Application of catalyst materials
Patent Information
- Application Number
- TW114101713
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-12-24
- Filing Date
- 2025-01-15
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-01-14
AI Technical Summary
Existing AMC removal technologies are inefficient for trace amounts of VOCs, energy-intensive, and have environmental drawbacks, while current single-atom catalysts are cumbersome and costly to produce.
A simplified process to synthesize single-atom catalysts without a mesoporous template, using transition metals on supports like Fe-Ni oxide, Al-Si oxide, or TiO2, achieving precise dispersion and high catalytic activity for VOCs treatment.
The catalysts efficiently treat VOCs at ppb to ppm concentrations, reducing production costs and enabling large-scale industrial application in filter media.
Smart Images

Figure TWG2TB001920425_001 
Figure TWG2TB001920425_002 
Figure TWG2TB001920425_003
Abstract
Description
Technical Field
[0001] This invention relates to catalyst materials, particularly catalyst materials for decomposing aerosolized molecular pollutants and their applications. Prior Technology
[0002] With the booming development of the semiconductor industry, a large number of chemicals, such as acid and alkali solutions and organic solvents, used in the manufacturing process often evaporate or are emitted naturally after etching or cleaning, and are collected in the exhaust system. These volatile chemicals are collectively referred to as airborne molecular contamination (AMC). As the amount of AMC waste gas generated increases daily, it not only threatens the health of personnel in the working environment but also negatively impacts product yield and may even cause environmental pollution through emission pipes. Therefore, how to effectively treat and remove these trace (ppb to ppm) contaminants has become a topic of great concern in the industry.
[0003] Previous technologies have developed and applied various AMC removal techniques, including physical methods (such as gas-phase adsorption and chemical filters) and chemical methods (such as solvent immersion and chemical cleaning agent treatment). Physical methods are generally efficient and environmentally friendly; however, these technologies may suffer from incomplete removal when dealing with trace amounts (ppb level) of AMC pollutants. Chemical methods have stronger removal capabilities, but their cumbersome post-treatment steps may have adverse environmental impacts. Furthermore, these traditional methods are not always effective against specific volatile organic compounds (VOCs), and treatment methods relying on simple filter adsorption or high-temperature incineration are energy-intensive and not sustainable in the long run. Therefore, how to treat these pollutants in a mild environment using highly efficient catalysts has become an urgent problem to be solved.
[0004] Most current catalytic technologies focus on micrometer (µm) or nanometer (nm) catalytic materials. However, while catalysts of this size can provide effective catalytic activity in some applications, their efficiency is limited when faced with much smaller pollutants (e.g., VOCs at ppb concentrations). Therefore, designing catalysts down to the single-atom level has become a key research direction for improving catalyst performance. Single-atom-level catalysts possess a large number of dispersed and highly active metal centers, theoretically providing more active sites and significantly improving catalytic efficiency.
[0005] It is worth noting that patent document TWI733200B provides a method for preparing a single-atom catalyst, which involves preparing a mesoporous transition metal oxide through a mesoporous template method and anchoring a single-atom noble metal to form the catalyst. However, this process involves the use of a mesoporous template, making the process relatively cumbersome and increasing production costs and time. Furthermore, the preparation of the mesoporous carrier requires precise template control and removal steps, which can be inefficient in large-scale industrial production. Therefore, although this technology has advantages in the preparation of single-atom catalysts, its application in actual production is somewhat limited. Summary of the Invention
[0006] To overcome the aforementioned technical problems, the present invention aims to provide a catalyst material and its application. Without using a mesoporous template method, a simplified process is employed to directly synthesize a high-efficiency single-atom catalyst material, achieving precise dispersion of single-atom-level metals while maintaining extremely high catalytic activity. This material can treat volatile pollutants at concentrations from ppb to ppm, significantly improving treatment efficiency. Furthermore, the catalyst material of this invention can be further added to a support material through impregnation, coating, mixing, or spraying techniques to form filter media, enabling its successful application in filter media and further expanding its application potential in the field of filter media technology. Thus, due to the simplified process of this invention, production costs are effectively reduced, and it can be flexibly applied to large-scale industrial production, possessing broad application prospects. It is particularly suitable for the gaseous pollutant treatment needs in modern chemical industries, becoming a promising solution.
[0007] To achieve the above objectives, the present invention provides a catalyst material, wherein the catalyst material comprises... A carrier; and A first transition metal and a second transition metal, wherein the first transition metal and the second transition metal are respectively loaded in or supported on the support in the form of a single atom; The carrier system is selected from one of the groups consisting of iron-nickel oxide (FexNiyOz), silicon-aluminum oxide (AlxSiyOz), aluminum oxide (Al2O3), and titanium oxide (TiO2); the first transition metal system is Fe, Cu, Ir, or Pt, and the second transition metal system is Pd, Ni, or Co. Based on 100 wt% of the catalyst material, the sum of the weight percentages of the first and second transition metals is between 0.2 wt% and 2.5 wt%; and, based on the sum of the moiré fractions of the second and first transition metals being 100%, the moiré fraction of the second transition metal is 1 to 2 times that of the moiré fraction of the first transition metal.
[0008] According to the present invention, when the carrier is an iron-nickel oxide (FexNiyOz), if x=1, then y=1 or 2, z=3 or 4; if x=2, then y=1, z=4; if x=5, then y=1, z=8. In one embodiment, the FexNiyOz can specifically be FeNiO3, FeNi2O4, Fe2NiO4, or Fe5NiO8.
[0009] According to the present invention, when the carrier is aluminum silicon oxide (AlxSiyOz), if x=1, then y=1, 2, 3 or 4, and z=3, 6, 8 or 10; if x=2, then y=1 or 2, and z=5, 6, 7 or 9. In one embodiment, the AlxSiyOz can specifically be AlSiO3, AlSi2O6, AlSi3O8, AlSi4O10, Al2SiO5, Al2SiO6, Al2Si2O6, Al2Si2O7 or Al2Si2O9.
[0010] According to the present invention, when the carrier is aluminum silicon oxide (AlxSiyOz), the first transition metal can be selected from Fe or Cu, and the second transition metal can be selected from Pd, Ni or Co.
[0011] According to the present invention, when the support is titanium oxide (TiO2), the first transition metal can be Ir and the second transition metal can be Pd.
[0012] According to the present invention, when the carrier is an iron-nickel oxide (FexNiyOz), the first transition metal can be Pt, and the second transition metal can be Pd.
[0013] According to the present invention, when the carrier is aluminum oxide (Al₂O₃), the first transition metal can be Pt, the second transition metal can be Pd, and the Pt is deposited or coated on the surface of the Pd.
[0014] In one embodiment, when the first transition metal is Fe, the precursor of Fe can be selected from Fe(NO 3) 3·9H 2O (Iron nitrate), FeCl 3 (Ferric chloride), FeSO 4·7H 2O (Ferrous sulfate heptahydrate), FeCl 2·4H 2O (Ferrous chloride tetrahydrate), Fe(CH 3COO) 2 (Ferrous acetate), Fe(CO) 5 (Iron pentacarbonyl) or Fe 2(SO 4) 3 (Ferric sulfate).
[0015] In one embodiment, when the first transition metal is Cu, the precursor of Cu can be selected from Cu(NO3)2 (Copper(II) nitrate), CuSO4·5H2O (Copper sulfate pentahydrate), CuCl2·2H2O (Copper chloride dihydrate), Cu(CH3COO)2 (Copper acetate), Cu(acac)2 (Copper acetylacetonate), CuBr2 (Copper bromide) or Cu(CO)4 (Copper carbonyl).
[0016] In one embodiment, when the first transition metal is Ir, the precursor of Ir can be selected from IrCl 3·xH 2O (Iridium trichloride hydrate), Ir(NO 3) 3 (Iridium(III) nitrate), Ir(CO) 2Cl (Iridium(III) dichlorocarbonyl), Ir(acac) 3 (Iridium(III) acetylacetonate), IrBr 3 (Iridium(III) bromide), IrI 3 (Iridium(III) iodide), Ir(OH) 3 (Iridium(III) hydroxide), Ir(CO) 4 (Iridium(I) carbonyl) or IrCl 4 (Iridium(IV) chloride).
[0017] In one embodiment, when the first transition metal is Pt, the precursor of Pt can be selected from H 2PtCl 6·6H 2O (Chloroplatinic acid hexahydrate), Pt(C 5H 7O 2) 2 (Platinum acetylacetonate), PtCl 2 (Platinum chloride), PtBr 2 (Platinum bromide), PtI 2 (Platinum iodide), Pt(NH 3) 2Cl 2 (cis-diamminedichloroplatinum), Na 2PtCl 6·6H 2O (Sodium hexachloroplatinate hexahydrate) or K 2PtCl 6·6H 2O (potassium hexachloroplatinate hexahydrate).
[0018] In one embodiment, when the second transition metal is Pd, the precursor of Pd can be selected from Pd(C5H7O2)2 (Palladium acetylacetonate), PdCl2 (Palladium chloride), PdBr2 (Palladium bromide), PdI2 (Palladium iodide), K2PdCl4 (Potassium chloropalladite), K2PdCl6 (Palladium hexachloroplatinate), Pd(NO3)2·2H2O (Palladium nitrate dihydrate), Na2PdCl4·xH2O (Sodium tetrachloropalladate(II) hydrate) or Na2PdCl6·4H2O (Sodium hexachloropalladate(IV) tetrahydrate).
[0019] In one embodiment, when the second transition metal is Ni, the precursor of Ni can be selected from Ni(NO 3) 2·6H 2O (Nickel nitrate hexahydrate), NiCl 2·6H 2O (Nickel chloride hexahydrate), NiSO 4·6H 2O (Nickel sulfate hexahydrate), Ni(CH 3COO) 2·4H 2O (Nickel acetate tetrahydrate), Ni(CO) 4 (Nickel tetracarbonyl), Ni(OH) 2 (Nickel hydroxide) or Ni(acac) 2 (Nickel acetylacetonate).
