Sulfide solid electrolyte for lithium secondary batteries

TWI945573BActive Publication Date: 2026-11-11LOTTE ENERGY MATERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
TW113134855
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-09-18
Filing Date
2024-09-13
Publication Date
2026-11-11
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

Sulfide solid electrolytes face challenges in atomization due to soft material properties, leading to reduced recovery and impurities, and liquid-phase synthesis results in low ionic conductivity and high electronic conductivity.

Method used

A sulfide solid electrolyte with a chemical formula Li xPS (5.7-0.9y)Ha y, where Ha is Cl, Br, or I, and a method involving mixing sources in an organic solvent, followed by stirring and sintering, to achieve high ionic conductivity and low electronic conductivity.

Benefits of technology

The solution provides sulfide solid electrolytes with ionic conductivity of 1.6 mS/cm or higher and brightness, overcoming the limitations of traditional synthesis methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001920318_001
    Figure TWG2TB001920318_001
  • Figure TWG2TB001920318_002
    Figure TWG2TB001920318_002
  • Figure TWG2TB001920318_003
    Figure TWG2TB001920318_003
Patent Text Reader

Abstract

This invention relates to a sulfide solid electrolyte for lithium secondary batteries, wherein the composition of the sulfide solid electrolyte is LixPS(5.7-0.9y)Hay (where Ha is at least one atom selected from the group consisting of Cl, Br and I, x = 6.4-0.8y, and 0.5y ≤ 1.7).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] [Cross-reference to related applications]

[0002] This application claims priority based on Korean Patent Application No. 10-2023-0123830 filed in the Korean Intellectual Property Office on September 18, 2023, and the disclosure of that patent is hereby incorporated by reference in its entirety into this application.

[0003] The present disclosure relates to a solid electrolyte for a lithium secondary battery, and in particular to a sulfide solid electrolyte for a lithium secondary battery. Prior Art

[0004] All-solid-state batteries (ALLSBAs) replace traditional liquid electrolytes with solid electrolytes in their battery cells. These batteries eliminate the need for the electrolyte and separators found in traditional lithium-ion batteries, using solid electrolytes instead. Compared to conventional batteries using liquid electrolytes, ALLSBAs offer reduced risk of explosion or fire, simplified manufacturing processes, and the potential for high energy density. As a result, they are attracting significant attention as the next generation of secondary batteries.

[0005] Among inorganic solid electrolytes, sulfide solid electrolytes have attracted considerable attention as solid electrolytes (SSEs) for all-solid-state batteries. However, most sulfide solid electrolytes are typically obtained by mixing raw materials (e.g., Li2S, P2S5, and LiCl), subjecting the mixture to a long, high-energy milling process, and then sintering to increase crystallinity and thus improve ionic conductivity. However, this sintering process increases the particle size of the solid electrolyte. Therefore, the synthesized materials used for assembly need to be appropriately atomized based on the location of the solid electrolyte in the battery. However, the atomization process of sulfide solid electrolytes is difficult due to their soft material properties. Furthermore, the solid electrolyte atomized by mechanical milling may adhere to or re-aggregate on the milling media, resulting in reduced solid electrolyte recovery. In particular, the introduction of wet milling during the atomization process may result in residual impurities, such as the solvent used as the dispersion medium, which can reduce the ionic conductivity of the solid electrolyte.

[0006] To address the issues associated with solid-phase synthesis, existing technologies utilize liquid-phase synthesis to produce sulfide solid electrolytes. Compared to solid-phase synthesis, liquid-phase synthesis allows for the synthesis of sulfide solid electrolytes in a shorter time and with less energy, making it suitable for large-scale production. However, liquid-phase synthesis also has drawbacks, such as low ionic conductivity due to impurities, high electronic conductivity due to sulfur vacancies or carbonization of organic solvents, and the production of dark and uneven color. Summary of the Invention

[0007] For example, in the traditional method of liquid-phase synthesis of sulfide solid electrolytes (LPSCl), a two-stage synthesis method is adopted, in which Li3PS4 is first synthesized, and then Li2S and LiCl are additionally introduced. The following is the reaction formula of this two-stage synthesis method: 3Li 2S + P 2S 5→ 2Li 3PS 4 [Reaction 1] Li 3PS 4 + Li 2S + LiCl → Li 6PS 5Cl [Equation 2]

[0008] In this regard, the inventors discovered that the Cl introduced during the reaction combines with P, while the S in the existing PS 4 3-bond is in an unstable binding state and is lost during the heat treatment, resulting in the manufactured LPSCl having high electronic conductivity and a dark color.

