Uv-curable precursor solutions for deposition of mixed metal oxide films containing titanium, and optical elements formed by liquid phase deposition of metal oxide films
Patent Information
- Application Number
- TW115109380
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-08-01
- Filing Date
- 2024-07-26
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Existing methods for forming titanium oxide films often result in cracking due to shrinkage during curing, which can lead to light scattering and component failure, especially in applications requiring thicker films or those with complex geometries.
The use of acid-stabilized precursor solutions containing titanium ions and additional metal ions, such as lanthanum or tellurium, along with photolytic and/or thermally degradable ligands and acids, to form low-crack and crack-free titanium oxide films through liquid-phase deposition, which reduces crystallinity and suppresses cracking during curing.
The method produces films with reduced cracking, enabling better optical performance and thicker films suitable for diffractive optical elements and dielectric layers in TFTs, while maintaining low temperatures and avoiding costly deposition techniques.
Smart Images

Figure TWG2TB001921117_001 
Figure TWG2TB001921117_002 
Figure TWG2TB001921117_003
Abstract
Description
Technical Field
[0001] This invention relates to a method for forming titanium oxide films and a precursor solution. Prior Technology
[0002] Titanium oxide is commonly used as an optical material, such as in diffractive optical elements. This use is at least in part due to TiO2's relatively high refractive index and its low light absorption coefficient across the entire visible light spectrum. Summary of the Invention
[0003] The provided summary presents a selection of concepts in a simplified form, which will be further illustrated in the following embodiments. This summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to limit the scope of the claimed subject matter. Furthermore, the claimed subject matter is not limited to embodiments that address any or all the shortcomings mentioned in any part of this disclosure.
[0004] The disclosed examples relate to acid-stabilized precursor solutions for forming low-crack and crack-free titanium oxide films. One example provides a method for forming a titanium oxide film by liquid-phase deposition. This method includes coating a substrate with an acid-stabilized aqueous precursor solution to form a thin film. The acid-stabilized aqueous precursor solution includes titanium ions and one or more other metal ions, photolytic and / or thermally degradable ligands, and an acid. This method further includes exposing the thin film to one or more heat or light.
[0005] The disclosed examples also relate to the formation of optical elements by liquid-phase deposition of metal oxide films. One example provides a method for forming a metal oxide film, the method comprising coating a substrate with an acid-stabilized precursor solution to form a thin film, the acid-stabilized precursor solution comprising metal ions, photolytic and / or thermally degradable ligands, and an acid. The method further includes a first region of a UV-curable thin film, a second region of a non-UV-curable thin film, and heating the thin film. Simple Explanation of the Diagram
[0006] Figure 1 shows a flowchart of an example method for forming titanium oxide films using an acid-stabilized precursor solution.
[0007] Figure 2 shows a cross-sectional view of an example waveguide including optical elements, which include a titanium oxide film.
[0008] Figure 3 shows a top view of an example titanium oxide film formed on a waveguide with multiple gaps on its surface, showing cracks formed in the oxide film during curing.
[0009] Figure 4 shows a top view of an example titanium / lanthanum / aluminum oxide film formed on a waveguide with gaps in its surface, which shows relatively fewer cracks than the example in Figure 3.
[0010] Figure 5 shows an example top view of an example titanium / lanthanum / tellurium oxide film formed on a waveguide with gaps on its surface, showing no cracks.
[0011] Figure 6 shows a flowchart of an example method for forming a holographic grating by liquid-phase deposition of an acid-stabilized precursor solution to form an inorganic film.
[0012] Figures 7A-7D schematically show example structures that can be formed using the method in Figure 6.
[0013] Figure 8-11 shows a graph of the refractive indices of the UV-cured portion and the non-UV-cured portion of the example film on different substrates.
[0014] Figure 12 shows an example graph illustrating the absorption of the thin film as the concentration of Te increases. Implementation
[0015] Liquid phase deposition processes can be used to form metal oxide films. These films can be used as coatings on optical components. For example, features can be formed on a substrate. Spin-coating deposition can be performed to form a film on the substrate surface, thereby filling the feature with a precursor solution. The film is then cured. Example curing methods include UV curing, thermal curing, laser curing, and particle beam curing. The curing process helps remove solvents and volatile substances from the film and forms a metal ion-oxygen network.
[0016] However, during curing, the film shrinks as solvents and volatile substances are expelled. In some examples, this can lead to cracking. For instance, when forming a titanium oxide film on a waveguide surface including raised regions and gaps between them, the titanium oxide film may crack during curing and shrinkage. In some examples, metal oxide nanoparticles (e.g., TiO2 nanoparticles) can be added to the precursor solution to help reduce shrinkage during the curing process. However, even some oxide films containing titanium nanoparticles may crack during film curing.
[0017] Therefore, some examples involving the formation of low-crack and crack-free titanium oxide films by liquid phase deposition using acid-stabilized metal oxide precursor solutions are disclosed. In short, in the liquid phase deposition process, an acid-stabilized precursor solution is coated onto a substrate to form a thin film. In some examples, the acid-stabilized precursor solution includes titanium ions and one or more other metal ions. Examples of other metal ions include one or more of tellurium ions, bismuth ions, tin ions, aluminum ions, or antimony ions. The acid-stabilized precursor solution further includes photolyzable and / or pyrolyzable ligands, and an acid. In some examples, the acid-stabilized precursor solution further includes components that slow solvent evaporation, such as polyols (alcohols having two or more hydroxyl groups (e.g., diols)). The precursor solution can remain stable over a relatively long period of time (e.g., weeks, months, or even years in the various examples). After coating the substrate, the thin film is exposed to one or more forms of light or heat. This will solidify the film to form an oxide film.