[0020] In one embodiment, when the second transition metal is Co, the precursor of Co can be selected from Co(NO3)2·6H2O (Cobaltous(II) nitrate hexahydrate), CoCl2·6H2O (Cobalt(II) chloride hexahydrate), CoSO4·7H2O (Cobalt(II) sulfate heptahydrate), Co(CH3COO)2·4H2O (Cobalt(II) acetate tetrahydrate), Co(acac)2 (Cobalt(II) acetylacetonate), CoBr2 (Cobalt(II) bromide), Co(OH)2 (Cobalt(II) hydroxide) or Co(CO)4 (Cobalt(I) carbonyl).
[0021] According to the present invention, when the support is the iron-nickel oxide (FexNiyOz), the Fe precursor of the support can be selected from FeCl3 (Ferric chloride), FeSO4·7H2O (Ferrous sulfate heptahydrate), FeCl2·4H2O (Ferrous chloride tetrahydrate), Fe(CH3COO)2 (Ferrous acetate), Fe(CO)5 (Iron pentacarbonyl), or Fe2(SO4)3 (Ferric sulfate); the Ni precursor of the support can be selected from NiCl2·6H2O (Nickel chloride hexahydrate), NiSO4·6H2O (Nickel sulfate hexahydrate), Ni(CH3COO)2·4H2O (Nickel acetate tetrahydrate), Ni(CO)4 (Nickel tetracarbonyl), Ni(OH)2 (Nickel hydroxide), or Ni(acac)2 (Nickel... acetylacetonate).
[0022] In one embodiment, the surfactant used in the preparation of the iron-nickel oxide (FexNiyOz) can be selected from Triton TMX-100 (Polyethylene glycol tert-octylphenyl ether), Triton TMX-114 (Polyethylene glycol n-dodecyl ether), Triton TMX-405 (Polyethylene glycol nonylphenyl ether), Tween 20 (Polysorbate 20), Tween 80 (Polysorbate 80), Pluronic ⓇF-127 (Polyethylene glycol-polypropylene glycol block copolymer), Brij Ⓡ35 (Polyoxyethylene lauryl ether), Myrj Ⓡ52 (Polyoxyethylene sorbitan monolaurate), Sorbitan esters (Span series), SDS (Sodium dodecyl sulfate), CTAB (Cetyltrimethylammonium bromide), Brij 35 (Polyoxyethylene lauryl ether), Span 80 (Sorbitan monooleate) or Dodecylbenzene sulfonic acid (DBSA).
[0023] According to the present invention, when the support is the aluminum silicon oxide (Al xSi yO z), the Al precursor of the support can be selected from Al(NO 3) 3·9H 2O (Aluminum nitrate), Al(OC 3H 7) 3 (Aluminum isopropoxide), Al 2(SO 4) 3 (Aluminum sulfate), AlCl 3 (Aluminum chloride), Al(OH) 3 (Aluminum hydroxide), NaAlO 2 (Sodium aluminate) or Al(OC 4H 9) 3 (Aluminum sec-butoxide); the Si precursor of the support can be selected from Si(OC 2H 5) 4 (Tetraethyl orthosilicate, TEOS), SiO 2 (Fumed silica, Colloidal silica), Si(OH) 4 (Silicic acid), Na 2SiO 3 (Sodium metasilicate) or SiCl 4 (Silicon tetrachloride).
[0024] In one embodiment, the template additive used in the preparation of the silicon aluminum oxide (AlxSiyOz) can be selected from [(C3H7)4N]OH (Tetra-n-propylammonium hydroxide, TPAH), N(CH3)4OH (Tetramethylammonium hydroxide, TMAH), N(C4H9)4OH (Tetrabutylammonium hydroxide, TBAH), C6H12N4 (Hexamethylenetetramine, HMTA), C2H5NH2 (Ethylamine), (C2H5)2NH2 (Diethylamine), (C2H5)3N (Triethylamine), C4H9N (Pyrrolidine), R4N +X- (Quaternary ammonium salts, where R is an alkyl group and X is a halogen) or C16H3N(CH3)3Br2 (Cetyltrimethylammonium bromide, CTAB).
[0025] According to the present invention, when the carrier is alumina (Al₂O₃), the carrier may be commercial alumina with a specific surface area (BET) greater than 200 m² / g; the brand of commercial alumina may be selected from Alfa Aesar, Sigma-Aldrich or BASF.
[0026] According to the present invention, when the support is titanium dioxide (TiO2), the support can be commercial titanium dioxide with a specific surface area (BET) greater than 50 m2 / g; the brand of commercial titanium dioxide can be Chemours or Evonik.
[0027] In one embodiment, with the catalyst material comprising 100 wt%, the weight percentage of the first transition metal and the second transition metal may optionally be 0.2 wt%, 0.4 wt%, 0.6 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.4 wt%, 1.6 wt%, 1.8 wt%, 2 wt%, 2.2 wt%, 2.4 wt%, or 2.5 wt%; the weight percentage of the first transition metal and the second transition metal may fall within the range of any two of the above values, but is not limited thereto.
[0028] In one embodiment, taking the sum of the moiré fraction of the second transition metal and the moiré fraction of the first transition metal as 100%, the moiré fraction ratio of the second transition metal to the first transition metal can optionally be 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1 or 2:1; the moiré fraction ratio of the second transition metal to the first transition metal can be within the range formed by any two of the above values, but is not limited thereto.
[0029] According to the present invention, both the first transition metal and the second transition metal can be monatomic metals.
[0030] In one embodiment, the dimensions of the first transition metal and the second transition metal can each be independently between 0.2 nm and 3.0 nm. Optionally, the dimensions of the first transition metal and the second transition metal can each be independently between 0.2 nm, 0.4 nm, 0.6 nm, 0.8 nm, 1 nm, 1.2 nm, 1.4 nm, 1.6 nm, 1.8 nm, 2 nm, 2.2 nm, 2.4 nm, 2.6 nm, 2.8 nm, or 3 nm; the dimensions of the first transition metal and the second transition metal can each be independently within the range formed by any two of the above values, but are not limited thereto.
[0031] In one embodiment, the size of the catalyst material can be from 29 nm to 412 nm, and the D50 can be from 37.9 nm to 337.3 nm.
[0032] Optionally, the size of the catalyst material may be 29nm, 30nm, 90nm, 120nm, 150nm, 180nm, 210nm, 240nm, 270nm, 300nm, 330nm, 360nm, 390nm, 400nm or 412nm; the size of the catalyst material may be within the range of any two of the above values, but is not limited thereto.
[0033] Optionally, the D50 of the catalyst material can be 37.9nm, 40nm, 70nm, 100nm, 130nm, 160nm, 190nm, 220nm, 250nm, 280nm, 310nm or 337.3nm; the size of the catalyst material can be within the range of any two of the above values, but is not limited thereto.
[0034] In one embodiment, the specific surface area (BET) of the catalyst material can be from 119.4 m² / g to 402.1 m² / g. Optionally, the specific surface area (BET) of the catalyst material can be 119.4 m² / g, 120 m² / g, 150 m² / g, 180 m² / g, 210 m² / g, 240 m² / g, 270 m² / g, 300 m² / g, 330 m² / g, 360 m² / g, 390 m² / g, or 402.1 m² / g; the specific surface area (BET) of the catalyst material can be within the range formed by any two of the above values, but is not limited thereto.
[0035] In one embodiment, the total pore volume of the catalyst material can be from 0.19 cm³ / g to 0.81 cm³ / g. Optionally, the total pore volume of the catalyst material can be 0.19 cm³ / g, 0.2 cm³ / g, 0.3 cm³ / g, 0.4 cm³ / g, 0.5 cm³ / g, 0.6 cm³ / g, 0.7 cm³ / g, 0.8 cm³ / g, or 0.81 cm³ / g; the total pore volume of the catalyst material can be within the range of any two of the above values, but is not limited thereto.
[0036] In one embodiment, the pore size of the catalyst material can be from 9.2 nm to 47.2 nm. Optionally, the pore size of the catalyst material can be 9.2 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, or 47.2 nm; the pore size of the catalyst material can be within the range formed by any two of the above values, but is not limited thereto.
[0037] Another object of the present invention is to provide an application of the aforementioned catalyst material, wherein the catalyst material is added to a support material so that the catalyst material and the support material together form a filter element for filtering an aerosolized molecular contaminant (AMC), the filter element being used to contact and decompose the aerosolized molecular contaminant.
[0038] According to the present invention, the catalyst material is added to the support material through impregnation, coating, mixing or spraying techniques, so that the catalyst material and the support material together form the filter element for contacting and decomposing the air-suspended molecular pollutants.
[0039] In one embodiment, the support material is prepared according to a "method for preparing a filter element for suspended gaseous pollutants" disclosed in Republic of China Patent Publication No. TW202404683A. In this embodiment, the support material is a cloth-like material, which is immersed in a co-solvent containing a catalyst material and then dried and shaped to form the filter element; wherein, based on the total weight of the filter element being 100 wt%, the amount of catalyst material added to the cloth-like material is 0.1 wt% to 30 wt%. Specifically, the co-solvent can be an ethanol-containing solvent.
[0040] In another embodiment, the support material is selected from a fabric formed by needle-knitting a fiber mixture; the fabric defines a filtering region and a flat region, wherein the flat region surrounds the filtering region, and the filtering region is formed into a plurality of parallel straight-line corrugations by vacuum forming. The fiber mixture is selected from polyester fiber, nylon, rayon, hot-melt cotton, moisture-absorbing cotton, or a combination thereof.
