Method for manufacturing aluminum hydroxide powder
Patent Information
- Application Number
- TW115103156
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-07
- Filing Date
- 2022-07-04
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-07-03
Abstract
Description
Technical Field
[0001] This instruction pertains to aluminum hydroxide powder and its manufacturing method. Prior Technology
[0002] The demand for aluminum hydroxide powder as a filler in resin molded materials (sealing materials, heat interface materials, artificial marble, etc.) is gradually increasing. For example, Patent Document 1 discloses a method for manufacturing aluminum hydroxide for use as a filler, characterized in that the raw material aluminum hydroxide is crushed using a screw-type kneader with a compression capacity of 5 to 500 kgf / cm2. [Previous Technical Documents] [Patent Literature]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 2001-322813 Summary of the Invention
[0004] [The problem that the invention aims to solve] However, it was learned that the prior art disclosed in Patent Document 1 had concerns about the tendency to increase viscosity when aluminum hydroxide powder was added to the resin.
[0005] The present invention was made in view of this situation, and one of its objectives is to provide aluminum hydroxide powder that can sufficiently suppress viscosity increase when resin is added, and a method for manufacturing the same. [Methods used to solve problems]
[0006] The present invention is a sample 1 of aluminum hydroxide powder, which has a density of 1.59~2.00 g / cm3 when formed at 10 MPa, and the ratio of the diffraction intensity of the (002) plane to the diffraction intensity of the (110) plane in the XRD pattern is 2.0~7.5.
[0007] The second state of the present invention is aluminum hydroxide powder as in the first state, wherein 90% by mass of the particle diameter (D90) is less than 100 μm.
[0008] The state sample 3 of the present invention is aluminum hydroxide powder as in state sample 1 or 2, wherein the mass-based particle size distribution has one or two peaks in the particle size range of 1 to 200 μm. When there is one peak, the frequency of the peak is 4.0% by mass or more. When there are two peaks, the frequency of one peak is 4.0% by mass or more, and the frequency of the other peak is more than 0% by mass and less than 4.0% by mass.
[0009] Sample 4 of the present invention is a method for manufacturing aluminum hydroxide powder, which includes: pulverizing 50% by mass of aluminum hydroxide powder with a particle size (D50) of 10-200 μm and a pore volume of 0.05-1 μm radius of 0.01-1 mL / g under a pressure of 49.0-294.0 MPa, and then disintegrating it at a collision speed of less than 92 m / s. [Invention Effects]
[0010] According to an embodiment of the present invention, an aluminum hydroxide powder that can sufficiently suppress viscosity increase when added to a resin and a method for manufacturing the same are provided. Implementation
[0011] In order to achieve an aluminum hydroxide powder that can sufficiently suppress the increase in viscosity (hereinafter also referred to as "resin viscosity") when added to resin, the inventors examined various aspects. As a result, they found that by controlling the density during molding at 10 MPa (hereinafter also referred to as "molding density") and the ratio of the diffraction intensity of the (002) plane to the diffraction intensity of the (110) plane in the XRD pattern (hereinafter also referred to as "(002) / (110) diffraction intensity ratio") within a specified range, the increase in resin viscosity can be sufficiently suppressed. It was found that in order to control the molding density and the (002) / (110) diffraction intensity ratio within a specified range, it is important to control the particle size and pore volume of the raw material aluminum hydroxide powder within a specified range, and to crush it with a pressure greater than that of the previous technology (500~3000 kgf / cm2, i.e. 49.0~294.0 MPa), and then to disintegrate it with a relatively weak collision velocity of less than 92 m / s.
[0012] The following details the requirements specified in the embodiments of the present invention.
[0013] <1. Aluminum hydroxide powder> The aluminum hydroxide powder of the embodiment of the present invention has a density of 1.59~2.00 g / cm3 when formed at 10 MPa, and the ratio of the diffraction intensity of the (002) plane to the diffraction intensity of the (110) plane in the XRD pattern is 2.0~7.5. In this way, the increase in resin viscosity can be effectively suppressed.
[0014] If the molding density is less than 1.59 g / cm3, the resin viscosity will increase. There is no particular limit to the upper limit of molding density, but for example, to make it exceed 2.00 g / cm3, detailed manufacturing conditions must be set, and considering productivity, it is better to make it below 2.00 g / cm3.
