Ag alloy bonding wires for semiconductor devices

TWI945145BActive Publication Date: 2026-11-11NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
TW110138512
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-20
Filing Date
2021-10-18
Publication Date
2026-11-11
Estimated Expiration
2041-10-17

AI Technical Summary

Technical Problem

Existing Ag alloy bonding wires face challenges in achieving a consistent crimping shape for solder balls during high-density packaging, leading to issues like anisotropic deformation, reduced joint strength, and short circuits due to poor bonding reliability.

Method used

An Ag alloy bonding wire containing specific concentrations of Te, Bi, and Sb, optionally with Pd, Pt, or In, to enhance the crimping shape and bonding reliability by suppressing crystal grain growth and inhibiting intermetallic compound formation.

Benefits of technology

The Ag alloy wire achieves a crimping shape close to a true circle, preventing short circuits and ensuring maximum bonding area, while significantly improving bonding reliability in high-density packaging applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention provides a novel Ag alloy bonding wire for semiconductor devices, which exhibits excellent solder ball crimping shape required for solder ball bonding in high-density packaging. The Ag alloy bonding wire for semiconductor devices comprises an Ag alloy containing one or more elements selected from the group consisting of Te, Bi, and Sb, and satisfies at least one of the following conditions (1) to (3). (1) The concentration of Te is 5 to 500 at.ppm. (2) The concentration of Bi is 5–500 at.ppm. (3) The concentration of Sb is 5 to 1500 at.ppm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to an Ag alloy bonding wire for a semiconductor device. Furthermore, this invention relates to a semiconductor device comprising the Ag alloy bonding wire. [Previous Technology]

[0002] In a semiconductor device, electrodes formed on a semiconductor element are connected to external electrodes on a lead frame or substrate via bonding wires. The bonding wire connection process is completed by heating and melting the end of a metal wire by an electric arc, forming a free air ball (FAB) by surface tension, pressing the solder ball (hereinafter referred to as solder ball bonding) onto the electrode on the semiconductor element, forming a circuit, and then pressing the metal wire (hereinafter referred to as wedge bonding) onto the external electrode on the lead frame or substrate.

[0003] Gold (Au) is the mainstream material for bonding wires. However, in recent years, with the soaring price of Au, there has been active development of bonding wires using cheaper materials to replace Au. Copper (Cu) and silver (Ag) have been studied as low-cost alternatives to Au. Ag is considered a promising material for bonding wires due to its equal or higher conductivity than Au and its lower hardness than Cu (which reduces the likelihood of problems when connecting to electrodes). For example, Patent Documents 1 and 2 disclose Ag alloy metal wires containing Pt, Pd, and Au, and describe the good bonding reliability exhibited by these Ag alloy metal wires. [Prior Art Documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. Hei 11-288962 [Patent Document 2] Japanese Patent Application Publication No. 2012-169374 [Summary of the Invention]

[0005] [The problem the invention aims to solve]

[0006] In recent years, with the further advancements in the performance and miniaturization of semiconductor devices, there is a strong demand for bonding lines capable of handling high-density packaging. For the narrow-pitch connections required in high-density packaging, a technology is needed that can not only control the fineness of the lines and the formation of small solder balls, but also control the crimping shape of the solder balls during bonding. Problems related to the crimping shape of the solder balls include: during solder ball bonding, the solder balls deform into a petal shape, or the solder balls preferentially deform in the direction of ultrasonic application, resulting in anisotropic solder ball deformation (hereinafter also referred to as "abnormal shape defects"). Such abnormal shape defects can lead to defects such as reduced bonding strength due to insufficient ultrasonic transmission during solder ball bonding, and short circuits caused by contact between adjacent solder balls. Therefore, regarding the crimping shape of the solder balls, it is preferable to have a shape that is close to a perfect circle when viewed from directly above the electrode. In this respect, compared with Au or Cu metal wires, Ag metal wires are often inferior in the crimping shape of solder balls. Even with Ag alloy metal wires described in Patent Documents 1 and 2, the crimping shape sometimes becomes poor.

[0007] The objective of this invention is to provide a novel Ag alloy bonding wire for semiconductor devices, which exhibits excellent solder ball crimping shape required for solder ball bonding in high-density packaging. [Technical Means for Solving the Problem]

[0008] The inventors have conducted intensive research on the above-mentioned problems and found that the above-mentioned problems can be solved by a bonding wire having the following structure, thereby completing the present invention. That is, the present invention includes the following. [1] An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element"), and satisfying at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm (2) the concentration of Bi is 5 to 500 at.ppm (3) the concentration of Sb is 5 to 1500 at.ppm. [2] The Ag alloy bonding wire described in [1] further contains one or more elements selected from the group consisting of Pd, Pt, In and Ga (hereinafter referred to as "the second element"), and the total concentration of the second element is 0.05 to 3 at.%. [3] An Ag alloy bonding line as described in [1] or [2], wherein when the total concentration of the first element is set to x1 [at.%], the total concentration of one or more elements selected from the group consisting of Pd, Pt, In and Ga (the second element) is set to x2 [at.%], and the concentration of Ag is set to xAg [at.%], the total concentration of other elements obtained by the following formula (1) is less than 0.1 at%: Formula (1): 100 - (x1 + x2 + xAg) [at.%]. [4] An Ag alloy bonding line as described in any one of [1] to [3], wherein the remainder of the Ag alloy contains Ag and unavoidable impurities. [5] An Ag alloy bonding line as described in any one of [1] to [4], wherein the concentration of Sb in condition (3) is 900 to 1500 at.ppm. [6] An Ag alloy bonding wire as described in any one of [1] to [5], wherein the concentration of each element is determined by ICP (Inductively Coupled Plasma) emission spectroscopy or ICP mass spectrometry. [7] A semiconductor device comprising an Ag alloy bonding wire as described in any one of [1] to [6]. [Effects of the Invention]

[0009] According to the present invention, a novel Ag alloy bonding wire for semiconductor devices can be provided, which has excellent solder ball crimping shape for solder ball bonding required in high-density packaging.