[0041] In another embodiment, based on a total weight of 100 wt% for the filter element, the filter element is a nonwoven sheet filter element formed by uniformly mixing 70 wt% to 99.9 wt% of a polymer composition with 0.1 wt% to 30 wt% of the catalyst material, and then using melt-blowing and spinning techniques. The polymer composition includes at least a plastic material and a binder material. The binder material is used to enhance processability during production and stability between dissimilar materials (e.g., between the catalyst material and the plastic material). The binder material can be polyvinyl alcohol, polyethylene oxide, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyacrylic acid, or polyurethane, but is not limited thereto. The plastic material can be polyethylene, polypropylene, polyethylene terephthalate, polyethylene terephthalate, cyclohexanediol, or nylon, but is not limited thereto. Specifically, the meltblown technology refers to spraying a uniformly mixed polymer composition and catalyst material through a nozzle surrounded by high-speed blow molding gas onto a spinneret to spin out a filter element in the form of a nonwoven sheet with randomly deposited catalyst material. In other words, the support material is a nonwoven fabric composed of a polymer composition, and at least a portion of the catalyst material is coated on the surface of the nonwoven fabric and can contact aerosolized molecular pollutants.
[0042] In one embodiment, based on the total weight of the filter element as 100 wt%, the filter element comprises 1.7 to 28.3 wt% of the catalyst material, 0.1 to 5 wt% of the binder material, and 66.7 to 98 wt% of the plastic material.
[0043] In one embodiment, based on the total weight of the filter element as 100 wt%, the filter element comprises 4.8 to 28.3 wt% of the catalyst material, 0.1 to 5 wt% of the binder material, and 66.7 to 95.1 wt% of the plastic material.
[0044] In one embodiment, based on the total weight of the filter element being 100wt%, the amount of catalyst material added can be greater than 0wt% to less than or equal to 30wt%. In another embodiment, based on a total weight of 100wt% for the catalyst material and the support material, the amount of catalyst material added can be 0.1wt%, 0.5wt%, 1.5wt%, 2.5wt%, 3.5wt%, 4.8wt%, 5.5wt%, 6.5wt%, 7.5wt%, 8.5wt%, 9.5wt%, 10.5wt%, 11.5wt%, 12.5wt%, 13.5wt%, 14.5wt%, 15.5wt%, 16.5wt%, 17.5wt%, 18.5wt%, 19.5wt%, 20.5wt%, 21.5wt%, 22.5wt%, 23.5wt%, 24.5wt%, 25.5wt%, 26.5wt%, 27.5wt%, 28.3wt%, or 30wt%. The amount of catalyst material added can be within the range of any two of the above values, but is not limited thereto.
[0045] According to the present invention, the aerosolized molecular contaminant includes acetone, isopropanol (IPA), ethanol, ethyl acetate, toluene, xylene, trichloroethylene, propylene glycol monomethyl ether (PGME), propylene glycol monomethyl ether ester (PGMEA), dimethyl sulfoxide (DMSO), or N-methylpyrrolidone (NMP). Specifically, the catalyst material of the present invention is particularly suitable for treating any of the aerosolized molecular contaminants at concentrations from 10 ppb to 5000 ppm; preferably, the catalyst material of the present invention is particularly suitable for treating any of the aerosolized molecular contaminants at concentrations from 10 ppb to 1000 ppm; more preferably, the catalyst material of the present invention is particularly suitable for treating any of the aerosolized molecular contaminants at concentrations from 500 ppb to 100 ppm.
[0046] According to the present invention, the catalyst material achieves a removal rate of 90.5% for the aerosolized molecular pollutant at room temperature. In one embodiment, the catalyst material achieves a removal rate of 32.5% to 90.5% for the aerosolized molecular pollutant at room temperature. Specifically, the removal rate of the catalyst material for the aerosolized molecular pollutant at room temperature can be 32.5%, 37.2%, 38.5%, 39.6%, 40.7%, 42.3%, 46.5%, 49.3%, 49.6%, 54.3%, 59.6%, 66.5%, 76.2%, or 90.5%; the removal rate of the catalyst material for the aerosolized molecular pollutant at room temperature can be within the range of any two of the above values, but is not limited thereto.
[0047] According to the present invention, the reaction temperature (T 90) at which the catalyst material achieves a 90% removal efficiency of aerosolized molecular contaminants is lower than or equal to 171.4°C. In one embodiment, the reaction temperature (T 90) at which the catalyst material achieves a 90% removal efficiency of aerosolized molecular contaminants can be from 25°C to 171.4°C (25°C ≤ T 90 ≤ 171.4°C). Specifically, the reaction temperature (T 90) at which the catalyst material achieves a 90% removal efficiency of aerosolized molecular contaminants can be 25°C, 63.2°C, 82.1°C, 92.5°C, 99.5°C, 103.4°C, 117°C, 121°C, 133.2°C, 135°C, 151.2°C, 164.5°C, 167°C, or 171.4°C; the reaction temperature (T 90) at which the catalyst material achieves a 90% removal efficiency of aerosolized molecular contaminants can fall within the range of any two of the above values, but is not limited thereto.
[0048] Regarding the techniques, means, and other effects adopted by the present invention to achieve the above objectives, preferred embodiments are described in detail below with reference to the accompanying drawings. Simple Explanation of the Diagram
[0049] Figure 1 is a TEM image of the catalyst material with loaded metal in Embodiment 1 of the present invention. Figure 2 is a TEM image of the catalyst material with loaded metal in Embodiment 3 of the present invention. Figure 3 is a TEM image of the catalyst material with loaded metal in Embodiment 7 of the present invention. Figure 4 is a bar graph showing the isopropanol removal efficiency of the catalyst material added to the cloth at different amounts in Example 4 of the present invention. Implementation
[0050] The following examples illustrate the implementation of the catalyst material of the present invention and its application. Those skilled in the art can easily understand the advantages and effects of this invention through the following examples and comparative examples. It should be understood that the examples listed in this specification are merely illustrative of the implementation of the present invention and are not intended to limit the scope of the present invention. Those skilled in the art can make various modifications and alterations based on their knowledge without departing from the spirit of the present invention to implement or apply the content of the present invention.
[0051] [Preparation of Catalyst Materials] []
[0052] As shown in Table 1 below, the present invention provides catalyst materials for Examples 1 to 7 (E1 to E7) and Comparative Examples 1 to 9 (C1 to C9). Taking Example 1 (E1) as an example, the catalyst material is represented as "Pt 1Pd 1 / Fe xNi yO z", where the part after the " / " refers to the composition name of the carrier of the catalyst material, such as "Fe xNi yO z", and the part before the " / " refers to the composition name of the loaded metal of the catalyst material, such as "Pt 1Pd 1". Taking Example 6 (E6) as an example, the catalyst material is represented as "Pt / PdO / Al 2O 3", where the part after the second " / " refers to the composition name of the carrier of the catalyst material, such as "Al 2O 3", and the part before the second " / " refers to the composition name of the loaded metal of the catalyst material, such as "Pt / PdO".
[0053] Table 1: Metal loading and TEM dimensions of the negative contact metals of the catalyst materials in Examples 1 to 7 (E1 to E7) and Comparative Examples 1 to 9 (C1 to C9). sample code name Catalyst materials (Loaded metal / carrier) Metal loading (wt%) Loaded metal TEM size (nm) E1 Pt 1Pd 1 / Fe xNi yO z 0.5 0.2-2 C1 Pt 1 / Fe xNi yO z 0.5 0.2–2 C2 Pd 1 / Fe xNi yO z 0.5 0.2–2 E2 Fe 1Pd 2 / Al xSi yO z 0.5 0.2–2 E3 Cu 1Pd 2 / Al xSi yO z 0.5 1.0-2.0 E4 Faith 1Ni 2 / Al xSi yO z 0.5 0.2–2 E5 Fe 1Co 2 / Al xSi yO z 0.5 0.2–2 C3 Cu 1 / Al xSi yO z 0.5 <1 C4 Pd 1 / Al xI yO z 0.5 0.2–2 C5 Faith 1Ni 2 / Al xSi yO z 0.5 3.7–10.9 C6 Mn 1Co 2 / Al xSi yO z 0.5 4.3–12.8 E6 Pt / PdO / Al 2O 3 0.2 2.0-3.0 C7 Pt / PdO / Al 2O 3 0.1 2.0-3.0 E7 Ir 1Pd 1 / TiO 2 2.5 0.2-2 C8 Ir 1 / TiO 2 2.5 0.2-2 C9 Pd1 / TiO2 2.5 0.2-2
[0054] The following describes the preparation methods of the catalyst materials of Examples 1 to 7 (E1 to E7) and Comparative Examples 1 to 9 (C1 to C9) in Table 1 above.
[0055] [Example] [1(E1)] [:] [Pt, 1, Pd, 1, / ] [Fe, x , Ni , y , O , z , ] [Method of preparation] []
[0056] The preparation steps of the FexNiyOz support include: weighing appropriate amounts of nickel nitrate (Ni(NO3)2·6H2O, Sigma-Aldrich, 99.9%) and ferric nitrate (Fe(NO3)3·9H2O, Sigma-Aldrich, 99.9%), dissolving them in an appropriate amount of deionized water, wherein the weight ratio of nickel nitrate:ferric nitrate:deionized water is 28.9:29.7:200, and stirring for at least 30 minutes. Subsequently, titration is performed with a 2N potassium hydroxide (KOH, Sigma-Aldrich, 85%) solution, and the redox potential of the mixed solution is monitored to be -0.1783V; the mixing process is carried out at 500 rpm and 35°C for 1 hour. The solid and liquid phases were then separated by a continuous centrifuge; after washing and drying, the mixture was dried at 60°C for one day; subsequently, it was calcined in a high-temperature furnace at a rate of 5°C per minute from room temperature to 400°C to 600°C, and held at that temperature for 12 hours to obtain Fe xNi yO z powder; the Fe xNi yO z powder can be composed of FeNiO 3, FeNi 2O 4, Fe 2NiO 4, Fe 5NiO 8 or a mixture thereof.