[0018] Because of the presence of one or more additional metal ions besides titanium in the precursor solution, the oxide film can be more amorphous (i.e., glassy) than a titanium oxide film. In other words, the presence of different metals can help suppress the crystallization of the oxide film compared to TiO2 films cured under similar conditions. This helps reduce cracking during the curing process compared to examples that omit such metals. In some examples, substantially crack-free oxide films can be formed. In some such examples, crack-free titanium-containing oxide films can be formed by liquid-phase deposition using an acid-stabilized precursor solution comprising one or more of titanium ions, lanthanum ions, and tellurium ions, bismuth ions, tin ions, or antimony ions. Since cracks can scatter light, substantially crack-free oxide films can provide better optical performance than oxide films with a relatively high concentration of cracks. Therefore, using an acid-stabilized precursor solution according to the examples described herein helps to form thin films with better performance than optical elements formed using other precursor solutions.
[0019] According to the disclosed examples, the use of acid-stabilized precursor solutions can also form films that are relatively thicker than titanium dioxide films, while avoiding cracking. Some applications may require relatively thicker metal oxide films compared to relatively thin films. For example, when used as diffractive optical elements, relatively thick films (e.g., films with a thickness of 100-1000 nm) can increase light interaction within the grating compared to gratings formed by relatively thin films. Another example is that holographic elements require thicker films compared to other types of elements.
[0020] The titanium oxide films disclosed herein can be used in any suitable device. For example, the oxide films can be used on waveguides. Another example is that the oxide films can be used as light extraction layers in organic light-emitting diode (OLED) display panels. Further examples include use in optical cladding and optical elements such as dichroic beam splitters, light scatterers, anti-reflective layers, cold mirrors, and hot mirrors. Example optical devices will be described in detail below.
[0021] The titanium oxide films disclosed in this paper can also be used in thin-film transistors (TFTs). Some TFTs include a dielectric to insulate the gate from the active layer. For example, indium-gallium-zinc-oxide (IGZO) TFTs may include a SiO2 dielectric layer between the gate and the active IGZO layer. The dielectric layer may be formed, for example, during patterning or gap-filling processes. Atomic layer deposition (ALD) is commonly used for dielectric gap filling. However, voids and seams can be generated during ALD gap filling, leading to device failure. Furthermore, the film must exhibit atomic-level smoothness and be deposited at relatively low temperatures to avoid or reduce SiGe outward diffusion. Performing gap-free ALD gap filling at low temperatures is challenging and costly compared to other deposition techniques.
[0022] Therefore, the disclosed titanium oxide film can be used for liquid phase deposition to form a void-free passivation layer and / or dielectric layer in a TFT at low temperatures (down to 150°C). In some such examples, the substrate is coated with an acid-stabilized precursor solution comprising titanium ions and one or more other metal ions to form a thin film. The thin film is cured to form the dielectric layer of the TFT, comprising an oxide film containing titanium and one or more other metal ions. Examples of other metal ions include lanthanum, tellurium, tin, bismuth, and antimony ions. Other examples are as follows. In some examples, a pattern is imprinted on the thin film prior to curing. In some examples, the liquid phase deposition process includes forming the thin film within gaps on the substrate. As mentioned above, the different metal oxides in the film can reduce the crystallinity of the oxide film compared to TiO2 films cured under similar conditions. The reduced crystallinity results in fewer cracks during the curing process compared to examples omitting such metals. This contributes to the formation of a void-free, crack-free dielectric layer. Therefore, the examples disclosed herein provide a liquid phase deposition method for forming dielectric layers of TFTs that is less complex, faster, and less costly than other methods (such as ALD interstitial filling).
[0023] Example acid-stabilizing precursor solutions may include titanium and any other suitable metal ions of appropriate concentration. In some examples, the acid-stabilizing precursor solution contains titanium ions and one or more of the following ions: Al, Ga, Bi, Sc, Cu, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Nb, Mo, In, Sn, Sb, Hf, Ta, W, Ir, Pt, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Te, Yb, or Lu. Metal ions can be introduced into the acid-stabilizing precursor solution in any suitable manner. In some examples, metal ions are introduced into the acid-stabilizing precursor solution in the form of metal chlorides. As an example, solid lanthanum chloride (LaCl3) and solid tellurium chloride (TeCl4) can be added to a 3% aqueous solution of titanium chloride (TiCl3) in hydrochloric acid. In other examples, any other suitable compound, such as metal sulfates or metal nitrates, can be used.
[0024] Example acid-stabilized precursor solutions may include any suitable photolytic and / or pyrolytic ligands. In some examples, the acid-stabilized precursor solution includes hydrogen peroxide (H₂O₂). Alternatively, formic acid (CH₂O₂) may also be used. Alternatively, nitrate ions (NO₃⁻) may also be used. Organic compounds, such as alkoxy ligands, may be omitted from the example acid-stabilized precursor solutions, and therefore can be deposited, dried, and cured at lower temperatures than precursor solutions containing organic compounds. Furthermore, the use of UV-curable ligands, such as peroxides, formic acid, or nitrate ions, helps to provide a precursor solution that is curable upon exposure to UV light.
[0025] Example acid-stabilized precursor solutions may include any suitable acid. Examples include hydrochloric acid (HCl), nitric acid (HNO3), and sulfuric acid (H2SO4). Using an acid in the precursor solution helps prevent the precipitation of metallic substances. Therefore, the example acid-stabilized precursor solutions described herein may have relatively long shelf lives, depending on the time it takes for precipitate formation to be observed.
[0026] According to the disclosed examples, acid-stabilized precursors may also include other components to address various problems encountered in some applications. For example, during the drying process of thick films, the solvent may evaporate before the film components rearrange into a stable configuration. This can cause cracking. Therefore, one or more components can be added to help slow down solvent evaporation during curing. Components that can slow down solvent evaporation during curing include polyhydric alcohols (polyols), such as glycols. In one experiment, adding ethylene glycol to an acid-stabilized precursor solution yielded films with a thickness >400 nm and substantially crack-free films.