Implementation Method

[0010] Hereinafter, the present invention will be described in detail according to preferred embodiments of the present invention.

[0011] [Ag alloy bonding wire for semiconductor devices] The Ag alloy bonding wire for semiconductor devices of the present invention (hereinafter also referred to as "metal wire of the present invention" or "metal wire") is characterized in that it comprises an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter also referred to as "the first element"), and satisfies at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm (2) the concentration of Bi is 5 to 500 at.ppm (3) the concentration of Sb is 5 to 1500 at.ppm

[0012] -Te, Bi, Sb (First Element)- The metal wire of the present invention comprises an Ag alloy containing one or more elements selected from the group consisting of Te, Bi, and Sb as the first element, and satisfying at least one of the following conditions: (1) the concentration of Te is 5 to 500 at.ppm, (2) the concentration of Bi is 5 to 500 at.ppm, and (3) the concentration of Sb is 5 to 1500 at.ppm. In this way, the metal wire of the present invention can reduce the anisotropy of solder ball deformation during solder ball bonding, achieving a near-perfectly spherical crimp shape. Although the detailed mechanism is not yet clear, it is believed that by causing these specific first elements to segregate at grain boundaries, etc., grain coarsening can be suppressed, thereby achieving a good crimp shape.

[0013] --Condition (1)-- Condition (1) relates to the concentration of Te in the metal wire. From the viewpoint of achieving a good crimp shape during solder ball bonding, the concentration of Te in the metal wire is 5 at.ppm or more, preferably 10 at.ppm or more, 20 at.ppm or more, 30 at.ppm or more, 40 at.ppm or more, or 50 at.ppm or more. In particular, if the concentration of Te in the metal wire is 50 at.ppm or more, an exceptionally good crimp shape can be achieved during small solder ball bonding, and therefore it is more suitable. The concentration of Te in the metal wire is more preferably 60 at.ppm or more, 70 at.ppm or more, or 80 at.ppm or more.

[0014] From the viewpoint of achieving a good FAB shape and thus a good crimping shape, the upper limit of the Te concentration in the metal wire is 500 at.ppm or less, preferably 480 at.ppm or less, 460 at.ppm or less, 450 at.ppm or less, 440 at.ppm or less, 420 at.ppm or less, or 400 at.ppm or less.

[0015] --Condition (2)-- Condition (2) concerns the concentration of Bi in the metal wire. From the viewpoint of achieving a good crimp shape during solder ball bonding, the concentration of Bi in the metal wire is 5 at.ppm or more, preferably 10 at.ppm or more, 20 at.ppm or more, 30 at.ppm or more, 40 at.ppm or more, or 50 at.ppm or more. In particular, if the concentration of Bi in the metal wire is 50 at.ppm or more, an exceptionally good crimp shape can be achieved during small solder ball bonding, and therefore it is more suitable. The concentration of Bi in the metal wire is more preferably 60 at.ppm or more, 70 at.ppm or more, or 80 at.ppm or more.

[0016] From the viewpoint of achieving a good FAB shape and thus a good crimping shape, the upper limit of the concentration of Bi in the metal wire is 500 at.ppm or less, preferably 480 at.ppm or less, 460 at.ppm or less, 450 at.ppm or less, 440 at.ppm or less, 420 at.ppm or less, or 400 at.ppm or less.

[0017] --Condition (3)-- Condition (3) relates to the concentration of Sb in the metal wire. From the viewpoint of achieving a good crimp shape during solder ball bonding, the concentration of Sb in the metal wire is 5 at.ppm or more, preferably 10 at.ppm or more, 20 at.ppm or more, 30 at.ppm or more, 40 at.ppm or more, or 50 at.ppm or more. In particular, if the concentration of Sb in the metal wire is 50 at.ppm or more, an exceptionally good crimp shape can be achieved during small solder ball bonding, and therefore it is more suitable. The concentration of Sb in the metal wire is more preferably 60 at.ppm or more, 70 at.ppm or more, 80 at.ppm or more, or 90 at.ppm or more. Furthermore, the concentration of Sb in the metal wire can also be set higher. For example, the concentration of Sb in the metal wire can be 900 at.ppm or higher, 920 at.ppm or higher, 940 at.ppm or higher, 950 at.ppm or higher, 960 at.ppm or higher, 980 at.ppm or higher, or 1000 at.ppm or higher. From the viewpoint of achieving a good FAB shape, and thus a good crimping shape, it is more appropriate to set the upper limit of the concentration of Te and Bi to 500 at.ppm or lower. However, it has been found that even with a higher concentration of Sb, a good FAB shape can be maintained. Therefore, in one embodiment, the concentration of Sb in condition (3) is 900 to 1500 at.ppm.

[0018] From the viewpoint of achieving a good FAB shape and thus a good crimping shape, the upper limit of the Sb concentration in the metal wire is 1500 at.ppm or less, preferably 1450 at.ppm or less, 1400 at.ppm or less, 1380 at.ppm or less, 1360 at.ppm or less, or 1350 at.ppm or less.

[0019] As described above, the metal wire of the present invention satisfies at least one of conditions (1) to (3). It may satisfy only one of conditions (1) to (3), or any two of conditions (1) to (3), or all of conditions (1) to (3).

