., cassette 842 or cassette 844). Cassette 842 or 844 may be a front-opening wafer transfer cassette (FOUP). FOUPs are designed to securely and safely hold substrates in a controlled environment and allow substrates to be removed by tools equipped with appropriate loading ports and machine operating systems for processing or measurement. The automated tool 840 may use vacuum attachment or some other attachment mechanism to hold the substrate.

[0224] Automatic tool 840 can engage with wafer handling station 832, cassette 842 or 844, transfer station 850, or alignment device 848. Automatic tool 840 can access substrates from transfer station 850. Transfer station 850 can be a slot or location from which automatic tools 840 and 846 can transfer substrates, or transfer substrates to, the slot or location, without passing through alignment device 848. However, in some embodiments, alignment device 848 can be used to align automatic tool 846 with the substrate to ensure proper alignment of the substrate on automatic tool 846 for accurate delivery to the plating module. Automatic tool 846 can also deliver substrates to one of plating modules 802, 804, or 806, or to one of the three separate modules 812, 814, and 816 configured for various processing operations.

[0225] An example of the processing operation according to the above method is as follows: (1) electrodepositing copper or another material onto the substrate in electroplating module 804; (2) rinsing and drying the substrate in the SRD of module 812; and (3) removing the crystal edge in module 814. Another method includes: (1) electrodepositing copper or another material onto the substrate in electroplating module 804; (2) rinsing and drying the substrate in the SRD of module 812; and (3) depositing SRP onto the substrate in module 814. Yet another method includes: (1) electrodepositing copper or another material onto the substrate in electroplating module 804; (2) rinsing and drying the substrate in the SRD of module 812; (3) acid cleaning the substrate in module 814; and (4) depositing SRP onto the substrate in module 816.

[0226] An apparatus configured to allow efficient recycling of substrates through sequential electroplating, rinsing, drying, and PEM processing operations is practical for implementations used in manufacturing environments. To achieve this, module 812 can be configured as a rotary rinse-dryer and a die edge removal chamber. Using this module 812, the substrate will only need to be transferred between the electroplating module 804 and module 812 for copper electroplating and EBR operations. In some embodiments, the methods described herein will be implemented in a system including electroplating equipment and a stepper.

[0227] Figure 9 schematically illustrates an alternative embodiment of the electrodeposition apparatus 900. In this embodiment, the electrodeposition apparatus 900 has a set of plating tanks 907 arranged in pairs or multiple "double" configurations, each plating tank containing an electroplating bath. In addition to its inherent electroplating, the electrodeposition apparatus 900 can perform a variety of other electroplating-related processes and sub-steps, such as spin rinsing, spin drying, wet etching of metals and silicon, electrodeposition-free processes, pre-wetting and pre-chemical treatment, reduction, annealing, electro-etching and / or electro-polishing, photoresist stripping, and surface pre-activation. In Figure 9, the electrodeposition apparatus 900 is schematically shown as a top-down view, and only a single layer or "floor" is revealed in the figure. However, it will be readily understood by those skilled in the art to which this invention pertains that this apparatus (e.g., the Lam Sabre™ 3D tool) may have two or more layers "stacked" on top of each other, wherein each of these layers may have the same or different types of processing stations.

[0228] Referring again to Figure 9, the substrate 906 to be electroplated is typically fed to the electrodeposition apparatus 900 via a front-end loading FOUP 901. In this example, the substrate 906 is carried from the FOUP to the main substrate processing area of ​​the electrodeposition apparatus 900 by a front-end robot 902. This front-end robot 902 is driven by a spindle 903 to retract the substrate and move it from one station to another in multiple dimensions. In this example, two front-end accessible stations 904 and 908 are shown. Front-end accessible stations 904 and 908 may include, for example, a pretreatment station and a spin rinse-dry (SRD) station. Lateral movement between the sides of the front-end robot 902 is achieved using machine tracks 902a. Each of the substrates 906 may be held by a cup-shaped / cone-shaped assembly (not shown), which is driven by a spindle 903 connected to a motor (not shown), and the motor may be attached to a mounting bracket 909. Additionally, four "dual" plating tanks 907 are shown in this example, for a total of eight plating tanks 907. A system controller (not shown) may be coupled to the electrodeposition apparatus 900 to control some or all of the properties of the electrodeposition apparatus 900. The system controller may be programmed or otherwise configured to execute instructions according to the processes described earlier herein.

[0229] Figure 10 shows a simplified cross-sectional view of an electroplating apparatus. The apparatus includes an electroplating tank 1001, in which a substrate 1002 is located within a substrate holder 1003. The substrate holder 1003 is often referred to as a cup and supports the substrate 1002 at its periphery. An anode 1004 is located near the bottom of the electroplating tank 1001. The anode 1004 is separated from the substrate 1002 by a permeable membrane 1005, which is supported by a permeable membrane frame 1006. The permeable membrane frame 1006 is sometimes referred to as an anode chamber permeable membrane frame because it defines the top of the anode chamber that houses the anode. Furthermore, the anode 1004 is separated from the substrate 1002 by an ion-resistive element 1007. The ion-resistive element 1007 includes an opening that allows electrolyte to pass through the ion-resistive element 1007 and impact the substrate 1002. The front insert 1008 is located above the ion-resistance element 1007 and near the periphery of the substrate 1002. As shown, the front insert 1008 can be annular and can be non-uniformly oriented. The front insert 1008 is sometimes also referred to as a lateral flow restriction ring.

[0230] The anode chamber 1012 is located below the permeable membrane 1005 and is where the anode 1004 is located. The ion-resistance element manifold 1011 is located above the permeable membrane 1005 and below the ion-resistance element 1007. The inlet 1016 (which can be connected to the irrigation channel 1040) delivers cathodic solution to the ion-resistance element manifold 1011 and can rinse the permeable membrane 1005 during electroplating. In this example, the inlet 1016 and the irrigation channel 1040 are supplied with electrolyte through the cathodic solution inlet 1018. The lateral flow manifold 1010 is located above the ion-resistance element 1007 and below the substrate 1002. The height of the lateral flow manifold is considered to be the distance between the plane of the substrate 1002 and the plane of the ion-resistance element 1007 (excluding the rib 1015 on the upper surface of the ion-resistance element 1007, if present). In some cases, the lateral flow manifold may have a height between about 1 mm and 4 mm, or between about 0.5 mm and 15 mm. The side of the lateral flow manifold 1010 is defined by a front insert 1008, which is used to receive the lateral flow electrolyte within the lateral flow manifold 1010. A side inlet 1013 to the lateral flow manifold 1010 is provided in an orientationally opposite manner to a side inlet 1014 to the lateral flow manifold 1010. The side inlet 1013 and the side outlet 1014 may be formed at least partially by the front insert 1008.

[0231] As shown by the arrows in Figure 10, the electrolyte flows from the cathode liquid inlet 1018 through the side inlet 1013, into the transverse flow manifold 1010, and exits at the side outlet 1014. Alternatively, the electrolyte may flow through one or more inlets of the ion-resistive element manifold 1011 (e.g., inlets in the irrigation channel 1040 and / or other inlets), into the ion-resistive element manifold 1011, through the opening of the ion-resistive element 1007, into the transverse flow manifold 1010, and exit at the outlet 1014. After passing through the side outlet 1014, the electrolyte is splashed onto the weir wall 1009. The electrolyte can be recovered and recycled.

[0232] In some embodiments, the ion-resistive element 1007 approximates a nearly constant and uniform current source near the substrate (cathode), and is therefore referred to in some contexts as a high-resistance virtual anode (HRVA) or channel ion-resistive element (CIRP). Generally, the ion-resistive element 1007 is positioned near the wafer. Conversely, an anode, also close to the substrate, will be significantly less inclined to supply a nearly constant current to the wafer, instead supporting only a constant potential plane at the anode metal surface, thus allowing the current to be maximized while minimizing the net resistance from the anode plane to the termination (e.g., peripheral device contacts on the wafer). Therefore, while the ion-resistive element 1007 is referred to as a high-resistance virtual anode (HRVA), this does not imply that the two are electrochemically interchangeable. Under certain operating conditions, the ion-resistive element 1007 will be more closely and perhaps more preferably described as a virtual uniform current source, where the nearly constant current originates from various points on the upper plane of the ion-resistive element 1007.