[0027] Figure 1 is a flowchart of an example method 100 for forming a titanium oxide film by liquid phase deposition. Method 100 includes, at 102, depositing a film on a substrate using an acid-stabilized precursor solution to form a thin film. The acid-stabilized precursor solution includes titanium ions and one or more other metal ions. The acid-stabilized precursor solution further includes photolytic and / or thermally degradable ligands and an acid. In addition to Ti, example metal ions that can be used include Al, Ga, Bi, Sc, Cu, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Nb, Mo, In, Sn, Sb, Hf, Ta, W, Ir, Pt, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Te, Yb, or Lu ions.
[0028] In some examples, at position 104, the acid-stabilized precursor solution includes titanium chloride, and one or more of lanthanum chloride, bismuth chloride, tin chloride, aluminum chloride, or antimony chloride. Alternatively or additionally, in some examples, one or more nitrates (e.g., titanium nitrate, lanthanum nitrate, aluminum nitrate, tellurium nitrate), nanoclusters (e.g., Al13(OH)24(H2O)24(NO3)15), and / or sulfates (e.g., titanium sulfate, lanthanum sulfate, tellurium sulfate) may also be used. In some examples, at position 106, the acid includes one or more of hydrochloric acid, nitric acid, or sulfuric acid. Furthermore, in some examples, at position 108, the photolyzable and / or pyrolyzable ligands include one or more of hydrogen peroxide, formic acid, or nitrate ions. In some examples, at position 110, the acid-stabilized precursor solution further comprises a polyol. For example, in some examples, the acid-stabilizing precursor solution may include one or more of ethylene glycol, propylene glycol, or 1,3-butanediol. In other examples, any other suitable polyol may be used. In some examples, the acid-stabilizing precursor solution may further include metal oxide nanoparticles, such as TiO2 nanoparticles. Continuing, method 100 further includes, at 120, exposing the film to one or more of heat or light. This will cure the film to form an oxide film comprising titanium and one or more other metal ions. Examples include aluminum, lanthanum, tellurium, bismuth, tin, and / or antimony. In some examples, at 122, method 100 further includes imprinting a pattern onto the film before exposing the film to heat or light. In some examples, at 123, method 100 further includes vacuum drying the film before exposing it to heat or light. In some examples, at 124, exposing the film to heat includes thermally curing the film at a temperature of 60ºC to 650ºC. Unless otherwise specified, numerical ranges include endpoints, i.e., "X to Y" includes values X and Y. In some examples, films cured at relatively high temperatures (e.g., >300ºC) may have a higher light absorption coefficient in the blue range of the visible light spectrum than films cured at relatively low temperatures (e.g., <300ºC). In some examples, at 126, exposing the film to light includes UV curing the film. In some such examples, UV-curable ligands, such as hydrogen peroxide, formic acid, and / or nitrate ions, may be used. In some such examples, nitric acid may be used, which facilitates UV curing. In some examples, exposing the film to light includes exposing the film to a laser. In some examples, at 128, method 100 further includes annealing the film after UV curing. Annealing can be performed at any suitable temperature, such as 60ºC to 650ºC.
[0029] In some examples, at 130, a thin film is formed on an optical element. In some such examples, at 132, the optical element includes a waveguide. For example, method 100 may include forming a diffraction grating on the waveguide. In some examples, the waveguide may be incorporated into a near-eye device. In some examples, the thin film is deposited onto a substrate as part of a TFT manufacturing process. In some examples, at 134, the oxide film includes a dielectric layer in the TFT. In some examples, at 136, the oxide film includes a passivation layer in the TFT.
[0030] Figure 2 shows a cross-sectional view of an example optical element 200 including an oxide film. For example, the optical element 200 can be formed using method 100. The optical element 200 is formed on the surface of a substrate 202 including features 204. As shown in Figure 2, the features 204 are approximately 562 nanometers high. In this example, a thin film is deposited on the substrate 202 using spin-coating to fill the gaps 206 between the features 204. For example, the optical element 200 can be formed by curing the thin film by exposing it to heat or light.
[0031] Figure 3 shows a top view of an example oxide film 300 including titanium atoms. The oxide film 300 is formed between features 304 on a substrate. The oxide film 300 is formed using a precursor solution that omits other metal ions. Therefore, the oxide film 300 shrinks and cracks during curing. This forms cracks 310 in the oxide film 300. Cracks 310 can cause light scattering and component failure.
[0032] Figure 4 shows a top view of another example oxide film 400 comprising titanium, lanthanum, and aluminum. For example, oxide film 400 may comprise a mixture of titanium oxide, lanthanum oxide, and aluminum oxide, and is at least partially amorphous. Oxide film 400 is formed between features 404 on a substrate. Oxide film 400 includes cracks 410. Oxide film 400 is formed using a precursor solution comprising titanium ions, lanthanum ions, and aluminum ions. Therefore, compared to the example in Figure 3, the titanium-containing oxide film 400 is more amorphous and exhibits relatively fewer cracks. Therefore, the addition of lanthanum and aluminum ions to the acid-stabilized precursor solution can help reduce cracking in the liquid-phase deposition of titanium-containing oxide films.