[0015] Furthermore, the molding density is determined by the following operation. 3.00g of aluminum hydroxide powder was placed into a cylindrical uniaxial forming mold with an inner diameter of 20.0mm. Using a universal testing machine (e.g., A&D Corporation, TENSILON RTG-1310), the aluminum hydroxide powder was compressed and filled to a pressure of 10MPa at a compression speed of 1mm / min. The weight / volume ratio was taken as the forming density.
[0016] If the (002) / (110) diffraction intensity ratio exceeds 7.5, the aluminum hydroxide powder, which is usually in a near-spherical shape, will become distorted into a plate-like shape, and the resin viscosity will increase. Preferably, the (002) / (110) diffraction intensity ratio is 6.0 or less. There is no particular limitation on the lower limit of the (002) / (110) diffraction intensity ratio, but in order to make the (002) / (110) diffraction intensity ratio less than 2.0, more detailed manufacturing conditions must be set. Considering productivity, it is preferable to make it 2.0 or more.
[0017] Furthermore, the (002) / (110) diffraction intensity ratio is obtained by the following operation. After compacting and filling the measuring glass box with aluminum hydroxide powder, the XRD pattern was measured using a powder X-ray diffraction measuring device (e.g., RINT-2000, manufactured by Riko Corporation) at a step width of 0.02 deg, a scanning speed of 0.04 deg / sec, an accelerating voltage of 40 kV, and an accelerating current of 30 mA. Cu-Kα was used as the X-ray source. In the obtained XRD pattern, the peak appearing at 2θ=18.3° was taken as the peak of the (002) plane, and the peak appearing at 2θ=20.3° was taken as the peak of the (110) plane. The ratio of the diffraction intensity (peak height) of the peak of the (002) plane to the diffraction intensity (peak height) of the peak of the (110) plane was taken as the (002) / (110) diffraction intensity ratio.
[0018] In the embodiments of the present invention, the 90% mass particle diameter of the aluminum hydroxide powder (i.e., the particle diameter whose cumulative frequency from the microparticle side in the mass-based particle size distribution is 90% and is also referred to as D90) is preferably less than 100 μm. This effectively suppresses appearance defects when aluminum hydroxide powder is filled into resin molded articles and makes it easier to ensure sufficient strength of the resin molded articles. D90 is preferably 90 μm or less, more preferably 65 μm or less, and even more preferably 45 μm or less. In the embodiments of the present invention, the aluminum hydroxide powder preferably has a D90 of 20 μm or more. This helps to suppress poor dispersion of the aluminum hydroxide powder in a liquid.
[0019] The aluminum hydroxide powder of this invention preferably has one or two peaks in the particle size range of 1 to 200 μm in a mass-based particle size distribution. This suppresses appearance defects when aluminum hydroxide powder is filled into a resin molded article, and also suppresses poor dispersion when the aluminum hydroxide powder is dispersed in a liquid. When there is one peak, the frequency of that peak is 4.0% by mass or more. When there are two peaks, one peak has a frequency of 4.0% by mass or more, and the other peak has a frequency of more than 0% by mass and less than 4.0% by mass. In this case, it is preferable to have only one peak in the particle size range of 1 to 200 μm in a mass-based particle size distribution. This further suppresses appearance defects and poor dispersion in the aforementioned resin molded article.
[0020] In the embodiment of the present invention, the aluminum hydroxide powder has one or more peaks in one or both of the particle size ranges of less than 1 μm and more than 200 μm in the mass-based particle size distribution. The frequency of the aforementioned peaks can be more than 0% by mass and less than 0.5% by mass, or there may be no peaks in the particle size range of less than 1 μm and more than 200 μm.
[0021] In the embodiments of the present invention, the 50% mass particle diameter of the aluminum hydroxide powder (i.e., the particle diameter at which the cumulative frequency from the microparticle side in the mass-based particle size distribution becomes 50% by mass, also referred to as D50) is preferably 30 μm or less. This suppresses appearance defects when aluminum hydroxide powder is filled into resin molded articles and makes it easier to ensure the strength of the resin molded articles. In this embodiment of the invention, the aluminum hydroxide powder preferably has a D50 of 7 μm or higher. This helps to suppress poor dispersion of the aluminum hydroxide powder in a liquid.
