Method for screening nanoparticle megalibrary for electrocatalytic activity
Patent Information
- Application Number
- PCT/US2024/017007
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-31
- Filing Date
- 2024-02-23
- Publication Date
- 2024-10-24
AI Technical Summary
The widespread adoption of proton-exchange membrane water electrolyzers for hydrogen production is limited due to the scarcity and geographical localization of IrO2, which is used as the anodic oxygen evolution reaction catalyst, and alternative catalysts like RuO2 suffer from insufficient stability and activity, making it difficult to identify effective and scalable electrochemical catalysts for decarbonization strategies.
A method for screening nanoparticle megalibraries using a scanning droplet cell with cyclic voltammetry measurements across a substrate to identify electrochemically active surface areas and correlate them with specific activity, allowing for the rapid discovery of high-efficiency electrochemical catalysts like Ru52Co33Mn9Cr6 oxide, which can replace traditional catalysts.
This approach enables the rapid identification of promising electrocatalyst candidates, such as Ru52Co33Mn9Cr6 oxide, that match or exceed the activity and stability of IrO2, facilitating the development of scalable and efficient decarbonization strategies by correlating chip-based catalyst activity with scaled-up versions.
Smart Images

Figure US2024017007_24102024_PF_FP_ABST
Abstract
Description
Docket No.30938 / 2023-039 METHOD FOR SCREENING NANOPARTICLE MEGALIBRARY FOR ELECTROCATALYTIC ACTIVITY CROSS-REFERENCE TO RELATED APPLICATION
[0001] The benefit of priority U.S. Provisional Patent Application Nos.63 / 448,182 filed February 24, 2023, and 63 / 529,865 filed July 31, 2023, is hereby claimed and the disclosures are incorporated herein by reference in their entireties. FIELD
[0002] The invention is generally directed to methods of screening the electrochemical activity of a plurality of nanoparticles for catalytic activity and more particularly, to methods of screening electrochemically activity of a plurality of nanoparticles arranged in nanoparticle megalibraries. BACKGROUND
[0003] Production of hydrogen via water electrolysis using renewable electricity represents a promising approach to the decarbonization of chemicals and fuels. The proton-exchange membrane water electrolyzer (PEMWE) produces hydrogen with encouraging energy efficiency; however, its widespread adoption is limited because it relies on IrO2as the anodic oxygen evolution reaction (OER) catalyst, and global supply of Ir is limited and geographically localized, with >90% in South Africa. Indeed, the world needs catalysts that meet or exceed the activity and stability of IrO2 in the context of the OER, and while many advances have been made, the catalysts that have been identified suffer from insufficient activity and stability or elemental scarcity. For example, while RuO2exhibits better activity than IrO2, its inferior stability makes it a nonviable replacement. Efforts have been directed toward improving the stability of Ru-based catalysts while maintaining high activity by introducing additional elements (e.g., Co, Ni, Mn, Cr, and Ti) or tailoring catalyst morphology, phase, and structure, but no comprehensive solution has been identified. The number of possible candidates through the systematic combination of the elements is daunting, and it is unlikely that optimum structures will be identified serendipitously or through serial intuition-based methods.
[0004] While important advances have been made through the development of high- throughput techniques, such as thin film deposition and inkjet printing, they are limited to 100- 2,000 features per library and are typically comprised of features that are highly compositionally variable, making it difficult to create scaled up forms that match the properties identified through library screening. Recently, we introduced the concept of material megalibraries, made possibleDocket No.30938 / 2023-039 through a combination of polymer pen lithography (PPL) and scanning probe block copolymer lithography (SPBCL). Megalibraries can consist of hundreds of millions of positionally encoded, well-defined nanostructures (particles) on a surface, allowing one to look at a much broader parameter set within the confines of a 2 cm x 2 cm chip. Each of these features is generated from a single nanoreactor where all metal precursors are converted into a single particle product. Thus far, the megalibrary platform has been utilized to rapidly identify thermal catalysts for single-walled carbon nanotube growth, photocatalysts for pollutant degradation, halide perovskites for record blue-light emissivity, and polyelemental heterostructured materials. SUMMARY
[0005] Discovery of high efficiency electrochemical catalysts is needed to further develop PEMWE and other decarbonization strategies. A high-throughput method is highly desirable to systematically screen potential candidates and identify the most promising compositions.