[0057] The preparation steps of Pt 1Pd 1 / Fe xNi yO z catalyst material include: adding the aforementioned Fe xNi yO z powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an Fe xNi yO z aqueous solution. Subsequently, appropriate amounts of Triton X-100 (Sigma-Aldrich), hexachloroplatinic acid (H₂PtCl₆·6H₂O, Sigma-Aldrich, 99.9%), and potassium tetrachloropalladate (K₂PdCl₄, Sigma-Aldrich, 98%) were weighed and prepared into 2.5 mM, 12.8 mM, and 23.5 mM mother liquors, respectively. These were then added sequentially to the aforementioned Fe₂xNi₂O₂ aqueous solution, stirred continuously for 30 minutes, and heated to 65°C at a rate of 5°C per minute. When the temperature reached 65°C, 45 mM sodium borohydride (NaBH₄, Sigma-Aldrich, 98%) was added. After observing the change in redox potential from 0.057 V to 0.065 V, the mixture was cooled to room temperature under a nitrogen atmosphere, followed by solid-liquid separation. The mixture was then dried at 60°C for one day to obtain the Pt₁Pd₁ / Fe₂O₃ of Example 1 (E1). xNi yO z catalyst materials.
[0058] [Example] [2(E2)] [:] [Fe, 1, Pd, 2, / Al, x , Si , y , O , z , ] [Method of preparation] []
[0059] The preparation steps of AlxSiyOz support include: weighing appropriate amounts of aluminum nitrate (Al(NO3)3·9H2O, Sigma-Aldrich, 98%), sodium silicate (Na2SiO3, Sigma-Aldrich, 95%), and tetrapropylammonium hydroxide (TPAH, Sigma-Aldrich, 99%), dissolving them in an appropriate amount of deionized water, wherein the weight ratio of aluminum nitrate:sodium silicate:tetrapropylammonium hydroxide:deionized water is 55.62:26.07:5:200, stirring for at least 30 minutes, then transferring to a high-pressure reactor, heating to 155°C at 5°C per minute for 6 hours, then separating the solid and liquid using a continuous centrifuge, washing and drying with water, drying at 60°C for one day, and then calcining in a high-temperature furnace at 5°C per minute from room temperature to 450°C to 550°C, holding the calcination temperature for 12 hours to obtain AlxSiyOz powder; the AlxSiyOz... The yO z powder can be composed of AlSiO 3, AlSi 2O 6, AlSi 3O 8, AlSi 4O 10, Al 2SiO 5, Al 2SiO 6, Al 2Si 2O 6, Al 2Si 2O 7, Al 2Si 2O 9 or a mixture thereof.
[0060] The preparation steps of the Fe1Pd2 / AlxSiyO2 catalyst material include: adding the aforementioned AlxSiyO2 powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an AlxSiyO2 aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich), ferric nitrate (Fe(NO3)3·9H2O, Sigma-Aldrich, 99.9%) and potassium tetrachloropalladate (K2PdCl4, Sigma-Aldrich, 98%), and preparing 2.5 mM, 16.43 mM, and 23.5 mM stock solutions respectively, and adding them sequentially to the AlxSiyO2 aqueous solution, stirring continuously for 30 minutes, and heating to 65°C at 5°C per minute. When the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH2O2) 4, Sigma-Aldrich (98%), after observing the change in redox potential from 0.057V to 0.0981V, it was cooled to room temperature under nitrogen coating, followed by solid-liquid separation, and dried at 60°C for one day to obtain the Fe1Pd2 / AlxSiyO2 catalyst material of Example 2 (E2).
[0061] [Example] [3(E3)] [:] [Cu, 1, Pd, 2, / Al, x , Si , y , O , z , ] [Method of preparation] []
[0062] The preparation steps of the Al xSi yO z support are the same as those of the Al xSi yO z support in Example 2 (E2) to obtain Al xSi yO z powder; the Al xSi yO z powder can be composed of AlSiO 3, AlSi 2O 6, AlSi 3O 8, AlSi 4O 10, Al 2SiO 5, Al 2SiO 6, Al 2Si 2O 6, Al 2Si 2O 7, Al 2Si 2O 9 or a mixture thereof.
[0063] The preparation steps of the Cu1Pd2 / AlxSiyO2 catalyst material include: adding the aforementioned AlxSiyO2 powder to an appropriate amount of deionized water, stirring at 500 rpm for 30 minutes at 35°C to form an AlxSiyO2 aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich), copper nitrate (Cu(NO3)2·3H2O, Sigma-Aldrich, 98%), and potassium tetrachloropalladate (K2PdCl4, Sigma-Aldrich, 98%), and preparing 2.5 mM, 74.88 mM, and 23.5 mM stock solutions respectively, and adding them sequentially to the aforementioned AlxSiyO2 aqueous solution, stirring continuously for 30 minutes, and heating to 65°C at 5°C per minute; when the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH2O2). 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.057V to 0.0981V, the material was cooled to room temperature under nitrogen coating, followed by solid-liquid separation and drying at 60°C for one day to obtain the Cu 1Pd 2 / Al xSi yO z catalyst material of Example 3 (E3).
[0064] [Example] [4(E4)] [:] [Fe, 1, Ni, 2, / ] [Al , x , Si , y , O , z , ] [Method of preparation]
[0065] The preparation steps of the Al xSi yO z support are the same as those of the Al xSi yO z support in Example 2 (E2) to obtain Al xSi yO z powder; the Al xSi yO z powder can be composed of AlSiO 3, AlSi 2O 6, AlSi 3O 8, AlSi 4O 10, Al 2SiO 5, Al 2SiO 6, Al 2Si 2O 6, Al 2Si 2O 7, Al 2Si 2O 9 or a mixture thereof.
[0066] The preparation steps of the Fe1Ni2 / AlxSiyO2 catalyst material include: adding AlxSiyO2 powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an AlxSiyO2 aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich), ferric nitrate (Fe(NO3)3·9H2O, Sigma-Aldrich, 99.9%), and nickel nitrate (Ni(NO3)2·6H2O, Sigma-Aldrich, 99.9%), and preparing 2.5 mM, 44.77 mM, and 42.60 mM stock solutions respectively, and adding them sequentially to the aforementioned AlxSiyO2 aqueous solution, stirring continuously for 30 minutes, and increasing the temperature to 65°C at 5°C per minute. When the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH2O) 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.057V to 0.0981V, the material was cooled to room temperature under nitrogen coating, followed by solid-liquid separation and drying at 60°C for one day to obtain the Fe1Ni2 / AlxSiyO2 catalyst material of Example 4 (E4).
[0067] [Example] [5(E5)] [:] [Fe, 1, Co, 2, / ] [Al , x , Si , y , O , z , ] [Method of preparation]
[0068] The preparation steps of the Al xSi yO z support are the same as those of the Al xSi yO z support in Example 2 (E2) to obtain Al xSi yO z powder; the Al xSi yO z powder can be composed of AlSiO 3, AlSi 2O 6, AlSi 3O 8, AlSi 4O 10, Al 2SiO 5, Al 2SiO 6, Al 2Si 2O 6, Al 2Si 2O 7, Al 2Si 2O 9 or a mixture thereof.
[0069] The preparation steps of the Fe1Co2 / AlxSiyO2 catalyst material include: adding AlxSiyO2 powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an AlxSiyO2 aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich), ferric nitrate (Fe(NO3)3·9H2O, Sigma-Aldrich, 99.9%) and cobalt nitrate (Co(NO3)2·6H2O, Sigma-Aldrich, 99.9%), and preparing 2.5 mM, 44.77 mM, and 42.42 mM stock solutions respectively, and adding them sequentially to the aforementioned AlxSiyO2 aqueous solution, stirring continuously for 30 minutes, and increasing the temperature to 65°C at 5°C per minute. When the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH2O) 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.057V to 0.0981V, the material was cooled to room temperature under nitrogen coating, followed by solid-liquid separation and drying at 60°C for one day to obtain the Fe1Co2 / AlxSiyO2 catalyst material of Example 5 (E5).
[0070] [Example] [6(E6)] [:] [Pt / PdO / Al, 2, O, 3, ] [Method of preparation]
[0071] The Al₂O₃ support used commercial alumina (Al₂O₃) powder (Alfa Aesar, BET > 200 m² / g).
[0072] The preparation steps of the Pt / PdO / Al₂O₃ catalyst material include: adding the aforementioned Al₂O₃ powder to an appropriate amount of deionized water, stirring at 500 rpm for 30 minutes at 35°C to form an Al₂O₃ aqueous solution. Subsequently, appropriate amounts of Triton™ X-100 (Sigma-Aldrich), hexachloroplatinic acid (H₂PtCl₆·6H₂O, Sigma-Aldrich, 99.9%), and potassium tetrachloropalladate (K₂PdCl₄, Sigma-Aldrich, 98%) were weighed and prepared into 2.5 mM, 12.8 mM, and 23.5 mM stock solutions, respectively. These were then added sequentially to the aforementioned Al₂O₃ aqueous solution, and stirred continuously for 30 minutes. The temperature was increased to 65°C at a rate of 5°C per minute. When the temperature reached 65°C, 45 mM sodium borohydride (NaBH₄, Sigma-Aldrich, 98%) was added. The redox potential was observed to change from 0.057 V to 0.065 V. The solution was then cooled to room temperature under a nitrogen atmosphere, followed by solid-liquid separation. The solution was dried at 60°C for one day to obtain the Pt / PdO / Al₂O₃ of Example 6 (E6). 3 Catalyst materials.
[0073] [Example] [7(E7)] [:] [Ir, 1, Pd, 1, / TiO, 2, ] [Method of preparation]
[0074] The TiO2 support used commercial titanium dioxide (TiO2) powder (Chemours, BET >50 m2 / g).