[0233] In many, but not all, embodiments, the ion-resistive element 1007 includes a plurality of vias of micro-sized dimensions (typically less than 0.04”), which are spatially and ionically isolated from each other and do not form interconnecting channels within the body of the ion-resistive element. Such vias are often referred to as non-connecting vias. They typically extend in one dimension, which is often, but not necessarily, perpendicular to the plated surface of the wafer (in some embodiments, the non-connecting vias tend to be at an angle to the wafer, where the wafer is generally parallel to the front surface of the ion-resistive element). Typically, the vias are parallel to each other. Typically, the vias are arranged in a square array. At other times, the arrangement is in a biased spiral pattern. These vias differ from 3D porous networks (where the channels extend in three dimensions and form an interconnected via structure) because the vias reorganize ion currents and (in some cases) fluid flows parallel to the surfaces therein, and straighten the paths of both current and fluid flows toward the wafer surface. However, in some embodiments, this porous plate (with an interconnected via network) can be used as an ion-resistive element. When the distance from the top surface of the plate to the wafer is small (e.g., a gap of about 1 / 10 of the wafer radius, for example less than about 5 mm), the divergence of current and fluid flows is locally confined, transmitted, and aligned using the channels of the ion-resistive element.

[0234] One example of the ion-resistive element 1007 is a disk made of a solid, non-porous dielectric material (which is ionic and electrically resistive). This material is also chemically stable in the plating solution used. In some cases where the ion-resistive element 1007 is made of ceramic materials (e.g., mixtures of aluminum oxide, tin oxide, titanium oxide, or metal oxides) or plastic materials (e.g., polyethylene, polypropylene, polyvinylidene fluoride (PVDF), polytetrafluoroethylene, polysulphone, polyvinyl chloride (PVC), polycarbonate, etc.), it has non-connecting vias between approximately 6000 and 12000. In many embodiments, the ion-resistive element 1007 is co-elongated with the wafer (e.g., when using a 300mm wafer, the ion-resistive element 1007 has a diameter of approximately 300mm) and close to the wafer, for example, directly below the wafer in a wafer-facing plating apparatus. Preferably, the electroplated surface of the wafer is located within approximately 10 mm of the surface of the nearest ion-resistive element, more preferably within approximately 5 mm. Therefore, the top surface of the ion-resistive element 1007 can be flat or substantially flat. Typically, both the top and bottom surfaces of the ion-resistive element 1007 are flat or substantially flat. However, in several embodiments, the top surface of the ion-resistive element 1007 includes a series of linear ribs, as further described below.

[0235] As described above, the total ionic capacitance and flow resistance of plate 1007 depend on both the plate's thickness and total porosity (the area fraction through which flow can pass) and the size / diameter of the pores. Plates with lower porosity will have higher impingement flow rates and ionic capacitance. Comparing multiple plates with the same porosity, the one with smaller diameter 1-D pores (and therefore a larger number of 1-D pores) will have a more uniform current distribution on the wafer due to the presence of more independent current sources, and will also have a higher total pressure drop (high viscosity flow resistance), where the independent current sources act more like point sources that can spread across the same gap.

[0236] In some cases, approximately 1-10% of the ion-resistive element 1007 is the open area through which ion current can pass (and through which electrolyte can pass if no other element obstructs the opening). In a particular embodiment, approximately 2-5% of the ion-resistive element 1007 is the open area. In a particular example, the open area of ​​the ion-resistive element 1007 is approximately 3.2%, and the effective total open cross-sectional area is approximately 23 cm². In some embodiments, non-connected vias formed in the ion-resistive element 1007 have a diameter of approximately 0.01 to 0.08 inches. In some cases, the vias have a diameter of approximately 0.02 to 0.03 inches, or between approximately 0.03 and 0.06 inches. In various embodiments, the diameter of the vias is at most 0.2 times the gap distance between the ion-resistive element 1007 and the wafer. The vias are generally circular in cross-section, but this is not mandatory. Furthermore, for ease of construction, all vias in the ion-resistive element 1007 may have the same diameter. However, this is not always the case; the individual size and density of the holes can vary above the surface of the ion-resistive element as may be required by specific needs.

[0237] The ion-resistive element 1007 shown in Figure 10 includes a series of linear ribs 1015 extending into / out of the paper plane. Ribs 1015 are sometimes referred to as protrusions. Ribs 1015 are located on the top surface of the ion-resistive element 1007 and, in many cases, are oriented so that their length (e.g., their longest dimension) is perpendicular to the direction of the transverse electrolyte flow. In certain embodiments, ribs 1015 may be oriented so that their length is parallel to the direction of the transverse electrolyte flow. Ribs 1015 influence fluid flow and current distribution within the transverse flow manifold 1010. For example, the transverse flow of the electrolyte is largely confined to the region above the top surface of the ribs 1015, where high-speed transverse electrolyte flow occurs. In the region between adjacent ribs 1015, the upward current delivered through the ion-resistive element 1007 is redistributed and becomes more uniform before being delivered to the substrate surface.

[0238] In Figure 10, the direction of the transverse flow of electrolyte is from left to right (e.g., from side inlet 1013 to side outlet 1014), and the rib 1015 is oriented so that its length extends into / out of the paper surface. In some embodiments, the rib 1015 may have a width between about 0.5 mm and 1.5 mm, or between about 0.25 mm and 10 mm (measured from left to right in Figure 10). The rib 1015 may have a height between about 1.5 mm and 3.0 mm, or between about 0.25 mm and 7.0 mm (measured from top to bottom in Figure 10). The rib 1015 may have a height-to-width ratio (height / width) between about 5 / 1 to 2 / 1, or between about 7 / 1 to 1 / 7. The rib 1015 may have a pitch between about 10 mm and 30 mm, or between about 5 mm and 150 mm. Ribs 1015 may have a variable length extending across the surface of the ion-resistive element 1007 (measured in / out of the paper in FIG. 10). The distance between the upper surface of rib 1015 and the surface of substrate 1002 may be between about 1 mm and 4 mm, or between about 0.5 mm and 15 mm. Ribs 1015 may be provided at various locations in a region approximately co-linear with the substrate, as shown in FIG. 10. Channels / openings in the ion-resistive element 1007 may be located between adjacent ribs 1015, or may extend through ribs 1015 (in other words, ribs 1015 may or may not form channels). In some other embodiments, the ion-resistive element 1007 may have a flat upper surface (e.g., excluding ribs 1015). The electroplating apparatus shown in Figure 10, including the ion-resistive element with ribs at the top, is further described in U.S. Patent No. 9,523,155 entitled "ENHANCEMENT OF ELECTROLYTE HYDRODYNAMICS FOR EFFICIENT MASS TRANSFER DURING ELECTROPLATING", the entire contents of which are incorporated herein by reference.

[0239] Depending on the specific application requirements, the device may include various additional elements. In some cases, an edge flow element may be provided near the periphery of the substrate within the lateral flow manifold. The shape and position of the edge flow element may be designed to promote a high degree of electrolyte flow (e.g., lateral flow) near the substrate edge. In some embodiments, the edge flow element may be annular or arcuate and may be oriented uniformly or non-uniformly. The edge flow element is further described in U.S. Patent Application No. 14 / 924,124 (which was filed October 27, 2015, entitled "EDGE FLOW ELEMENT FOR ELECTROPLATING APPARATUS"), the entire contents of which are incorporated herein by reference.

[0240] In some cases, the device may include a sealing element that temporarily seals the transverse flow manifold. The sealing element may be annular or arc-shaped and may be located near the edge of the transverse flow manifold. An annular sealing element may seal the entire transverse flow manifold, while an arc-shaped sealing element may seal a portion of the transverse flow manifold (in some cases, leaving the side outlet open). During electroplating, the sealing element may be repeatedly engaged and disengaged to seal and unseal the transverse flow manifold. The sealing element may be engaged and disengaged by moving a substrate holder, an ion-resistance element, a front insert, or other parts of the device that engage with the sealing element. The sealing element and the method for regulating lateral flow are further described in the following U.S. patent applications, the entire contents of which are incorporated herein by reference: U.S. Patent Application No. 15 / 225,716, filed August 1, 2016, entitled "DYNAMIC MODULATION OF CROSS FLOW MANIFOLD DURING ELECTROPLATING" (which has been granted U.S. Patent No. 10,364,505); and U.S. Patent Application No. 15 / 161,081, filed May 20, 2016, entitled "DYNAMIC MODULATION OF CROSS FLOW MANIFOLD DURING ELECTROPLATING" (which has been granted U.S. Patent No. 10,233,556).