[0006] A method of screening a nanoparticle megalibrary for catalytic activity in accordance with the disclosure can include disposing a substrate comprising the nanoparticle megalibrary in a scanning droplet cell. The scanning droplet cell can include a scanning droplet cell head comprising a reference electrode and a counter electrode arranged within the scanning droplet cell head, and an electrolyte in fluid communication with the scanning droplet cell head and adapted to be circulated into the scanning droplet cell head. The method can further include forming a droplet of the electrolyte at the scanning droplet cell head, the droplet having a diameter of less than about 500 micrometers and arranged such that a gap of about 50 micrometers to about 100 micrometers is disposed between the substrate and the droplet; and obtaining an electrochemically active surface area (ESCA) of the sample via a set of cyclic voltammetry measurements across the substrate using at least four different scan rates. The ESCA can be obtained by disposing the scanning droplet cell head with the droplet of electrolyte in a first region of the substrate and measuring a cyclic voltammetry signal at each of the at least four different scan rates, moving the scanning droplet cell head with the droplet of electrolyte to a second region of the substrate and measuring a cyclic voltammetry signal at each of the at least four different scan rates at the second region, a distance between the first region and the second region of the substrate being no more than 2000 micrometers, and repeating moving the scanning droplet cell head and measuring a cyclic voltammetry signal at further regions of the substrate such that a cyclic voltammetry signal is measured at the at least four different scan rates at a plurality of regions across the substrate, with a distance betweenDocket No.30938 / 2023-039 each adjacent region being no more than 2000 micrometers. The method further includes moving the scanning droplet cell head with the droplet of the electrolyte across the substrate at a substantially constant rate and substantially constant applied potential and collecting electrochemical signal data at discrete locations as the scanning droplet cell head is moved across the substrate; and correlating the set of cyclic voltammetry measurements to an electrochemically active surface area and forming a position-to-specific activity mapping of the substrate by subtracting a background current of the substrate and normalizing the electrochemical signal data measured across the substrate.
[0007] The megalibrary can include at least 100,000 nanoparticles arranged on the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 is a schematic illustration of megalibrary synthesis, screening, and catalyst scale-up for electrocatalyst discovery in accordance with the disclosure.
[0009] Figure 2A is an optical image of nanoreactors patterned on a polystyrene film-coated glassy carbon (GC) substrate. Scale bars = 5 mm (left) and 50 µm (right).
[0010] Figures 2B to 2E are representative SEM images of a metal oxide nanoparticle array at selected regions (single particle yield >95%). Scale bars = 1 µm.
[0011] Figures 2F to 2I are AFM height images of a metal oxide nanoparticle array at selected regions and corresponding statistical analysis. Scale bars = 2 µm.
[0012] Figure 2J is an OER SA mapping image of a representative RuCoMnCr oxide megalibrary measured in 0.5 M H2SO4at 1.7 V versus RHE. The white dashed square area corresponds to the PPL patterning region. The dashed circles highlight the highest activity regions.
[0013] Figure 3A is a representative high-resolution HAADF-STEM image of a Ru52Co33Mn9Cr6oxide catalyst. The plane spacing of 0.23 nm corresponds with the (200) facet of RuO2. Scale bar = 5 nm.
[0014] Figures 3B to 3G are a HAADF-STEM image and corresponding EDX elemental maps of a Ru52Co33Mn9Cr6oxide nanoparticle, suggesting a uniform elemental distribution. Scale bars = 10 nm.