[0020] In the metal wire of the present invention, from the viewpoint of achieving a good FAB shape and thus a good crimping shape, the total concentration of the first element is preferably 2000 at.ppm or less, more preferably 1800 at.ppm or less, and even more preferably 1700 at.ppm or less or 1600 at.ppm or less. There is no particular limitation on the lower limit of this total concentration, as long as at least one of the above conditions (1) to (3) is met.

[0021] - Pd, Pt, In, Ga (Second Element) - The metal wire of the present invention preferably contains one or more elements selected from the group consisting of Pd, Pt, In, and Ga as a second element. Thereby, the inventors have discovered that, in conjunction with the improved bonding shape during solder ball bonding resulting from the inclusion of the first element in a specific amount, the bonding reliability required in high-density packaging can be significantly improved, as described below.

[0022] It has been found that previous bonding wires using Ag exhibited worse bonding reliability than Au bonding wires. Specifically, in order to evaluate the bonding lifetime under actual semiconductor device operating conditions, bonding reliability assessments such as high-temperature placement tests and high-temperature and high-humidity tests have been conducted. It has been found that in bonding reliability assessments (especially high-temperature and high-humidity tests), the solder ball bonding lifetime of Ag bonding wires is worse than that of Au bonding wires. Furthermore, the high-temperature and high-humidity test (HAST) includes bHAST (Biased Highly Accelerated Stress Test) with applied bias voltage and uHAST (Un-biased High Accelerated Temperature and Humidity Stress Test) without applied bias voltage. However, applying bias voltage accelerates corrosion, therefore bHAST is a more stringent test than uHAST.

[0023] In the technologies described in Patent Documents 1 and 2 above, dopants such as Pd are added to improve the bonding reliability of Ag bonding wires. However, it has been found that in high-density packaging where small solder ball bonding is performed, sufficient bonding reliability is sometimes not achieved even when using this technology. Regarding this, when using metal wires with a wire diameter of ϕ15–25 μm, in normal bonding, solder balls with a diameter 1.7–2.0 times that of the metal wire are formed for bonding. In contrast, in high-density packaging applications, to cope with narrower pitch, solder balls with a diameter 1.5–1.6 times that of the metal wire are often formed for bonding, which is smaller than normal solder balls. In high-density packaging, since small solder ball bonding is performed in this manner, the bonding area becomes smaller, which further makes it difficult to ensure the bonding life of the solder ball bonding portion.

[0024] In contrast, the metal wire of the present invention, which contains an Ag alloy with a specific amount of the first element, can reduce the anisotropy of solder ball deformation during solder ball bonding, thereby achieving a near-circular crimp shape. This prevents short circuits caused by contact between adjacent solder balls, even in small solder ball bonding, and maximizes the area conducive to bonding. When the metal wire of the present invention further includes the aforementioned second element, the effects of including the first element in a specific amount and the improved bonding reliability brought about by including the second element are synergistically achieved, thereby stably achieving a near-circular crimp shape and significantly improving the bonding reliability required in high-density packaging.

[0025] From the viewpoint that the combination with the first element can significantly improve the bonding reliability required in high-density packaging, the metal wire of the present invention preferably contains, as described above, one or more elements selected from the group consisting of Pd, Pt, In, and Ga as the second element. The inventors have discovered that by including the aforementioned specific second element in the combination with the first element, a stable press-fit shape can be achieved, and bonding reliability can be improved. Although the detailed mechanism is not yet clear, it is believed that these specific second elements inhibit the growth of intermetallic compounds between Ag and electrode metals (such as Al) that cause corrosion at the bonding interface of the solder ball joint, thereby improving bonding reliability.

[0026] From the viewpoint that the combination with the first element can significantly improve the bonding reliability required in high-density packaging, the total concentration of the second element in the metal wire is preferably 0.05 at.% or more, more preferably 0.1 at.% or more, 0.2 at.% or more, 0.3 at.% or more, 0.4 at.% or more, 0.5 at.% or more, 0.6 at.% or more, 0.8 at.% or more, or 1 at.% or more. In particular, if the total concentration of the second element is 0.3 at.% or more, better bonding reliability can be achieved, and if it is 0.5 at.% or more, exceptionally good bonding reliability can be achieved, and therefore it is more suitable.

[0027] From the viewpoint of suppressing hardening of metal lines and thus suppressing wafer damage, the upper limit of the total concentration of the second element in the metal lines is preferably 3 at.% or less, more preferably 2.9 at.% or less, 2.8 at.% or less, 2.7 at.% or less, 2.6 at.% or less, or 2.5 at.% or less. By containing the second element in combination with the first element, the metal lines of the present invention can improve the bonding reliability required in high-density packaging without excessively increasing the amount of the second element added.

[0028] Therefore, in a preferred embodiment, the metal wire of the present invention further contains one or more elements selected from the group consisting of Pd, Pt, In and Ga ("second element"), and the total concentration of the second element is 0.05 to 3 at.%.

[0029] In the metal wire of the present invention, the second element may contain one or more of Pd, Pt, In and Ga, or may contain all four elements, any three or two elements, or only one element.

[0030] In one embodiment, the metal wire of the present invention substantially contains only one of the elements Pd, Pt, In, and Ga in the second element. Here, "substantially contains only one of the elements Pd, Pt, In, and Ga" means that it contains any one of the elements Pd, Pt, In, and Ga, and the concentrations of the other three elements are each below 50 at.ppm. In this case, the concentrations of the other three elements can also be below 40 at.ppm, below 30 at.ppm, below 20 at.ppm, and below 10 at.ppm, respectively.

[0031] When Pd is contained as the second element, the concentration of Pd in ​​the metal wire is not particularly limited, as long as the preferred value of the total concentration mentioned above is met in relation to the concentrations of Pt, In and Ga, for example, it can be less than 1 at.%, less than 1 at.%, less than 0.8 at.%, less than 0.8 at.%, less than 0.75 at.%, or less than 0.7 at.%.