[0009] To solve this problem, the present invention aims to provide a sulfide solid electrolyte that can achieve high ionic conductivity regardless of the reaction mechanism of LPSCl and a method for producing the same.

[0010] According to one embodiment of the present invention, a sulfide solid electrolyte is provided, having a chemical formula of Li xPS (5.7-0.9y)Ha y (wherein Ha is at least one element selected from the group consisting of Cl, Br, and I, x = 6.4-0.8y, and 0.5≤y≤1.7).

[0011] The sulfide solid electrolyte may have an argyrodite-type crystal structure.

[0012] In this composition chemical formula, y may satisfy 0.8≤y≤1.5.

[0013] In this composition formula, Ha may be Cl.

[0014] The ionic conductivity of the solid electrolyte may be 1.6 mS / cm or higher, or 2.0 mS / cm or higher.

[0015] The sulfide solid electrolyte may have a lightness (L*) value of 60 or more in the CIE L*a*b* color space.

[0016] According to another embodiment of the present invention, a method for manufacturing a sulfide solid electrolyte is provided. The method includes: mixing a lithium source, a phosphorus source, a sulfur source, and a halogen source according to the chemical formula Li xPS (5.7 + 0.665x - 1.565y) Ha y (wherein Ha is at least one element selected from the group consisting of Cl, Br, and I, x = 6.4-0.8y, and 0.5 ≤ y ≤ 1.7); and synthesizing a Li xPS (5.7-0.9y) Ha y compound through a mixing reaction of the source materials.

[0017] Mixing may include dissolving each source material in an organic solvent followed by stirring.

[0018] The mixing may include the following steps: mixing a lithium source, a phosphorus source, and a sulfur source to generate an LPS compound; and mixing a halogen source with the LPS compound.

[0019] The LPS compound may include Li 3PS 4 .

[0020] The synthesis may include sintering the reaction product at a temperature of 300 to 600°C.

[0021] The synthesized compound may have an argyrodite-type crystal structure.

[0022] In this composition chemical formula, y may satisfy 0.8≤y≤1.5.

[0023] In this composition formula, Ha may be Cl.

[0024] According to the present disclosure, a sulfide solid electrolyte powder having high ionic conductivity and low electronic conductivity can be provided.

[0025] Furthermore, a method for producing sulfide solid electrolyte powder with high ionic conductivity and low electronic conductivity based on a liquid phase synthesis method is provided. Simple diagram description

[0026] The above and other aspects, features and advantages of the present disclosure will become more apparent from the following detailed description in conjunction with the accompanying drawings. FIG1 is a flow chart of a method for manufacturing a sulfide solid electrolyte according to one embodiment of the present invention. FIG2 is a flow chart illustrating a two-stage synthesis process according to an embodiment of the present invention. FIG3 and FIG4 are graphs showing the results of X-ray diffraction analysis of a powder sample according to an embodiment of the present invention. Implementation Method

[0027] The preferred embodiments of the present disclosure will be described below with reference to the accompanying drawings.

[0028] Here, "LPS compound" or "LPS" refers to a compound obtained from a ternary composition of lithium (Li), phosphorus (P), and sulfur (S); while "LPSHa compound" or "LPSHa" refers to a compound obtained from a quaternary composition of lithium (Li), phosphorus (P), sulfur (S), and Ha (where Ha is at least one selected from the group consisting of Cl, Br, and I). In the present disclosure, an LPS or LPSHa compound may be a mixture of two or more compounds.

[0029] LPS may include not only ternary compounds but also binary compounds such as Li2S or P2S5 as unreacted products or by-products, which can be obtained from Li, P and S as raw materials. This definition also applies to LPSHa compounds.

[0030] FIG1 is a flow chart illustrating a method for manufacturing a sulfide solid electrolyte according to one embodiment of the present disclosure.