[0033] Figure 5 shows a top view of another example oxide film 500 comprising titanium, lanthanum, and tellurium. For example, oxide film 500 may comprise a mixture of titanium oxide, lanthanum oxide, and tellurium oxide, and is at least partially amorphous. Film 500 is formed by spin deposition of a precursor solution comprising 3 mL TiCl3·3HCl (30%) (aq) + 1 g TeCl4 (s) + 1 g LaCl3 (s) + 1 mL H2O2 (aq) (30%). The film is thermally cured at 200ºC. Oxide film 500 (light-colored portion) is formed between features 504 (dark-colored portion) on the substrate. Oxide film 500 is formed using a precursor solution according to the example described herein, the precursor solution comprising titanium ions, lanthanum ions, tellurium ions, photolytic and / or thermally degradable ligands, and an acid. Therefore, oxide film 500 does not crack during curing. This is because, compared to oxide films omitting such metal ions, the addition of lanthanum and tellurium to titanium-containing oxide films contributes to the formation of more amorphous and less prone-to-cracking oxide films. As described above, the acid-stabilized precursor solution according to the disclosed example can be used to form diffractive optical elements. Diffractive optical elements can be used to guide light in optical systems. Examples of diffractive optical elements include diffractive relief gratings and volume holographic gratings. For example, these elements can be integrated into waveguide combiners to combine real-world images with displayed images. Such waveguide combiners can be used in virtual reality and augmented reality systems.
[0034] Volumetric holographic gratings are typically formed using organic photopolymers. Interference patterns are generated by superimposing wavefronts and recorded in a holographic medium. Laser light can be used to generate fringe patterns in the holographic medium to form the volumetric holographic grating. For example, such gratings can be used in diffraction waveguides.
[0035] However, organic films degrade over time. For example, UV radiation and oxidation can cause organic films to absorb blue light, giving them a pale yellow hue. Organic films also become brittle over time. Furthermore, organic polymers may have a relatively low refractive index dynamic range, for example, Δn ≤ 0.04. The dynamic range Δn refers to the difference in refractive index values between different materials. A lower dynamic range results in relatively low diffraction efficiency (less diffracted light). Organic films may also have relatively high haze (i.e., light scattering), which may reach 0.2% or higher in some examples. Finally, organic films may undergo self-deformation due to heat, leading to a deterioration in dynamic range.
[0036] Therefore, this example discloses the use of metal oxide films as holographic media and the formation of diffractive optical elements by liquid-phase deposition of metal oxide films. Due to differences in film density, UV-cured and heated metal oxide films have different refractive indices than heated but not UV-cured metal oxide films. UV exposure removes organic matter in these areas, increasing the density of the exposed areas. After heating, the UV-exposed film portions have a higher density and a higher refractive index compared to the unexposed areas. In the unexposed areas, organic matter is simultaneously burned off during hard baking. Therefore, the film does not become dense and has a lower refractive index.
[0037] Therefore, UV light can be used to record holographic data and / or form holographic optical elements in metal oxide films, which are then heated to shape the thin film. In short, liquid phase deposition is used to deposit inorganic precursor solutions to form thin films on a substrate. The precursor solution includes metal ions, acids, and photolyzable and / or thermally diffusible ligands, as described above. Holographic images are recorded on the thin film by UV laser curing. Due to the interference pattern, the UV laser light cures and increases the density of a first region of the film, but does not cure the other second regions. The film is then baked. Baking the film changes the refractive index of both the first and second regions. Because UV curing increases the density of the first region, the refractive index differs from that of the annealed second region. Therefore, this method can be used to record holographic images. In some examples, holographic data can be recorded into a metal oxide film. In some examples, UV laser interference patterns can be recorded into a metal oxide film to form a volumetric holographic grating. For example, this can be used to form a diffraction grating on a waveguide.
[0038] Compared to organic thin films, the disclosed metal oxide films can exhibit higher dynamic range, longer durability, and lower haze. Furthermore, metal oxide films are less prone to yellowing than some organic thin films. Holographic media can include any suitable metal oxide, including those deposited using an acid-stabilized precursor solution according to the examples disclosed herein. As described below, in some examples, both the UV-cured and non-UV-cured portions of the metal oxide film can achieve a refractive index dynamic range of 0.10 or greater. Furthermore, vacuum drying the film prior to UV curing can increase the dynamic range. Additionally, the refractive index can be relatively large compared to organic thin films (e.g., 1.7 < n < 2.5). For example, Group IV oxides (such as TiO2, ZrO2, and HfO2) can provide such refractive indices and low optical absorption coefficients across the entire visible spectrum. Volumetric holographic gratings comprising metal oxide films according to the disclosed examples can exhibit higher diffraction efficiency compared to organic thin films. This allows for better performance with thinner films in waveguide systems compared to organic thin films.
[0039] Various precursor solutions can be formed and used for liquid-phase deposition of the disclosed metal oxide films. In some examples, the acid-stabilized precursor aqueous solution according to this disclosure may include one or more Group 4 or 13 ions and one or more other ions from Group 1 and / or Group 2 and / or Group 3, and / or Group 4, and / or Group 5, and / or Group 13 and / or Group 14 and / or Group 15 and / or F-block ions, referring to groups in the periodic table. Examples of these examples include TiO2, AlxTiyOn, AlwTixLayBizOnTexTiyOn, NbxTiyOn, TiO2 / TiO2 nanoparticle complexes, other metal oxide / metal oxide nanoparticle complexes, ZrO2, ZrxTiyOn, CexTiyOn, LaxTiyOn, LixLayTizOn, LixBiyTizOn, NbwLaxLiyTizOn, and AlvNbwLaxLiyTizOn. Further examples include metal oxides comprising one or more of Ti, La, and Te, Bi, or Sb, such as LaxTeyTizOn, LaxBiyTizOn, and LaxSbyTizOn.
[0040] Metal oxide films prepared using the disclosed acid-stabilized precursor solution can be used for a wide range of potential applications. Examples include optical thin films, energy storage, semiconductor devices, photonic integrated circuits (PICs), and biomedical devices. As a more specific example, TiO2 and mixed metal oxide / TiO2 acid-stabilized precursor solutions according to the disclosed examples can be used to deposit titanium oxide films with high thermal stability (>800ºC), high optical transparency (>90% @550nm), and tunable refractive index (1.7 < n < 2.5). Composition and post-deposition treatments can be controlled to adjust the refractive index and optical transparency.