[0032] When Pt is contained as the second element, the concentration of Pt in the metal wire is not particularly limited, as long as the preferred value of the total concentration mentioned above is satisfied in relation to the concentrations of Pt, In and Ga, for example, it can be 0.4 at.% or more, 0.45 at.% or more, 0.5 at.% or more, 0.55 at.% or more, or 0.6 at.% or more.

[0033] When In is contained as the second element, there is no particular limitation on the concentration of In in the metal wire, as long as the preferred value of the total concentration mentioned above is met in relation to the concentrations of Pd, Pt and Ga, for example, it can be 0.03 at.% (300 at.ppm) or more, 0.035 at.% or more, 0.04 at.% or more, 0.045 at.% or more, or 0.05 at.% or more.

[0034] When Ga is contained as the second element, the concentration of Ga in the metal wire is not particularly limited, as long as the preferred value of the total concentration mentioned above is satisfied in relation to the concentrations of Pd, Pt and In, for example, it can be 0.3 at.% or more, 0.35 at.% or more, 0.4 at.% or more, 0.45 at.% or more, or 0.5 at.% or more.

[0035] The metal wire of the present invention comprises an Ag alloy, which contains a first element in a specific amount and, if necessary, also contains the aforementioned second element. The remainder of the Ag alloy contains Ag. From the viewpoint of better enjoying the effects of the present invention, the concentration of Ag in the metal wire relative to the entire metal wire is preferably 95 at.% or more, more preferably 96 at.% or more, 96.5 at.% or more, 96.6 at.% or more, 96.7 at.% or more, or 96.8 at.% or more.

[0036] Without impairing the effects of the present invention, the metal wire of the present invention may further contain elements other than the first element, the second element and Ag (hereinafter also referred to as "other elements"). The total concentration of other elements in the metal wire is not particularly limited, as long as it is within the range that does not impair the effects of the present invention. The total concentration of other elements may be, for example, 0.5 at.% or less. Therefore, when the total concentration of the first element is set as x1 [at.%], the total concentration of the second element is set as x2 [at.%], and the concentration of Ag is set as xAg [at.%], the total concentration of other elements obtained by the following formula (1) may be 0.5 at.% or less, Formula (1): 100-(x1+x2+xAg)[at.%].

[0037] The total concentration of elements other than element 1, element 2, and Ag can be lower, for example, below 0.4 at.%, below 0.3 at.%, below 0.2 at.%, below 0.15 at.%, below 0.1 at.%, below 0.08 at.%, below 0.06 at.%, below 0.05 at.%, below 0.04 at.%, below 0.02 at.%, or below 0.011 at.% or 0.01 at.%. There is no particular limitation on the lower limit of the total concentration of other elements, and it can be 0 at.%.

[0038] For example, when Ca and rare earth elements are included as other elements, the total concentration of Ca and rare earth elements in the metal wire may not reach 20 at.ppm. The total concentration of Ca and rare earth elements in the metal wire may be even lower, for example, below 18 at.ppm, below 16 at.ppm, below 15 at.ppm, below 14 at.ppm, below 12 at.ppm, below 10 at.ppm, below 8 at.ppm, below 6 at.ppm, or below 5 at.ppm. There is no particular limitation on the lower limit of this total concentration, and it may be 0 at.ppm.

[0039] In a preferred embodiment, the metal wire of the present invention comprises an Ag alloy, the Ag alloy comprising a first element and a second element, and the remainder comprising Ag and unavoidable impurities.

[0040] The concentrations of the first element, the second element, or other elements contained in the metal wire of the present invention can be detected by dissolving the metal wire in a strong acid, and then analyzing the resulting liquid using an ICP emission spectrometer or an ICP mass spectrometer to detect the concentrations of the elements contained in the entire metal wire. The concentrations of each element shown in the present invention are based on concentrations measured by ICP emission spectrometry or ICP mass spectrometry.

[0041] Preferably, the metal wire of the present invention does not have a coating with metals other than Ag as the main component. Therefore, in a preferred embodiment, the metal wire of the present invention does not have a coating with metals other than Ag as the main component. Here, "coating with metals other than Ag as the main component" means a coating with the content of metals other than Ag being 50 at.% or more.

[0042] The diameter of the metal wire of the present invention is not particularly limited, and can be appropriately determined according to the specific purpose. It is preferably 15 μm or more, 18 μm or more, or 20 μm or more. The upper limit of the diameter is not particularly limited, for example, it can be less than 100 μm, less than 90 μm, or less than 80 μm.

[0043] <Method for manufacturing metal wire> An example of a method for manufacturing Ag alloy bonding wire for semiconductor devices of the present invention will be described.

[0044] Prepare raw material Ag with a purity of 3 N to 5 N (99.9 to 99.999% by mass). Then, weigh the raw material Ag, the first element, the second element, and the other elements as starting materials, in such a way that the concentration of the first element (and the concentration of the second element and other elements in the case of containing the second element and other elements) is within the above-mentioned specific range, and melt and mix them to obtain an Ag alloy. Alternatively, a master alloy containing the first element, the second element, and the other elements can be used as raw materials. The Ag alloy is processed into a large diameter by continuous casting, and then thinned to the final wire diameter by wire drawing.

[0045] Wire drawing can be performed using a continuous wire drawing device capable of setting up a plurality of diamond-coated eyelets. If necessary, pickling can be performed before wire drawing, or heat treatment can be performed during wire drawing.