[0031] 1 , a lithium source, a phosphorus source, a sulfur source, and a halogen source are mixed to satisfy the following composition formula (step S110): LixPS (5.7+0.665x-1.565y)Hay (x=6.4-0.8y and 0.5≤y≤1.7) [Composition Formula 1]

[0032] The mixed components are stirred and sintered to synthesize an LPSHa compound having the following chemical formula (step S120): LixPS (5.7-0.9y)Hay(x=6.4-0.8y and 0.5≤y≤1.7) [Composition formula 2]

[0033] Thus, in Composition Formula 1 and Composition Formula 2, the subscript numbers (such as x or y) below the symbols of each element represent the number of moles of each element constituting the synthesized compound, and the number of moles is expressed based on 1 mole of P.

[0034] In embodiments of the present disclosure, the LPSHa compound has high ionic conductivity. The ionic conductivity of the LPSHa compound may be 1.6 mS / cm or higher, 2.0 mS / cm or higher, 2.5 mS / cm or higher, 3 mS / cm or higher, 3.5 mS / cm or higher, or 4 mS / cm or higher.

[0035] In embodiments of the present disclosure, the LPSHa compound has high brightness. The LPSHa compound may have a brightness (L*) value of 65 or higher, 66 or higher, 67 or higher, 68 or higher, 69 or higher, or 70 or higher.

[0036] The sulfide solid electrolyte composition described in the present disclosure can be manufactured through a two-stage process based on Reaction Formula 1 and Reaction Formula 2. This will be described below.

[0037] First, a precursor for LPS production is provided (step S210), wherein the precursor includes a lithium (Li) source, a phosphorus (P) source, and a sulfur (S) source.

[0038] For example, the precursor may include a lithium sulfide and a phosphorus sulfide. In the present disclosure, examples of lithium sulfide may include at least one compound selected from the group consisting of Li2S2, Li2S3, Li2S4, Li2S6, and Li2S8. In the present disclosure, the phosphorus sulfide may include P2S5. In the present disclosure, the lithium sulfide and phosphorus sulfide in the precursor may be mixed according to the mixing ratio in Reaction Formula 1 above.

[0039] In the present disclosure, an excess amount of sulfur (S) can be used in the one-stage synthesis for LPS production according to the composition formula 1. In the present disclosure, S8 can be used as an excess sulfur source.

[0040] Subsequently, the precursors are dissolved in an organic solvent, such as THF (tetrahydrofuran), DMC (dimethyl carbonate), ACN (acetonitrile), or DME (dimethyl ether), and stirred to synthesize the LPS compound (step S220). Specifically, stirring can be performed at a temperature of 50 to 80°C and a speed of 200 to 500 rpm for 1 to 10 hours. Preferably, the stirring step is performed in an inert gas environment, such as argon (Ar).

[0041] Optionally, the LPS compound produced by stirring can be dried. For example, the LPS compound can be dried at a temperature of 80 to 140° C. for 1 to 24 hours.

[0042] Subsequently, a lithium halide is added to the synthesized LPS compound to synthesize the LPSHa compound. For example, the LPSHa compound can be synthesized by mixing the LPS compound with LiHa in a suitable organic solvent (e.g., THF) and stirring at 200 to 500 rpm for 1 to 10 hours at 50 to 80°C, or by milling the mixture in a ball mill at 100 to 500 rpm for 1 to 10 hours. The synthesized LPSHa can be sintered in an inert atmosphere at 300 to 600°C to produce LPSHa with high crystallinity.

[0043] According to the present disclosure, an all-solid-state secondary battery comprising the above-mentioned solid electrolyte can be provided. The all-solid-state secondary battery disclosed herein can include a positive electrode comprising a positive electrode active material, a negative electrode comprising a negative electrode active material, and a solid electrolyte layer disposed between the positive electrode and the negative electrode.

[0044] In the present disclosure, the positive electrode active material is not limited to any positive electrode active material commonly used in secondary batteries. For example, the positive electrode active material may be a lithium transition metal oxide, a transition metal sulfide, or the like. For example, at least one composite oxide formed of lithium and a metal selected from the group consisting of cobalt, manganese, nickel, and combinations thereof may be used as the positive electrode active material.

[0045] In the present disclosure, the negative electrode active material may include at least one selected from the following groups: lithium metal, lithium metal alloy or a combination thereof, a metal alloyed with lithium, a transition metal oxide, a non-transition metal oxide, and a carbon-based material.

