Optical device and method for fabricating such optical device
Patent Information
- Application Number
- TW114120194
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-22
- Filing Date
- 2021-07-08
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-07-07
AI Technical Summary
Conventional physical vapor deposition (PVD) processes for forming optical elements result in either high manufacturing costs and complexity due to the need for specialized hardware at low temperatures or the formation of heterogeneous polycrystalline films at higher temperatures, which are birefringent and have large surface roughness, while amorphous films require uniform refractive index and low absorption loss properties.
A method involving the deposition of a doped optical element film by varying power levels to form an optical element layer and incorporate dopant material, maintaining a uniform refractive index and low absorption loss, with a temperature processing margin expanded by the dopant material to prevent crystallization.
The method achieves amorphous optical elements with uniform refractive index greater than 2.0 and low absorption loss, reducing manufacturing complexity and costs by inhibiting crystallization within a broader temperature range.
Smart Images

Figure TWG2TB001920604_001 
Figure TWG2TB001920604_002 
Figure TWG2TB001920604_003
Abstract
Description
Technical Field
[0001] The embodiments disclosed herein generally relate to the fabrication of optical elements. More specifically, the embodiments described herein provide doped optical element films, optical elements having doped structures, and methods for forming doped optical element films and structures. Prior Technology
[0002] Optical components (such as waveguides, planar optical elements, metasurfaces, color filters, and anti-reflective coatings) are processed to exhibit high refractive index and low absorption loss properties. Conductive materials possess high refractive index and low absorption loss, enabling efficient, large-scale manufacturing of optical components.
[0003] Optical elements with polycrystalline films are heterogeneous, have large surface roughness, and can be birefringent, while amorphous films are homogeneous, smooth, and have a uniform refractive index. However, the conventional physical vapor deposition (PVD) process used to form amorphous films for optical elements is performed at substrate temperatures below 30°C to suppress crystallization. Processing temperatures below 30°C for titanium dioxide increase manufacturing costs and complexity due to the need for specialized hardware, while processing temperatures above approximately 30°C result in a large amount of heterogeneous polycrystalline titanium dioxide films. In addition, processing temperatures of approximately 200°C or higher produce significant crystals in the film.
[0004] Therefore, there is a need in the art for improved doped optical element films, optical elements with doped structures, and methods for forming doped optical element films and structures. Summary of the Invention
[0005] In one embodiment, a method is provided. The method includes placing an optical element substrate on a substrate support. The substrate support is disposed in a chamber. The chamber includes an optical element material target disposed in the chamber and a dielectric target disposed in the chamber. The optical element material target includes an optical element material and the dielectric target includes a dopant material. A doped optical element film is deposited on the optical element substrate. Depositing the doped optical element film includes depositing the optical element material to form an optical element layer on a surface of the optical element substrate, and depositing the dopant material into the optical element layer to form the doped optical element film. Depositing the optical element material includes providing a first power level to the optical element material target to deposit the optical element layer at a first deposition rate. Depositing the dopant material into the optical element layer includes providing a second power level to the dielectric target to deposit the dielectric target at a second deposition rate. The first deposition rate and the second deposition rate are different. In one embodiment, the doped optical element film has a plurality of regions extending vertically from a surface of the optical element substrate to a top surface of the doped optical element film. In one embodiment, the method further includes the step of oxidizing the surface of the optical element substrate.
[0006] In another embodiment, a method is provided. The method includes placing an optical element substrate in a chamber, the chamber including a target having a pre-doped optical element material. The pre-doped optical element material includes an optical element material at a first concentration and a dopant material at a second concentration. Power is provided to the target to deposit a doped amorphous optical element layer on the optical element structure.
[0007] In another embodiment, a method is provided. The method includes mounting an optical element substrate on a substrate support. The substrate support is mounted in a chamber. The chamber includes an optical element material target mounted in the chamber and a dielectric target mounted in the chamber. The optical element material target includes a metallic material and the dielectric target includes a dopant material. A doped optical element film is deposited on the optical element substrate. Depositing the doped optical element film includes depositing an optical element material to form an optical element layer on the surface of the optical element substrate, and depositing the dopant material into the optical element layer to form the doped optical element film. Depositing the optical element material includes providing a first power level to the optical element material target and providing oxygen-containing gas to the chamber to deposit the optical element layer at a first deposition rate. Depositing the dopant material into the optical element layer includes providing a second power level to the dielectric target to deposit the dielectric target at a second deposition rate. The first deposition rate and the second deposition rate are different.
[0008] In one embodiment, a method is provided. The method includes the steps of: placing an optical element substrate in a chamber; flowing an optical element material precursor into the chamber at a first flow rate to deposit an optical element layer on a surface of the optical element substrate; and flowing a dopant precursor into the chamber at a second flow rate to form a doped optical element film on the optical element substrate, the doped optical element film having a plurality of regions extending vertically from a surface of the optical element substrate to a top surface of the doped optical element film, wherein the dopant material is distributed in each of the plurality of regions within the range. In one embodiment, the step of flowing the optical element material precursor into the chamber includes the step of introducing an oxygen-containing precursor into the chamber.
[0009] In another embodiment, an optical element is provided. The optical element includes an amorphous optical element layer disposed above the surface of an optical element substrate. The amorphous optical element layer includes an amorphous optical element material and a dopant material, wherein the dopant material is incorporated into the amorphous optical element material.
[0010] In another embodiment, an optical element is provided. The optical element includes a doped optical element film disposed above a surface of an optical element substrate. The doped optical element film includes: a plurality of regions extending perpendicularly from a surface of the optical element substrate to a top surface of the doped optical element film; an amorphous optical element material; and a dopant material, wherein the dopant material is incorporated into the amorphous optical element material, and wherein the dopant material is distributed in each of the plurality of regions. Simple Explanation of the Diagram
[0011] To gain a more detailed understanding of the features described above, a more specific description of the disclosure, which has been briefly summarized above, can be obtained with reference to the embodiments, some of which are illustrated in the accompanying drawings. However, it will be noted that the drawings illustrate exemplary embodiments only and are not intended to limit the scope thereof, and may allow for other equivalent embodiments.
[0012] Figure 1 is a cross-sectional view of an optical element comprising a doped optical element film disposed on an optical element substrate, according to an embodiment.
[0013] Figure 2A is a schematic cross-sectional view of a binary optical element structure mounted on an optical element substrate according to an embodiment.
[0014] Figure 2B is a schematic cross-sectional view of an angled optical element structure mounted on an optical element substrate according to an embodiment.
[0015] Figure 3 is a schematic cross-sectional view of a physical vapor deposition (PVD) processing chamber according to an embodiment.
[0016] Figure 4 is a schematic cross-sectional view of a chemical vapor deposition (CVD) processing chamber according to an embodiment.
[0017] Figure 5 is a schematic top view of the clustering tool according to an embodiment.