[0041] The disclosed example precursor solutions can be deposited on a substrate by any suitable method. Examples include spin coating, dip coating, doctor blade coating, spray coating, electrodeposition, and printing methods (e.g., inkjet printing, screen printing, etc.). The disclosed example precursor solutions can be formed from various different metal-containing compounds. For example, the precursor solution used to form a TiO2 film can be formed from titanium-containing materials such as TiO2, TiCl3·xHCl (x=0-200), and / or TiCl4(l). The precursor solution according to this disclosure can be an aqueous solution and / or may include another suitable solvent.
[0042] The acid-stabilized precursor solution used to form a holographic recording medium (e.g., for fabricating diffractive optical elements) may comprise any suitable metal ions of any appropriate concentration. In some examples, the metal ions include one or more ions selected from Al, Ga, Bi, Sc, Cu, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Nb, Mo, In, Sn, Sb, Hf, Ta, W, Ir, Pt, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Te, Yb, or Lu. In some examples, the acid-stabilized precursor solution includes one or more Group 4 or 13 ions and one or more other ions from Group 1 and / or Group 2 and / or Group 3, and / or Group 4, and / or Group 5, and / or Group 13 and / or Group 14 and / or Group 15 and / or F-block ions. In some examples, the acid-stable precursor solution includes Ti and Te. In some examples, the acid-stable precursor solution contains one or more of Ti, La, and Te, Bi, or Sb ions. In some examples, the acid-stable precursor solution contains Ti, La, and Al. In some examples, the acid-stable precursor solution contains Te, Bi, or Sn ions. Some illustrative examples include TiO2, AlxTiyOn, TexTiyOn, NbxTiyOn, TiO2 / TiO2 nanoparticle complexes, other metal oxide / metal oxide nanoparticle complexes, ZrO2, ZrxTiyOn, CexTiyOn, LaxTiyOn, LixLayTizOn, LixBiyTizOn, NbwLaxLiyTizOn, and AlvNbwLaxLiyTizOn. Further examples include metal oxides containing one or more of Ti, La, and Sn, Te, Bi, or Sb, such as LaxTeyTizOn, LaxBiyTizOn, and LaxSbyTizOn.
[0043] Metal ions can be introduced into the acid-stabilized precursor solution in any suitable form. In some examples, metal ions are introduced into the acid-stabilized precursor solution in the form of metal chlorides. As illustrative examples, solid lanthanum chloride (LaCl3) and solid tellurium chloride (TeCl4) can be added to an aqueous solution of titanium chloride (TiCl3) in 3% hydrochloric acid. In other examples, any other suitable compound, such as metal sulfates or metal nitrates, can be used.
[0044] As described above, acid-stabilized precursor solutions may include photolyzable and / or pyrolyzable ligands. The term "photolyzable and / or pyrolyzable ligand" refers to a ligand that decomposes or leaves a thin film when the precursor solution is exposed to light (e.g., UV light) and / or sufficient heat (e.g., temperatures from 60ºC to 650ºC). Photolyzable and / or pyrolyzable ligands may include oxygen-containing coordinations that facilitate the formation of metal-ion-oxygen networks. Examples of photolyzable and / or pyrolyzable ligands include hydrogen peroxide, formic acid, and nitrate ions.
[0045] To enable curing using UV laser light, the precursor solution according to this disclosure may include UV-curable ligands. For example, hydrogen peroxide may be used as a UV-curable ligand. In other examples, other suitable UV-curable ligands may also be used. Examples include other peroxides (e.g., lithium peroxide, sodium peroxide, etc.), formic acid or other carboxylic acids, and nitrate ions. Using UV-curable ligands can alter the density of the film and allow holographic encoding into the metal oxide film using UV laser light. Furthermore, example acid-stabilized precursor solutions may omit organic compounds, such as alkoxy ligands, and therefore can be deposited, dried, and cured at lower temperatures than precursor solutions containing organic compounds. In some examples, the precursor solution may include one or more ligands in addition to the UV-curable ligand.
[0046] In addition, in some examples, organic peroxides or acids can be used as photolytically and / or thermally degradable ligands. However, due to the potentially low stability and flammability of organic peroxides, additional safety measures may be required. Formic acid and hydrogen peroxide offer additional advantages because the carbon in formic acid is converted into CO2 gas during the curing of the deposited film, thus eliminating the need for a relatively high-temperature post-deposition heating step to remove carbon from the organic material. As an illustrative example, titanium-containing precursor solutions may include, for example, TiX3 (x = Cl-, Br-, I-, NO3-, OOCH-, etc.) + H2O2, TiX4 (x = Cl-, Br-, I-, NO3-, OOCH-, etc.) + H2O2, or TiOSO4 + H2O2 as metal source / ligand combinations. In some examples, the precursor solution may include metal nitrates (e.g., titanium nitrate) or metal sulfates (e.g., titanium sulfate).
[0047] Example acid-stabilized precursor solutions may include any suitable acid. Examples include hydrochloric acid (HCl), nitric acid (HNO3), and sulfuric acid (H2SO4). Using an acid in the precursor solution helps prevent the precipitation of metallic substances. Therefore, the example acid-stabilized precursor solutions described herein may have relatively long shelf lives, depending on the time it takes for precipitate formation to be observed.
[0048] As described above, in some examples, the acid-stabilized precursor solution may include components that help reduce the solvent evaporation rate of the film formed using the acid-stabilized precursor solution. In some examples, polyols, such as diols, may be used to reduce the solvent evaporation rate of the film formed using the acid-stabilized precursor solution. Example polyols include ethylene glycol ((CH2OH)2), propylene glycol (CH3CH(OH)CH2OH), 1,3-butanediol, and 1,4-butanediol.