[0046] In the present disclosure, the solid electrolyte may include the above-mentioned sulfide solid electrolyte. The above-mentioned sulfide solid electrolyte may also be used as a positive electrode active material.

[0047] According to the present disclosure, an all-solid-state secondary battery with reduced internal resistance and improved cycle characteristics is provided. [Detailed description of preferred embodiments] []

[0048] Hereinafter, preferred embodiments of the present disclosure will be described in detail. [Example] [1]

[0049] Raw materials were mixed according to the chemical formula Li xPS (5.7 + 0.665x - 1.565y) Cl y, with varying values of y within a range of 0.5 ≤ y ≤ 2.2. Li 2S, P 2S 5, S 8, and LiCl were used as the sources of Li, P, S, and Cl, respectively. First, Li 2S, P 2S 5, and S 8 were mixed to prepare the LPS compound. ACN was used as the stirring solvent, and the mixture was stirred at 300 rpm in an Ar atmosphere at 55°C for 5 hours. The mixed solution was then dried under vacuum at a temperature range of 80 to 140°C for 1 to 24 hours. LiCl was then added to synthesize the LPSCl compound, which was then sintered at a temperature of 350 to 600°C in an inert atmosphere. [A. LPSCl] [Compound composition analysis] []

[0050] The composition of the prepared LPSCl compound was analyzed using ion chromatography (IC), inductively coupled plasma atomic emission spectrometry (ICP-AES), and a C / S-dedicated analyzer.

[0051] Specifically, the quantitative values of Li and P were measured by analytical analysis using a Thermo Fisher Scientific iCAP 7400 ICP-AES.

[0052] Cl was quantified using IC analysis using a Dionex ICS 6000 instrument. Samples were pumped through an analytical column (Dionex AS11-HC) at a flow rate of 0.25 ml / min, and conductivity was measured using an ion chromatography conductivity detector.

[0053] The quantitative value of S was measured using a LECO CS844 device by the following method: (1) Place an empty ceramic crucible on a balance and tar it. Then, add approximately 1 g of sample to the crucible and weigh it with a weight. Then, install the crucible in a high-frequency induction furnace for automatic analysis. (2) NaOH is used to remove CO 2 contained in the O 2 gas as a carrier (see reaction formula 3 below), while H 2O is removed by MgClO 4 as a reagent (see reaction formula 4 below). NaOH + CO₂ → NaCO₃ [Equation 3] MgClO 4 + H 2O → MgCl(OH) 4 [Equation 4] (3) The C gas generated in the high-frequency induction furnace in the sample combines with O2 as combustion gas to generate CO and CO2; while the S gas combines with O2 to generate SO2. (4) Remove moisture and dust that may affect the analysis by using MgClO 4 and quartz wool. (5) The sulfur content in the form of SO 2 gas is measured using a SO 2 infrared absorption detector. (6) Since the carbon content is measured by an infrared absorption detector of CO 2 , all gases present in the form of CO are converted to CO 2 by CuO (see reaction formula 5 below). CO + CuO → CO 2 + Cu [Equation 5] (7) The carbon content in the form of CO 2 gas is measured using a CO 2 infrared absorption detector. [B.] [Measurement] [LPSCl] [Ionic conductivity of the compound (] [IC] [) and electronic conductivity (] [EC] [)] []

[0054] The ionic conductivity (IC) of the prepared LPSCl compound was measured. First, 100 mg of the prepared LPSCl compound powder was pressed at a pressure of 3 ton / cm² for 1 minute to produce sample pellets with a thickness of approximately 800 μm and a diameter of approximately 10 mm. The particle impedance of the sample was measured using a two-probe method using an impedance analyzer (Biologic, VSP400) with indium electrodes placed on both sides. The measurement frequency range was 0.1 Hz to 1 MHz, and the voltage amplitude was 100 mV. The measurements were performed in a dry air environment at 25°C. The resistance value was calculated from the arcs in the Nyquist plot of the impedance measurement results, and the ionic conductivity was calculated taking into account the sample area and thickness. The measurement results are shown in Table 1. [C.] [Measurement] [LPSCl] [Brightness of the compound] []

[0055] Lightness (L*) values were measured according to the CIE L*a*b* color space. The prepared LPSCl powder was evenly packed into a 30 mm diameter sample holder and then measured using a spectrophotometer (Konica Minolta, CM-2600d). Specifically, D65 illuminant was used as the measurement light source.