[0018] Figure 6 is a flowchart of a method for manufacturing a doped optical element film according to an embodiment.
[0019] Figure 7 is a flowchart of a method for manufacturing a doped optical element film according to an embodiment.
[0020] Figure 8 is a flowchart of a method for manufacturing a doped optical element film according to an embodiment.
[0021] Figure 9 is a flowchart of a method for manufacturing a doped optical element film according to an embodiment.
[0022] For ease of understanding, the same element symbols have been used to identify common elements in the figures where possible. It is anticipated that elements and features of one embodiment may be advantageously incorporated into other embodiments without further description. Implementation
[0023] The embodiments described herein relate to the fabrication of optical elements. Specifically, the embodiments described herein provide doped optical element films, optical elements having doped structures, and methods for forming doped optical element films and structures. The embodiments described herein provide doped optical element films and structures having optical element layers, wherein the doped optical element film and structure have optical element material concentrations and dopant concentrations throughout their thickness.
[0024] The optical element materials described and referenced herein have a refractive index of about 2.0 or greater. The dopant materials described and referenced herein have a dopant refractive index of less than 2.0. In combination, the optical element materials and uniformly distributed dopant materials therein constitute a doped optical element film having an optical element refractive index of about 2.0 or greater. An optical element layer is formed when the optical element material is oxidized, nitrated, or oxynitrated and deposited or flowed over an optical element substrate. In one embodiment, which may be combined with other embodiments described herein, the optical element material comprises a uniform distribution of dopant material.
[0025] In one embodiment that can be combined with other embodiments described herein, the optical element material is a metallic material. Metallic materials include, but are not limited to, metals, metal oxides, metal nitrides, or metal oxynitrides. In another embodiment that can be combined with other embodiments described herein, the optical element material is a semiconductor material. Semiconductor materials include, but are not limited to, silicon (Si), germanium (Ge), silicon-germanium-silicon (SiGe), III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, transparent conductive oxides, or combinations thereof. In other embodiments, the semiconductor material is an oxide, oxynitride, nitride, or carbide of silicon (Si), germanium (Ge), silicon-germanium (SiGe), a III-V semiconductor, II-IV semiconductor, ternary semiconductor, quaternary semiconductor, or a transparent conductive oxide. Dopant materials include, but are not limited to, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides.
[0026] In one embodiment, a method includes mounting an optical element substrate on a substrate support disposed in a chamber. Optical element material is deposited to form an optical element layer over a surface of the optical element substrate. Depositing the optical element material includes providing a first power level to an optical element material target to deposit the optical element material at a first deposition rate. Dopant material is uniformly deposited into the optical element layer to form a doped optical element film. Depositing the dopant material includes providing a second power level to a dielectric target to deposit the dopant material at a second deposition rate.
[0027] Figure 1 is a cross-sectional view of the optical element 100. According to the embodiments described herein, a doped optical element film 101 is disposed above the surface 103 of an optical element substrate 102. The doped optical element film 101 is formed by methods 600, 700, 800, and 900 described herein. The optical element substrate 102 is any suitable optical element substrate on which an optical element can be formed. In one embodiment, the optical element substrate 102 includes, but is not limited to, silicon (Si), silicon nitride (SiN), silicon dioxide (SiO2), fused silica, quartz, silicon carbide (SiC), germanium (Ge), silicon germanium (SiGe), indium phosphide (InP), gallium arsenide (GaAs), gallium oxide (GaO), diamond, lithium niobate (LiNbO3), gallium nitride (GaN), sapphire, tantalum oxide (Ta2O5), titanium dioxide (TiO2), or combinations thereof. The optical element substrate 102 may comprise an optically transparent perovskite material.
[0028] The doped optical element film 101 includes an optical element layer comprising an optical element material. The doped optical element film 101 also includes a dopant material distributed within the optical element layer. The doped optical element film 101 is amorphous to achieve optical properties, including a uniform refractive index greater than about 2.0 and low absorption loss. The optical element layer is formed when the optical element material is oxidized, nitrated, or oxynitrated and deposited or flowed over the optical element substrate 102. Examples of doped optical element films 101 that can be formed by the reaction of the optical element material with a dopant material include, but are not limited to, tantalum pentoxide (Ta₂O₅), zirconium dioxide (ZrO₂), indium oxide (In₂O₃), or hafnium oxide (HfO₂).
[0029] The doped optical element film 101 has a thickness of 110. The thickness 110 is divided into regions 115. In one embodiment, which may be combined with other embodiments described herein, the thickness 110 has a uniform or substantially uniform distribution of dopant material throughout the entire range of region 115. In one embodiment, the doped optical element film 101 includes an optical element refractive index greater than about 2.0 uniformly throughout the thickness 110. In another embodiment, the doped optical element film 101 includes an optical element refractive index of about 2.6 to about 2.7 uniformly throughout the thickness 110.
[0030] The dopant materials described and referenced herein have a dopant refractive index of less than 2.0. In combination, the optical element materials constituting the optical element layer and the dopant materials distributed therein constitute a doped optical element film 101 having an optical element refractive index of about 2.0 or greater.
[0031] The doped optical element film 101 includes an optical element material at an optical element material concentration and a dopant material at a dopant material concentration. The optical element material includes one or both of metallic and semiconductor materials. The tuning of the optical element material concentration, the optical element material refractive index, the dopant material concentration, and the dopant material refractive index will determine the optical properties of the optical element film 101, such as the optical element refractive index.
[0032] In one embodiment, which may be combined with other embodiments described herein, the doped optical element film 101 comprises an optical element material concentration of about 85% to about 100% atomic percentage. In another embodiment, which may be combined with other embodiments described herein, the doped optical element film 101 comprises a dopant material at a dopant concentration of from about 0% to 15% atomic percentage. A dopant concentration of about 0% to about 50% affects the morphology of the doped optical element film 101 without a significantly detrimental increase in the refractive index of the optical element layer.
[0033] To achieve desired optical properties, dopant materials can be distributed within the optical element layer and maintained within a temperature processing margin. In some embodiments, the dopant material is uniformly distributed within the optical element layer. The temperature processing margin is a temperature range at which the optical element layer is amorphously formed to achieve optical properties, including uniform high refractive index and low absorption loss. In the absence of dopant material, the optical element layer is amorphously formed within a certain temperature processing margin and forms a crystalline structure when the optical element layer exceeds the temperature processing margin. The optical element layer without dopant material is amorphously formed within a temperature processing margin of less than 30°C and becomes crystalline at temperatures above 30°C. As described in methods 600, 700, 800, and 900, the dopant material uniformly incorporated into the optical element layer inhibits the growth of the crystal structure and expands the temperature processing margin of the formed doped optical element film 101. An optical element layer having a dopant material uniformly incorporated into the optical element layer at a dopant concentration (e.g., 5% atomic percentage) extends the temperature processing margin at which the doped optical element film 101 is amorphously formed to a temperature greater than about 30°C, for example, a temperature processing margin between about 30°C and 300°C.