[0015] Figure 4A is a graph showing the experimental validation of the SA obtained from the particle megalibrary.Docket No.30938 / 2023-039
[0016] Figure 4B is a set of OER polarization curves of scaled-up Ru52Co33Mn9Cr6oxide and commercial RuO2measured on a glassy carbon rotating disk electrode at 1,600 rpm.
[0017] Figure 4C is a representative HAADF-STEM image of a Ru52Co33Mn9Cr6oxide catalyst as-prepared at scale (20 mg). Scale bar = 100 nm.
[0018] Figure 4D is a representative high-resolution HAADF-STEM image of Ru52Co33Mn9Cr6 oxide catalyst. Inset: the corresponding fast Fourier transform (FFT). Scale bars = 5 nm and 10 nm-1for inset, respectively.
[0019] Figure 4E to 4J are the HAADF-STEM image, and corresponding EDX elemental mapping of Ru52Co33Mn9Cr6 oxide. Scale bar = 10 nm
[0020] Figures 5A to 5D are representative SEM images of a metal nanoparticle array at selected metal-rich regions showing single particle formation.
[0021] Figures 5E to 5H are AFM height images of metal nanoparticle arrays at selected metal-rich regions and corresponding statistic particle size analysis.
[0022] Figures 6A and 6B are CV measurements from a representative area in the catalyst megalibrary (approximate coordinates: X= 5838 µm, Y = 1689 µm) and the corresponding linear capacitance fitting (R2= 0.9992). CV curves were measured at different scan rates from 100 mV / s to 400 mV / s.
[0023] Figures 6C and 6D are CV measurements from a representative area with less or no catalyst (approximate coordinates: X= 14835 µm, Y = 5688 µm, boundary of the megalibrary) and the corresponding linear capacitance fitting (R2= 0.9992). CV curves were measured at different scan rates from 100 mV / s to 400 mV / s.
[0024] Figure 7A is the catalytic current mapping of a representative RuCoMnCr oxide nanoparticle megalibrary measured in 0.5 M H2SO4 at 1.7 V versus RHE.
[0025] Figure 7B is the ECSA mapping of a representative RuCoMnCr oxide nanoparticle megalibrary measured in 0.5 M H2SO4 at 1.7 V versus RHE.
[0026] Figure 7C is the SA mapping of a representative RuCoMnCr oxide nanoparticle megalibrary measured in 0.5 M H2SO4 at 1.7 V versus RHE. Areas enclosed in boxes represent the most active regions.
[0027] Figure 7D is an optical image of a RuCoMnCr oxide megalibrary after electrochemical screening. The circle in the bottom left corner represents the origin point (0, 0) during the screening, which was used to correct the coordinates.Docket No.30938 / 2023-039
[0028] Figure 7E is an optical image of nanoreactors patterned on top of a polystyrene thin coated glassy carbon substrate. The full circle in the bottom left corner represents the scanning origin point corresponding with the circle in Figure 7D.
[0029] Figure 8 is a representative high-resolution HAADF-STEM image of a Ru52Co33Mn9Cr6nanoparticle prepared by DPN. Plane spacing of 0.21 nm corresponds to (200) facets of Ru metallic nanoparticles. Scale bar = 5 nm.
[0030] Figures 9A to 9F shows an HAADF-STEM image (9A) and corresponding EDX elemental maps (9B-9F) of a DPN-prepared Ru52Co33Mn9Cr6 nanoparticle. Scale bars = 5 nm.
[0031] Figure 10 is an EDX elemental spectrum of a DPN-prepared Ru52Co33Mn9Cr6 nanoparticle. Nitrogen, Silicon, and some of the Oxygen signals are attributed to the use of a SiNx TEM grid as sample substrate.
[0032] Figure 11 is an EDX elemental spectrum of a Ru52Co33Mn9Cr6 oxide nanoparticle. Nitrogen, Silicon, and some of the Oxygen signals are attributed to the use of a SiNx TEM grid as sample substrate.