[0046] After wire drawing, a final heat treatment is performed. For the final heat treatment temperature, for example, with a fixed wire feeding speed, only the furnace temperature is varied. The heat treatment temperature is determined by confirming the elongation at break of the heat-treated metal wire and ensuring that this elongation at break is within a specific range. The heat treatment temperature can be, for example, in the range of 200–700°C. The heat treatment time is preferably set to 10 seconds or less (preferably 5 seconds or less, 4 seconds or less, or 3 seconds or less). For the heat treatment atmosphere, inert gases such as nitrogen or argon, or inert gases containing hydrogen such as constituent gases (5% H2-N2), can be used.

[0047] The metal wire of the present invention can be used in the manufacture of semiconductor devices to connect a first electrode on a semiconductor element to a second electrode on a lead frame or circuit board. The first connection (1st bonding) to the first electrode on the semiconductor element can be a solder ball bonding, and the second connection (2nd bonding) to the electrode on the lead frame or circuit board can be a wedge bonding. In solder ball bonding, the end of the metal wire is heated and melted by electric arc heating, and a solder ball (FAB) is formed by surface tension. Then, the solder ball is bonded to the electrode of the heated semiconductor element by applying ultrasonic waves and pressure. In wedge bonding, no solder ball is formed. The metal wire is pressed onto the electrode by applying heat, ultrasonic waves, and pressure. The metal wire of the present invention, which contains an Ag alloy containing a specific amount of the first element, can reduce the anisotropy of solder ball deformation in solder ball bonding and achieve a near-circular crimped shape. Therefore, even when bonding small solder balls, short circuits caused by contact between adjacent solder balls can be prevented, and the bonding area is maximized. Furthermore, when the second element is included in a specific amount, the aforementioned effects of including the first element in a specific amount and the improved bonding reliability brought about by including the second element synergistically enhance the bonding reliability required in high-density packaging. Therefore, the metal wire of the present invention is suitable for semiconductor devices, and particularly suitable for high-density packaged semiconductor devices.

[0048] [Method for manufacturing a semiconductor device] A semiconductor device can be manufactured by connecting the electrodes on a semiconductor element to the electrodes on a lead frame or circuit board using the Ag alloy bonding wires for semiconductor devices of the present invention.

[0049] In one embodiment, the method for manufacturing a semiconductor device of the present invention (hereinafter also simply referred to as "the method of the present invention") includes the step of connecting a first electrode on a semiconductor element to a second electrode on a lead frame or circuit board using the metal wires of the present invention. The first connection between the first electrode and the metal wires of the present invention can be implemented by solder ball bonding, and the second connection between the second electrode and the metal wires of the present invention can be implemented by wedge bonding.

[0050] By using the metal wire of the present invention, which contains an Ag alloy in a specific amount of the first element, the anisotropy of solder ball deformation during solder ball bonding can be reduced, thereby achieving a near-circular crimp shape. This prevents short circuits caused by contact between adjacent solder balls, even in small solder ball bonding, and maximizes the area conducive to bonding. The metal wire of the present invention is also well-suited for narrow-pitch connections of 50 μm or less, significantly contributing to the application of Ag metal wires in high-density packaging applications.

[0051] [Semiconductor Device] A semiconductor device can be manufactured by connecting the electrodes on a semiconductor element to the electrodes on a lead frame or circuit board using the Ag alloy bonding wires of the present invention.

[0052] In one embodiment, the semiconductor device of the present invention is characterized in that it includes a circuit board, a semiconductor element, and a bonding line for making the circuit board and the semiconductor element conductive, wherein the bonding line is a metal wire of the present invention.

[0053] In the semiconductor device of the present invention, there are no particular limitations on the circuit board and semiconductor elements, and any known circuit board and semiconductor elements that can be used to constitute a semiconductor device can be used. Alternatively, a lead frame can be used instead of a circuit board. For example, as shown in the semiconductor devices described in Japanese Patent Application Publication No. 2020-150116 or Japanese Patent Application Publication No. 2002-246542, the device can be configured as a semiconductor device including a lead frame and a semiconductor element mounted on the lead frame.

[0054] Examples of semiconductor devices include those used in electrical products (e.g., computers, mobile phones, digital cameras, televisions, air conditioners, solar power systems, etc.) and transportation vehicles (e.g., locomotives, automobiles, trams, ships, and aircraft). Among these, high-density packaged semiconductor devices that require strict control over the compression shape of the solder ball joints during small solder ball bonding are preferred. [Example]

[0055] Hereinafter, embodiments are shown to specifically describe the present invention. However, the present invention is not limited to the embodiments shown below.

[0056] (Sample) The Ag used as raw material has a purity of 99.9 at.% or higher and the remainder contains unavoidable impurities. The first element (Te, Bi, and Sb) and the second element (Pd, Pt, In, and Ga) have a purity of 99.9 at.% or higher and the remainder contains unavoidable impurities.

[0057] The Ag alloy used in the bonding wire is manufactured in the following manner: the raw material is loaded into a carbon crucible that has been processed into a cylindrical shape, and the raw material is melted by heating it to 1080 to 1600°C in a vacuum or in an inert gas atmosphere such as nitrogen or argon in a high-frequency furnace. Then, a metal wire of ϕ4 to 6 mm is manufactured by continuous casting.

[0058] The obtained Ag alloy is drawn using a die to produce a metal wire with a diameter of ϕ300–600 μm. Then, by repeatedly performing intermediate heat treatment at 200–700°C and drawing, the final wire diameter ϕ20 μm is achieved. A commercially available lubricant is used during drawing, and the wire feed rate is set to 20–600 m / min. The intermediate heat treatment is performed while continuously sweeping the metal wire in an argon atmosphere. The wire feed rate during intermediate heat treatment is set to 20–100 m / min.