[0022] Furthermore, the quality reference particle size distribution (including D50 and D90) is obtained through the following operation. For the process of dispersing aluminum hydroxide powder in a 0.2% (w / w) sodium hexametaphosphate aqueous solution by irradiating with a 25W ultrasonic wave for 120 seconds, a mass-based particle size distribution (including D50 and D90) is determined using a laser scattering particle size distribution measuring device. This particle size distribution is determined by dividing the particle size range of 0.02 μm to 2000 μm into 132 segments on a logarithmic scale and measuring the mass of aluminum hydroxide with particle sizes in each segment. Furthermore, considering machine differences and integration with this embodiment, it is preferable to use a Microtrac MT-3300EXII (manufactured by Nikkiso Corporation) or an equivalent device as the laser scattering particle size distribution measuring device. Also, when measuring particle size distribution, the concentration of the aluminum hydroxide powder should be appropriately adjusted to a concentration that the measuring device can measure before measurement.
[0023] In this embodiment of the invention, the aluminum hydroxide powder preferably has a BET specific surface area of 2.0 m² / g or less. This helps to suppress poor dispersion of the aluminum hydroxide powder in the liquid. Furthermore, the BET specific surface area is obtained by nitrogen adsorption using a fully automated specific surface area measuring device (e.g., Macsorb HM-1201, manufactured by Mountech) according to the method specified in JIS-Z-8830:2013.
[0024] The aluminum hydroxide powder of this invention can contain Na2O as an impurity. The Na2O content is preferably 0.13% by mass or less. This helps to suppress resin degradation and insulation degradation when filled into a resin molded body. Here, the Na2O content is determined by dissolving the aluminum hydroxide powder in an aqueous solution of an inorganic acid and then using an ICP-based spectrophotometer. Specifically, the intensity of sodium at its wavelength (589.592 nm) is measured, converted to Na2O, and the mass of Na2O is calculated. The ratio of this Na2O mass to the mass of the dissolved aluminum hydroxide powder is taken as the Na2O content (mass %). Furthermore, the aluminum hydroxide powder of this invention, in addition to containing Al(OH)3 and Na2O, may also contain unavoidable impurities. These unavoidable impurities include elements introduced from the raw materials, materials, manufacturing equipment, etc.
[0025] When the aluminum hydroxide powder of the embodiment of the present invention is added to the resin, the viscosity increase can be effectively suppressed, making it suitable as a filler in resin molded articles (sealing materials, heat interface materials, artificial marble, etc.). Examples of suitable resins include thermosetting resins such as unsaturated polyester resins, epoxy resins, phenolic resins, and polyurethane resins; and thermoplastic resins such as polyethylene, polypropylene, copolymers of ethylene and propylene, copolymers of ethylene and / or propylene with other α-olefins such as butene-1, pentene-1, hexene-1, heptene-1, octene-1, nonene-1, 4-methylpentene-1, decene-1, etc., including styrene (co)polymers, methyl methacrylate (co)polymers, polyamide, polycarbonate, ethylene-vinyl acetate copolymers, polyacetal, acrylonitrile-butadiene-styrene copolymers, polyphenylene ether, polyether ether, polyaryl esters, polyether ether ketone, polymethylpentene, etc. The aluminum hydroxide powder in the embodiments of the present invention is not limited to the above-mentioned resin, and can also be used as a filler for other synthetic resins, natural resins or paper.
[0026] <2. Method for manufacturing aluminum hydroxide powder> The method for manufacturing aluminum hydroxide powder according to an embodiment of the present invention includes: (a) preparing 50% by mass of aluminum hydroxide powder with a particle size (D50) of 10-200 μm and a cumulative pore volume of 0.01-1 mL / g with a radius of 0.05-1 μm; (b) pulverizing the powder under a pressure of 49.0-294.0 MPa; and (c) disintegrating the powder at a collision velocity of 92 m / s or less. The details of each step are described below.
[0027] [(a) Steps for preparing aluminum hydroxide powder] First, prepare aluminum hydroxide powder as raw material (hereinafter also referred to as "raw aluminum hydroxide powder"). The raw aluminum hydroxide powder must have a particle size (D50) of 10~200μm at 50% by mass and a cumulative pore volume (hereinafter also referred to as "cumulative pore volume") of 0.01~1mL / g with a radius of 0.05~1μm. This makes it easy to obtain the desired molding density. Preferably, the cumulative pore volume is 0.02~1mL / g. This makes it easy to obtain the desired D90 and the desired mass-based particle size distribution of aluminum hydroxide powder.