[0056] Table 1 below summarizes the composition, ionic conductivity, electronic conductivity, and brightness measurement results of the synthesized LPSCl compounds. [Table 1] sample composition S 8 additives Ionic conductivity IC (mS / cm) Electronic conductivity EC (nS / cm) Lightness (L*) value Li (x) P S Cl (y) #1 6.0 1.0 5.2 0.5 O 0.52 1.5 72.9 #2 5.8 1.0 5.0 0.8 The 1.79 2.9 64.7 #3 5.6 1.0 4.8 1 The 2.90 5.5 71.0 #4 5.3 1.0 4.5 1.34 The 5.40 1.5 75.2 #5 5.2 1.0 4.4 1.5 The 4.30 2.8 66.7 #6 5.1 1.0 4.2 1.7 The 0.67 2.5 50.3 #7 4.8 1.0 3.9 2 The - - 51.4 #8 4.7 1.0 3.7 2.2 O - - 49.4

[0057] As shown in Table 1, the ionic conductivity values of samples #2 through #5 all reached 1 mS / cm or above, which is considered ideal. When the y value is less than 0.8 or greater than 1.5, the ionic conductivity drops below 1. Furthermore, as the y value increases, the brightness (L*) of the sample powders generally decreases. [D. LPSCl] [Compound] [X] [Radial diffraction analysis] []

[0058] The prepared LPSCl compound powder was analyzed by X-ray diffraction. Figure 3 shows the results of the X-ray diffraction analysis.

[0059] Referring to Figure 3, it can be confirmed that significant LiCl peaks are present in samples #1, #7, and #8. Meanwhile, samples #1 to #6, and especially samples #2 to #5, exhibit highly crystalline LPSCl compounds with minimal levels of impurities such as Li2S and LiCl. [Example] [2]

[0060] LPS compounds with the same composition as samples #3 and #4 in Example 1 were prepared using a solid-phase method.

[0061] Li2S, P2S5, and LiCl were weighed according to the chemical formula 1, and an excess of S8 was added. Subsequently, the mixture was placed in a ball mill along with zirconia balls and subjected to high-energy ball milling at 300 rpm for 10 hours to synthesize LPSCl.

[0062] As a control, Li 2S, P 2S 5 and LiCl raw materials without excess S 8 were weighed according to the composition chemical formula 2, and LPSCl was synthesized by high-energy ball milling.

[0063] The composition of the synthesized LPSCl powder was analyzed, and its ionic conductivity, electronic conductivity and brightness were measured. X-ray diffraction analysis was also performed on the powder.

[0064] Table 2 summarizes the analysis results, and Figure 4 is a graph of the X-ray diffraction analysis results. [Table 2] sample composition S 8 additives Ionic conductivity IC (mS / cm) Electronic conductivity EC (nS / cm) Lightness (L*) value Li P S Cl #9 5.6 1.0 4.8 1 O 2.22 1.6 70.1 #10 5.3 1.0 4.5 1.34 O 3.95 1.1 70.3 #11 5.6 1.0 4.8 1 X - - 71.8 #12 5.3 1.0 4.5 1.34 X - - 70.6

[0065] As shown in Table 2, samples #9 and #10, which fall within the scope of the disclosed compositional formula 1, exhibited relatively high ionic conductivity values when synthesized using the solid-phase method. However, compared to samples #3 and #4 with the same composition synthesized using the liquid-phase method in Example 1, the ionic conductivity values of samples #9 and #10 were slightly lower.

[0066] For reference, samples #11 and #12 fall within the range of composition formula 2. [Comparative Example] [1]

[0067] The compounds were prepared by liquid phase synthesis according to the compositions listed in Table 3.