[0241] In various embodiments, one or more electrolyte nozzles may be provided to deliver additional electrolyte over the ion-resistive element. The electrolyte nozzle may deliver electrolyte to a location near the periphery of the substrate, or closer to the center of the substrate, or both. The electrolyte nozzle may be oriented in any location and may deliver lateral flow electrolyte, impinging electrolyte, or a combination thereof. The electrolyte nozzle is further described in U.S. Patent Application No. 15 / 455,011 (and published as U.S. Patent Application Publication No. 2018 / 0258546), filed March 9, 2017, entitled "ELECTROPLATING APPARATUS AND METHODS UTILIZING INDEPENDENT CONTROL OF IMPINGING ELECTROLYTE," the entire contents of which are incorporated herein by reference.

[0242] The described SRP removal process can be performed in a chamber, which may be part of a substrate processing system. This substrate processing system may further include one or more additional substrate processing tools for processing substrates (including SRP deposition and upstream and downstream processing). Referring now to FIG11, the substrate processing system 1100 includes one or more substrate processing tools 1102 (substrate processing tools 1102a and 1102b are shown for illustrative purposes), and a substrate storage area 1130 or other substrate storage device. Substrate processing tools 1102a and 1102b each include a plurality of processing chambers 1104a, 1104b, 1104c, etc. (collectively referred to as processing chamber 1104). By way of example only, each of these processing chambers 1104 may be configured to perform substrate processing. In some examples, the substrate may be loaded into one of the processing chambers 1104, processed, then moved to one or more of the other processing chambers 1104, and / or removed from the substrate processing system 1100 (e.g., if all chambers are subjected to the same processing).

[0243] The substrate to be processed is loaded into substrate processing tools 1102a and 1102b via the port of the loading station of the atmosphere-to-vacuum (ATV) transfer module 1108. In some examples, the ATV transfer module 408 includes an equipment front-end module (EFEM). The substrate is then transferred to one or more of the processing chambers 1104. For example, a transfer robot 1112 is configured to transfer the substrate from the loading station 1116 to the load lock chamber 1120. A vacuum transfer robot 1124 of the vacuum transfer module 1128 is configured to transfer the substrate from the load lock chamber 1120 to the various processing chambers 1104.

[0244] After processing in one or more of substrate processing tools 1102a and 1102b, the substrate can be transferred to the outside of the vacuum environment. For example, the substrate can be moved to a storage location (e.g., substrate storage area 1130). In other examples, the substrate can be moved directly from one substrate processing tool to another substrate processing tool for subsequent processing, or directly from substrate storage area 1130 to another substrate processing tool for subsequent processing.

[0245] Exposing a substrate to the surrounding environment can cause defects or otherwise negatively impact downstream processing. Before exposure to the environment, a sacrificial capping layer, including SRP, can be added to the metal features or substrate. In some examples, the coating of the sacrificial capping layer is performed in a substrate processing tool before transferring the substrate to a substrate storage area for storage or to another substrate processing tool, such as for thermocompression bonding. In other examples, the coating of the sacrificial capping layer is performed in another processing chamber (independent of the substrate processing tool).

[0246] The sacrificial capping layer is removed as described herein before further processing of the substrate (e.g., before bonding the metal features). For example, after the substrate has been stored in the substrate storage area 1130 for a period of time, or after processing in the substrate processing tool 1102a, it can be transferred to the substrate processing tool 1102b. The sacrificial capping layer can be removed in one of the processing chambers in the substrate processing tool 1102b, or in another processing chamber (unrelated to the substrate processing tool 1102b). In some embodiments, the sacrificial capping layer is removed in the load lock chamber 1120.

[0247] In some examples, the coating of the sacrificial capping layer is performed in a processing chamber within the same substrate processing tool (which performs electroplating or substrate processing) before exposure to the surrounding environment. Since the substrate processing tool operates under vacuum, exposure of the substrate to the surrounding environment is avoided. In some examples, the sacrificial layer is deposited after a wet cleaning or plasma processing step. In this case, oxides and residues can be removed via the wet cleaning or plasma processing step, and the sacrificial capping layer is deposited immediately before or after wafer drying. In some examples, this process is not performed under vacuum, but rather without exposing the dried, clean surface to the surrounding environment. In other examples, the substrate is transferred from the substrate processing tool to another processing chamber located outside the substrate processing tool where the sacrificial capping layer is applied. This method limits or reduces the time the substrate is exposed to the surrounding environment. Exposure is limited to the brief transfer from the substrate processing tool to the processing chamber where the sacrificial capping layer is applied. The substrate can be stored for a longer period without additional exposure to the surrounding environment.

[0248] Next, the sacrificial capping layer can be removed before subsequent processing. In some examples, the sacrificial capping layer is removed in a vacuum environment in another substrate processing tool before substrate processing is performed in the processing chamber of the same substrate processing tool. In other examples, the substrate is transferred to the processing chamber where the sacrificial capping layer has been removed, and then transferred to the substrate processing tool for subsequent processing. This method also limits the exposure of the surrounding environment between the processing chamber and the substrate processing tool or other environments. In one example, the sacrificial capping layer is formed immediately after etching, deposition, or other processing by exposing the substrate to small molecule vapors, causing them to condense on the surface. This can be done directly inside the tool performing the etching or deposition (e.g., substrate processing tool 1102a), and can be performed in the same processing chamber where etching or deposition is performed. The substrate is then carried to a next processing tool (e.g., substrate processing tool 1102b). Once the substrate is no longer exposed to the surrounding environment (e.g., carried in a vacuum or in an atmosphere purged with inert gas), the aforementioned vacuum and compounds, and other stimuli (in some cases), are applied to induce film degradation and remove it from the substrate. This can be done inside the aforementioned processing chamber (e.g., processing chamber 1104a of substrate processing tool 1102b).

[0249] The metal-to-metal bonding process described herein can be performed in a bonding chamber, which may be part of a substrate processing system. Alternatively, the metal-to-metal bonding tool may be located near a processing chamber for SRP removal, wherein a transfer channel, transfer chamber, and / or handling robot regulate the movement of the wafer from the SRP removal chamber to the bonding tool. The bonding tool or chamber may be configured to provide the bonding temperature or bonding pressure described herein. Non-limiting bonding tools and chambers include thermocompression bonding tools or other bonding platforms, such as the EVG®500 series bonding modules from EV Group (EV Group Europe & Asia / Pacific GmbH, Sankt Florian am Inn, Austria), the XBS200 platform or SB6 / 8 Gen2 platform from SÜSS MicroTec SE (Garching, Germany), the Esec series for die bonding and the Datacon series for die attachment (e.g., Datacon 8800 TC) from BE Semiconductor Industries NV (Duiven, Netherlands), and the Fineplacer series for bonding from Finetech GmbH & Co. KG (Berlin, Germany).

[0250] In various embodiments, the system controller is used to control processing conditions during processing, including SRP removal and / or metal bonding formation. The controller typically includes one or more memory devices and one or more processors. The processor may include a CPU or computer, analog and / or digital input / output connections, a stepper motor controller board, etc.

[0251] The controller manages all activities related to the removal of the device. The system controller executes system control software, which includes a set of instructions for controlling the timing of a specific process, gas mixing, chamber pressure, chamber temperature, wafer temperature, wafer chuck or pedestal position, plasma power, and other parameters. In some embodiments, other computer programs stored in memory associated with the controller may be used.

[0252] Typically, a user interface will exist associated with the controller. This user interface may include a display screen, an image software display of the device and / or processing conditions, and user input devices such as pointing devices, keyboards, touch screens, and microphones.

[0253] System control logic can be configured by any suitable method. Generally, this logic can be designed or configured in hardware and / or software. Control instructions for the drive circuitry can be hard-coded or provided as software. Instructions can be provided through "programming." This programming is understood to include hard-coded logic in any form of logic, including digital signal processors, application-specific integrated circuits, and other devices having specific algorithms implemented as hardware. Programming is also understood to include software or firmware instructions executable on a general-purpose processor. System control software can be encoded in any suitable computer-readable programming language.

[0254] The computer program code used to control reactant pulses, purge gas flow, and other processes in the processing sequence can be written in any well-known computer-readable programming language: such as Assembly Language, C, C++, Pascal, Fortran, etc. The compiled object code or script is executed by the processor to perform the tasks specified in the program. Alternatively, as mentioned above, the program code can be hard-coded.

[0255] The controller parameters relate to processing conditions, such as the composition and flow rate of the processed gas, temperature, pressure, substrate temperature, and plasma power. These parameters are provided to the user in the form of a formula and can be input via a user interface.