[0049] Figure 6 illustrates an example method 600 for forming a volumetric holographic grating. At 601, method 600 optionally includes coating an antireflective film on a substrate. When a pattern is recorded in a holographic medium, the substrate surface can reflect light through an optically transparent film during curing, resulting in unwanted curing of parts of the film. This can cause pattern blurring and ghosting. Therefore, an antireflective film can be applied to the substrate surface before the deposition and patterning of the holographic medium to reduce pattern blurring. For example, the antireflective film may comprise a multilayer dielectric film, which may be adjusted according to the wavelength of light used to record the hologram.
[0050] At 602, method 600 includes coating a substrate with an acid-stabilized precursor solution to form a thin film. The acid-stabilized precursor solution includes metal ions, photolytic and / or thermally degradable ligands, an acid, and optionally a polyol. In some examples, the metal ions include one or more ions selected from Al, Ga, Bi, Sc, Cu, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Nb, Mo, In, Sn, Sb, Hf, Ta, W, Ir, Pt, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Te, Yb, or Lu. In some examples, the acid-stabilized precursor solution includes one or more Group 4 or 13 ions, and one or more other ions from Group 1 and / or Group 2 and / or Group 3, and / or Group 4, and / or Group 5, and / or Group 13 and / or Group 14 and / or Group 15 and / or F-block ions.
[0051] In some examples, at 608, the photolyzable and / or pyrolyzable ligand includes one or more of hydrogen peroxide, nitrate ions, or formic acid. In other examples, any other suitable photolyzable and / or pyrolyzable ligand may be used. In some examples, at 610, the acid comprises one or more of hydrochloric acid, nitric acid, or sulfuric acid. In other examples, any other suitable acid may be used. In some examples, at 612, the acid-stabilizing precursor optionally further comprises one or more polyols, such as ethylene glycol, propylene glycol, or 1,3-butanediol. In other examples, any other suitable polyol may be used. Method 600 optionally includes, at 614, vacuum drying of the film prior to UV curing, as described below.
[0052] Continuing, at 620, method 600 further includes a first region of UV-curable film and a second region of non-UV-curable film. This increases the density of the first region of film. In some examples, at 622, method 600 includes curing the first region of film by constructive interference of UV laser light. In other examples, a mask may be used. In some such examples, at 624, method 600 includes recording a hologram onto the film. In some such examples, at 626, method 100 includes forming a diffraction grating on a waveguide. The diffraction grating may have any suitable orientation. In some examples, the diffraction grating may be oriented perpendicularly to the plane of the substrate. In other examples, the diffraction grating may be oriented at another angle (e.g., obliquely) relative to the plane of the substrate. Continuing, at 630, method 100 includes heating the film. In some examples, at 632, heating the film includes heating the film to a temperature of 60ºC to 650ºC. Heating the film changes the refractive index of both the first and second regions of the film and stabilizes the film (shapes the film). In this way, the refractive index of the film will not change after heating. Heating the film can expel the solvent (e.g., water) from the film. This causes the film to shrink. In some examples, the first region shrinks more after heating than the second region. As mentioned above, due to UV curing of the first region and the increase in film density, the refractive index n1 of the first region is greater than the refractive index n2 of the second region. Here, the dynamic range of the film is Δn = n1 - n2. In some examples, at 634, the refractive index of the first region of the film is at least 0.01 greater than that of the second region. In other words, Δn ≥ 0.01. In some examples, the annealing temperature can be selected to help control the refractive index and / or dynamic range of the metal oxide film. For example, the refractive index can be adjusted by the electromagnetic radiation dose (e.g., UV, laser, IR, X-ray, gamma, etc.). In some examples, the dynamic range can be adjusted by electromagnetic radiation. Alternatively or additionally, in some examples, the film density can be adjusted by electromagnetic radiation. In some examples, the refractive indices of the first and second regions can be adjusted by means of the film composition, drying process, curing temperature, UV exposure time, and / or UV exposure power. In some examples, the dynamic range can be adjusted by means of the film composition, drying process, curing temperature, UV exposure time, and / or UV exposure power.
[0053] Figures 7A-7D show schematic cross-sectional views of example structures that can be formed using method 600. Figure 7A shows a substrate 700. The substrate 700 may include any suitable material on which a volumetric holographic grating can be formed. In some examples, the substrate 700 includes a waveguide. Figure 7B shows a thin film 702 deposited on the substrate 700, for example, by performing step 602 of method 600. The thin film 702 is deposited using an acid-stabilized precursor solution according to the examples disclosed herein. The precursor solution includes metal ions, photolyzable and / or thermally soluble ligands, and an acid, and in some cases, a polyol (e.g., a diol) or other components configured to slow down the rate of solvent evaporation. In some examples, the thin film 702 is vacuum-dried prior to curing (not shown in Figures 7A-7D).
[0054] Figure 7C shows, for example, that by performing step 620 of method 600, the first region 704 is exposed to UV light 706 for curing. As shown in Figure 7C, the second region 708 is not exposed to UV light 706. In this example, the two wavefronts from the UV laser create an interference pattern. The first region 704 represents the region of constructive interference. This provides UV curing for the first region 704. The second region 708 represents the region of destructive interference. Therefore, the second region 708 is not UV cured. In other examples, the pattern can be created using a mask (not shown in Figure 7).
[0055] Figure 7D shows the substrate 700 after the heating step, for example, by performing step 630 of method 600. The heating step stabilizes the thin film 702 (shapes the film). Due to UV curing and higher density, the refractive index n1 of the first region 704 is greater than the refractive index n2 of the second region 708, which has been heated but not UV cured. Figure 7D also schematically illustrates the shrinkage of the first region 704 and the second region 708. As shown, the first region 704 shrinks more than the second region 708. In some examples, the first and second regions may shrink by similar amounts.