[0033] Figure 12 is a high-resolution HAADF-STEM image of a Ru52Co33Mn9Cr6 oxide particle after electrochemical measurement. The plane spacing of 0.13 nm corresponds to (301) facets of rutile phase RuO2. Scale bar = 5 nm.
[0034] Figures 13A to 13F show a HAADF-STEM image (13A) and corresponding EDX elemental maps (13B-13F) of the Ru52Co33Mn9Cr6 oxide nanoparticle in Figure 12. Scale bars = 10 nm.
[0035] Figure 14 is an EDX elemental spectrum of the Ru52Co33Mn9Cr6 oxide nanoparticle in figure 13. Nitrogen, Silicon, and some of the oxygen signals are attributed to the use of a SiNx TEM grid as sample substrate.
[0036] Figure 15 shows OER polarization curves of scaled-up catalysts with different levels of performance. The graphs correspond to each of “Excellent”, “Good”, “Medium”, and “Bad” performance quartiles.
[0037] Figure 16 is an EDX elemental spectrum of the Ru52Co33Mn9Cr6 catalyst in Figure 4E. Nitrogen, silicon, and some of the oxygen signals are attributed to the use of a SiNxTEM grid as sample substrate. Titanium peaks are from the Ti felt.Docket No.30938 / 2023-039
[0038] Figure 17 are the XRD patterns of Ru52Co33Mn9Cr6catalysts as prepared (top first spectrum) and the reference patterns for Ti [PDF #44-1294], Co3O4[PDF #42-1467], and RuO2[PDF #40-1290].
[0039] Figure 18 is the XPS survey spectrum of a scaled up Ru52Co33Mn9Cr6oxide catalyst.
[0040] Figure 19A is a high-resolution XPS spectrum of the scaled up Ru52Co33Mn9Cr6 oxide on Ti felt catalyst showing the Ru 3d region, which overlaps with the C 1s peak.
[0041] Figure 19B is a high-resolution XPS spectrum of the scaled up Ru52Co33Mn9Cr6oxide on Ti felt catalyst showing the Ru 3p, which slightly overlaps with Ti 2p.
[0042] Figure 19C is a high-resolution XPS spectrum of the scaled up Ru52Co33Mn9Cr6 oxide on Ti felt catalyst showing the Co 2p region.
[0043] Figure 19D is a high-resolution XPS spectrum of the scaled up Ru52Co33Mn9Cr6 oxide on Ti felt catalyst showing the Mn 2p region.
[0044] Figure 19E is a high-resolution XPS spectrum of the scaled up Ru52Co33Mn9Cr6 oxide on Ti felt catalyst showing the Mn 3s region.
[0045] Figure 19F is a high-resolution XPS spectrum of the scaled up Ru52Co33Mn9Cr6 oxide on Ti felt catalyst showing the Cr 2p region. DETAILED DESCRIPTION
[0046] Methods in accordance with the disclosure provide for screening of a megalibrary of nanoparticles for catalytic activity. The methods of the disclosure can advantageously allow for catalytic screening on the megalibrary scale, which can allow for a significant increase in the pace of discovery of catalysts. The observed correlation between chip-based catalyst activity and scaled-up versions of the catalysts confirmed this approach for rapid screening of megalibraries to identify promising new electrocatalyst candidates, such as, for example, for OER and other reactions. Additionally, the methods of the disclosure can be used in combination with machine learning to inform and extract catalyst design features for a given reaction and to further reduce materials cost.
[0047] Methods of screening a nanoparticle megalibrary for catalytic activity in accordance with the disclosure can include disposing a substrate comprising the nanoparticle megalibrary in a scanning droplet cell, forming a droplet of the electrolyte at the scanning droplet cell head opening, and obtaining an electrochemically active surface area (ESCA) of the sample via a setDocket No.30938 / 2023-039 of cyclic voltammetry measurements across the substrate using at least four different scan rates. The method further includes moving the scanning droplet cell head with the droplet of the electrolyte across the substrate at a substantially constant rate and with a substantially constant applied potential and collecting electrochemical signal data at discrete points across the substrate; and correlating the set of cyclic voltammetry measurements to an electrochemically active surface area and forming a position-to-specific activity mapping of the substrate by subtracting a background current of the substrate and normalizing the electrochemical signal data measured across the substrate.