[0256] Signals used to monitor the processing can be provided via analog and / or digital input connectors of the system controller. Signals used to control the processing are output to the system's analog and digital output connectors.

[0257] System software can be designed or configured in many ways.

[0258] For example, various chamber component subroutines or control objects can be programmed to control the operation of the chamber components required to perform the deposition process according to the disclosed embodiments. Examples of programs or program portions for this purpose include substrate positioning codes, process gas control codes, pressure control codes, and heater control codes.

[0259] Figure 12 shows an example of a deposition chamber (e.g., for vapor-based deposition such as SRP). As shown, it illustrates an apparatus 1200 with a processing chamber 1202, which includes a cover 1208. The processing chamber 1202 may include a wafer transfer channel 1204 passing through one wall of the processing chamber 1202. The wafer transfer channel 1204 is sized to allow a substrate 1222 to pass through and enter the interior of the processing chamber 1202, whereby the substrate 1222 can be placed on a wafer support 1224. The wafer transfer channel 1204 may have a gate valve 1206 or a similar gate mechanism operable to seal or unseal the wafer transfer channel, thereby allowing the environment within the processing chamber 1202 to be isolated from the environment on the other side of the gate valve 1206. For example, the substrate 1222 may be provided to the processing chamber 1202 via a wafer handling robot adjacent to the transfer chamber. Such a transmission chamber may, for example, have a plurality of processing chambers 1202 arranged around its periphery, wherein each processing chamber 1202 is connected to the transmission chamber via a corresponding gate valve 1206.

[0260] The wafer support 1224 may include, for example, an electrostatic chuck (ESC) 1226, which can be used to provide a wafer support surface for supporting the substrate 1222. The ESC 1226 may include, for example, a base plate 1234 engaged with a top plate 1228, wherein the top plate 1228 is located on top of the base plate 1234. The top plate 1228 may be made of, for example, a ceramic material, and may embed several other components therein. In the illustrated example, the top plate 1228 has two discrete electronic systems embedded therein. One such system may be an electrostatic clamping electrode system having one or more clamping electrodes 1232, wherein the clamping electrodes 1232 can be used to generate a charge within the substrate 1222, causing the substrate 1222 to be attracted by the wafer support surface of the top plate 1228. In the embodiment of Figure 12, although two clamping electrodes 1232 are present to provide a bipolar electrostatic clamping system, some embodiments may use only a single clamping electrode 1232 to provide a unipolar electrostatic clamping system.

[0261] Other systems are thermal control systems that can be used to control the temperature of substrate 1222 during processing conditions. In Figure 12, this thermal control system is characterized by a plurality of region thermal control systems for four annular resistance heater tracks 1230a, 1230b, 1230c, and 1230d, wherein these annular resistance heater tracks are concentric and positioned below the clamping electrode 1232. In some embodiments, the central resistance heater track 1230a may fill a generally circular region, and each resistance heater track 1230a / b / c / d may follow a generally zigzag or otherwise meandering path within its respective annular region. Each resistance heater track 1230a / b / c / d can be independently controlled to provide various radial heating profiles within the top plate 1228; in some cases, such a four-region heating system can be controlled, for example, to maintain substrate 1022 with a temperature uniformity of ±0.5°C. Although the device 1200 of Figure 12 is characterized as a four-zone heating system in ESC 1226, other embodiments may use a single-zone heating system or a plurality of zone heating systems with more or fewer than four zones.

[0262] In some embodiments of the temperature control mechanism described above, a heat pump may be used instead of a resistance heating track. For example, in some embodiments, a Peltier junction, or other similar device that can be controlled to "draw" heat from one side to the other, may be used to replace or extend the resistance heater track. This mechanism may be used, for example, to draw heat from the top plate 1228 (and therefore from the substrate 1222) and direct it to the bottom plate 1234 and the heat exchange channel 1236, thereby allowing for faster and more efficient cooling of the substrate 1222 when needed.

[0263] ESC 1226 may also include a base plate 1234, which can be used to provide structural support for the underside of the top plate 1228 and can also serve as a heat dissipation system. For example, the base plate 1234 may include one or more heat exchange channels 1236 arranged in a generally dispersed pattern at various locations on the base plate 1234, such as following a zigzag, circular, or spiral pattern around the center of the base plate 1234. During use, a heat exchange medium (e.g., water, or an inert fluorinated liquid) can circulate through the heat exchange channels 1236. The flow rate and temperature of the heat exchange medium can be externally controlled to create specific heating or cooling behavior within the base plate 1234.

[0264] ESC 1226 may be supported, for example, by a wafer support housing 1242, which is connected to or supported by a wafer support pillar 1244. The wafer support pillar 1244 may have a routing channel 1248 or other pathway for routing cables, fluid flow conduits, and other devices to the underside of the base plate 1234 and / or the top plate 1228. For example, although not shown in FIG. 12, cables supplying power to the clamping electrode 1232 may be routed via the routing channel 1248, as may cables supplying power to the resistance heater tracks 1230a / b / c / d. Other cables (e.g., temperature sensor cables) may also be routed via the routing channel 1248 to locations within the wafer support 1224. In an embodiment with a temperature-controlled base plate 1234, the conduits that transfer the heat exchange medium to or from the base plate 1234 can also be routed via route channels 1248. To avoid excessive clutter, these cables and conduits are not shown in Figure 12, but it should be understood that they will still be present.

[0265] The device 1200 of Figure 12 also includes a wafer support z-actuator 1246, which provides movable support for the wafer support pillar 1244. The wafer support z-actuator 1246 can be actuated to move the wafer support pillar 1244 and the supported wafer support member 1224 vertically upward or downward within the reaction space 1220 of the processing chamber 1202, for example, up to several inches. When this is done, the gap distance X between the substrate 1222 and the bottom side of the spray head 1210 can be adjusted depending on various processing conditions.

[0266] In some embodiments, the wafer support 1224 may also include one or more edge rings for controlling and / or fine-tuning various processing conditions. In Figure 12, for example, an upper edge ring 1238 is provided on top of lower edge rings 1240a and 1240b, which are thus supported by the wafer support housing 1242 and a third lower edge ring 1240c. For example, the upper edge ring 1238 typically experiences the same processing environment as the substrate 1222, while the lower edge rings 1240a / b / c are typically shielded from this environment. Due to the increased exposure of the upper edge ring 1238, it may have a more limited lifespan than the lower edge rings 1240a / b / c and may require more frequent replacement or cleaning.

[0267] The apparatus 1200 may also include a system for removing process gases from the process chamber 1202 during or after processing. For example, the process chamber 1202 may include an annular gas chamber 1256 surrounding the wafer support pillar 1244. Therefore, the annular gas chamber 1256 may be in fluid communication with a vacuum pre-line 1252, which may, for example, be connected to a vacuum pump located below a subfloor beneath the apparatus 1200. A regulator valve 1254 may be provided between the vacuum pre-line 1252 and the process chamber 1202, and may be actuated to control the flow into the vacuum pre-line 1252. In some embodiments, a baffle 1250 may be provided to reduce the possibility of gradual flow non-uniformity in the reactants flowing over the entire substrate 1222, wherein the baffle 1250 is, for example, an annular plate or other structure that allows the airflow entering the annular gas chamber 1256 to be more uniformly distributed around the periphery of the wafer support pillar 1244.

[0268] As shown in the figure, the spray head 1210 is a dual-chamber spray head and includes a first chamber 1212 that provides processing gas via a first inlet 1216, and a second chamber 1214 that provides processing gas via a second inlet 1218. In some embodiments, the spray head 1210 has more than two chambers. In some instances, a single chamber is used to transport SRP into the reaction space 1220 of the processing chamber 1202. Each chamber may have a set of corresponding gas distribution ports, which are fluidly connected to the reaction space 1220 via a panel of the spray head 1210 (which is part of the spray head 1210 located between the lowermost chamber and the reaction space 1220).

[0269] The first inlet 1216 and the second inlet 1218 of the spray head 1210 may be supplied with processing gas via a gas supply system that may be configured to provide one or more SRPs as described herein.