[0034] Figure 2A is a schematic cross-sectional view of a binary optical element structure 201a mounted on an optical element substrate 102. Figure 2B is a schematic cross-sectional view of an angled optical element structure 201b mounted on an optical element substrate 102. Optical elements 200a and 200b include optical element structures 201a and 201b mounted on a surface 103 of the optical element substrate 102. Optical element structures 201a and 201b can be formed, for example, by etching a doped optical element film 101, which is formed by methods 600, 700, 800, and 900 described herein.
[0035] As shown in Figure 2A, the optical element structure 201a is a binary (i.e., vertical) structure. As shown in Figure 2A, the optical element structure 201a includes a top surface 204 parallel to the surface 103 of the optical element substrate 102. The first sidewall 205 and the second sidewall 206 are parallel to the third sidewall 207 and the fourth sidewall 208. The sidewalls 205, 206, 207, and 208 are orthogonally oriented to the principal axis of the optical element substrate 102.
[0036] As shown in Figure 2B, the optical element structure 201b is an angled structure. As shown in Figure 2B, the optical element structure 201b includes a first sidewall 205 and a second sidewall 206 parallel to the third sidewall 207 and the fourth sidewall 208. The sidewalls 205, 206, 207, and 208 are inclined relative to the surface 103 of the optical element substrate 102.
[0037] The optical element structures 201a and 201b formed by the optical element film 101 include optical element material of optical element material concentration and dopant material of dopant material concentration distributed throughout the entire thickness 110 of the optical element film 101. The distribution of dopant material throughout the entire thickness 110 provides a uniform refractive index greater than about 2.0 and low absorption loss.
[0038] Figure 3 is a schematic cross-sectional view of the PVD chamber 300. It will be understood that the PVD chamber 300 described below is an exemplary PVD chamber, and other PVD chambers (including PVD chambers from other manufacturers) may be used with or modified to implement the specifications disclosed herein. The PVD chamber 300 can be used in the methods 600, 700, 800, and 900 described herein.
[0039] The PVD chamber 300 is used to form a doped optical element film 101. The PVD chamber 300 includes a plurality of cathodes attached to a chamber body 308, including at least one dielectric target cathode 302 having a plurality of corresponding targets and at least one optical element material target cathode 303, including at least one dielectric target 304 and at least one optical element material (e.g., metal or semiconductor) target 306. Although Figure 3 depicts a dielectric target 304 and an optical element material target 306, the PVD chamber 300 may include one or more dielectric targets 304 and / or one or more optical element material targets 306. For example, three to five targets selected from at least one of the dielectric target 304 or the optical element material target 306 may be included in the PVD chamber 300. In embodiments having one or more dielectric targets 304 and one or more optical element material targets 306, each dielectric target 304 is operable to deposit different dopant materials and / or each optical element material target 306 is operable to deposit different optical element materials.
[0040] The PVD chamber 300 is configured to include a substrate support 310 having a support surface 312 for supporting the optical element substrate 102. The PVD chamber 300 includes an opening 334 (e.g., a slit valve) through which the optical element substrate can enter the processing volume 305.
[0041] In the embodiment shown in Figure 3, the substrate support 310 includes an RF bias power supply 314 disposed therein and coupled to the bias electrode 316. The PVD chamber 300 includes a sputtering gas source 336 for providing a sputtering gas (such as argon (Ar)). The PVD chamber 300 includes a reaction gas source 338 for providing a reaction gas (such as an oxygen-containing gas or a nitrogen-containing gas).
[0042] The substrate support 310 includes a mechanism (not shown) for securing the optical element substrate 102 to a support surface 312 of the substrate support 310, such as an electrostatic chuck, a vacuum chuck, a substrate clamp, or the like. The substrate support 310 is configured to include a cooling conduit 318 disposed within the substrate support 310, wherein the cooling conduit 318 controllably cools the substrate support 310 and the optical element substrate 102 positioned thereon to a predetermined temperature, for example, between about 30°C and about 300°C. The cooling conduit 318 is coupled to a cooling fluid source 320 to provide cooling fluid. The substrate support 310 is further configured to include a heater 322 embedded therein. The heater 322 (e.g., a resistive element) disposed within the substrate support 310 is coupled to an optional heater power supply 324 and controllably heats the substrate support 310 and the optical element substrate 102 positioned thereon to a predetermined temperature, for example, between about 30°C and 300°C. Each target (e.g., dielectric target 304 or optical element material target 306) has a DC power supply 326 or an RF power supply 328 and an associated magnetron. Multiple power supplies enable both DC-powered and RF-powered processes to occur in the same PVD chamber 300.
[0043] The PVD chamber 300 includes a process gas supplier 330 for supplying a predetermined process gas to the process volume 305 of the PVD chamber 300. For example, the process gas supplier 330 supplies oxygen-containing gas to the process volume 305 to create an oxidation environment in the process volume 305. The PVD chamber 300 may also include a precursor gas source 332 controlled by a precursor gas flow controller 331 for supplying precursor gases, such as gaseous dopant precursors.
[0044] Figure 4 is a schematic cross-sectional view of the CVD chamber 400. It will be understood that the CVD chamber 400 described below is an exemplary CVD chamber, and other CVD chambers (including CVD chambers from other manufacturers) may be used with or modified to implement the pattern of this disclosure.
[0045] The CVD chamber 400 has a chamber body 408, which includes a processing volume 405 in which a substrate support 410 is disposed to support an optical element substrate 102. The substrate support 410 includes a heating / cooling conduit 414 and a mechanism for fixing the optical element substrate 102 to a support surface 412 of the substrate support 410, such as an electrostatic chuck, a vacuum chuck, a substrate clamp, or the like. The substrate support 410 is coupled to the processing volume 405 and is movably disposed in the processing volume 405 by means of a rod 406 connected to a lifting system (not shown), which moves the substrate support 410 between a raised processing position and a lowered position, thereby facilitating the transfer of the optical element substrate 102 through an opening 420 into and from the CVD chamber 400.
[0046] CVD chamber 400 includes flow controllers 418a, 418b, such as mass flow control (MFC) devices disposed between a first gas source 402, a second gas source 403, and chamber body 408 to control the flow rate of process gas from the first gas source 402 and the second gas source 403 to a nozzle 404 for distributing process gas across a process volume 405. The first gas source 402 is operable to include optical element material. The second gas source 403 is operable to include dopant material. Although Figure 4 depicts two gas sources 402, 403, CVD chamber 400 may include one or more first gas sources 402 and / or one or more second gas sources 403. For example, three to five gas sources selected from at least one of the first gas source 402 or the second gas source 403 may be included in chamber 300. In embodiments having one or more first gas sources 402 and one or more second gas sources 403, each first gas source 402 is operable to deposit different optical element materials and / or each second gas source 403 is operable to deposit different dopant materials.