[0048] Referring to Fig.1, the scanning droplet cell head can include a reference electrode, a counter electrode, a working electrode, and a flowing electrolyte. The electrolyte is flowed to the scanning droplet cell head to generate the droplet for performing the measurements on the megalibrary. For example, the electrolyte can be pumped to the scanning droplet cell head via a pump operating at a rotating speed, for example, of about 1 rpm to 4 rpm to form a suitable electrolyte droplet.
[0049] The reference electrode can be, for example, a saturated calomel electrode. The counter electrode can be, for example, graphite. Other suitable electrode materials can also be used herein. In the method disclosed, the megalibrary constitutes the working electrode.
[0050] During the scanning, an electrolyte droplet is arranged above the substrate such that a gap is defined between the droplet and the substrate. The scanning droplet cell head can be used to scan the droplet across the substrate of the megalibrary. The electrolyte droplet has a diameter less than about 500 micrometers. For example, the electrolyte droplet can have a diameter of about 300 to about 500 micrometers. The gap between the droplet and the substrate can be about 50 micrometers to about 100 micrometers.
[0051] The electrolyte can be an acid electrolyte with a pH of about 0 to about 4. The electrolyte can be, for example, one or more of HClO4, H2SO4, HNO3, and HCl. The electrolyte can optionally be saturated with Argon before being loaded in the scanning droplet cell device. Other non-acidic electrolytes are also contemplated herein.
[0052] The specific activity mapping of the sample is determined in the methods of the disclosure by obtaining a position to electrochemical activity (ECSA) map and a catalytic current activity map. The correlation can further include subtracting the background current of the substrate from the catalytic current data and normalizing this data with the interpolated ECSA map.Docket No.30938 / 2023-039
[0053] The ECSA map can be generated from a series of stationary cyclic voltammetry measurements in the non-faradaic region of 0.9-1.0 V vs RHE using at least 4 scan rates. The scan rates can be selected from the range of about 10 mV / s to about 500 mV / s. The scan rates can be for example, 400, 200, 150, and 100 mV / s. The SDC head can be further programed to collect a cyclic voltammetry signal at each of the at least four different scan rates at regular intervals across the substrate. For example, the stationary cyclic voltammetry measurements can be performed every 2000 micrometers to every 1000 micrometers, or every 1000 micrometers to every 500 micrometers, or every 500 micrometers to 200 micrometers in the x and / or y directions. The specific capacitance at each point can be calculated by linear interpolation of the measured current by the voltage scan rate. Automated data processing can be used to perform these calculations at each data point to generate a position-dependent array of ECSA values. Delaunay triangulation and barycentric interpolation can be applied to the ECSA map to match the resolution of the catalytic current activity map when different data collection intervals are used.
[0054] The catalytic current activity map can be measured at a constant applied potential. The applied potential can be between about 1.5 V and 1.8 V vs RHE. The applied potential can be, for example 1.7 V. Measurements at the substantially constant applied potential can be made while moving the scanning droplet cell head across the substrate at a substantially constant rate and collecting measurement data at discrete locations during the movement. For example, measurement data can be collected every 50 µm to 500 µm in the x direction and every 500 µm to 1000 µm in the y direction. The scanning droplet cell head can be moved across the substrate at a rate of about 50 micrometers / s to about 500 micrometers / s. Other suitable rates include about 50 micrometers / s to about 100 micrometers / s, about 150 micrometers / s to about 300 micrometers / s, about 250 micrometers / s to about 500 micrometers / s or about 200 micrometers / s to about 400 micrometers / s. For example, the rate can be about 50, 75, 100, 125, 150, 175, 200, 225, 250, 275, 300, 325, 350, 375, 400, 425, 450, 475, or 500 micrometers / s, or any values therebetween or ranges defined by such values. For example, the scanning droplet cell head can be moved across the megalibrary at a rate of 300 µm / s.