[0270] A first valve manifold 1268a may be configured to supply SRP to a first inlet 1216, while a second valve manifold 1268b may be configured to supply another SRP or other reactant to a second inlet 1218. In this example, the first valve manifold 1268a may include, for example, a plurality of valves A1-A5. Valve A2 may be, for example, a three-way valve having a port fluidly connected to a first vaporizer 1272a, another port fluidly connected to a bypass line 1270a, and a third port fluidly connected to a port on another three-way valve A3. Similarly, valve A4 may be another three-way valve having a port fluidly connected to a second vaporizer 1272b, another port fluidly connected to a bypass line 1270a, and a third port fluidly connected to a port on another three-way valve A5. One of the other ports on valve A5 may be fluidly connected to the first inlet 1216, and the remaining ports on valve A5 may be fluidly connected to one of the remaining ports on valve A3. Therefore, the remaining ports on valve A3 may be fluidly connected to valve A1, which is fluidly positioned between valve A3 and a purge gas source 1274, wherein the purge gas source 1274 is, for example, nitrogen, argon, or other suitable inert gas (for SRP). In some embodiments, only the first valve manifold is used.

[0271] For the purposes of this disclosure, the term "fluid connection" is used to refer to volumes, chambers, orifices, etc., that can be connected to each other to form a fluid connection, just as the term "electrical connection" is used to refer to components that are connected to each other to form an electrical connection. When the term "fluid medium" is used, it refers to a component, volume, chamber, or orifice that is fluidly connected to at least two other components, volumes, chambers, or orifices such that fluid flowing from one of these other components, volumes, chambers, or orifices to the other or one of these other components, volumes, chambers, or orifices will first flow through the component of the "fluid medium" before reaching that other or one of these other components, volumes, chambers, or orifices. For example, if a pump system has fluid between a storage tank and an outlet, then fluid flowing from the storage tank to the outlet will first flow through the pump before reaching the outlet.

[0272] The first valve manifold 1268a may, for example, be controllable, allowing vapor from one or both of vaporizers 1272a and 1272b to flow into the processing chamber 1202, or to enter the vacuum pre-line 1252 via the first bypass line 1270a. The first valve manifold 1268a may also be controllable, allowing purge gas to flow from the purge gas source 1274 into the first inlet 1216.

[0273] For example, to allow steam from the first vaporizer 1272a to flow into the reaction space 1220, valve A2 can be actuated to allow steam from the first vaporizer 1272a to first flow into the first bypass path 1270a. This flow can be maintained for a period of time sufficient to allow the steam flow to reach steady-state flow conditions. After sufficient time (or, if using a flow meter, after its indicated flow rate has stabilized), valves A2, A3, and A5 can be actuated to direct steam from the first vaporizer 1272a to the first inlet. A similar operation can be performed using valves A4 and A5 to direct steam from the second vaporizer 1272b to the first inlet 1216. In some instances, it may be necessary to actuate valves A1, A3, and A5 to allow purge gas from the purge gas source 1274 to flow into the first inlet 1216 to purge one of the steam from the first gas chamber 1212. In some additional embodiments, it may be necessary to simultaneously introduce steam from one of the vaporizers 1272a and 1272b into the first inlet 1216 along with the gas flowing from the purge gas stream. This embodiment can be used to dilute the concentration of reactants contained in the steam.

[0274] It will be understood that the second valve manifold 1268b can be controlled in a similar manner (e.g., via control valves B1-B5) to supply steam from vaporizers 1272c and 1272d to the second inlet 1218 or to the second bypass line 1270b. It will be further understood that different manifold configurations can also be used, including a single-unit manifold, wherein the single-unit manifold includes multiple valves for controlling the flow of SRP or other reactants to the first inlet 1216 and the second inlet 1218.

[0275] As mentioned earlier, some devices 1200 may be characterized by a smaller number of steam sources, such as only two vaporizers 1272. In this case, the valve manifold 1268 may be modified to have a smaller number of valves, such as only valves A1-A3.

[0276] As described above, the apparatus can be configured to maintain a specific temperature profile within the processing chamber 1202, such as an apparatus 1200 used for dry deposition of films. In particular, this apparatus 1200 can be configured to maintain the substrate 1222 at a lower temperature, for example, 25°C to 50°C, which is lower than most configurations of the apparatus 1200 that are in direct contact with the SRP. Alternatively, the temperature of the configuration of the apparatus 1200 in direct contact with the SRP can be maintained at a higher level, sufficiently high to prevent vaporized reactants from condensing on the surface of the configuration. Simultaneously, the temperature of the substrate 1222 can be controlled at a level that promotes reactant condensation, or at least deposition, on the substrate 1222.

[0277] To provide such temperature control, various heating systems may be included within the device 1200. For example, the processing chamber 1202 may have a receptacle for receiving a cartridge heater 1258 (e.g., for a processing chamber 1202 having a generally cylindrical internal volume but a square or rectangular external shape), and vertical holes for receiving the cartridge heater 1258 may be drilled into the four corners of the housing of the chamber 1202. In some embodiments, a heater cover 1260 may be used to cover the spray head 1210, wherein the heater cover 1260 can be used to apply heat to the entire exposed upper surface of the spray head 1210, thereby maintaining a rising temperature of the spray head. Heating various gas lines used to guide vaporized reactants from the vaporizer 1272 to the spray head 1210 may also be beneficial. For example, a resistance heater may be wrapped around these gas lines and used to heat them to a higher temperature. As shown in Figure 12, all gas lines (including bypass line 1270) are heated as illustrated, and these gas lines may have SRP flowing through them. The only exception is the gas line from valve manifold 1268 to first inlet 1216 and second inlet 1218, which can be relatively short and can be indirectly heated by spray head 1210. Of course, these gas lines can even be actively heated if needed. In some embodiments, a heater can be provided near gate valve 1206 to similarly heat the gate valve.

[0278] The various operating systems of device 1200 can be controlled by controller 1284, which may include one or more processors 1286 and one or more memory devices 1288, which are interconnected and communicate with various systems and subsystems of device 1200 to provide control functions to these systems. For example, controller 1284 may be configured to control valves A1-A5 and B1-B5, various heaters 1258 and 1260, carburetor 1272, regulator valve 1254, gate valve 1206, wafer support z-actuator, etc.

[0279] Another feature that the device 1200 may include is shown in FIG. 13, which illustrates a close-up side cross-section and plan view of the substrate 1222 portion, the top plate 1228, and the upper edge ring 1238 of FIG. 12. As shown, in some embodiments, the substrate 1222 can be lifted away from most of the top plate 1228 by a plurality of small platforms 1276, which may be hollow bosses that protrude a short distance from the nominal upper surface of the top plate 1228 to provide a back clearance 1278 between the underside of the substrate 1222 and most of the top plate 1228. A circumferential wall feature 1277 may be provided at the periphery of the top plate 1228. The circumferential wall feature 1277 may extend around the overall circumference of the top plate 1228 and is nominally at the same height as the small platforms 1276. During processing, a general-purpose inert gas (e.g., helium) can flow into the back side gap 1278 via one or more gas ports 1282. This gas can then flow radially outward before reaching the circumferential wall feature 1277. This path then restricts this radial outward flow, trapping a higher-pressure region of gas between the substrate 1222 and the top plate 1228. Inert gas leaking through the circumferential wall 1277 can eventually escape through a radial gap 1280 between the outer edge of the substrate 1222 and a portion of the upper edge ring 1238. This gas protects the underside of the substrate 1222 from undesirable effects by the processing operation by preventing gas released from the spray head 1210 from reaching the underside of the substrate 1222. Simultaneously, the gas released into the back side gap 1278 region also enhances the thermal coupling between the substrate 1222 and the top plate 1228, allowing the top plate 1228 to heat or cool the substrate 1222 more efficiently. Due to the higher pressure provided by the circumferential wall, the gas in the region of the back gap 1278 can also have a higher density than the gas in the rest of the chamber, thus providing more efficient thermal coupling between the substrate 1222 and the top plate 1228.

[0280] The controller 1284 can be configured, for example, by executing computer-executable instructions to cause the device 100 to perform various operations consistent with the present disclosure provided above.

[0281] After depositing the SRP layer on the substrate 1222, the substrate 1222 can be transferred to one or more subsequent processing chambers or tools for additional operations (e.g., any of those described herein) as described above. Further deposition apparatus is described in International Patent Application No. PCT / US2020 / 038968, filed June 22, 2020, entitled "APPARATUS FOR PHOTORESIST DRY DEPOSITION," the entire contents of which are incorporated herein by reference.

[0282] Solvent- or liquid-based deposition can be performed using equipment with a liquid dispensing system and a heater. Figure 14 shows an example of the equipment, in which a rotating chuck 10 is designed to hold and rotate a wafer W of a predetermined diameter (e.g., 300 mm or 450 mm). The wafer W is held by a series of circular clamping pins 16, in this embodiment, there are six clamping pins 16. The pins 16 pass through openings in a transparent plate 25 made of quartz or sapphire. The plate 25 is secured to the chuck 10 by screws 26 and rotates with the chuck 10. When the wafer W is on the chuck, the wafer W is held above the plate 25 such that the lower surface of the wafer is parallel to the plate 25 and separated from it by a small gap.