[0047] Nozzle 404 is connected to RF power supply 416 via RF feed 422 for generating plasma from process gas in process volume 405. RF power supply 416 provides RF energy to nozzle 404 to facilitate plasma generation between nozzle 404 and substrate support 410. Rod 406 is configured to move substrate support 410 to an elevated process position.
[0048] Figure 5 is a schematic diagram of clustering tool 502 in factory environment 501. It will be understood that clustering tool 502 described herein is an exemplary cluster, and other clustering tools may be used in conjunction with or modified to implement the specifications disclosed herein. Clustering tool 502 described herein can be used in methods 700, 800, and 900 described herein.
[0049] Clustering tool 502 includes a transfer chamber 506 surrounded by one or more processing chambers 504. Processing chambers 504 may include any suitable type of processing chamber for forming the doped optical element film 101 described herein. In one embodiment that may be combined with other embodiments described herein, processing chamber 504 may be a PVD chamber 300. In another embodiment that may be combined with other embodiments described herein, processing chamber 504 may be a CVD chamber 400. In yet another embodiment that may be combined with other embodiments described herein, processing chamber 504 may be a combination of PVD chamber 300 and CVD chamber 400.
[0050] Furthermore, the clustering tool 502 includes a substrate access chamber 508 coupled to the loading gate chamber 510. In one embodiment, the substrate access chamber 508 can be used to connect a factory environment 501 at atmospheric pressure to a loading gate chamber 510 under vacuum pressure. In one embodiment that can be combined with other embodiments described herein, the clustering tool 502 can be used in a single-chamber process, such as in a PVD chamber 300 having at least two targets (e.g., dielectric target 304 or optical element material target 306). In another embodiment that can be combined with other embodiments described herein, the clustering tool 502 can be used in a multi-chamber process, such as in methods 600-900, wherein a plurality of processing chambers 504 are PVD chambers 300, CVD chambers 400, or a combination of both. The clustering tool 502 will transfer an optical element substrate 102 between the plurality of processing chambers 504 such that an optical element layer or dopant material can be deposited in each region of a range of regions 115 in each processing chamber 504. The optical element substrate will enter each processing chamber 504 through openings 334 and 420 of PVD chamber 300 and CVD chamber 400, respectively.
[0051] Figure 6 is a flowchart of a method 600 for fabricating a doped optical element film 101. For ease of explanation, Figure 6 will be described with reference to the PVD chamber 300 of Figure 3 and the clustering tool 502 of Figure 5. However, it will be noted that a PVD chamber different from the PVD chamber 300 of Figure 3 may be used in conjunction with method 600. It will also be noted that a clustering tool different from the clustering tool 502 of Figure 5 may be used in conjunction with method 600. As described above, clustering tool 502 may be used, wherein processing chamber 504 is PVD chamber 300. Method 600 deposits optical element material onto optical element substrate 102 to form an optical element layer. In one embodiment, which may be combined with other embodiments described herein, the dopant material may be deposited uniformly throughout the entire thickness 110 of the optical element layer.
[0052] At operation 601, the optical element substrate 102 intended for coating is placed on a substrate support in the PVD chamber 300. For example, the optical element substrate 102 is placed on a substrate support 310.
[0053] At operation 602, optical element material is deposited. The optical element material is deposited from one or more optical element material targets 306 to form an optical element layer over the optical element substrate 102. The optical element material contains one or both of a metallic material and a semiconductor material. The optical element material is deposited via a PVD process. In one embodiment that can be combined with other embodiments described herein, the PVD process is a sputtering process. In another embodiment that can be combined with other embodiments described herein, the PVD process is an evaporation process.
[0054] In an embodiment, when the optical element material is metallic, an optical element layer is formed when the deposited metal of one or more optical element material targets 306 reacts with a reactive gas to form an optical element layer over the optical element substrate 102. A reactive gas source 338 provides a reactive gas, such as an oxygen-containing gas or a nitrogen-containing gas. For example, pure titanium optical element material is deposited and reacted with a reactive gas (such as oxygen) to form titanium dioxide (TiO2). In an embodiment, when the optical element material is a metal oxide, metal nitride, or metal oxynitride, an optical element layer is formed when the optical element material is deposited over the optical element substrate 102. An optical element material target cathode 303 coupled to one or more optical element material targets 306 is set to a first power level to deposit optical element material at a first deposition rate. When the first power level is applied, the first power level can be kept constant during operations 602 and 603. The PVD chamber 300 may include one or more optical element material targets 306. For example, three to five targets selected from at least one of the optical element material targets 306 may be included in the PVD chamber 300. In embodiments having one or more optical element material targets 306, each optical element material target 306 may be operable to deposit a different optical element material.
[0055] The first power level of the target cathode is in the range of about 0% to about 100%. For example, the first power level of the target cathode is about 80%, and the corresponding first deposition rate is about 0.35 nm / s. In one embodiment, the optical element layer comprises an optical element material concentration of about 85% to about 100% atomic percentage. In one embodiment, the optical element material comprises a first refractive index. The first refractive index is greater than 2.0. For example, the first refractive index is between about 2.0 and about 2.8. In embodiments, when the optical element material is a metallic material, the metallic material includes, but is not limited to, metals, metal oxides, metal nitrides, or metal oxynitrides, such as titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2). In embodiments, when the optical element material is a semiconductor material, the semiconductor material includes, but is not limited to, silicon (Si), germanium (Ge), germanium-silicon (SiGe), III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, transparent conductive oxides, and combinations thereof. In other embodiments, the semiconductor material is an oxide, oxynitride, nitride, or carbide of Si, Ge, SiGe, a III-V semiconductor, a II-IV semiconductor, a ternary semiconductor, a quaternary semiconductor, or a transparent conductive oxide.
[0056] At operation 603, dopant material is deposited. The dopant material is deposited by dielectric target 304 to form a doped optical element film 101 on optical element substrate 102. In one embodiment, which may be combined with other embodiments described herein, the dopant material is deposited such that it is uniformly concentrated in the optical element layer to form one or more regions of the doped optical element film 101. The dielectric target cathode 302 coupled to dielectric target 304 is set to a second power level to deposit the dopant material at a second deposition rate. The second power level of dielectric target cathode 302 is in the range of about 0% to about 100%. For example, the second power level of dielectric target cathode 302 is about 80% and the second deposition rate is about 0.35 nm / s. In one embodiment, the doped optical element film 101 comprises dopant material at a dopant concentration of about 0% to 15% atomic percentage. Dopant materials include, but are not limited to, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides. The PVD chamber 300 may include one or more dielectric targets 304. For example, three to five targets selected from at least one of the dielectric targets 304 may be included in the PVD chamber 300. In embodiments having one or more dielectric targets 304, each dielectric target 304 is operable to deposit a different dopant material.