[0075] The preparation steps of the Ir 1Pd 1 / TiO 2 catalyst material include: adding the aforementioned TiO 2 powder to an appropriate amount of deionized water / alcohol (ratio 1:1), stirring at 500 rpm for 30 minutes at 30°C to form a TiO 2 aqueous solution. Subsequently, appropriate amounts of Triton™ X-100 (Sigma-Aldrich), iridium platinum chloride (IrCl3·xH2O, Sigma-Aldrich, 99.9%), and potassium tetrachloropalladate (K2PdCl4, Sigma-Aldrich, 98%) were weighed and prepared into 2.5 mM, 13.1 mM, and 23.5 mM stock solutions, respectively. These were then added sequentially to the aforementioned TiO2 aqueous solution, stirred continuously for 30 minutes, and heated to 85°C at a rate of 5°C per minute. When the temperature reached 85°C, 80 mM urea (Sigma-Aldrich, 99.5%) was added. The redox potential was observed to change from 0.057 V to 0.065 V. The solution was then cooled to room temperature under a nitrogen atmosphere, followed by a solid-liquid separation step. The solution was dried at 60°C for one day to obtain the Ir1Pd1 / TiO2 catalyst material of Example 7 (E7).
[0076] [Comparative Example] [1(C1)] [:] [Pt, 1, / ] [Fe, x , Ni , y , O , z , ] [Method of preparation]
[0077] The preparation steps of the Fe xNi yO z support are the same as those of the Fe xNi yO z support in Example 1 (E1) to obtain Fe xNi yO z powder; the Fe xNi yO z powder can be a powder composed of FeNiO 3, FeNi 2O 4, Fe 2NiO 4, Fe 5NiO 8 or a mixture thereof.
[0078] The preparation steps of the Pt 1 / Fe xNi yO z catalyst material include: adding the aforementioned Fe xNi yO z powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an Fe xNi yO z aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich) and hexachloroplatinic acid (H 2PtCl 6·6H 2O, Sigma-Aldrich, 99.9%), preparing 2.5 mM and 12.8 mM stock solutions respectively, and adding them sequentially to the aforementioned Fe xNi yO z solution, stirring continuously for 30 minutes, and heating to 65°C at 5°C per minute; when the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH 2) 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.35V to 0.36V, it was cooled to room temperature under nitrogen coating, followed by solid-liquid separation and drying at 60°C for one day.
[0079] [Comparative Example] [2(C2)] [:] [Pd, 1, ] [ / ] [Fe, x , Ni , y , O , z , ] [Method of preparation]
[0080] The preparation steps of the Fe xNi yO z support are the same as those of the Fe xNi yO z support in Example 1 (E1) to obtain Fe xNi yO z powder; the Fe xNi yO z powder can be a powder composed of FeNiO 3, FeNi 2O 4, Fe 2NiO 4, Fe 5NiO 8 or a mixture thereof.
[0081] The preparation steps of the Pd1 / FexNiyOz catalyst material include: adding the aforementioned FexNiyOz powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an FexNiyOz aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich) and potassium tetrachloropalladate (K2PdCl4, Sigma-Aldrich, 98%), preparing 2.5 mM and 23.5 mM stock solutions respectively, and adding them sequentially to the aforementioned FexNiyOz solution, stirring continuously for 30 minutes, and increasing the temperature to 65°C at 5°C per minute; when the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH2O2). 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.32V to 0.33V, it was cooled to room temperature under nitrogen cover, followed by solid-liquid separation and drying at 60°C for one day.
[0082] [Comparative Example] [3(C3)] [:] [Cu, 1, / Al, x , Si , y , O , z , ] [Method of preparation]
[0083] The preparation steps of the Al xSi yO z support are the same as those of the Al xSi yO z support in Example 2 (E2) to obtain Al xSi yO z powder; the Al xSi yO z powder can be composed of AlSiO 3, AlSi 2O 6, AlSi 3O 8, AlSi 4O 10, Al 2SiO 5, Al 2SiO 6, Al 2Si 2O 6, Al 2Si 2O 7, Al 2Si 2O 9 or a mixture thereof.
[0084] The preparation steps of Cu 1 / Al xSi yO z catalyst material include: adding Al xSi yO z powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an Al xSi yO z aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich) and copper nitrate (Cu(NO 3) 2.3H 2O (Sigma-Aldrich, 98%), preparing 2.5 mM and 74.88 mM stock solutions respectively, and adding them sequentially to the aforementioned Al xSi yO z solution, stirring continuously for 30 minutes, and increasing the temperature to 65°C at 5°C per minute. When the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH) 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.35V to 0.37V, it was cooled to room temperature under nitrogen coating, followed by solid-liquid separation and drying at 60°C for one day.
[0085] [Comparative Example] [4(C4)] [:] [Pd, 1, / Al, x , Si , y , O , z , ] [Method of preparation]
[0086] The preparation steps of the Al xSi yO z support are the same as those of the Al xSi yO z support in Example 2 (E2) to obtain Al xSi yO z powder; the Al xSi yO z powder can be composed of AlSiO 3, AlSi 2O 6, AlSi 3O 8, AlSi 4O 10, Al 2SiO 5, Al 2SiO 6, Al 2Si 2O 6, Al 2Si 2O 7, Al 2Si 2O 9 or a mixture thereof.
[0087] The preparation steps of the Pd 1 / Al xSi yO z catalyst material include: adding the aforementioned Al xSi yO z powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an Al xSi yO z aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich) and potassium tetrachloropalladium (K 2PdCl 4, Sigma-Aldrich, 98%), preparing 2.5 mM and 23.5 mM stock solutions respectively, and adding them sequentially to the aforementioned Al xSi yO z solution, stirring continuously for 30 minutes, and increasing the temperature to 65°C at 5°C per minute; when the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH 2) 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.40V to 0.41V, it was cooled to room temperature under nitrogen cover, followed by solid-liquid separation and drying at 60°C for one day.
[0088] [Comparative Example] [5(C5)] [:] [Fe, 1, Ni, 2, / ] [Al , x , Si , y , O , z , ] [Method of preparation]
[0089] The preparation steps of the Al xSi yO z support are the same as those of the Al xSi yO z support in Example 2 (E2) to obtain Al xSi yO z powder; the Al xSi yO z powder can be composed of AlSiO 3, AlSi 2O 6, AlSi 3O 8, AlSi 4O 10, Al 2SiO 5, Al 2SiO 6, Al 2Si 2O 6, Al 2Si 2O 7, Al 2Si 2O 9 or a mixture thereof.
[0090] The preparation steps of the Fe1Ni2 / AlxSiyO2 catalyst material include: adding the aforementioned AlxSiyO2 powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an AlxSiyO2 aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich), ferric nitrate (Fe(NO3)3·9H2O, Sigma-Aldrich, 99.9%), and nickel nitrate (Ni(NO3)2·6H2O, Sigma-Aldrich, 99.9%), and preparing mother liquors of 7.5 mM, 134.3 mM, and 42.60 mM respectively, and adding them sequentially to the aforementioned AlxSiyO2 solution, stirring continuously for 30 minutes, and heating to 65°C at 5°C per minute; when the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH2O) 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.45V to 0.46V, it was cooled to room temperature under nitrogen cover, followed by solid-liquid separation and drying at 60°C for one day.
[0091] [Comparative Example] [6(C6)] [:] [Mn, 1, Co, 2, / ] [Al , x , Si , y , O , z , ] [Method of preparation]
[0092] The preparation steps of the Al xSi yO z support are the same as those of the Al xSi yO z support in Example 2 (E2) to obtain Al xSi yO z powder; the Al xSi yO z powder can be composed of AlSiO 3, AlSi 2O 6, AlSi 3O 8, AlSi 4O 10, Al 2SiO 5, Al 2SiO 6, Al 2Si 2O 6, Al 2Si 2O 7, Al 2Si 2O 9 or a mixture thereof.
[0093] The preparation steps of the Mn1Co2 / AlxSiyO2 catalyst material include: adding the aforementioned AlxSiyO2 powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an AlxSiyO2 aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich), manganese nitrate (Mn(NO3)2·4H2O, Sigma-Aldrich, 99%) and cobalt nitrate (Co(NO3)2·6H2O, Alfa, 98%), and preparing mother liquors of 7.5 mM, 100.4 mM, and 100.6 mM respectively, and adding them sequentially to the aforementioned AlxSiyO2 solution, stirring continuously for 30 minutes, and heating to 65°C at 5°C per minute. When the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH2O) 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.41V to 0.42V, it was cooled to room temperature under nitrogen cover, followed by solid-liquid separation and drying at 60°C for one day.
[0094] [Comparative Example] [7(C7)] [:] [Pt / PdO / Al, 2, O, 3, ] [Method of preparation]
[0095] The Al₂O₃ support used commercial alumina (Al₂O₃) powder (Alfa Aesar, BET > 200 m² / g).
[0096] The preparation steps of the Pt / PdO / Al₂O₃ catalyst material include: adding the aforementioned Al₂O₃ powder to an appropriate amount of deionized water, stirring at 35°C and 500 rpm for 30 minutes to form an Al₂O₃ aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich), hexachloroplatinic acid (H₂PtCl₆·6H₂O, Sigma-Aldrich, 99.9%), and potassium tetrachloropalladate (K₂PdCl₄, Sigma-Aldrich, 98%), and preparing 2.5 mM, 6.4 mM, and 23.5 mM stock solutions respectively, and adding them sequentially to the aforementioned Al₂O₃ solution, stirring continuously for 30 minutes, and heating to 65°C at 5°C per minute; when the temperature reaches 65°C, adding 45 mM sodium borohydride (NaBH₂O) 4. Sigma-Aldrich (98%), after observing the change in redox potential from 0.45V to 0.46V, it was cooled to room temperature under nitrogen cover, followed by solid-liquid separation and drying at 60°C for one day.
[0097] [Comparative Example] [8(C8)] [:] [Ir, 1, / TiO, 2, ] [Method of preparation]
[0098] The TiO2 support used commercial titanium dioxide (TiO2) powder (Chemours, BET >50 m2 / g).