[0283] A radiant heating assembly 50 is installed below the transparent plate 25, which will be described in more detail below.

[0284] The boom arm 30 is mounted adjacent to the chuck 10 and pivots about its drive motor 34. The arm 30 is supplied with a treatment and / or rinsing liquid system, which is discharged downwards via its discharge nozzle 32. The boom arm 30 is movable between a standby position shown by the solid line in FIG. 14 and a center position shown by the dashed line. Therefore, the discharge nozzle 32 can scan across the entire radius of the wafer W and distribute liquid onto the entire upward-facing surface of the wafer W as the wafer W is rotated by the chuck 10.

[0285] Referring now to Figure 15, the rotating chuck 10 is composed of a lower chuck body 12 and an upper chuck body 14, which are fastened together and have journals for rotation about a fixed central post 20. In this embodiment, the pins 16 and the transparent plate 25 also rotate with the chuck 10, as do the ring gear 18, which continuously meshes with each of the clamping pins 16 via gear teeth located at the base of these clamping pins 16. The ring gear 18 can also rotate relative to the chuck 10 to a limited extent, causing the pins 16 to rotate about their respective axes and moving the uppermost eccentric clamping portion between its open and closed positions in a manner known to the art.

[0286] The fixed post 20 is mounted on the machine frame 40 of the device as a stator 44, while the rotor 42 is fastened to the chuck body 12, wherein the stator 44 and the rotor 42 constitute a magnetic motor that drives the chuck 10 to rotate. Further details of the overall chuck structure are described, for example, in commonly owned U.S. Patent No. 9,245,777.

[0287] In this embodiment, the radiant heating assembly 50 is mounted on the fixed post 20 and therefore does not rotate, but is enclosed by a rotating structure comprising chucks including elements 25, 14, and 16. In this embodiment, the radiant heating assembly 50 includes a plurality of blue light-emitting diodes (LEDs) 51 mounted facing the transparent plate 25, and a controller 52 (e.g., an onboard controller (not shown) mounted on the underside of the heating assembly 50). The controller 52 controls the on / off state and power of the blue LEDs 51, and is also wirelessly connected to the motor 34 of the boom arm 30.

[0288] As shown in Figure 16, the radiant heating assembly 50 is made of an aluminum substrate, which is formed by an upper part 54 and a lower part 55 soldered together with copper. The aluminum substrate serves as a heat sink to prevent overheating of the structure below the blue LED element 51. A printed circuit board (PCB) 53 is mounted on top of the upper part 54, on which the traces for forming the LED element are formed, and the LED element 51 is mounted.

[0289] The onboard chip 56 is mounted on a printed circuit board 60, which is fastened to the lower side of the lower part 55. The wire 58 connecting the output pin of the onboard chip 56 to the input terminal of the trace formed on the PCB 53 is housed in a pocket 57, which passes through the aluminum substrates 53 and 54.

[0290] As shown in Figure 17, the PCB 53 of this embodiment is formed in four quadrants, which are joined together by connectors 59. The LED elements 51 are formed in groups of 16, i.e., the configuration of the onboard chips 56 and the connection from these chips to the PCB 53, accompanied by the onboard controller 52 allowing the LEDs to be independently powered in groups of as few as 16.

[0291] As shown in Figure 17, the LED 51 series is configured in 12 concentric circles, and the number of LEDs in each circle is a multiple of 16. Therefore, with the above configuration, each concentric circle can be independently controlled as a separate heating zone.

[0292] The blue LED 51 has maximum intensity at a wavelength of approximately 450 nm. Other radiation sources can be used, but it is preferred to use a source that emits radiation with maximum intensity in the wavelength range of 390 nm to 550 nm, and even more preferably in the wavelength range of 400 nm to 500 nm.

[0293] Although most of the radiation system of this wavelength characteristic is transmitted by plate 25, the same radiation system is significantly absorbed by the semiconductor material of wafer W, especially when wafer W is silicon.

[0294] This configuration allows for very rapid localized heating of the wafer W in a manner that vaporizes the rinsing fluid before a damaging meniscus can form. For example, each LED 51 can have a power consumption of 10W and provide 3W of optical power, which can be generated almost instantaneously. Additionally, when needed, the power supply to the selected LED 51 can be pulsed, for example, at 500Hz, in a manner known per se, to generate a smaller optical power for the selected LED 51.

[0295] Figures 18-19 show an alternative embodiment, wherein the chuck is located within a closed chamber 80 and is driven to rotate by a stator 72 located outside the chamber 80 by a magnetic annular rotor 70. The wafer W is held by a clamping element 71 protruding downward from the annular rotor 70.

[0296] As shown in Figure 19, the chamber 80 can be opened for loading and unloading of the wafer W. The heating assembly 50' is incorporated into the lower part of the housing 80 and is generally similar to the heating assembly described in relation to the previous embodiments, except that in this embodiment, the transparent plate 25' is fixed and does not rotate with the magnetic rotor 70.

[0297] Furthermore, in this embodiment, a series of fixed liquid dispensing nozzles 74, supplied via manifold 73, are provided instead of a radially movable liquid dispenser 30. The rinsing liquid can be continuously supplied to these nozzles 74, starting from the center and continuing to the periphery, approximating the dispensing action of the boom arm 30 in the previous embodiment. Therefore, in this case, the controller 52 will control the power supply to the selected group of LEDs 51 based on which nozzle 74 is dispensing liquid. Further devices and components are described in U.S. Patent No. 10,720,343 to Mui et al., entitled "METHOD AND APPARATUS FOR PROCESSING WAFER-SHAPED ARTICLES," the entire contents of which are incorporated herein by reference.

[0298] In some embodiments, the controller is part of a system, and the system may be part of the examples described above. This system may include semiconductor processing equipment, which includes one or more processing tools, one or more chambers, one or more processing platforms, and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems may be integrated with electronic components to control their operation before, during, and after processing semiconductor wafers or substrates. The electronic components may be referred to as a "controller," which controls various components or sub-components of one or more systems. Depending on processing requirements and / or system type, the controller may be programmed to control any of the processes disclosed herein, including the transport of processing gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid transport settings, positioning and operation settings, wafer transfer into and out of a tool and other transport tools and / or load chamber connected or coupled to a specific system.

[0299] In a broad sense, a controller can be defined as an electronic component having various integrated circuits, logic, memory, and / or software to receive instructions, send instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits may include a chip storing program instructions in firmware, a digital signal processor (DSP), a chip defined as an application-specific integrated circuit (ASIC), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). Program instructions may be instructions transmitted to the controller in various independent settings (or program files) to define operational parameters for performing specific steps on, or for, a semiconductor wafer, or on a system. In some embodiments, the operational parameters may be part of a recipe defined by a process engineer to complete one or more processing steps during the fabrication of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or wafer dies.

[0300] In some embodiments, the controller may be part of a computer, or coupled to a computer integrated and coupled to the system, or otherwise networked to the system, or a combination thereof. For example, the controller may reside in the "cloud," or be part of the FAB host computer system, allowing remote access to the board processing. The computer may enable remote access to the system to monitor the current progress of processing operations, view the history of past processing operations, view trends or performance metrics from multiple processing operations, change parameters of the current processing, set processing steps after the current processing, or start a new processing. In some examples, the remote computer (e.g., a server) may provide processing recipes to the system via a network, which may include a local area network or the Internet. The remote computer may include a user interface that allows input or programming of parameters and / or settings, which are then transmitted from the remote computer to the system. In some examples, the controller receives instructions in the form of data, wherein the instructions specify parameters used for each processing step to be performed during one or more operations. It should be understood that the parameters may be specific to the type of step to be performed and the type of tool the controller is configured to connect to or control. Therefore, as described above, the controller may be distributed, for example, by including one or more discrete controllers, which are networked together and operate toward a common purpose (e.g., the steps and control described herein). An example of a controller distributed for this purpose would be one or more integrated circuits located on a chamber, which are connected to one or more integrated circuits at a remote location (e.g., located at a platform layer or as part of a remote computer) and combined to control the processing on the chamber.