[0028] When D50 is less than 10μm or more than 200μm, and / or the cumulative pore volume is less than 0.01mL / g or more than 1mL / g, it becomes difficult to obtain the desired molding density.
[0029] Furthermore, the cumulative volume of the fine pores is determined by the following operation. Aluminum hydroxide powder was dried at 120°C for 4 hours to remove adsorbed moisture. Subsequently, approximately 0.5–0.6 g was weighed using a precision balance and filled into a measuring box with a diameter of 15 mm and a height of 24 mm. This measuring box was then installed in an automatic porosimeter (e.g., Micromeritics Autopore III 9420), and measurements were taken on both the low-pressure side (1–10000 psi) and the high-pressure side (10000–60000 psi). These measurement data were combined and calculated to determine the pore volume distribution in the region with a pore radius of 0.002 μm to 100 μm, and the cumulative volume in the region with a pore radius of 0.05 μm to 1.0 μm was also calculated.
[0030] The crystalline structure of the raw material aluminum hydroxide powder is, for example, gibbsite or bayerite, with gibbsite being preferred.
[0031] The raw material aluminum hydroxide powder can be manufactured by adding seed crystals to a supersaturated sodium aluminate solution, stirring and simultaneously hydrolyzing to precipitate aluminum hydroxide, filtering and washing the obtained aluminum hydroxide, and then drying it. Here, by appropriately adjusting the precipitation conditions (and / or dissolving a portion of the precipitated material, and / or pulverizing or disintegrating the precipitated material), raw material aluminum hydroxide powder with the aforementioned particle size and pore volume can be obtained. Furthermore, commercially available aluminum hydroxide powder can also be used as long as the aforementioned particle size and pore volume are met.
[0032] [(b) The pulverizing step under a pressure of 49.0~294.0 MPa] Next, the above-mentioned raw material aluminum hydroxide powder is pulverized under a pressure of 49.0~294.0 MPa. Here, "pulverization" means applying a certain amount of energy to solid particles (e.g., primary particles) of a certain size, causing them to become smaller than their original size.
[0033] If the crushing pressure is less than 49.0 MPa, the desired molding density will not be obtained. A pressure exceeding 49.0 MPa is preferable, and more preferably above 68.6 MPa. There is no particular upper limit to the crushing pressure, but considering productivity, a pressure below 294.0 MPa is preferable.
[0034] Examples of pulverizers that perform pulverization under the aforementioned pressure include, for example, co-kneaders, onlators, self-cleaning kneaders, gear compounders, single-shaft screw kneaders, and twin-shaft screw kneaders. This type of device can be used individually or in combination with two or more other types. Furthermore, pulverizers can be used in either batch or continuous operation; however, continuous operation is preferable from the viewpoint of reducing pulverization energy per unit weight. When using a continuous pulverizer, the aluminum hydroxide material inside the pulverizer does not necessarily need to be pulverized entirely; for example, the degree of pulverization can be sequentially increased in the direction of transport (axial direction) of the aluminum hydroxide material. In the case of screw kneaders, the compression capacity can be adjusted by, for example, the shape, length, or rotational speed of the screw, and the rotational speed of the rotor (which achieves the function of transporting the material to the screw).
[0035] The pulverizer contains aluminum hydroxide powder as a solid phase, and also typically contains air as a gas phase and water as a liquid phase. Since these states within the pulverizer affect the physical properties of the resulting aluminum hydroxide powder, pulverization is preferably carried out in a state where the solid, liquid, and gas phases are (i) a dry state where the solid and gas phases are continuous and the liquid phase is essentially absent; (ii) a pendular state where the solid and gas phases are continuous and the liquid phase is discontinuous; or (iii) a funicular I state where the solid, gas, and liquid phases are continuous. This type of filling configuration results in a smooth, even dry, mixed system.
[0036] The grinding process should aim to achieve a dry, oscillating, or cable-like state during grinding. It is best to adjust the liquid content of the raw aluminum hydroxide powder before grinding. The liquid content can be adjusted, for example, by drying the raw aluminum hydroxide powder or by adding liquids such as water or alcohol. The optimal liquid content varies depending on the particle size distribution of the raw aluminum hydroxide and cannot be generalized. For example, 30% by weight or less is preferably 10% by weight or less, and 1% by weight or more is preferably 5% by weight or more. If the liquid content becomes too high, it becomes difficult to efficiently grind the raw aluminum hydroxide.