[0056] In some examples, thin film 702 can serve as a holographic medium for recording holographic data. In some examples, thin film 702 can be used as a diffraction optical element, such as a volumetric holographic grating on a waveguide. Although depicted as a vertically oriented grating, in other examples, the grating element may be obliquely oriented relative to substrate 700. In some examples, one or more additional layers may be deposited on thin film 702. For example, method 600 may be repeated to deposit an additional volumetric holographic grating on top of thin film 702. In some examples, two or more volumetric holographic gratings may be stacked. In some such examples, each volumetric holographic grating is configured to diffract light of different wavelengths (e.g., red, green, and blue light) from the display.
[0057] In one experiment, six silicon wafer substrates were cut into approximately 1-inch squares. The substrates were then subjected to plasma treatment for 10 minutes. The thin film was then coated in a vacuum chamber at a maximum rotational speed of 3000 rpm and an acceleration of 3000 rpm / s for 60 seconds. The thin film was coated using a precursor solution according to the example disclosed herein.
[0058] A shield is created by padding a 2-inch square glass sheet covered with aluminum foil to create sufficient height between the film and the glass, thereby avoiding direct contact and heat conduction, and reducing reflected light reaching the substrate.
[0059] Following spin coating, the substrates were UV-cured at a dose of 5 J / cm². During this step, half of the film area on each substrate was UV-cured. However, the other half of the film area was covered by a mask and not UV-cured, resulting in a lower density. After UV curing, the films were baked in an oven at 400ºC for 15 minutes. In another experiment, the films were baked at 250ºC for 10 minutes.
[0060] Figure 8 shows a graph 800 of the refractive index of a UV-cured and non-UV-cured portion of a thin film on a substrate. The thin film is titanium aluminum oxide, of which 75% is titanium and 25% is aluminum (molar percentage). Graph 800 shows the refractive index according to the Cauchy equation (…). The fitting results of the refractive index measurement were obtained. The film was UV-cured at a dose of 5 J / cm² and baked at 400ºC for 15 minutes. A mask was used to UV-cur half of the film area and leave the other half uncured. According to the fitting results, the UV-cured portion of the film has n = 1.957, and the uncured portion has n = 1.913. Therefore, the Δn of the film is 0.044. Furthermore, after baking, the thickness of the UV-cured portion of the film is 98 nm, while the thickness of the uncured portion is 105 nm.
[0061] Figure 9 shows the Cauchy equation fitting results for the refractive index of the titanium oxide film. The titanium oxide film was UV-cured at a dose of 5 J / cm² (half of the film area was covered with a mask) and baked at 400ºC for 15 minutes. According to the fitting results, the UV-cured portion of the film has n = 2.278, while the non-UV-cured portion has n = 2.221. Therefore, the Δn of the second film is 0.057. Furthermore, after baking, the thickness of the UV-cured portion of the film is 63 nm, while the thickness of the non-UV-cured portion is 67 nm.
[0062] Figure 10 shows the Cauchy equation fitting results for the refractive index of the third film (Graph 1000). The third film was formed using a precursor solution comprising 33% Ti, 33% Te, and 33% La (molar percentage). The film was UV-cured at a dose of 5 J / cm² (half of the film area was covered with a mask) and baked at 250ºC for 10 minutes. According to the fitting results, the UV-cured portion of the film has n = 2.01, and the non-UV-cured portion has n = 1.91. Therefore, the Δn of the third film is 0.10. Furthermore, after baking, the thickness of the UV-cured portion of the film is 115 nm, while the thickness of the non-UV-cured portion is 140 nm.
[0063] Figure 11 shows the fitting results of the Cauchy equation for the refractive index of the fourth thin film (Graph 1100). The fourth thin film was formed using a precursor solution comprising 72% Ti and 28% Te (molar percentage). The film was UV-cured at a dose of 5 J / cm² (half of the film area was covered with a mask) and baked at 250ºC for 10 minutes. According to the fitting results, the UV-cured portion of the film has n = 2.20, and the non-UV-cured portion has n = 2.04. Therefore, the Δn of the fourth thin film is 0.16. Furthermore, after baking, the thickness of the UV-cured portion of the film is 95 nm, while the thickness of the non-UV-cured portion is 119 nm.
[0064] As described above, according to this disclosure, various metal oxides can be used as holographic films. Some examples include titanium dioxide (TiO2), zirconium dioxide (ZrO2), hafnium oxide (HfO2), lithium titanium oxide, strontium titanium oxide, yttrium titanium oxide, titanium zirconium oxide, niobium titanium oxide, aluminum titanium oxide, titanium tin oxide, bismuth titanium oxide, titanium lanthanum oxide, titanium lanthanum tellurium oxide, titanium lanthanum bismuth oxide, titanium lanthanum antimony oxide, titanium lanthanum aluminum oxide, cerium titanium oxide, lithium aluminum oxide, aluminum strontium oxide, yttrium aluminum oxide, niobium aluminate, aluminum tin oxide, bismuth aluminum oxide, aluminum lanthanum oxide, lithium lanthanum titanium oxide, and lithium bismuth titanium oxide.
[0065] According to this disclosure, the efficiency of recording holograms (e.g., diffractive optical elements) in metal oxide films can be improved by increasing the amount of light absorbed by the metal oxide film during hologram recording to form the diffractive optical element. This can be achieved by adding metal ions that absorb stronger light at the wavelength of the recorded hologram. Examples of metal ions that can be included in the metal oxide film to produce relatively high absorption compared to other ions include silver, bismuth, indium, tin, antimony, and tellurium. Figure 12 shows an example graph 1200 illustrating the absorption of tellurium-doped titanium dioxide (TiO2) films as the Te concentration increases. The absorption of 400 nm light increases as the Te ion concentration in the current substrate solution increases from 0% to 7.5%, to 15%, and to 30%.