[0068] The prepared compounds were analyzed for composition, and their ionic conductivity (IC), electronic conductivity (EC), and brightness were measured. Table 3 shows the analysis results for each sample, and Figure 4 shows the X-ray diffraction analysis results. [Table 3] sample composition S 8 additives Ionic conductivity IC (mS / cm) Electronic conductivity EC (nS / cm) Lightness (L*) value Li P S Cl #13 6.0 1.0 5.0 1 X 1.30 129 41.1 #14 5.5 1.0 4.5 1.5 X 1.50 200 46.4 #15 5.6 1.0 4.8 1 X - - 45.5 #16 5.3 1.0 4.5 1.34 X - - 46.5

[0069] Referring to Table 3, the compounds prepared by the liquid phase method exhibit lower ionic conductivity and higher electronic conductivity. Samples #15 and #16 contain significant amounts of impurities, resulting in ionic conductivities too low to provide meaningful data.

[0070] This disclosure has been described using exemplary embodiments and accompanying drawings, but these are intended only to facilitate a more comprehensive understanding of the disclosure and are not intended to limit the disclosure. Those skilled in the art will appreciate that various modifications and variations are possible without departing from the core features of the disclosure. Therefore, the spirit of the disclosure is defined by the appended claims, not by the foregoing description, and all variations and modifications falling within the claims or their equivalents are intended to be included within the spirit of the disclosure.

[0071] Industrial Utilization

[0072] The present disclosure is applicable to lithium secondary batteries and solid electrolytes used therein.

[0073] S110, S120: Steps S210, S220, S230, S240: Steps

Claims

1. A sulfide solid electrolyte having the chemical formula LixPS(5.7-0.9y)Hay (wherein, Ha is at least one element selected from the group consisting of Cl, Br and I, x = 6.4-0.8y, and 0.5 ≤ y ≤ 1.7), and is manufactured by mixing a lithium source, a phosphorus source, a sulfur source and a halogen source according to the chemical formula LixPS(5.7+0.665x-1.565y)Hay (where Ha is at least one element selected from the group consisting of Cl, Br and I, x = 6.4-0.8y, and 0.5 ≤ y ≤ 1.7), wherein the mixing comprises dissolving each of the above sources in an organic solvent and then stirring.

2. The sulfide solid electrolyte as claimed in claim 1, wherein, This sulfide solid electrolyte has an argyrodite-type crystal structure.

3. The sulfide solid electrolyte as claimed in claim 1, wherein, 0.8≤y≤1.5。 4. The sulfide solid electrolyte as claimed in claim 1, wherein, Ha is Cl.

5. The sulfide solid electrolyte as claimed in claim 1, wherein, The ionic conductivity of this sulfide solid electrolyte is 1.6 mS / cm or higher.

6. The sulfide solid electrolyte as claimed in claim 1, wherein, The ionic conductivity of this sulfide solid electrolyte is 2.0 mS / cm or higher.

7. The sulfide solid electrolyte as claimed in claim 1, wherein, The ionic conductivity of this sulfide solid electrolyte is 10 mS / cm or lower.

8. The sulfide solid electrolyte as claimed in claim 1, wherein, In the CIE L*a*b* color space, this sulfide solid electrolyte has a degree (L*) value of 60 or higher.

9. A method for manufacturing a sulfide solid electrolyte, the method comprising: According to the chemical formula LixPS(5.7+0.665x-1.565y)Hay, wherein Ha is at least one element selected from the group consisting of Cl, Br and I, x=6.4-0.8y, and 0.5≤y≤1.7, a lithium source, a phosphorus source, a sulfur source and a halogen source are mixed; and a LixPS(5.7-0.9y)Hay compound is synthesized by reacting the above sources; wherein the above mixing includes dissolving each of the sources in an organic solvent and then stirring.

10. The method as described in claim 9, wherein, The above mixing includes: mixing a lithium source, a phosphorus source and a sulfur source to generate an LPS compound; and mixing a halogen source with the LPS compound.

11. The method as described in claim 9, wherein, The LPS compound includes Li3PS4.

12. The method as described in claim 9, wherein, The above synthesis includes sintering the reaction products at a temperature of 300 to 600°C.

13. The method as described in claim 9, wherein, The synthesized compound has an argyrodite-type crystal structure.

14. The method as described in claim 9, wherein, 0.8≤y≤1.5。 15. The method as described in claim 9, wherein, Ha is Cl.

Citation Information

Patent Citations

  • Sulfide-based solid electrolyte for lithium ion batteries

    CN105518923A

  • Manufacturing Methods of LPSCl Solid Electrolyte For Li Based Secondary Batteries

    KR102314201B1

  • Solid electrolyte and method for producing same

    TW202301727A