[0057] In one embodiment that can be combined with other embodiments described herein, operations 602 and 603 are repeated by sequentially applying a first power level to the optical element material target cathode 303 at time intervals and applying a second power level to the dielectric target cathode 302 at time intervals. In another embodiment, deposition of dopant material at the second power level is performed by pulses of the second power level at a predetermined frequency during the deposition of the optical element material. In yet another embodiment that can be combined with other embodiments described herein, the optical element material and dopant material are simultaneously deposited by simultaneously applying the first power level and the second power level to a target (e.g., dielectric target 304 or optical element material target 306) to form a doped optical element film 101.
[0058] In one embodiment that can be combined with other embodiments described herein, operations 602 and 603 are performed in a single operation to form all regions of a range 115. In another embodiment, operations 602 and 603 are performed in a single operation to form a portion of a doped optical element film 101, wherein the portion may correspond to one or more regions of a range 115. Each region of a range 115 may be 20 nm to 25 nm of thickness 110. Operations 602 and 603 are repeated until a predetermined thickness 110 is reached. In one embodiment that can be combined with other embodiments described herein, operations 602 and 603 may be performed in a PVD chamber 300 having at least two targets (e.g., dielectric target 304 or optical element material target 306). In another embodiment that can be combined with other embodiments described herein, operations 602 and 603 may be performed in multiple processing chambers 504 of a clustering tool 502. For example, an optical element substrate 102 is transferred between at least two processing chambers 504. At least one of the processing chambers 504 is a PVD chamber 300 comprising an optical element material target 306, and at least another of the processing chambers 504 is a PVD chamber 300 comprising a dielectric target 302.
[0059] Figure 7 is a flowchart of a method 700 for manufacturing a doped optical element film 101. For ease of explanation, Figure 7 will be described with reference to the PVD chamber 300 of Figure 3 and the clustering tool 502 of Figure 5. However, it will be noted that a PVD chamber different from the PVD chamber 300 of Figure 3 may be used in conjunction with method 700. It will also be noted that a clustering tool different from the clustering tool 502 of Figure 5 may be used in conjunction with method 700. As described above, clustering tool 502 may be used, wherein processing chamber 504 is PVD chamber 300.
[0060] At operation 701, the optical element substrate 102 intended for coating is placed on a substrate support in the PVD chamber 300. For example, the optical element substrate 102 is placed on a substrate support 310.
[0061] At operation 702, pre-doped optical element material is deposited. The pre-doped optical element material is deposited from one or more optical element material targets 306 to form one or more regions 115 of a doped optical element film 101 over an optical element substrate 102. The pre-doped optical element material includes optical element material and dopant material. The pre-doped optical element material may include one or both of a metallic material and a semiconductor material. Metallic materials include, but are not limited to, metals, metal oxides, metal nitrides, or metal oxynitrides, such as titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2). Semiconductor materials include, but are not limited to, silicon (Si), germanium (Ge), germanium-silicon (SiGe), III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, transparent conductive oxides, or combinations thereof. In other embodiments, the semiconductor material is an oxide, oxynitride, nitride, or carbide of Si, Ge, SiGe, a III-V semiconductor, a II-IV semiconductor, a ternary semiconductor, a quaternary semiconductor, or a transparent conductive oxide.
[0062] In one embodiment, the pre-doped optical element material is a metal, and the deposited metal reacts with a reactive gas to form one or more regions 115 of a doped optical element film 101 over the optical element substrate 102. The pre-doped optical element material further includes a dopant material, including but not limited to silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides. In one embodiment, which may be combined with other embodiments described herein, the dopant material is uniformly pre-doped in the pre-doped optical element material. The PVD chamber 300 may include one or more optical element material targets 306. For example, three to five targets selected from at least one of the optical element material targets 306 may be included in the PVD chamber 300. In embodiments having one or more optical element material targets 306, each optical element material target 306 is operable to deposit a different pre-doped optical element material. In one embodiment, the pre-doped optical element material has a first refractive index. The first refractive index is greater than 2.0. For example, the first refractive index is between about 2.0 and about 2.8.
[0063] The optical element material target cathode 303, coupled to the optical element material target 306, is set to a first power level to deposit pre-doped optical element material at a first deposition rate. When the first power level is applied, it remains constant during operation 702. The pre-doped optical element material provided by the optical element material target 306 has a predetermined concentration corresponding to the concentration of the doped optical element film 101. In one embodiment, which may be combined with other embodiments described herein, the pre-doped optical element material comprises an optical element material concentration of about 85% to about 100% atomic percentage and a dopant material concentration of about 0% to 15% atomic percentage. For example, the pre-doped optical element material is a titanium dioxide (TiO2) optical element material having a dopant material, such as silicon dioxide (SiO2), at a 5% atomic percentage concentration. In one embodiment, the deposition temperature of the predoped optical element material is maintained at about 270°C or lower to prevent the formation of titanium dioxide (TiO2) grains in the doped optical element film 101.
[0064] In another embodiment, which may be combined with other embodiments described herein, a single application operation 702 forms all regions of a range 115. In another embodiment, repeated operation 702 forms a portion of a doped optical element film 101, wherein this portion may correspond to one or more regions of a range 115.
[0065] In yet another embodiment, which may be combined with other embodiments described herein, one or more optical element material targets 306 are operable to deposit pre-doped metal-containing material and pre-doped semiconductor material. The pre-doped metal-containing material may be deposited simultaneously with the pre-doped semiconductor material to form a region 115. The pre-doped metal-containing material and the pre-doped semiconductor material may be deposited independently with the same optical element material target 306 or with different optical element material targets 306.
[0066] In yet another embodiment, which may be combined with other embodiments described herein, one or more optical element material targets 306 are operable to deposit pre-doped metal-containing material from two or more optical element material targets 306 to form a region 115. The pre-doped metal-containing material may be deposited independently with the same optical element material target 306 or with different optical element material targets 306.
[0067] Figure 8 is a flowchart of an exemplary method 800 for fabricating a doped optical element film 101. For ease of explanation, Figure 8 will be described with reference to the PVD chamber 300 of Figure 3, the CVD chamber 400 of Figure 4, and the clustering tool 502 of Figure 5. However, it will be noted that a PVD chamber different from the PVD chamber 300 of Figure 3 may be used in conjunction with method 800. It will also be noted that a CVD chamber different from the CVD chamber 400 of Figure 4 may be used in conjunction with method 800. It will also be noted that a clustering tool different from the clustering tool 502 of Figure 5 may be used in conjunction with method 800. As described above, clustering tool 502 may be used, wherein processing chamber 504 is either PVD chamber 300 or CVD chamber 400. In one embodiment, the processing chamber is a modified PVD chamber, such as a modified version of the PVD chamber 300 described in Figure 3, equipped to supply dopant precursors, for example, dopant precursors supplied from a precursor gas source 332 controlled by a precursor gas flow controller 331.