[0037] When adding liquids such as water during pulverization, or when pulverizing raw material aluminum hydroxide powder containing water, the pulverized aluminum hydroxide powder is usually dried. Drying can be carried out, for example, by using a known dryer, or by heating a part of a continuous pulverizer during pulverization.
[0038] [(c) The step of breaking up at a collision velocity of 92 m / s or less] After step (b) above, the fragmentation is performed at a collision velocity of 92 m / s or less. Here, "fragmentation" means the operation of breaking down and refining (e.g., creating primary particles) fine particles that have been aggregated into a single mass (e.g., secondary particles).
[0039] If the collision velocity during fragmentation exceeds 92 m / s, the desired (002) / (110) diffraction intensity ratio will not be obtained. For example, fragmentation can be carried out at the above collision velocity by using an impact crusher.
[0040] The method for manufacturing aluminum hydroxide powder according to embodiments of the present invention may also include other steps (such as surface treatment steps) within the scope of achieving the purpose of the present invention. [Example]
[0041] The following examples illustrate the embodiments of the present invention in more detail. The embodiments of the present invention are not limited to the following examples; suitable modifications can be made to implement the invention within the scope of the foregoing and following descriptions, and these modifications are all included within the technical scope of the embodiments of the present invention.
[0042] The raw material aluminum hydroxide powder (D50: 81μm, cumulative pore volume: 0.09mL / g) was adjusted to a moisture content of 5wt% and continuously fed into a pulverizer (single-shaft screw type kneader) for pulverization. The pressure of the pulverizer was adjusted to 196.0MPa by regulating the feeding speed. Furthermore, regarding the pulverizer pressure, the relationship between the pressure and D90 of the same raw material aluminum hydroxide powder was investigated in advance, and the pulverizer pressure was easily calculated from the D90 of the pulverized aluminum hydroxide powder. The obtained pulverized material was dried at 120°C and then fed into an impact pulverizer (free pulverizer, Nara Machinery) for further pulverization to obtain the aluminum hydroxide powder of Example 1. The impact speed of the impact pulverizer was set to 46 m / s. Furthermore, based on the manufacturing method of Example 1 above, the conditions were changed as shown in Table 1 below to obtain aluminum hydroxide powders of Examples 2-4 and Comparative Examples 1-2. Commercially available aluminum hydroxide powders were used as Comparative Example 3 (Sumitomo Chemical, CW-308), Comparative Example 4 (Sumitomo Chemical, C-305), and Comparative Example 5 (Sumitomo Chemical, CM-3080).
[0043]
[0044] For the aluminum hydroxide powders of Examples 1-4 and Comparative Examples 1-5, the molding density, (002) / (110) diffraction intensity ratio, mass-based particle size distribution (including D50 and D90), BET specific surface area and Na2O content were determined by the following methods.
[0045] [Molding density] 3.00g of aluminum hydroxide powder was placed into a cylindrical uniaxial forming mold with an inner diameter of 20.0mm. Using a universal testing machine (A&D Corporation, TENSILON RTG-1310), the aluminum hydroxide powder was compressed and filled at a compression speed of 1mm / min until a pressure of 10MPa was achieved. The weight / volume ratio was taken as the forming density.
[0046] [(002) / (110) diffraction intensity ratio] After compacting and filling the measuring glass box with aluminum hydroxide powder, the XRD pattern was measured using a powder X-ray diffraction measuring device (RIK Corporation, RINT-2000) at a step width of 0.02 deg, a scanning speed of 0.04 deg / sec, an accelerating voltage of 40 kV, and an accelerating current of 30 mA. Cu-Kα was used as the X-ray source. In the obtained XRD pattern, the peak appearing at 2θ=18.3° was taken as the peak of the (002) plane, and the peak appearing at 2θ=20.3° was taken as the peak of the (110) plane. The ratio of the diffraction intensity (peak height) of the peak of the (002) plane to the diffraction intensity (peak height) of the peak of the (110) plane was taken as the (002) / (110) diffraction intensity ratio.