[0059] The metal wire after drawing is subjected to final heat treatment to achieve a final elongation at break of approximately 9-25%. The final heat treatment is performed in the same manner as the intermediate heat treatment. The feed rate of the metal wire during the final heat treatment is the same as that during the intermediate heat treatment, set to 20-100 m / min. The final heat treatment temperature is set to 200-700℃, and the heat treatment time is set to 0.2-1.0 seconds.

[0060] The concentrations of the first and second elements in the junction line are detected by dissolving the junction line with a strong acid and analyzing the resulting liquid using an ICP emission spectrometer and an ICP mass spectrometer to detect the concentrations of the elements contained in the entire junction line.

[0061] (Test and evaluation methods) The test and evaluation methods are described below.

[0062] [Crimping Shape] The crimping shape (flattened shape of the solder ball) of the solder ball joint is evaluated as follows: a commercially available wire bonder (manufactured by K&S, Iconn Plus) is used to bond electrodes with an Al film of 1.0 μm thickness on a Si substrate, and the results are observed from directly above using an optical microscope (evaluation number N = 100). Furthermore, while nitrogen gas + 5% hydrogen gas is flowing in at a flow rate of 0.4–0.6 L / min, solder balls are formed, with the ball diameter set to be 1.5–1.6 times the diameter of the metal wire. Regarding the determination of the flattened shape of the solder ball, a shape close to a perfect circle is considered good; an elliptical or petal-shaped shape is considered poor. Then, the evaluation is performed according to the following criteria.

[0063] Evaluation Criteria: ◎: No defects ○: 1-4 defects (no problems in actual use) ×: 5 or more defects

[0064] [FAB Shape] The evaluation of FAB shape is performed as follows: a FAB is fabricated on the lead frame using a commercially available wire bonding machine, and observed using a scanning electron microscope (SEM) (evaluation number N=100). Furthermore, a FAB is formed while nitrogen gas + 5% hydrogen gas is flowing in at a flow rate of 0.4–0.6 L / min, and the diameter of the FAB is set within the range of 1.5–1.6 times the diameter of the metal wire. Regarding the determination of FAB shape, a true spherical shape is considered good, while off-center or irregular shapes are considered poor. Then, the evaluation is performed according to the following criteria.

[0065] Evaluation Criteria: ◎: 5 ​​or fewer defects ○: 6 to 10 defects (no problems in actual use) ×: 11 or more defects

[0066] [Evaluation of Bonding Reliability] The samples used for bonding reliability evaluation were prepared by bonding electrodes with a 1.0 μm thick Al film formed on a Si substrate on a general metal frame using a commercially available wire bonder, and sealing them with commercially available epoxy resin. Furthermore, while nitrogen gas + 5% hydrogen gas was flowing in at a flow rate of 0.4–0.6 L / min, solder balls were formed, with the ball diameter set in the range of 1.5–1.6 times the diameter of the metal wire.

[0067] The bonding reliability is evaluated using a high temperature and high humidity test (bHAST). Specifically, an unsaturated pressure cooker is used to expose the bonding reliability evaluation samples to a high temperature and high humidity environment of 130°C and 85% relative humidity, with a bias voltage of 5V applied. Regarding the bonding life of the solder ball joints, a shear test is performed on the solder ball joints every 48 hours. The bonding life of the solder ball joint is defined as the time when the shear strength value reaches half of the initial shear strength. The shear test is performed after removing the resin through acid treatment, exposing the solder ball joints.

[0068] The shear testing machine used for HAST evaluation was a testing machine manufactured by DAGE Corporation. The shear strength value was the average of the measurements taken at 10 randomly selected solder ball joints. Then, the evaluation was performed according to the following criteria.

[0069] Evaluation Criteria: ◎◎: Bond life of 288 hours or more ◎: Bond life of 144 hours or more but less than 288 hours ○: Bond life of 96 hours or more but less than 144 hours ×: Bond life of less than 96 hours

[0070] [Wafer Damage] The assessment of wafer damage is performed as follows: using a commercially available wire bonder, electrodes with a 1.0 μm thick Al film formed on a Si substrate are bonded with solder balls. The metal wires and Al electrodes are dissolved with a chemical solution to expose the Si substrate. The Si substrate directly below the solder ball bonding area is then observed using an optical microscope (N=50). The assessment is then performed according to the following criteria.

[0071] Evaluation criteria: ○: No cracks or joint marks △: Although there are no cracks, there are fewer than 3 places where joint marks can be observed ×: Other conditions

[0072] [Experimental Example 1] The evaluation results of the example and comparative example with changes in whether or not the first element was added and the amount added are shown in Table 1.

[0073] [Table 1] (Table 1) Element 1 (at.ppm) Element 2 (at.%) crimping shape FAB shape wafer damage Te Bi Sb Pd Pt In Ga Reality Shi example 1 5 〇 ◎ 〇 2 100 ◎ ◎ 〇 3 495 〇 〇 〇 4 5 〇 ◎ 〇 5 100 ◎ ◎ 〇 6 495 〇 〇 〇 7 5 〇 ◎ 〇 8 200 ◎ ◎ 〇 9 1495 〇 〇 〇 Compare Comparison example 1 4 × 〇 〇 2 3 × 〇 〇 3 4 × 〇 〇 4 510 × × 〇 5 505 × × 〇 6 1560 × × 〇 7 0.6 × ◎ 〇 8 0.4 × ◎ 〇 9 0.5 × ◎ 〇 10 0.4 × ◎ 〇

[0074] It has been confirmed that the concentration of the first element in the Ag alloy bonding wires of Examples 1 to 9 is within the scope of the present invention, and the crimping shape of the solder balls is excellent. On the other hand, the concentration of the first element in the Ag alloy bonding wires of Comparative Examples 1 to 10 exceeds the lower or upper limit of the scope of the present invention, and the crimping shape of the solder balls is poor.