[0068] At operation 801, the substrate intended for coating is placed on a substrate support in the PVD chamber 300. For example, the optical element substrate 102 is placed on the substrate support 310.
[0069] At operation 802, optical element material is deposited. The optical element material is deposited from one or more optical element material targets 306 to form an optical element layer over the optical element substrate 102. The optical element material may include one or both of a metallic material or a semiconductor material. In one embodiment of operation 802, the processing chamber is a PVD chamber, such as the multi-cathode PVD chamber in Figure 3, and includes an optical element material target cathode 303. The optical element material target cathode 303 operates at a first power level to deposit the optical element material at a first deposition rate. The optical element material is deposited on the surface of the optical element substrate 102 by setting the optical element material target cathode 303 to the first power level to form an optical element layer at a first deposition rate. For example, the first power level of the optical element material target cathode 303 is in the range of about 0% to about 100%. For example, the first power level of the optical element material target cathode 303 is about 80% and the first deposition rate is about 0.35 nm / s. The PVD chamber 300 may include one or more optical element material targets 306. For example, three to five targets selected from at least one of the optical element material targets 306 may be included in the PVD chamber 300. In embodiments having one or more optical element material targets 306, each optical element material target 306 may be operable to deposit a different optical element material.
[0070] The optical element layer comprises an optical element material at an optical element material concentration. For example, the optical element material concentration is from about 85% to 100% atomic percentage. In one embodiment, the optical element material comprises a first refractive index. The first refractive index is greater than 2.0. For example, the first refractive index is between about 2.0 and about 2.8.
[0071] At operation 803, a dopant precursor is flowed. The dopant precursor includes dopant material flowing from a precursor gas source 332 corresponding to PVD chamber 300 or from a second gas source 403 corresponding to CVD chamber 400. The dopant precursor flows therein to form a doped optical element film 101 on the optical element substrate 102. The dopant precursor includes, but is not limited to, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides. In one embodiment, which may be combined with other embodiments described herein, the dopant precursor flows therein such that it is uniformly concentrated in the optical element layer to form one or more regions of the doped optical element film 101. The optical element material reacts with the dopant precursor to form the doped optical element film 101 on the surface of the optical element substrate 102.
[0072] The dopant precursor flows at a second power level to deposit the dopant precursor at a flow rate. In one embodiment, which may be combined with other embodiments described herein, a precursor gas flow controller 331 coupled to the precursor gas source 332 is set to the second power level. In another embodiment, which may be combined with other embodiments described herein, a second flow controller 418b coupled to the second gas source 403 is set to the first power level. The PVD chamber 300 may include one or more precursor gas sources 332. For example, three to five precursor gas sources 332 may be included in the PVD chamber 300. In embodiments having one or more precursor gas sources 332, each optical element material target 306 is operable to deposit a different optical element material. The CVD chamber 400 may include one or more second gas sources 403. For example, three to five second gas sources 403 may be included in the CVD chamber 400. In embodiments having one or more second gas sources 403, each second gas source 403 is operable to deposit different dopant precursors.
[0073] In one embodiment that can be combined with other embodiments described herein, the deposition rate of the optical element material is greater than the deposition rate of the dopant precursor, such that the dopant material has a lower concentration in the doped optical element film 101 compared to the optical element material. When a second power level is applied, the second power level remains constant throughout operation 803. In one embodiment that can be combined with other embodiments described herein, the first power level and the second power level may be different. The optical element material provided by the optical element material target 306 and the dopant precursor provided by the precursor gas source 332 or the second gas source 403 have predetermined concentrations, and the combined concentrations of the optical element material and the dopant material correspond to the concentration of the doped optical element film 101. In one embodiment that can be combined with other embodiments described herein, the optical element material comprises an optical element material concentration of about 85% to about 100% atomic percentage, while the dopant precursor comprises a dopant material concentration of from about 0% to 15% atomic percentage.
[0074] In one embodiment, which may be combined with other embodiments described herein, operations 802 and 803 are repeated by time intervals of applying a first power level to the optical element material target cathode 303 and time intervals of applying a second power level to the precursor flow controller 331 or the second flow controller 418b. In another embodiment, the flow of the dopant precursor at the second power level is performed by pulses of the second power level at a predetermined frequency during the deposition of the metallic optical element material. In yet another embodiment, which may be combined with other embodiments described herein, the optical element material is deposited and the dopant precursor flows simultaneously by applying both the first and second power levels to form the doped optical element film 101.
[0075] In one embodiment, which may be combined with other embodiments described herein, operations 802 and 803 are performed in a single operation to form all regions of a defined range 115 of the doped optical element film 101. In another embodiment, operations 802 and 803 are performed in a single operation to form a portion of the doped optical element film 101, which may correspond to one or more regions of the defined range 115. Each region of the defined range 115 may be 20 nm to 25 nm of thickness 110. Operations 802 and 803 are repeated until a predetermined thickness 110 of the doped optical element film 101 is achieved.
[0076] In one embodiment that can be combined with other embodiments described herein, operations 802 and 803 can be performed in a PVD chamber 300 having at least an optical element material target 306 and a precursor gas source 332. In another embodiment that can be combined with other embodiments described herein, operations 801 and 802 can be performed in multiple processing chambers 504 of a cluster tool 502. For example, an optical element substrate 102 is transferred between at least two processing chambers 504. At least one of the processing chambers 504 is a PVD chamber 300 comprising the optical element material target 306, and at least another of the processing chambers 504 is a PVD chamber 300 comprising the precursor gas source 332. In yet another example, at least one of the processing chambers 504 is a PVD chamber 300 comprising the optical element material target 306, and at least another of the processing chambers 504 is a CVD chamber 400 comprising a second gas source 403.
[0077] Figure 9 is a flowchart of an exemplary method 900 for fabricating a doped optical element film 101. For ease of explanation, Figure 9 will be described with reference to the CVD chamber 400 of Figure 4 and the clustering tool 502 of Figure 5. However, it will be noted that a CVD chamber different from the CVD chamber 400 of Figure 4 may be used in conjunction with method 900. It will also be noted that a clustering tool different from the clustering tool 502 of Figure 5 may be used in conjunction with method 900. As described above, clustering tool 502 may be used, wherein processing chamber 504 is CVD chamber 400.
[0078] At operation 901, the substrate intended for coating is placed on a substrate support in the CVD chamber 400. For example, the optical element substrate 102 is placed on the substrate support 410.