[0099] The preparation steps of the Ir 1 / TiO 2 catalyst material include: adding the aforementioned TiO 2 powder to an appropriate amount of deionized water / alcohol (weight ratio 1:1), stirring at 30°C and 500 rpm for 30 minutes to form a TiO 2 aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich) and iridium trichloride hydrate (IrCl 3.xH 2O, Sigma-Aldrich, 99.9%), preparing 2.5 mM and 13.1 mM stock solutions respectively, and sequentially adding the aforementioned TiO 1 / TiO 2 catalyst material. In the solution, stir continuously for 30 minutes, and increase the temperature to 85°C at a rate of 5°C per minute. When the temperature reaches 85°C, add 80mM urea (Urea4, Sigma-Aldrich, 99.5%). Observe the change in redox potential from 0.29V to 0.30V, cool to room temperature under nitrogen cover, and then perform solid-liquid separation. Dry at 60°C for one day.
[0100] [Comparative Example] [9(C9)] [:] [Pd, 1, / TiO, 2, ] [Method of preparation]
[0101] The TiO2 support used commercial titanium dioxide (TiO2) powder (Chemours, BET >50 m2 / g).
[0102] The preparation steps of the Pd1 / TiO2 catalyst material include: adding the aforementioned TiO2 powder to an appropriate amount of deionized water / alcohol (weight ratio 1:1), stirring at 30°C and 500 rpm for 30 minutes to form a TiO2 aqueous solution; subsequently, weighing appropriate amounts of Triton™ X-100 (Sigma-Aldrich) and potassium tetrachloropalladium (K2PdCl4, Sigma-Aldrich, 98%), preparing 2.5 mM and 23.5 mM stock solutions respectively, and sequentially adding the aforementioned TiO2... In the solution, stir continuously for 30 minutes, and increase the temperature to 85°C at a rate of 5°C per minute. When the temperature reaches 85°C, add 80mM urea (Urea4, Sigma-Aldrich, 99.5%). Observe the change in redox potential from 0.29V to 0.30V, cool to room temperature under nitrogen cover, and then perform solid-liquid separation. Dry at 60°C for one day.
[0103] [Testing of Catalyst Materials]
[0104] As shown in Table 1 above, in the cases of two transition metals, the TEM images obtained by transmission electron microscopy (TEM) of Examples 1 to 7 show that the size of the loaded metals in Examples 1 to 5 and 7 (E1 to E5, E7) is less than 2 nm, with the smallest size being only 0.2 nm and the largest size of the loaded metal reaching only 3 nm (E6). Compared with the comparative examples (C1 to C4, C8, C9) that only loaded a single transition metal, the catalyst materials of Examples 1 to 7 of the present invention can also bring about a significant synergistic effect due to the presence of bimetals. Compared with the comparative examples (C5, C6) that loaded two transition metals, the smaller TEM size of the loaded metals in Examples 1 to 7 can provide a higher density of active sites, improve the activity of the catalyst, increase the surface area, and improve the reaction selectivity and stability.
[0105] Figures 1 to 3 show TEM images of Examples 1, 3, and 7 of the present invention. As shown in Figure 1, the loaded metal particles in Example 1 are relatively uniformly distributed, with particle sizes ranging from approximately 0.2 nm to 2 nm, consistent with the data in Table 1. The particles in Figure 1 are relatively dispersed, indicating that the Pt and Pd loadings are uniformly distributed on the FexNiyOz surface, which helps improve catalyst activity. Furthermore, small particles contribute to increased specific surface area and catalytic activity, providing a synergistic effect in bimetallic catalysts and improving reaction efficiency. As shown in Figure 2, some larger particles, approximately 1.0 nm to 2.0 nm in size, can be observed in the loaded metal particles of Example 3, consistent with the TEM size description in Table 1. These particles form a clear dotted distribution on the matrix, indicating the presence of bimetallic particles. Moreover, the synergistic effect of the bimetallic Cu-Pd helps enhance the catalytic selectivity and activity of specific reactions. Unlike Example 1, the loaded metal particles in Example 3 are slightly larger, but still within a small range, contributing to high catalytic efficiency. As shown in Figure 3, the supported metal particles in Example 7 exhibit a relatively fine particle distribution, with particle sizes ranging from approximately 0.2 nm to 2 nm, consistent with the data in Table 1. The uniform particle distribution and small size on TiO2 demonstrate good dispersibility of the Ir-Pd particles, which is highly beneficial for improving catalytic performance. Furthermore, the good distribution of the Ir and Pd bimetallic system on the TiO2 support may enhance the stability and reactivity of the catalyst, especially in applications requiring high stability and long lifespan.
[0106] Table 2 below shows the test results of the catalyst material's dimensions, D50, specific surface area, total pore volume, and pore size parameters as described in Table 1.
[0107] This invention uses a particle size analyzer to detect the particle size of the catalyst materials. Comparison shows that the particle sizes of the bimetallic catalyst materials in Examples 1 to 7 (E1 to E7) are mostly concentrated in a small range. Taking E1 as an example, its particle size is 30 nm to 61 nm, which is significantly smaller than that of the monometallic catalysts in the comparative examples, such as C1 (29 nm to 62 nm) or C2 (33 nm to 66 nm). Smaller particle sizes provide more surface active sites, making it easier for reactants to contact the active surface, promoting the reaction, and effectively improving the catalytic activity. Furthermore, the D50 value is the median particle size. Compared with the corresponding comparative examples 1 to 9 (C1 to C9), E1 to E7 generally have smaller D50 values, indicating that the particle size distribution of the bimetallic catalyst materials E1 to E7 is more concentrated and uniform. For example, the D50 value of E1 is 47.5 nm, which is smaller than that of C1 (47.7 nm) and C2 (49.9 nm). Since smaller particles provide a larger surface area and active sites, the catalyst exhibits higher activity and stability during the reaction process. Therefore, E1 to E7, which have smaller D50 values, can help improve catalytic activity.
[0108] In terms of specific surface area, Examples 1 to 7 (E1 to E7) generally have a larger specific surface area than the corresponding Comparative Examples 1 to 9 (C1 to C9). For example, the specific surface area of E4 is 402.1 m² / g, compared to 339.4 m² / g of C5. Examples 1 to 7 have a sufficiently large surface area to provide ample active surface to promote the reaction, which is beneficial to improving the reaction rate and efficiency.
[0109] Regarding the total pore volume, Examples 1 to 7 (E1 to E7) generally have a smaller specific surface area compared to the corresponding Comparative Examples 1 to 9 (C1 to C9). For example, the total pore volume of E1 is 0.37 cm³ / g, which is slightly lower than that of C1 (0.39 cm³ / g) and C2 (0.38 cm³ / g). However, despite the smaller total pore volume, pore structure and size are more likely to have a positive impact on catalyst performance.
[0110] Regarding pore size, Examples 1 to 7 (E1 to E7) generally exhibit smaller pore sizes compared to the corresponding Comparative Examples 1 to 9 (C1 to C9). For example, the pore size of E3 is 9.2 nm, compared to 14.9 nm for C3 and 14.7 nm for C4. This demonstrates that the bimetallic catalyst material is more effective in promoting molecular diffusion and enhancing catalytic performance.
[0111] In general, bimetallic catalysts of grades E1 to E7, compared to those of grades C1 to C9, exhibit smaller particle sizes, providing more surface active sites to promote reaction and enhance catalytic activity. They also possess moderate specific surface areas and pore sizes to provide favorable molecular diffusion conditions, thus improving overall catalyst performance. Furthermore, their smaller D50 values result in more concentrated and uniform particle size distribution, contributing to reaction stability and improved selectivity. Compared to C1 to C9, bimetallic catalysts of grades E1 to E7 demonstrate significant synergistic effects, offering substantial advantages in enhancing reaction activity, selectivity, and stability.
[0112] Table 2: Dimensions, D50 values, specific surface area, total pore volume, and pore size of the catalyst materials of Examples 1 to 7 (E1 to E7) and Comparative Examples 1 to 9 (C1 to C9). sample code name Catalyst materials Catalyst materials size (nm) D 50 value (nm) Comparison Table area (m 2 / g) main hole volume (cm³ / g) Pores size (nm) E1 Pt 1Pd 1 / Fe xNi yO z 30~61 47.5 119.4 0.37 47.2 C1 Pt 1 / Fe xNi yO z 29~62 47.7 123.9 0.39 48.2 C2 Pd 1 / Fe xNi yO z 33~66 49.9 131.2 0.38 46.1 E2 Fe 1Pd 2 / Al xSi yO z 202~350 297.3 363.2 0.64 11.3 E3 Cu 1Pd 2 / Al xSi yO z 252~412 337.3 382.6 0.72 9.2 E4 Faith 1Ni 2 / Al xSi yO z 192~382 263.5 402.1 0.53 12.6 E5 Fe 1Co 2 / Al xSi yO z 195~402 303.9 348.7 0.81 15.2 C3 Cu 1 / Al xSi yO z 188~393 298.8 361.2 0.77 14.9 C4 Pd 1 / Al xI yO z 193~399 305.3 358.1 0.79 14.7 C5 Faith 1Ni 2 / Al xSi yO z 201~383 189.4 339.4 0.83 15.4 C6 Mn 1Co 2 / Al xSi yO z 207~407 304.6 383.2 0.84 15.9 E6 Pt / PdO / Al 2O 3 83~169 103.6 348.7 0.47 11.5 C7 Pt / PdO / Al 2O 3 82~179 111.5 357.3 0.49 12.2 E7 The presence of 1Pd 1 / TiO 29~62 37.9 243.5 0.19 20.1 C8 There are 1 / TiO 29~44 39.3 257.8 0.19 20.4 C9 Pd 1 / TiO 22~38 31.7 267.3 0.19 20.8
[0113] [The Degradation Effect of Catalyst Materials on Aerosol Molecular Pollutants]
[0114] To verify the degradation effects of the catalyst materials of Examples 1 to 7 (E1 to E7) and Comparative Examples 1 to 9 (C1 to C9) on aerosolized molecular pollutants, as shown in Table 3 below, under controlled factors such as different pollutant source gases (isopropanol (IPA) or acetone), whether or not an oxidant (O3) was added, and the initial concentration of the pollutant source (0.5 ppm or 100 ppm), the catalyst materials of each group of examples were expanded into groups A, B, and C. For example, Example 1 was expanded into Examples 1A to 1C (E1A to E1C); and each group of comparative examples was expanded into group A. For example, Comparative Example 1 was expanded into Comparative Example 1A (C1A). Specifically, 0.5 g of the catalyst material of each group of examples and comparative examples was evenly distributed on 0.1 g of quartz wool, and then the quartz wool and catalyst material were filled into a reaction tube (U-shaped glass tube, inner diameter 7 mm, tube length 150 mm) for isopropanol or acetone oxidation reaction tests at different temperatures. The isopropanol or acetone concentrations at the inlet of the reaction tube were 0.5 ppm and 100 ppm, respectively, while the GHSV of both isopropanol and acetone was 6250 h⁻¹. Isopropanol or acetone was introduced into reaction tubes at different temperatures, and the concentrations at the outlet were measured to confirm the efficiency of the catalyst material in removing isopropanol or acetone at different temperatures. The experimental results are shown in Table 4 below.