[0055] The megalibrary can be prepared on any suitable substrate. For example, the substrate can be a glassy carbon substrate. For example, the glassy carbon substrate can be obtained via annealing a multilayer of S1813 photoresist deposited on As-doped silicon. Megalibraries of nanoparticles can be prepared using any known methods. For example,Docket No.30938 / 2023-039 polymer pen lithography can be used to deposit megalibraries with a plurality of nanoparticles, for example, a megalibrary can have at least 100,000 nanoparticles. Megalibraries can include millions of nanoparticles. For example, a megalibrary can have about 200 million distinct nanoparticles in a 2 cm x 2 cm area. The nanoparticles can be made of a single element or contain multiple elements. For example, a four-metal nanoparticle megalibrary can be prepared by loading the polymer pen lithography unit with four inks each containing a different metal precursor. Such megalibrary can have at least 250,000 different compositions on a 4 cm2substrate.
[0056] The simultaneous deposition of multiple metals can lead to a concentration gradient along the substrate which can be divided by the pen separation to calculate the compositional variation between each pen position and furthermore to calculate the composition variation within a given area, for example the area covered by the electrolyte droplet. The composition gradient can be from 100% to 0% between adjacent corners of the substrate or any values therebetween or ranges defined by such values. For example, in a four-metal megalibrary, the composition of one element can vary from 84% to 7.5% between two adjacent corners of the substrate. This range divided by, for example, a 30-micrometer pen separation, results in an atomic composition variance of about 0.5%. The composition variance within a 500-micrometer droplet can be calculated to be about 1.27%.
[0057] The megalibrary can include a compositional difference of nanoparticles within the area of the droplet of less than 5%, less than 3%, or less than 1.5%. For example, the difference in compositions of the nanoparticles within the area of the droplet can be about 0.5% to about 5%, about 1% to about 2%, about 0.5% to about 1.5%, or about 3% to about 5%. Other suitable values of the compositional difference within an area of the droplet can be about 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8.3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, or 5% or any values therebetween or ranges defined by such values.
[0058] The nanoparticles in the megalibrary can be metal oxide particles. The metals can be one or more of Ru, Co, Mn, and Cr.
[0059] The methods of the disclosure can be used for scanning for a variety of catalytic activity, such as, for example, oxygen evolution reaction (OER), hydrogen evolution reaction (HER), hydrogen oxidation reaction (HOR), or oxygen reduction reaction (ORR). The applied potential used during the method of the disclosure for obtaining the CV measurements can beDocket No.30938 / 2023-039 about 1.5 V to about 1.8 V. A suitable value can be selected based on the type of catalytic activity to be screened.
[0060] Methods of the disclosure can include an alignment process performed before measuring the electrochemical signal of the substrate. For example, the alignment process can include positioning the scanning droplet cell head opening at a plurality of regions across the substrate and recording the height at each region. For example, the scanning droplet cell head opening can be positioned at each corner of the substrate. The substrate position can be adjusted until the height measurement at each of the plurality of regions is within 10 micrometers of each other. For example, the substrate can be measured at each corner until the height at each corner has a height difference of less than 10 micrometers. Other suitable height differences include 8 micrometers to about 5 micrometers, 5 micrometers to about 3 micrometers, 3 micrometers to about 1 micrometer. For example, the height differences can be about 10, 9, 8, 7, 6, 5, 4, 3, 2 or 1 micrometers, or any values therebetween or ranges defined by such values.