[0079] At operation 902, a flow optical element material precursor is formed. The optical element material precursor contains optical element material flowing from the first gas source 402 to form an optical element layer over the optical element substrate 102. The optical element material may include one or both of a metallic material and a semiconductor material. Metallic precursors include, but are not limited to, metals, metal oxides, metal nitrides, or metal oxynitrides, such as titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2). Semiconductor precursors include, but are not limited to, silicon (Si), germanium (Ge), silicon-germanium germanium (SiGe), III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, transparent conductive oxides, or combinations thereof. In other embodiments, the semiconductor precursor is an oxide, oxynitride, nitride, or carbide of Si, Ge, SiGe, a III-V semiconductor, a II-IV semiconductor, a ternary semiconductor, a quaternary semiconductor, or a transparent conductive oxide.
[0080] In an embodiment, when the optical element material is metallic, an optical element layer is formed when the flowing metal from the first gas source 402 reacts with the reactive gas to form an optical element layer over the optical element substrate 102. In an embodiment, when the optical element material is a metal oxide, metal nitride, or metal oxynitride, an optical element layer is formed when the optical element material flows over the optical element substrate 102. A first flow controller 418a coupled to the first gas source 402 is set to a first power level to flow at a flow rate in the optical element material precursor. When the first power level is applied, the first power position remains constant during operations 902 and 903. The CVD chamber 400 may include one or more first gas sources 402. For example, three to five first gas sources 402 may be included in the chamber 300. Each first gas source 402 can be operated to deposit a different optical element material. The CVD chamber 400 may include one or more second gas sources 403. For example, three to five second gas sources 403 may be included in the CVD chamber 400. In embodiments having one or more second gas sources 403, each second gas source 403 is operable to deposit different dopant precursors.
[0081] At operation 903, a dopant precursor is flowed. The dopant precursor comprises dopant material flowing from a second gas source 403. The dopant precursor flows therein to form a doped optical element film 101 on the optical element substrate 102. The dopant precursor includes, but is not limited to, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides. In one embodiment, which may be combined with other embodiments described herein, the dopant precursor flows therein such that it is uniformly concentrated in the optical element layer to form one or more regions of the doped optical element film 101. In an embodiment, when the optical element material precursor is a titanium precursor and the dopant precursor is oxygen (O2), a metal-containing precursor reacts with the precursor to form titanium dioxide (TiO2).
[0082] The dopant precursor flows at a second power level to deposit the dopant material at a flow rate. In one embodiment, which may be combined with other embodiments described herein, a second flow controller 418b coupled to a second gas source 403 is set to the second power level. In one embodiment, which may be combined with other embodiments described herein, the flow rate of the optical element material precursor is greater than the flow rate of the dopant precursor, such that the dopant material has a lower concentration in the doped optical element film 101 compared to the optical element material. When the second power level is applied, the second power level remains constant in operation 903. In one embodiment, which may be combined with other embodiments described herein, the first power level and the second power level may be different. The optical element material precursor provided by the first gas source 402 and the dopant precursor provided by the second gas source 403 have predetermined concentrations, and the combined concentrations of the optical element material and the dopant material correspond to the concentration of the doped optical element film 101. In one embodiment, which may be combined with other embodiments described herein, the optical element material precursor comprises an optical element material concentration of about 85% to about 100% atomic percentage and the dopant precursor comprises a dopant material concentration of about 0% to 15% atomic percentage. The CVD chamber 400 may include one or more second gas sources 403. For example, three to five second gas sources 403 may be included in the chamber 300. Each second gas source 403 is operable to deposit a different dopant precursor.
[0083] In one embodiment, which may be combined with other embodiments described herein, operations 902 and 903 are repeated by time intervals of applying a first power level to the first flow controller 418a and time intervals of applying a second power level to the second flow controller 418b. In another embodiment, the flow of the dopant precursor at the second power level is performed by pulses of the second power level at a predetermined frequency as it flows in the optical element material precursor. In yet another embodiment, which may be combined with other embodiments described herein, the optical element material precursor and the dopant precursor flow simultaneously by applying both the first and second power levels to form the doped optical element film 101.
[0084] In one embodiment that can be combined with other embodiments described herein, operations 902 and 903 are performed in a single operation to form all regions of a defined area 115 of the doped optical element film 101. In another embodiment, operations 902 and 903 are performed in a single operation to form a portion of the doped optical element film 101, which may correspond to one or more regions of the defined area 115. Operations 902 and 903 are repeated until a predetermined thickness 110 of the doped optical element film 101 is reached. In one embodiment that can be combined with other embodiments described herein, operations 902 and 903 may be performed in a CVD chamber 400 having at least a first gas source 402 and a second gas source 403. In another embodiment that can be combined with other embodiments described herein, operations 902 and 903 may be performed in multiple processing chambers 504 of a cluster tool 502. For example, the optical element substrate 102 is transferred between at least two processing chambers 504. At least one of the processing chambers 504 is a CVD chamber 400 comprising an optical element material target, and at least another of the processing chambers 504 is a CVD chamber 400 comprising a second gas source 403.
[0085] In one embodiment, the doped optical element film 101 of methods 600-900 is maintained at a temperature range that allows the doped optical element film 101 to remain amorphous. In embodiments that can be combined with other embodiments described herein, in methods 600-900, the doped optical element film 101 is maintained within this temperature range. In one embodiment, the optical element substrate 102 is maintained at a temperature greater than about 30°C, such as between about 30°C and 300°C. In one embodiment, the temperature is maintained by using cooling conduits 318, 414 to cool the substrate supports 310, 410 and the optical element substrate 102. For example, cooling fluid flows through the cooling conduit 318 disposed in the substrate support 310. In one embodiment, the temperature is maintained by using a heater 322 or a heating conduit 414 to heat the substrate supports 310, 410 and the optical element substrate 102.
[0086] In methods 600-900, the optical element material is exposed to a processing temperature of about 30°C or higher. The dopant material incorporated into the optical element layer enables the doped optical element film 101 to be formed amorphously at a temperature greater than about 30°C (e.g., between about 100°C and about 300°C). When the dopant material is incorporated into the optical element layer, the optical element material having the dopant material is formed amorphously, wherein the dopant material modifies the composition of the optical element material and interrupts the formation of crystal structures in the optical element layer that would otherwise be formed above a certain temperature specific to the optical element material. For example, titanium dioxide (TiO2) can be formed into polycrystalline titanium dioxide (TiO2) at temperatures between 30°C and 200°C, and can form distinct crystals at temperatures at or above 200°C.