[0115] Table 3: Test conditions and parameters for the catalyst material performance tests of Examples 1A to 7C (E1A to E7C) and Comparative Examples 1A to 9A (C1A to C9A), including pollutant gas, oxidant, relative humidity, and initial concentration of pollutant. sample code name Catalyst materials pollution source gas Oxidizing agent pollution source initial concentration (ppm) E1A Pt 1Pd 1 / Fe xNi yO z Isopropanol - 0.5 E1B Pt 1Pd 1 / Fe xNi yO z acetone - 0.5 E1C Pt 1Pd 1 / Fe xNi yO z acetone O 3 0.5 C1A Pt 1 / Fe xNi yO z Isopropanol - 0.5 C2A Pd 1 / Fe xNi yO z Isopropanol - 0.5 E2A Fe 1Pd 2 / Al xSi yO z Isopropanol - 0.5 E2B Fe 1Pd 2 / Al xSi yO z acetone - 0.5 E2C Fe 1Pd 2 / Al xSi yO z acetone O 3 0.5 E3A Cu 1Pd 2 / Al xSi yO z Isopropanol - 0.5 E3B Cu1Pd 2 / Al xSi yO z acetone - 0.5 E3C Cu1Pd 2 / Al xSi yO z acetone O 3 0.5 E4A Fe 1Ni 2 / Al xSi yO z Isopropanol - 0.5 E4B Fe 1Ni 2 / Al xSi yO z acetone - 0.5 E4C Fe 1Ni 2 / Al xSi yO z acetone O 3 0.5 E5A Fe 1Co 2 / Al xSi yO z Isopropanol - 0.5 E5B Fe 1Co 2 / Al xSi yO z acetone - 0.5 E5C Fe 1Co 2 / Al xSi yO z acetone O 3 0.5 C3A Cu 1 / Al xSi yO z Isopropanol - 0.5 C4A Pd 1 / Al xSi yO z Isopropanol - 0.5 C5A Fe 1Ni 2 / Al xSi yO z Isopropanol - 0.5 C6A Mn 1Co 2 / Al xSi yO z Isopropanol - 0.5 E6A Pt / PdO / Al₂O₃ Isopropanol - 100 E6B Pt / PdO / Al₂O₃ acetone - 100 E6C Pt / PdO / Al₂O₃ acetone O 3 100 C7A Pt / PdO / Al₂O₃ Isopropanol - 100 E7A Ir 1Pd 1 / TiO 2 Isopropanol - 0.5 E7B Ir 1Pd 1 / TiO 2 acetone - 0.5 E7C Ir 1Pd 1 / TiO 2 acetone O 3 0.5 C8A Ir 1 / TiO 2 Isopropanol - 0.5 C9A Pd1 / TiO2 Isopropanol - 0.5
[0116] Table 4: Results of the pollution source removal rate, test duration, and T90 value at 25°C for the catalyst material performance tests of Examples 1A to 7C (E1A to E7C) and Comparative Examples 1A to 9A (C1A to C9A). Sample Code Catalyst material Removal rate @25 oC (%) T 90 value (°C) E1A Pt 1Pd 1 / Fe xNi yO z 90.5 25.0 E1B Pt 1Pd 1 / Fe xNi yO z 76.2 63.2 E1C Pt 1Pd 1 / Fe xNi yO z 99.0 25.0 C1A Pt 1 / Fe xNi yO z 10.3 92.3 C2A Pd 1 / Fe xNi yO z - 254.3 E2A Fe 1Pd 2 / Al xSi yO z 37.2 135.0 E2B Fe 1Pd 2 / Al xSi yO z 39.6 121.0 E2C Fe 1Pd 2 / Al xSi yO z 99.0 25.0 E3A Cu 1Pd 2 / Al xSi yO z 59.6 92.5 E3B Cu 1Pd 2 / Al xSi yO z 49.3 103.4 E3C Cu 1Pd 2 / Al xSi yO z 99.0 25.0 E4A Faith 1Ni 2 / Al xSi yO z 46.5 151.2 E4B Faith 1Ni 2 / Al xSi yO z 40.7 164.5 E4C Faith 1Ni 2 / Al xSi yO z 99.0 25.0 E5A Fe 1Co 2 / Al xSi yO z 49.6 133.2 E5B Fe 1Co 2 / Al xSi yO z 38.5 171.4 E5C Fe 1Co 2 / Al xSi yO z 99.0 25.0 C3A Cu 1 / Al xSi yO z 86.3 165.0 C4A Pd 1 / Al xI yO z - 281.4 C5A Faith 1Ni 2 / Al xSi yO z 4.4 213.5 C6A Mn 1Co 2 / Al xSi yO z 16.4 >200 E6A Pt / PdO / Al₂O₃ 66.5 117.0 E6B Pt / PdO / Al₂O₃ 32.5 167.0 E6C Pt / PdO / Al₂O₃ 42.3 83.2 C7A Pt / PdO / Al₂O₃ 31.2 156.8 E7A Ir 1Pd 1 / TiO 2 54.3 82.1 E7B Ir 1Pd 1 / TiO 2 42.3 99.5 E7C Ir 1Pd 1 / TiO 2 98.5 27.3 C8A Ir 1 / TiO 2 55.1 82.1 C9A Pd1 / TiO2 - 299.4
[0117] Table 4 above shows the test results of the removal rate and T90 value of the catalyst materials of Examples 1A to 7C (E1A to E7C) and Comparative Examples 1A to 9A (C1A to C9A) at 25°C. In the experiment of this invention, the T90 value was determined by first confirming the temperature at which a removal rate of 90% was achieved through stepwise heating.
[0118] Comparing E1A and E1B with C1A and C2A, it is evident that at 25°C, the catalyst material of Example 1 (E1) exhibits significantly higher removal rates for both IPA and acetone than the catalyst material of Comparative Example 1 (C1). Furthermore, the removal time of E1A and E1B exceeds 6000 hours (approximately 8.3 months), while C1A becomes ineffective after only 12 hours. Due to the high T90 value of 254.3°C, the removal rate of C2A at room temperature cannot be measured. Moreover, the T90 values show that E1A and E1B achieve a 90% removal rate for the pollutant source gas at 25°C and 63.2°C, respectively. This indicates that E1A and E1B have significant advantages over C1A and C2A in terms of removal time (lifespan) and removal temperature (reduced treatment costs).
[0119] Comparing E3A and E3B with C3A and C4A, it is evident that at 25°C, the catalyst material of Example 3 (E3) exhibits lower removal rates for both IPA and acetone compared to the catalyst materials of Comparative Examples 3 and 4 (C3 and C4). However, the removal time of E3A and E3B can exceed 6000 hours (approximately 8.3 months), while C3A becomes ineffective after only 9 hours. Furthermore, due to the high T90 value of 281.4°C, the removal rate of C4A at room temperature cannot be measured. Moreover, the T90 values show that E3A and E3B achieve a 90% removal rate for the pollutant source gas at 92.5°C and 103.4°C, respectively. This indicates that E3A and E3B have significant advantages over C3A and C4A in terms of removal time (lifespan) and removal temperature (reduced treatment costs).
[0120] Comparing E4A and E4B with C5A, it is evident that at 25°C, the catalyst material of Example 4 (E4) exhibits significantly higher removal rates for both IPA and acetone than the catalyst material of Comparative Example 5 (C5). Furthermore, the removal time of E4A and E4B exceeds 6000 hours (approximately 8.3 months), while the removal rate of C5A at room temperature cannot be measured due to its high T90 value of 213.5°C. Moreover, the T90 values show that E4A and E4B achieve a 90% removal rate for the pollutant gas at 151.2°C and 164.5°C, respectively, indicating that E4A and E4B have significant advantages over C5A in terms of removal time (lifespan) and removal temperature (reduced treatment costs).
[0121] Comparing E5A and E5B with C6A, it is evident that at 25°C, the catalyst material of Example 5 (E5) exhibits significantly higher removal rates for both IPA and acetone than the catalyst material of Comparative Example 6 (C6). Furthermore, the removal time of E5A and E5B exceeds 6000 hours (approximately 8.3 months), while the removal rate of C6A at room temperature cannot be measured due to its T90 value being greater than 200°C. Moreover, the T90 values show that E5A and E5B achieve a 90% removal rate for the pollutant gas at 133.2°C and 171.4°C, respectively, indicating that E5A and E5B have significant advantages over C6A in terms of removal time (lifespan) and removal temperature (reduced treatment costs).
[0122] Comparing E6A and E6B with C7A, it is evident that at 25°C, the catalyst material of Example 6 (E6) exhibits significantly higher removal rates for both IPA and acetone compared to the catalyst material of Comparative Example 7 (C7). Furthermore, although the removal time of E6A, E6B, and C7A is also greater than 6000 hours (approximately 8.3 months), the T90 value shows that E6A achieves a 90% removal rate for the pollutant gas at 117°C, while C7A has a T90 value of 156.8°C. This indicates that E6A still has a considerable advantage over C6A in terms of removal time (lifespan) and removal temperature (reduced treatment costs).