[0061] Catalysts in accordance with the disclosure can include Ru52Co33Mn9Cr6 oxide, Ru29Co35Mn16Cr20 oxide, Ru23Co41Mn13Cr23 oxide, Ru14Co35Mn16Cr25 oxide, Ru49Co33Mn11Cr7 oxide, Ru36Co38Mn13Cr13 oxide, Ru60Co10Mn27Cr3 oxide, Ru36Co28Mn20Cr16 oxide, Ru24Co60Mn4Cr12 oxide, Ru26Co60Mn4Cr10 oxide or other oxides within the composition variance. For example, Ru51.2-52.8 Co32.5-33.5Mn8.9-9.1Cr5.9-6.1 oxide, Ru28.5-29.5Co34.5-35.5Mn15.8-16.2Cr19.7-20.3 oxide, Ru22.7-23.3Co40.4-41.6Mn12.8-13.2Cr22.7-23.3 oxide, Ru13.8-14.2Co34.5-35.5Mn15.8-16.2Cr24.6-25.4 oxide, Ru48.3-49.7Co32.5-33.5Mn10.8-11.2Cr6.9-7.1 oxide, Ru35.5-36.5Co37.4-38.6Mn12.8-13.2Cr12.8-13.2 oxide, Ru59.1- 60.9Co9.9-10.2Mn26.6-27.4Cr2.96-3.05 oxide, Ru35.5-36.5Co27.6-28.4Mn19.7-20.3Cr15.8-16.2 oxide, Ru23.6-24.4Co59.1- 60.9Mn3.9-4.1Cr11.8-12.2 oxide or Ru25.6-26.4Co59.1-60.9Mn3.9-4.1Cr9-10.2 oxide. Catalysts in accordance with the disclosure can be selected as having a specific activity, for example, in the top quantile as measured in a megalibrary or a minimum activity value, for example, catalysts with a specific activity of at least 1.19 mA / cm2. EXAMPLES
[0062] General Methods and Materials. Polystyrene (atactic; Mn 4,200 Mw / Mn = 1.05; 10,000 Mw / Mn = 1.09; 25,000 Mw / Mn = 1.04; 51,000 Mw / Mn = 1.03) and Poly(2-vinylpyridine)- b-poly(ethylene oxide) (Mn 1,500-b-2,800 Mw / Mn = 1.11) were purchased from Polymer Source and used as received. Ruthenium (III) chloride hydrate (99.9% trace metals basis), Cobalt (II) chloride hexahydrate (ACS reagent, 98%), Chromium(III) nitrate nonahydrate (99%), HCl (70%, redistilled, ^99.999%), acetylacetone, ethanol, and toluene were purchased from Sigma-AldrichDocket No.30938 / 2023-039 and used as received. Manganese (II) nitrate tetrahydrate (for analysis), Sylgard 184 PDMS and S1813 positive photoresist were purchased from Fisher Scientific. Ultra-high purity H2(99.999%), Ar (99.999%), and O2(99.994%) were purchased from Air-Gas. Deionized (DI) water used in all experiments was Millipore ultrapure water (18.2 MW·cm). Silicon substrates (As-doped, item number: 1113, 0.5 mm thick) were purchased from University Wafer. The Ti felt and commercial RuO2and IrO2were purchased from the Fuel Cell Store. Silicon nitride support film transmission electron microscopy (TEM) grids (15 nm with 9 each 0.1 x 0.1mm windows) were purchased from Ted Pella, Inc. Dip-pen nanolithography (DPN) 1D pen arrays (type M, no gold coating) were purchased from Nanoink, Inc.