[0087] In summary, this paper describes an improved method and materials for forming a doped optical element film 101 with optical properties, including uniform high refractive index and low absorption loss. To achieve the desired optical properties, a dopant material is distributed in the optical element layer at a dopant concentration, and the doped optical element film is maintained within a temperature processing margin that allows the doped optical element film to be formed amorphously (i.e., without forming a crystalline structure). The dopant material at a dopant concentration expands the temperature processing margin of the doped optical element film. The dopant material modifies the composition of the optical element layer such that crystal formation is interrupted at a given temperature. For example, in the case where the optical element layer has a dopant material uniformly distributed therein, crystal formation is interrupted at a temperature between approximately 30°C and 300°C. The 0-50% concentration of dopant atoms in the dopant material affects the morphology of the doped optical element film without a significantly detrimental increase in the refractive index of the optical element layer.
[0088] Although the foregoing relates to embodiments of the present disclosure, other and further embodiments of the present disclosure may be designed without departing from its basic scope, and the scope thereof is determined by the following claims.
[0089] 100: Optical Components 101: Doped optical element film 102: Optical component substrate 103: Surface 110: Thickness 115: Area 200a: Optical Components 200b: Optical Components 201a: Binary Optical Element Structure 201b: Angular optical element structure 204: Top surface 205: First sidewall 206: Second sidewall 207: Third sidewall 208: Fourth sidewall 300: PVD chamber 302: Dielectric target cathode 303: Optical Component Material Target Cathode 304: Dielectric target 305: Processing volume 306: Target 308: Main chamber 310: Substrate support 312: Supporting surface 314: RF Bias Power Supply 316: Bias electrode 318: Cooling duct 320: Cooling fluid source 322: Heater 324: Optional heater power supply 326: DC power supply 328: RF Power Supply 330: Processing gas supply unit 331: Precursor airflow controller 332: Precursor gas source 334: Opening 336: Sputter gas source 338: Reactor Gas Source 400: CVD Chamber 402: Primary Gas Source 403: Second gas source 404: Sprayer head 405: Processing volume 406: Pole 408: Main chamber 410: Substrate support 412: Support surface 414: Heating / cooling conduit 416: RF Power Supply 418A: Flow Controller 418B: Flow Controller 420: Opening 422: RF feed 501: Factory Environment 502: Clustering Tools 504: Processing Chamber 506: Chamber 508: Substrate access chamber 510: Loading gate chamber 600: Method 601: Operation 602: Operation 603: Operation 700: Method 701: Operation 702: Operation 800: Method 801: Operation 802: Operation 803: Operation 900: Method 901: Operation 902: Operation 903: Operation
Claims
1. A method for forming an optical element, comprising the steps of: placing an optical element substrate in a chamber; depositing a doped optical element film on the optical element substrate by means of the following steps: applying power to one or more cathodes, each of the one or more cathodes being coupled to one of one or more targets, each of the one or more targets having a pre-doped optical element material having a first concentration of an optical element material and a second concentration of a dopant material, wherein the first concentration is greater than or equal to 85% and less than 100% atomic percentage, and the second concentration is greater than 0% and less than or equal to 15% atomic percentage; and sputtering the pre-doped optical element material onto the optical element substrate; maintaining the optical element substrate at a temperature between 30°C and 300°C during the deposition of the doped optical element film on the optical element substrate; and etching the doped optical element film to form an optical element having a plurality of doped optical element structures.
2. The method of claim 1, wherein the optical element material comprises one or both of the following: a metallic material comprising titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2); and a semiconductor material comprising silicon (Si), germanium (Ge), germanium-silicon (SiGe), III-V semiconductor, II-IV semiconductor, ternary semiconductor, quaternary semiconductor, and transparent conductive oxide.
3. The method as claimed in claim 1, wherein the dopant material comprises: silicon (Si), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), hafnium (Hf), or oxides thereof, and the dopant material and the optical element material are different.
4. The method as described in request item 1, wherein: The plurality of doped optical element structures have a first refractive index; and the dopant material has a second refractive index, wherein the first refractive index is greater than the second refractive index.
5. The method of claim 1, further comprising the step of: oxidizing a surface of the optical element substrate.
6. A method for forming an optical element, comprising the steps of: placing an optical element substrate in a chamber; flowing an optical element material precursor into the chamber at a first flow rate, wherein the optical element material precursor comprises one or both of the following: a metallic material comprising titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2); and a semiconductor material comprising silicon (Si), germanium (Ge), germanium-silicon (SiGe), III-V semiconductor, II-IV semiconductor, ternary semiconductor, quaternary semiconductor, and transparent conductive oxide; and depositing a doped optical element film on a surface of the optical element substrate using the optical element material precursor. A dopant precursor is flowed into the chamber at a second flow rate to form a doped optical element film on the optical element substrate, wherein the dopant precursor comprises silicon (Si), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), hafnium (Hf), or oxides thereof, and wherein the dopant precursor and the optical element material precursor are different; the optical element substrate is maintained at a temperature between 30°C and 300°C during the flow of the optical element material precursor, the deposition of the plurality of optical element structures, and the flow of the dopant precursor; and the doped optical element film is etched to form an optical element having a plurality of doped optical element structures.
7. The method of claim 6, wherein the step of flowing the optical element material precursor into the chamber comprises the step of introducing an oxygen-containing precursor into the chamber.
8. The method of claim 7, wherein the optical element material precursor is a titanium precursor.
9. The method of claim 6, wherein the dopant precursor is silane (SiH4).
10. The method of claim 6, wherein the dopant precursor is deposited in the plurality of doped optical element structures at a concentration greater than 0% and less than or equal to 15% atomic percentage.
11. An optical element comprising: a plurality of doped optical element structures disposed on a surface of an optical element substrate, the doped optical element structures comprising: a plurality of regions extending perpendicularly from a surface of the optical element substrate to a top surface of the plurality of doped optical element structures; an amorphous optical element material; and a dopant material, wherein the dopant material is incorporated into the amorphous optical element material, wherein the dopant material is distributed in various regions of the plurality of regions, wherein the optical element substrate is maintained at a temperature between 30°C and 300°C during the deposition of the amorphous optical element material and the deposition of the dopant material.
12. The optical element as claimed in claim 11, wherein: The amorphous optical element material has a first refractive index; and the dopant material has a second refractive index, wherein the first refractive index is greater than the second refractive index.
13. The optical element as claimed in claim 11, wherein the dopant material has a concentration of greater than 0% and less than or equal to 15% atomic percentage in the plurality of doped optical element structures.
14. The optical element as claimed in claim 11, wherein the amorphous optical element material comprises one or both of the following: a metallic material comprising tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2); and a semiconductor material comprising silicon (Si), germanium (Ge), germanium-silicon (SiGe), III-V semiconductor, II-IV semiconductor, ternary semiconductor, quaternary semiconductor, and transparent conductive oxide.
15. The optical element as claimed in claim 11, wherein the dopant material comprises: silicon (Si), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), hafnium (Hf), or oxides thereof, and the dopant material is different from the material of the amorphous optical element.
Citation Information
Patent Citations
Transparent titanium oxide-aluminum and / or aluminum oxide coating with rutile structure
CN1741972A