[0123] Comparing E7A and E7B with C8A and C9A, it can be seen that at 25°C, the catalyst material of Example 7 (E7) has a removal rate for both IPA and acetone that is only slightly lower than that of Comparative Example 8 (C8), but higher than that of Comparative Example 9 (C9). Furthermore, the removal time of E7A and E7B can exceed 6000 hours (approximately 8.3 months), while C8A becomes ineffective after only 19 hours. Due to the high T90 value of C9A (299.4°C), the removal rate at room temperature cannot be measured. Moreover, the T90 values show that E7A and E7B achieve a removal rate of 90% for the pollutant gas at 82.1°C and 99.5°C, respectively. While C8A also has a T90 value of 82.1°C, C9A's T90 value is significantly higher. The 90 value is as high as 299.4°C, indicating that E7A and E7B still have considerable advantages over C8A and C9A in terms of removal time (lifespan) and removal temperature (reducing treatment costs) for pollution sources.
[0124] Based on the experimental results above, the catalyst materials of Examples 1 to 7 (E1 to E7) significantly outperformed the catalyst materials of Comparative Examples 1 to 9 (C1 to C9) in removing IPA and acetone, regardless of whether the removal was at room temperature or higher. In particular, their removal time exceeded 6000 hours under prolonged use. However, it should be emphasized that 6000 hours is not the failure time of the catalyst materials of Examples 1 to 7, but only a limitation based on the testing time allowed at the time of the current patent application; the actual service life is expected to be longer. Furthermore, the catalyst materials of the examples also showed a significant advantage in reducing the temperature (T 90°C) required for pollution source treatment, which helps to reduce operating costs.
[0125] It is also worth noting that although the content of precious metals in the formulation of some catalyst materials is relatively low, the filter material of the present invention is designed to be recyclable because it contains precious metals. This not only helps to reduce resource waste, but also further reduces the material cost for long-term use, thereby meeting the needs of large-scale industrial applications and achieving sustainable development.
[0126] [Application of Catalyst Materials]
[0127] To verify the degradation effect of the catalyst materials of Examples 1 to 7 (E1 to E7) of the present invention on airborne molecular pollutants when added to a support material in different amounts, the support material includes, but is not limited to, a cloth-like material (e.g., woven fabric or non-woven fabric), a porous structure filler, or a mesh conductive substrate, and at least a portion of the catalyst material is coated on the surface of the support material and can contact the airborne molecular pollutants. In an application example, a method for preparing a sheet-like filter element and its application (also referred to as an application of a catalyst material) is disclosed. Based on 100 wt% of the total weight of the filter element, the filter element includes 1.7 to 28.3 wt% of catalyst material, 0.1 to 5 wt% of binder material, and 66.7 to 98 wt% of plastic material. The catalyst material, binder material, and plastic material are made into a non-woven sheet filter element using melt-blowing and needle-punching techniques. The filter element is shaped into a rectangle with a thickness of 0.4mm to 1.5mm. Then, vacuum forming is used to create multiple parallel raised straight corrugations on the filter element. The height of the corrugations is 2.0mm to 8.0mm, the distance between the corrugations of adjacent corrugations is 2.5mm to 12.0mm, and the angle between the direction of the corrugations and the long side of the rectangular filter element is 45 degrees to 75 degrees.
[0128] Figure 4 shows an application example 1 of the present invention, which demonstrates the removal efficiency of isopropanol (IPA) after the catalyst material (Fe1Ni2 / AlxSiyO2) cloth-like material from Example 4 (E4) was used as a support material.
[0129] [Application Example] [1] Example 4 (E4) [Catalyst Material] (Fe1Ni2 / AlxSiyOz) [Add to fabric] []
[0130] In this application example 1, based on a total weight of 100wt% for the filter element, the filter element contains 0wt%, 1.7wt%, 4.8wt%, 11.5wt%, and 28.3wt% of the catalyst material (Fe1Ni2 / AlxSiyOz) from Example 4 (E4), 2.5wt% of a binder material of polyethylene oxide, and the balance being polyethylene terephthalate (PET). The above-mentioned catalyst material, binder material, and plastic material are fabricated into a nonwoven sheet filter element using melt-blowing and needle-punching techniques. The filter element is rectangular in shape with a thickness of 0.8mm. It is then processed using vacuum forming to create a plurality of parallel, raised, straight corrugations. The height of each corrugation peak is 6.0mm, the distance between adjacent corrugations is 7mm, and the angle between the corrugation's extension direction and the long side of the rectangular filter element is 65 degrees. The filter element was then cut into multiple 0.15 x 0.5 m² cubes and filled into a reaction tube (U-shaped glass tube, 7 mm inner diameter, 150 mm length) to achieve a packing volume of 0.15 m³. The reaction tube temperature was controlled at 25°C. Volatile isopropanol at 100 ppm was then introduced into the reaction tube inlet at a GHSV of 15000 h⁻¹, and the isopropanol concentration was measured at the reaction tube outlet to confirm the filter element's isopropanol removal efficiency. As shown in Figure 4, tests were conducted with no added catalyst and with four different catalyst addition ratios. Using a 90% isopropanol removal efficiency as a benchmark, without the addition of the catalyst material of this invention (0 wt%), 72.5 ± 3.3% of isopropanol can be removed solely by the adsorption capacity of the plastic material itself. However, with the increase of the amount of catalyst material added, even at a low addition amount such as 4.8 wt%, 91.4 ± 3.6% of isopropanol can be effectively removed; and with a further increase in the addition amount, such as reaching 28.3 wt%, the removal efficiency is further improved to 96.5 ± 1.9%. This shows that the catalyst material of this invention only needs to be added in small amounts to non-woven sheet-like fabrics to achieve excellent gaseous pollutant removal effects, and has good economic benefits and industrial application value.
[0131] In summary, the catalyst material of the present invention exhibited excellent gaseous pollutant removal performance in Application Example 1. In Application Example 1, a removal efficiency of 95.3% was achieved with an addition amount as low as 4.8 wt%, and the removal efficiency further improved with increasing addition amount. The results of the above application examples demonstrate that the catalyst material of the present invention can achieve stable and efficient pollutant removal performance in the application of support materials, and has significant industrial application potential and cost-effectiveness.
Claims
1. An application of a catalyst material, wherein a catalyst material is added to a support material, such that the catalyst material and the support material together form a filter element for filtering an aerosolized molecular contaminant (AMC), the filter element being used to contact and decompose the aerosolized molecular contaminant; wherein, Based on a total weight of 100 wt%, the filter element is a nonwoven sheet formed by uniformly mixing 70 wt% to 99.9 wt% of a polymer composition with 0.1 wt% to 30 wt% of a catalyst material and then using melt-blowing and spinning techniques. The polymer composition contains at least a plastic material and a binder material. The catalyst material includes: a carrier; and a first transition metal and a second transition metal, wherein the first transition metal and the second transition metal are respectively supported on the carrier in a single-atom form. The carrier system is selected from one of the group consisting of FeNiO3, FeNi2O4, Fe2NiO4, Fe5NiO8, AlSiO3, AlSi2O6, AlSi3O8, AlSi4O10, Al2SiO5, Al2SiO6, Al2Si2O6, Al2Si2O7, Al2Si2O9, alumina (Al2O3), and titanium oxide (TiO2); the first transition metal system is Fe, Cu, Ir, or Pt, and the second transition metal system is Pd, Ni, or Co; based on 100wt% of the catalyst material, the sum of the weight percentages of the first and second transition metals is between 0.2wt% and 2.5wt%; and based on the sum of the moiré fractions of the second and first transition metals being 100%, the moiré fraction of the second transition metal is 1 to 2 times that of the moiré fraction of the first transition metal.
2. The application of the catalyst material as described in claim 1, wherein, Both the first transition metal and the second transition metal are monatomic metals.
3. The application of the catalyst material as described in claim 1, wherein, The dimensions of the first transition metal and the second transition metal are from 0.2 nm to 3.0 nm.
4. The application of the catalyst material as described in claim 1, wherein, The catalyst material has a size ranging from 29 nm to 412 nm and a D50 ranging from 37.9 nm to 337.3 nm.
5. The application of the catalyst material as described in claim 1, wherein, The specific surface area (BET) of the catalyst material ranges from 119.4 m² / g to 402.1 m² / g.
6. The application of the catalyst material as described in claim 1, wherein, The total pore volume of the catalyst material ranges from 0.19 cm³ / g to 0.81 cm³ / g.
7. The application of the catalyst material as described in claim 1, wherein, The pore size of the catalyst material ranges from 9.2 nm to 47.2 nm.
8. The application of the catalyst material as described in claim 1, wherein, Based on a total weight of 100wt% of the filter element, the filter element contains 1.7 to 28.3wt% of the catalyst material, 0.1 to 5wt% of the binder material, and 66.7 to 98wt% of the plastic material.
9. The application of the catalyst material as described in claim 8, wherein, Based on a total weight of 100wt% of the filter element, the filter element contains 4.8 to 28.3wt% of the catalyst material, 0.1 to 5wt% of the binder material, and 66.7 to 95.1wt% of the plastic material.
10. The application of the catalyst material as described in claim 1, wherein, The plastic material is polyethylene, polypropylene, polyethylene terephthalate, polyethylene terephthalate, cyclohexanediol, or nylon.
11. The application of the catalyst material as described in claim 1, wherein, The adhesive material is polyvinyl alcohol, polyethylene oxide, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyacrylic acid, or polyurethane.
12. The application of the catalyst material as described in claim 1, wherein, The aerosolized molecular contaminants include acetone, isopropanol (IPA), ethanol, ethyl acetate, toluene, xylene, trichloroethylene, propylene glycol monomethyl ether (PGME), propylene glycol monomethyl ether ester (PGMEA), dimethyl sulfoxide (DMSO), or N-methylpyrrolidone (NMP).