[0301] Without limitation, exemplary systems may include plasma etching chambers or modules, deposition chambers or modules, spin-wash chambers or modules, metal plating chambers or modules, cleaning chambers or modules, edge etching chambers or modules, physical vapor deposition (PVD) chambers or modules, chemical vapor deposition (CVD) chambers or modules, atomic layer deposition (ALD) chambers or modules, atomic layer etching (ALE) chambers or modules, ion implantation chambers or modules, orbital chambers or modules, and any other semiconductor processing systems that may be used in the processing and / or fabrication of semiconductor wafers.

[0302] As described above, depending on the one or more processing steps to be performed by the tool, the controller may be connected to one or more other tool circuits or modules, other tool components, clustered tools, other tool interfaces, adjacent tools, neighboring tools, tools distributed throughout the plant, main computer, another controller, or tools used in material handling to bring the substrate container into and out of the tool location and / or loading port of the semiconductor manufacturing plant.

[0303] The controller may include various programs. The substrate positioning program may include programming code for controlling chamber components used to load the substrate onto a base or chuck, and for controlling the spacing between the substrate and other components of the chamber (e.g., gas inlets and / or targets). The process gas control program may include coding for controlling gas composition, flow rate, pulse duration, and optionally for gas flow into the chamber. The pressure control program may include coding for controlling the pressure within the chamber, for example, by adjusting a throttle valve in the chamber's exhaust system. The heater control program may include coding for controlling the current to a heating unit used to heat the substrate. Alternatively, the heater control program may control the transfer of a heat transfer gas (e.g., helium) to the wafer. The plasma control program may control plasma power.

[0304] Examples of chamber sensors that can be monitored during removal include mass flow controllers, pressure sensors (e.g., pressure gauges), and thermocouples located in a base or chuck. Appropriately programmed feedback and control algorithms can be used with data from these sensors to maintain the desired processing conditions.

[0305] The preceding description pertains to implementations of the disclosed embodiments in single-chamber or multi-chamber semiconductor processing tools. The apparatus and processes described herein can be used in conjunction with photolithography tools or processes for, for example, processing or manufacturing semiconductor devices, displays, LEDs, optoelectronic panels, etc. Generally, while not essential, such tools / processes will be commonly used or performed in shared manufacturing facilities. Photolithography patterning of films typically includes some or all of the following steps, each provided by a number of feasible tools: (1) applying photoresist to a workpiece (i.e., substrate) using a spin coater or spray coater; (2) curing the photoresist using a heated plate, furnace, or UV curing tool; (3) exposing the photoresist to visible light, UV light, or X-ray using a tool such as a wafer stepper; (4) developing the photoresist to selectively remove it, thereby patterning the photoresist using a tool such as a wet stage; (5) transferring the photoresist pattern to the underlying film or workpiece using a dry or plasma-assisted etching tool; and (6) removing the photoresist using a tool such as an RF or microwave plasma photoresist stripper. [in conclusion] []

[0306] While some details have been described for clarity of understanding of the foregoing embodiments, it will be apparent that certain changes and modifications may be made within the scope of the appended claims. The embodiments disclosed herein may be practiced without some or all of these specific details. In other instances, conventional processing operations have not been described in detail to avoid unnecessarily obscuring the disclosed embodiments. Furthermore, although the disclosed embodiments will be described in conjunction with specific embodiments, it will be understood that the specific embodiments are not intended to limit the disclosed embodiments. It should be noted that many alternative methods exist for implementing the processes, systems, and apparatuses of the presented embodiments. Therefore, the presented embodiments are to be considered illustrative rather than restrictive, and the embodiments are not limited to the details given herein.

[0307] 10: Rotate the chuck 12:Lower chuck body 14: Upper chuck body 16: Clamping pin 18: Ring Gear 20: Fixed central column 25,25': Transparent panel 26: Screws 30: boom swing arm 32: Exhaust nozzle 34: Motor 40: Machine Frame 42: Rotor 44: Stator 50: Radiant heating components 50': Heating component 51: Light Emitting Diode (LED) 52: Controller 53: Printed Circuit Board (PCB) 54: Upper part 55:lower part 56: Onboard chip 57: Bag Section 58: Conductor 59: Connector 60: Printed Circuit Board 70: Annular rotor 71: Clamping element 72: Stator 73: manifold 74: Liquid dispensing nozzle 80: Closed chamber 100: Method 101: Operation 102: Align 103, 103a, 103b: Operations 110: Features of the sealed section 114: Metal Feature Section 116:Substrate 118: SRP layer 120: Second sealing feature 124: Second metal feature section 126:Substrate 128: SRP layer 130: Connected assembly 134: Metal Structure 201,202,203,204,205,206,207: Operations 210: First sealing feature 211: Seed layer / barrier layer 212: Patterned photoresist 213: Opening 213a: Metal-plated column 213b: Released metal column 214: Independent / isolated metal feature 216:Substrate 218: SRP layer 220: Second sealing feature 224: Second metal feature section 226:Substrate 228: SRP layer 230: Connected assembly 234: Metal Structure 240: First sealing feature 248: Non-uniform SRP layer 250: Second sealing feature 254: Metal Feature Section 256:Substrate 258: Non-uniform SRP layer 260: Connected assembly 264: Metal Structure 301, 302, 303, 304, 305, 306, 307, 308: Operations 310: First sealing feature 311: Seed layer / barrier layer 312: Patterned photoresist 313: Opening 313a: Metal-plated column 313b: Released metal column 314: Independent / isolated metal feature 315: Gap Filling Layer 316:Substrate 318: SRP layer 320: Second sealing feature 324: Second metal feature section 325: Gap Filler Layer 326: Second substrate 328: Second SRP layer 330: Connected assembly 334: Metal Structure 400: Method 401, 403, 405, 407, 409, 409a, 409b: Operations 420, 440, 460: Method 500: Methods 501, 502, 503, 504, 505, 507, 509: Operations 600: Method 601, 603, 604, 605, 607, 609: Operations 701: Electroplating Equipment 703: Electroplating Bath 705: Level 707: Wafer 708: Vibration transducer 709:Substrate holder 711: Mandrel 713: Anode 714: Inert Anode 715: Transmissive membrane / Anodic membrane 717: Pump 719: Diffuser Plate 721: Overflow Channel 731: Reference Electrode 733: Separated Chamber 735: DC Power Supply 739: Negative Output Lead 741: Positive output lead 745: Heater 747: System Controller 800: Electrodeposition equipment 802, 804, 806: Electroplating Module 812, 814, 816: Modules 822: Chemical Dilution Module 824: Central electrodeposition chamber 826: Adjustment System 828: Filtering and Extraction Unit 830: System Controller 832: Wafer Operation Station 840: Automatic Tools 842, 844: Box 846: Automatic Tools 848: Aligner 850: Transfer Station 900: Electrodeposition equipment 901: Front-end loading FOUP 902: Front-end robot 902a: Machine track 903: Mandrel 904: Front-end accessible site 906:Substrate 907: Electroplating bath 908: Front-end accessible site 909: Install bracket 1001: Electroplating bath 1002:Substrate 1003:Substrate holder 1004: Anode 1005: Permeable membrane 1006: Permeable membrane framework 1007: Ion resistance element 1008: Front Embedded Object 1009: Dam 1010: Lateral Flow Manifold 1011: Ion resistance element manifold 1012: Anode Chamber 1013, 1014: Side input ports 1015: Ribs 1016: Input Port 1018: Cathode liquid inlet 1040: Irrigation flume 1100: Substrate Processing System 1102a, 1102b: Substrate processing tools 1104, 1104a, 1104b, 1104c: Processing chambers 1108: Atmosphere-to-vacuum (ATV) transmission module 1112: Transmission Robot 1116: Loading Station 1120: Load Lock Chamber 1124: Vacuum Transfer Robot 1128: Vacuum Transfer Module 1130: Substrate Temporary Storage Area 1200: Equipment 1202: Processing Chamber 1204: Wafer Transfer Channel 1206: Gate Valve 1208: Cover part 1210: Sprayer Head 1212: First air chamber 1214: Second air chamber 1216: First Entrance 1218: Second Entrance 1220: Reaction space 1222:Substrate 1224: Wafer support 1226: Electrostatic Chuck (ESC) 1228: Top Slab 1230a~1230d: Trajectory of resistance heater 1232: Clamping Electrode 1234: Base Plate 1236: Heat exchange channel 1238: Upper edge ring 1240a~1240c: Lower edge ring 1242: Wafer support casing 1244: Wafer support pillar 1246: Wafer Support Z-Actuator 1248: Route Passage 1250: baffle 1252: Vacuum foreline 1254: Regulator valve 1256: Annular air chamber 1258: Cartridge heater 1260: Heater Cover 1268a: First valve manifold 1268b: Second valve manifold 1270a: First bypass route 1270b: Second bypass pipeline 1272a~1272d: Carburetor 1274: Purge gas source 1276: Small Platform 1277: Circumferential wall feature 1278: Dorsal gap 1280: Radial clearance 1282: Gas Port 1284: Controller 1286: Processor 1288: Memory device A1~A5, B1~B5: Valves W: Wafer

Claims

1. A method of using a temporary covering material, the method comprising: Aligning a first capped feature with a second capped feature, wherein each of the first capped feature and the second capped feature independently includes a stimulus-responsive polymer (SRP) layer disposed on the surface of a metal feature; and bonding the first capped feature and the second capped feature in an environment in which the SRP is removed and a metal-metal bond is formed between the metal features.