[0075] [Experimental Example 2] The study on the effect of adding the second element changed the amount of the first element added, and changed the state of whether the second element was added and the amount added. The evaluation results of the implementation and comparative examples are shown in Table 2 and Table 3.

[0076] [Table 2] (Table 2) Element 1 (at.ppm) Element 2 (at.%) Other elements (at.%) crimping shape FAB shape Connection reliability wafer damage Te Bi Sb Pd Pt In Ga Reality Shi example 10 5 0.06 〇 ◎ 〇 〇 11 10 0.1 〇 ◎ 〇 〇 12 20 0.4 〇 ◎ ◎ 〇 13 30 0.7 〇 ◎ ◎◎ 〇 14 40 1 〇 ◎ ◎◎ 〇 15 50 2.8 ◎ ◎ ◎◎ 〇 16 100 2.9 ◎ ◎ ◎◎ 〇 17 200 3 ◎ ◎ ◎◎ 〇 18 300 0.7 ◎ ◎ ◎◎ 〇 19 395 1.8 ◎ ◎ ◎◎ 〇 20 450 0.5 0.5 〇 〇 ◎◎ 〇 21 495 0.3 0.5 〇 〇 ◎◎ 〇 22 5 0.06 〇 ◎ 〇 〇 23 10 0.1 〇 ◎ 〇 〇 24 20 0.4 〇 ◎ ◎ 〇 25 30 0.5 〇 ◎ ◎ 〇 26 40 0.6 〇 ◎ ◎ 〇 27 50 1 ◎ ◎ ◎◎ 〇 28 100 2.8 ◎ ◎ ◎◎ 〇 29 150 2.9 ◎ ◎ ◎◎ 〇 30 200 3 ◎ ◎ ◎◎ 〇 31 300 2 ◎ ◎ ◎◎ 〇 32 395 1 ◎ ◎ ◎◎ 〇 33 450 1 0.4 〇 〇 ◎◎ 〇 34 495 0.4 〇 〇 ◎ 〇 35 5 0.06 〇 ◎ 〇 〇 36 20 0.2 〇 ◎ 〇 〇 37 40 0.4 〇 ◎ ◎ 〇 38 60 0.75 ◎ ◎ ◎◎ 〇 39 80 0.8 ◎ ◎ ◎◎ 〇 40 100 1 ◎ ◎ ◎◎ 〇 41 200 2.8 ◎ ◎ ◎◎ 〇 42 300 2.9 ◎ ◎ ◎◎ 〇 43 400 3 ◎ ◎ ◎◎ 〇 44 500 1 0.2 ◎ ◎ ◎◎ 〇 45 600 0.8 ◎ ◎ ◎◎ 〇 46 700 0.6 ◎ ◎ ◎ 〇 47 900 0.05 ◎ ◎ 〇 〇 48 1100 0.1 ◎ ◎ 〇 〇 49 1200 0.3 ◎ ◎ ◎ 〇 50 1250 0.4 ◎ ◎ ◎ 〇 51 1300 0.5 ◎ ◎ ◎◎ 〇 52 1350 0.7 ◎ ◎ ◎◎ 〇 53 1400 2 〇 〇 ◎◎ 〇 54 1450 2.5 〇 〇 ◎◎ 〇 55 1495 2.9 〇 〇 ◎◎ 〇

[0077] [Table 3] (Table 3) Element 1 (at.ppm) Element 2 (at.%) Other elements (at.%) crimping shape FAB shape Connection reliability Chip damage Te Bi Sb Pd Ft In Ga Real Shi example 56 100 100 2.2 ◎ ◎ ◎◎ 〇 57 150 1400 0.8 ◎ ◎ ◎◎ 〇 58 150 1400 0.8 0.2 ◎ ◎ ◎◎ 〇 59 100 300 0.3 ◎ ◎ ◎ 〇 60 50 50 200 0.4 03 ◎ ◎ ◎◎ 〇 61 150 4 ◎ ◎ ◎◎ △ 62 150 3.1 ◎ ◎ ◎◎ △ 63 500 3.1 ◎ ◎ ◎◎ △ 64 1000 32 ◎ ◎ ◎◎ △ 65 20 0.4 Au: 0.2 〇 ◎ ◎ 〇 66 500 1 0.2 With: 0.3 ◎ ◎ 〇 〇 67 100 1.5 Cu: 0.18 P: 0.1 ◎ ◎ 〇 △ Compare Comparison example 1 4 × 〇 × 〇 2 3 × 〇 × 〇 3 4 × 〇 × 〇 4 510 × × × 〇 5 505 × × × 〇 6 1560 × × × 〇 7 0.6 × ◎ ◎ 〇 8 0.4 × ◎ ◎ 〇 9 0.5 × ◎ ◎◎ 〇 10 0.4 × ◎ ◎ 〇 11 3 0.04 × 〇 × 〇 12 4 0.03 × 〇 × 〇 13 4 0.03 × 〇 × 〇 14 4 0.04 × 〇 × 〇

[0078] It has been confirmed that the concentration of the first element in the Ag alloy bonding wires of Examples 10-60 and 65-67 is within the range of the present invention, and the concentration of the second element is within the preferred range of the present invention, and both the crimping shape and bonding reliability of the solder balls are excellent. Although the crimping shape and bonding reliability of the solder balls in the Ag alloy bonding wires of Examples 61-64 are also excellent, the concentration of the second element exceeds the upper limit of the preferred range of the present invention, and compared with other embodiments, there is a slight tendency for the chip damage to be slightly worse. On the other hand, the concentration of the first element in the Ag alloy bonding wires of Comparative Examples 1 to 14 exceeds the range of the present invention, and the crimping shape of the solder balls is poor. In addition, the bonding reliability of the metal wires of Comparative Examples 1 to 6 and 11 to 14, which do not contain the second element, is also poor.