[0047] [Quality reference particle size distribution (including D50 and D90)] For the dispersion of aluminum hydroxide powder in a 0.2% (w / w) sodium hexametaphosphate aqueous solution by irradiation with a 25W ultrasonic wave for 120 seconds, a laser scattering particle size distribution measurement device was used to determine the mass reference particle size distribution (including D50 and D90). This particle size distribution was determined by dividing the particle size range of 0.02μm to 2000μm into 132 logarithmic segments and measuring the mass of aluminum hydroxide with particle sizes in each segment. A Microtrac MT-3300EXII (manufactured by Nikkiso Corporation) was used as the laser scattering particle size distribution measurement device. Furthermore, during particle size distribution measurement, the concentration of aluminum hydroxide powder was appropriately adjusted to a concentration measurable by the aforementioned measurement device before measurement.
[0048] [BET specific surface area] The BET specific surface area was determined by nitrogen adsorption using a fully automated specific surface area measuring device (Macsorb HM-1201, manufactured by Mountech) according to the method specified in JIS-Z-8830:2013.
[0049] [Na2O content] After dissolving aluminum hydroxide powder in an aqueous solution of inorganic acid to prepare an aqueous solution, the Na₂O content is determined using an ICP-based spectrophotometer. Specifically, the intensity of sodium at its wavelength (589.592 nm) is measured, converted to Na₂O, and the mass of Na₂O is calculated. The ratio of this Na₂O mass to the mass of the dissolved aluminum hydroxide powder is taken as the Na₂O content (mass %).
[0050] The following method was used to determine the resin viscosity. A planetary mixer (THINKY Corporation, Deaerator Rentarō ARV-310) was used to mix 5.59 parts by weight of aluminum hydroxide powder and 1.86 parts by weight of bisphenol A type epoxy resin mixture (AQ010-8140, room temperature curing resin type 53 main agent) at 1000 rpm for 3 minutes to obtain a mixture. The mixture was then placed on a dynamic viscoelasticity measuring device (Rheosol-G3000) with parallel plates of 30 mm diameter. After standing for 10 minutes at 100°C with a gap of 0.50 mm between the parallel plates, the resin viscosity was measured at a shear rate of 40 s⁻¹. The results are summarized in Table 2 below. Furthermore, in Table 2, the "-" in the "Second Peak" column indicates that a second peak does not exist.
[0051]
[0052] From the results in Table 2, the following can be observed. Examples 1-4 in Table 2 are all examples that fully meet the requirements specified in the embodiments of the present invention, with resin viscosity below 10 Pa·s and sufficient suppression of resin viscosity increase. Among them, Examples 1-3 are preferred examples because D90 is less than 100 μm, thus sufficient suppression of appearance defects when filled into the resin molded body, and from the viewpoint of easily and sufficiently ensuring the strength of the resin molded body. In Example 4, since the cumulative pore volume of the raw material aluminum hydroxide powder is less than 0.02 mL / g, D90 is 100 μm or more. On the other hand, Comparative Examples 1 to 5 are examples that do not meet the requirements specified in the embodiments of the present invention, with resin viscosity exceeding 10 Pa·s and the increase in resin viscosity not being sufficiently suppressed.
[0053] In Comparative Example 1, since the collision velocity during disintegration exceeds 92 m / s, the (002) / (110) diffraction intensity ratio becomes more than 7.5, and the resin viscosity becomes more than 10 Pa·s.
[0054] In Comparative Example 2, because the pressure during crushing was less than 49.0 MPa, the molding density was less than 1.59 g / cm3, and the resin viscosity was more than 10 Pa·s.
[0055] Comparative Examples 3 and 4 had resin viscosities exceeding 10 Pa·s because their molding density was less than 1.59 g / cm3.
[0056] In Comparative Example 5, the resin viscosity exceeds 10 Pa·s because the (002) / (110) diffraction intensity ratio exceeds 7.5.
Claims
1. A method for manufacturing aluminum hydroxide powder, comprising: taking 50% by mass of aluminum hydroxide powder with a particle size (D50) of 10-200 μm and a pore volume of 0.05-1 μm radius of 0.01-1 mL / g, adjusting the moisture content to below 30% by weight before pulverization, pulverizing at a pressure of 49.0-294.0 MPa, drying the obtained pulverized material, and then crushing it at a collision speed of below 92 m / s.
Citation Information
Patent Citations
Mixed aluminum hydroxide powder
CN101970356A
Aluminum hydroxide for filling in resin and resin composition using the same
JP1997176367A
Aluminium hydroxide powder and method for producing same
TW201402461A