2. The method of using a temporary covering material as described in claim 1, wherein the SRP layer prevents oxidation of the metal feature.

3. The method of using a temporary covering material as described in any of claims 1 to 2, wherein the SRP layer has a thickness of about 10 nm to 10 µm.

4. The method of using a temporary covering material as described in any of claims 1 to 2, wherein the joining includes: The first capped feature and the second capped feature are exposed to the removal temperature for removing the SRP, thereby providing a plurality of exposed metal features; And to bring these exposed metal features into contact to form the metal-metal bond.

5. The method of using a temporary covering material as described in claim 4, wherein the removal temperature is from about 50°C to about 250°C.

6. The method of using a temporary covering material as claimed in claim 4, wherein the exposure includes the use of acidic vapors, heat, ultraviolet or vacuum ultraviolet light, plasma, metastable neutrals from inert gas plasma, or combinations thereof.

7. The method of using a temporary covering material as claimed in any of claims 1 to 2, wherein the bonding includes a bonding temperature from about 25°C to about 250°C.

8. A method of using a temporary covering material as claimed in any of claims 1 to 2, wherein the bonding includes using an inert atmosphere, a vacuum environment, a reducing gas, or ambient air.

9. The method of using a temporary covering material as described in any of claims 1 to 2, wherein the metallic feature includes copper (Cu), tin (Sn), silver (Ag), gold (Au), aluminum (Al), or an alloy thereof.

10. The method of using a temporary covering material as claimed in any of claims 1 to 2 further includes, prior to the alignment: (i) depositing a first SRP layer on the surface of the first metal feature to provide the first covered feature; and (ii) depositing a second SRP layer on the surface of the second metal feature to provide the second covered feature.

11. The method of using a temporary covering material as claimed in claim 10, wherein the first SRP layer is further deposited on the surface of the gap-filling layer surrounding the first metallic feature.

12. The method of using a temporary covering material as claimed in claim 11, wherein the second SRP layer is further deposited on the surface of the gap-filling layer surrounding the second metallic feature.

13. The method of using a temporary covering material as claimed in claim 10 further includes, prior to the deposition in (i) and / or (ii): pretreating the surfaces of the first metal feature and the second metal feature to clean the surfaces and / or remove the oxide layer.

14. The method of using a temporary covering material as claimed in claim 10, wherein the deposition in (i) and / or (ii) includes vapor-based or solvent-based deposition of the SRP.

15. A method of using a temporary covering material, the method comprising: A stimulus-responsive polymer (SRP) is deposited on the surface of a first metallic feature to form an SRP layer, thereby providing a first capped feature, wherein the first metallic feature includes electrical contacts, and wherein the SRP includes an upper temperature limit of less than about 300°C.

16. The method of using a temporary covering material as claimed in claim 15 further includes, after the deposition: removing the SRP layer to provide a first exposed metal feature; and contacting the first exposed metal feature with a second exposed metal feature to form a metal-metal bond between the exposed metal features.

17. A method of using a temporary covering material as described in any of claims 15 to 16, wherein the deposition includes vapor-based or solvent-based deposition of the SRP.

18. A method of using a temporary covering material as claimed in any of claims 15 to 16, wherein the removal includes exposing the SRP layer to heat, ultraviolet or vacuum ultraviolet light, metastable neutral substances from inert gas plasma, acidic vapors or alkaline vapors.

19. The method of using a temporary covering material as claimed in any of claims 15 to 16, wherein the SRP layer prevents oxidation of the first metal feature.

20. A method of using a temporary covering material as described in any of claims 15 to 16, wherein the SRP layer has a thickness of about 10 nm to 10 µm.

21. The method of using temporary covering material as described in claim 16 further includes: SRP is deposited on the surface of the second metal feature to form an SRP layer, thereby providing the second capped feature; And remove the SRP layer from the second covered feature to provide the second exposed metal feature.

22. The method of using temporary covering material as described in claim 21 further includes: Remove the SRP layer from the second covered feature to provide an exposed metal feature; And the first exposed metal feature and the second exposed metal feature are joined together to form a metal-metal joint.

23. The method of using a temporary covering material as claimed in any of claims 15 to 16, 21 and 22, wherein the electrical contact includes a protruding metal pillar, a bonding pad, a bump, a microbump, a metal contact surrounded by a dielectric, or an internal connector.

24. A method of using a temporary covering material, the method comprising: A stimulus-responsive polymer (SRP) is deposited on the surfaces of a first metal feature and a second metal feature to form an SRP layer, thereby providing a first capped feature and a second capped feature; the first capped feature and the second capped feature are aligned; the SRP layer is removed to provide a plurality of exposed metal features; and the exposed metal features are brought into contact to form a metal-metal bond between the exposed metal features.

25. The method of using a temporary covering material as described in claim 1 or 2, wherein the SRP includes an upper limit temperature of less than about 300°C.

26. The method of using a temporary covering material as described in claim 25, wherein the upper limit temperature is less than about 60°C.

27. The method of using a temporary covering material as claimed in claim 24, wherein the SRP further comprises an acid catalyst, an organic acid, a photoacid generator, or a thermal acid generator.

28. The method of using a temporary covering material as described in any of claims 1, 2, 15, 16, 21, 22 and 24, wherein the SRP further includes a metal bonding portion.

29. A method of using a temporary covering material as described in any of claims 1, 2, 15, 16, 21, 22, and 24, wherein the SRP comprises a structure of one of the chemical formulas (I)-(XII): , ... R1 is independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halogen; R2, R2', R2'', and R3 are independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; R4, R4', and R4'' are independently H or optionally substituted alkyl; Ar is optionally substituted aryl, optionally substituted alkyl, or optionally substituted aralkyl; L1 and L2 are independently covalent, optionally substituted alkylene, optionally substituted heteroalkylene, optionally substituted aryl, or optionally substituted cycloalkylene; Z1 and Z2 are independently -O-, -S-, -CR2R3O-, -OCR2R3O-, -OCR2R3-, -CR2R3S-, -SCR2R3S-, or -SCR2R3-; r1 is an integer from 1 to 4; and n is from about 3 to about 100,000; The SRP comprises a linear polymer or a cyclic polymer; and at least one of R1, R2, R2', R2'', R3, R4, R4', R4'', Ar, L1, L2, Z1 or Z2 further comprises a metal bonding portion.

30. A method of using a temporary covering material as described in any of claims 1, 2, 15, 16, 21, 22, and 24, wherein the SRP comprises a structure of chemical formula (Ia): or a salt thereof, wherein: R1 is each independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl or halogen; R2' and R2'' are each independently H, optionally substituted alkyl or optionally substituted aryl; r1 is an integer from 1 to 4; and n is from 4 to 100,000; and the SRP includes linear polymers or cyclic polymers.

31. A method of using a temporary covering material as described in any of claims 1, 2, 15, 16, 21, 22, and 24, wherein the SRP comprises a structure of chemical formula (Ib): or a salt thereof, wherein: R1, R5, and R6 are each independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halogen; R2', R2'', R3', R3'', R4', and R4'' are each independently H, optionally substituted alkyl, or optionally substituted aryl; Z1, Z2, Z3, Z4, Z5, and Z6 are each independently -O-, -S-, -CR2R3O-, -OCR2R3O-, -OCR2R3-, -CR2R3S-, -SCR2R3S-, or -SCR2R3-, wherein R2 and R3 are each independently H, optionally substituted alkyl, or optionally substituted aryl; r1, r5, and r6 are each independently an integer from 1 to 4; and n1 series from 1 to 100.

Citation Information

Patent Citations

  • Method of manufacturing a flexible substrate having metal wiring embedded therein,and flexible substrate manufactured by the method

    US20140000943A1