[0066] Therefore, the example acid-stabilized precursor solution can help avoid crack formation during liquid-phase deposition of titanium oxide films. In particular, acid-stabilized precursor solutions comprising one or more of titanium ions, lanthanum ions, and tellurium ions, bismuth ions, tin ions, or antimony ions can be used to form substantially crack-free oxide films. This can improve the performance of devices utilizing such titanium oxide films as optical elements (e.g., volumetric holographic gratings). Furthermore, the example acid-stabilized precursor solution can be used to deposit a void-free dielectric layer in thin-film transistors. Other applications include high-density data storage, three-dimensional (3D) displays for AR and MR, advanced optical components, enhanced security and anti-counterfeiting features, and improved medical imaging.
[0067] It is understood that the configurations and methods described herein are provided by way of example and should not be considered limiting, as many variations, extensions, and omissions are foreseeable. Any action of the various actions of the above methods may be performed in the order illustrated, in other orders, in parallel, or omitted. The subject matter of this disclosure includes all novel and non-obvious combinations and sub-combinations of the various configurations, methods, properties, and other features disclosed herein, as well as any and all equivalents thereof.
[0068] 100: Method 102: Steps 104: Steps 106: Steps 108: Steps 110: Steps 120: Steps 122: Steps 123: Steps 124: Steps 126: Steps 128: Steps 130: Steps 132: Steps 134: Steps 136: Steps 200: Optical Components 202:Substrate 204: Features 206: Gap 300: Oxide film 304: Features 310: Crack 400: Oxide film 404: Characteristics 410: Crack 500: Oxide film 504: Features 600: Method 601: Steps 602: Steps 608: Steps 610: Steps 612: Steps 614: Steps 620: Steps 622: Steps 624: Steps 626: Steps 630: Steps 632: Steps 634: Steps 700:Substrate 702:Thin film 704: Area 1 706: UV light 708: Second Area 800: Chart 900: Chart 1000: Chart 1100: Chart 1200: Chart
Claims
1. A method for forming a holographic optical element in a metal oxide film, the method comprising: A thin film is formed by coating a substrate with an acid-stabilized aqueous precursor solution, the acid-stabilized aqueous precursor solution comprising: a metal ion, a photolyzable and / or thermally degradable ligand, including one or more of hydrogen peroxide, formic acid, or nitrate ions, and an acid; and recording a hologram in the thin film by: UV laser curing a first region of the thin film and not UV laser curing a second region of the thin film, the first region and the second region being determined by an interference pattern of UV laser light, and baking the thin film, thereby changing the refractive index of the first region and the refractive index of the second region.
2. The method as described in claim 1 further includes coating the substrate with an antireflective coating before coating the substrate with the acid-stabilized aqueous precursor solution.
3. The method as described in claim 1, wherein recording the hologram in the film further includes vacuum drying the film prior to UV laser curing.
4. The method as described in claim 1, wherein baking the film includes heating the film to a temperature of 60ºC to 650ºC.
5. The method as described in claim 1, wherein the holographic optical element is a diffraction grating on a waveguide.
6. The method as described in claim 1, wherein the refractive index of the first region is at least 0.04 greater than the refractive index of the second region.
7. The method as described in claim 1, wherein the refractive index of the first region is between 1.7 and 2.
5.
8. The method as described in claim 1, wherein the acid comprises one or more of hydrochloric acid, nitric acid, or sulfuric acid.
9. The method as described in claim 1, wherein the acid-stabilized aqueous precursor solution further comprises a polyol.
10. An acid-stable aqueous precursor solution for forming a holographic recording medium, the acid-stable aqueous precursor solution comprising: Metal ions; UV-curable ligands include one or more of hydrogen peroxide, lithium peroxide, sodium peroxide, formic acid, another carboxylic acid, or nitrate ions; and an acid.
11. The acid-stabilized aqueous precursor solution as claimed in claim 10, wherein the metal ion includes one or more of titanium ions, tellurium ions, bismuth ions, tin ions, aluminum ions, or antimony ions.
12. An acid-stabilized aqueous precursor solution as claimed in claim 10, wherein the acid comprises one or more of hydrochloric acid, nitric acid, or sulfuric acid.
13. The acid-stabilized aqueous precursor solution as described in claim 10 further includes polyols.
14. An acid-stabilized aqueous precursor solution as described in claim 13, wherein the polyol comprises ethylene glycol, propylene glycol, or 1,3-butanediol.
15. The acid-stable aqueous precursor solution as described in claim 10, wherein the alkoxy ligand is omitted from the acid-stable aqueous precursor solution.
16. The acid-stabilized aqueous precursor solution as described in claim 10, wherein the acid-stabilized aqueous precursor solution comprises titanium chloride, lanthanum chloride, and tellurium chloride.
17. The acid-stable aqueous precursor solution as described in claim 10, wherein the acid-stable aqueous precursor solution comprises TiO2 nanoparticles.
18. A method for forming a holographic optical element in a titanium oxide film, the method comprising: A thin film is formed by coating a substrate with an acid-stabilized aqueous precursor solution, the acid-stabilized aqueous precursor solution comprising: titanium ions, one or more other metal ions, a photolyzable and / or thermally degradable ligand, including one or more of hydrogen peroxide, formic acid, or nitrate ions, and an acid; and recording a hologram in the thin film by: UV laser curing a first region of the thin film and not UV laser curing a second region of the thin film, the first region and the second region being determined by an interference pattern of UV laser light, and baking the thin film, thereby changing the refractive index of the first region and the refractive index of the second region.
19. The method as described in claim 18, wherein the one or more other metal ions include one or more of tellurium ions, bismuth ions, tin ions, aluminum ions, or antimony ions.
20. The method as described in claim 18, wherein the refractive index of the first region is at least 0.04 greater than the refractive index of the second region.
Citation Information
Patent Citations
Method of Synthesizing Hybrid Metal Oxide Materials and Applications Thereof
US20080022896A1