Claims

1. An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element"), and containing Ga, and satisfying at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm; (2) the concentration of Bi is 5 to 500 at.ppm; (3) the concentration of Sb is 5 to 1500 at.ppm.

2. An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element"), and containing In, satisfying at least one of the following conditions (1) to (3), and not having a coating with a metal other than Ag as the main component, (1) the concentration of Te is 5 to 500 at.ppm (2) the concentration of Bi is 5 to 500 at.ppm (3) the concentration of Sb is 5 to 1500 at.ppm 3. An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element"), and containing one or more elements selected from the group consisting of Pd, Pt, In and Ga (hereinafter referred to as "the second element"), and containing at least In as the second element, wherein the total concentration of elements not belonging to the first element, the second element and Ag (hereinafter referred to as "other elements") is 0 at.% to 0.5 at.%, and the Ag alloy satisfies at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm; (2) the concentration of Bi is 5 to 500 at.ppm; (3) the concentration of Sb is 5 to 1500 at.ppm.

4. An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element"), and containing at least Pt, wherein the concentration of Pt is less than 0.1 at.%, and satisfies at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm; (2) the concentration of Bi is 5 to 500 at.ppm; (3) the concentration of Sb is 5 to 1500 at.ppm.

5. An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element"), and containing at least Pt, wherein the concentration of Pt is less than 0.1% by mass, and satisfying at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm; (2) the concentration of Bi is 5 to 500 at.ppm; (3) the concentration of Sb is 5 to 1500 at.ppm.

6. An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element") and one or more elements selected from the group consisting of Pd, Pt, In and Ga (hereinafter referred to as "the second element"), wherein the total concentration of the second element is 0.05 to 1 at.%, and the Ag alloy satisfies at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm; (2) the concentration of Bi is 5 to 500 at.ppm; (3) the concentration of Sb is 5 to 1500 at.ppm.

7. An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing two or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element"), and satisfying at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm; (2) the concentration of Bi is 5 to 500 at.ppm; (3) the concentration of Sb is 5 to 1500 at.ppm.

8. An Ag alloy bonding wire for a semiconductor device, comprising an Ag alloy containing one or more elements selected from the group consisting of Te, Bi and Sb (hereinafter referred to as "the first element") and one or more elements selected from the group consisting of Pd, Pt, In and Ga (hereinafter referred to as "the second element"), wherein the second element substantially contains only one element selected from Pd, Pt, In and Ga, the total concentration of Ca and rare earth elements is 0 at.ppm or more but less than 20 at.ppm, and the Ag alloy satisfies at least one of the following conditions (1) to (3): (1) the concentration of Te is 5 to 500 at.ppm; (2) the concentration of Bi is 5 to 500 at.ppm; (3) the concentration of Sb is 5 to 1500 at.ppm.

9. The Ag alloy bonding wire of any one of claims 1 to 5, 7 and 8 contains one or more elements selected from the group consisting of Pd, Pt, In and Ga (hereinafter referred to as "second element"), and the total concentration of the second element is 0.05 to 3 at.%.

10. The Ag alloy bonding wire of any one of claims 1 to 8 contains at least Pt, and the concentration of Pt is less than 0.06 at.%.

11. The Ag alloy bonding wire of any one of the claims 1 to 8 satisfies at least two of the above conditions (1) to (3).

12. The Ag alloy bonding wire of any one of claims 2 to 8 contains at least Ga.

13. The Ag alloy bonding wire as requested in item 12, wherein the concentration of Ga is 0.06 at.% or more.

14. The Ag alloy bonding wire of any one of claims 1 and 4 to 8 contains at least In.

15. The Ag alloy bonding wire as requested in claim 14, wherein the concentration of In is 0.03 at.% or more.

16. The Ag alloy bonding wire of any of claims 1 and 3 to 8 does not have a coating with a metal other than Ag as the main component.

17. The Ag alloy bonding wire of any one of claims 1 to 3 and 6 to 8 contains at least Pt, and the concentration of Pt is less than 0.1 at.%.

18. For any of the Ag alloy bonding wires in claims 1 to 7, the total concentration of Ca and rare earth elements is above 0 at.ppm but less than 20 at.ppm.

19. An Ag alloy bonding wire as claimed in any of claims 1 to 8, wherein the total concentration of the first element is less than 2000 at.ppm.

20. For any of the Ag alloy bonding wires in claims 1 to 8, the total concentration of elements other than Ag, Te, Bi, Sb, Pd, Pt, In and Ga (hereinafter referred to as "other elements") is less than 0.1 at.%.

21. An Ag alloy bonding wire as claimed in any of claims 1 to 8, wherein the remainder of the Ag alloy comprises Ag and unavoidable impurities.

22. The Ag alloy bonding wire of any one of the claims 1 to 8, wherein the concentration of Sb in condition (3) is 900 to 1500 at.ppm.

23. For any of the Ag alloy bonding wires requested in items 1 to 8, the concentrations of each element are the concentrations measured by ICP emission spectroscopy or ICP mass spectrometry.

24. A semiconductor device comprising an Ag alloy bonding wire as claimed in any one of claims 1 to 23.

Citation Information

Patent Citations

  • Bonding wire

    JP2016025114A

  • Noble metal-coated silver wire for ball bonding and manufacturing method of the same, and semiconductor device using noble metal-coated silver wire for ball bonding and manufacturing method of the same

    JP2019186248A

  • Silver alloy bonding wire and method of manufacturing the same

    TW201639972A

  • Wire joining structure, bonding wire used in same, and semiconductor device

    TW202115799A