[0063] Scanning electron microscopy (SEM) was performed using a Hitachi SU8030 SEM with 5.0 kV acceleration voltage and 10 µA emission current. A high probe current for secondary electron imaging was performed using a JEOL JSM-7900FLV SEM with 5.0 kV acceleration voltage. DPN / SPBCL on silicon nitride TEM membranes and scanning transmission electron microscopy-energy dispersive spectroscopy (STEM-EDX) characterization were performed as previously described on a JEOL ARM200CF STEM microscope. Atomic force microscopy (AFM) was performed using a Bruker Dimension Icon AFM in tapping mode with an NCHR probe, and data analysis was performed using NanoScope Analysis. Optical microscopy was performed using a Zeiss Axio Imager with appropriate dark-field, brightfield, or fluorescence filters. Electron beam evaporation was performed using a Pro-Line PVD 75 system (Kurt J. Lesker). A Lindberg Blue tube furnace with quartz tubes was used for thermal annealing. Grazing incidence X-ray diffraction (GIXRD) was performed with a Smartlab Gen29 kW system. Inductively coupled plasma mass spectrometry (ICP-MS) was performed using a Thermo Element2 High-Resolution Magnetic Sector Field instrument. Air plasma treatments were performed in a Plasma Etch, Inc. plasma cleaner. The Xe arc lamp light source, power supply, and 435 nm long-pass filter used for photocatalysis were purchased from Newport Corporation. X-ray photoelectron spectroscopy (XPS) spectra were acquired on a Thermo Fisher NEXSA G2 surface analysis system with an Al-K^ X-ray source (1486.6 eV). A 500 ^m spot size with surface charge compensation was selected. The survey spectra and the high-resolution spectra were collected with pass energy of 150 eV (1 eV / step) and 50 eV (0.1 eV / step), respectively. Since the C 1s peak had significant overlap with other elements present in the sample, all spectra were calibrated to the obtained Co 2p3 / 2peaks at 779.7 eV (typical 2p3 / 2value for Co2+in CoOx). To calculate the relative element concentration during the durability tests, oxygen from TiO2on Ti felt was excluded from the total oxygen in the whole sample according to TiO2formula, and only oxygen from the catalysts was considered, i.e., oxygen in the catalystDocket No.30938 / 2023-039 [O]c=[O]-2×[Ti]. The relative concentrations of metal M (M%) were calculated using the following equation: M%=([M]t / [O]c,t) / ([M]0 / [O]c,0)×100%, where t is the durability testing time in seconds. The electrochemical screening was performed on the M470 scanning electrochemical workstation (from Bio-Logic). The scanning droplet cell head (SDC) was fabricated in Mattiq. Inc.
[0064] Substrate preparation for the polymer pen lithography (PPL). A 4-inch diameter As-doped silicon wafer was spin-coated with S1813 positive photoresist at 2,000 rpm and then placed on a hotplate set to 115 ºC for 1 min. This process was repeated four times to prepare a uniform layer. The resulting coated wafer was then cut into 2 cm x 2 cm pieces. The substrates were then annealed at 200 standard cubic centimeters per minute (sccm) of 10% H2 in Ar. The substrates were heated to 1000 ºC with an 8.5 h ramp and then held at 1000 ºC for 1 h before slowly cooling to room temperature to obtain the glassy carbon (GC) substrates. Polystyrene thin film coating was prepared according to a previous report (2). The substrates were first washed with isopropanol and dried under a stream of N2. A 5% w / v solution of polystyrene (Mn = 10,000) in toluene (50 mg / mL) was prepared and passed through a 0.2 µm PTFE syringe filter. Polystyrene thin films were prepared by spin coating 150 µL of the solution on the substrate at 2,500 rpm followed by placing the substrates on a hotplate set to 110 ºC for 2 min.
[0065] Preparation of Polymer Pen Arrays. Pen arrays were fabricated with modifications to previous report. Silicon masters etched with arrays of inverted pyramids with 30 µm bases and 30 µm pitches over 4 cm x 4 cm were purchased from Hawk Semiconductor.3 layers of scotch tape (from 3M) were put along the edges of the master to make rails about 175 nm thick. Sylgard 184 PDMS (curing agent: base agent = 1:10) was prepared and degassed then added to the edge of the master. A clean glass slide was passed along the tape rails to evenly spread the PDMS layer to mitigate the presence of air bubbles and dust particles. This was allowed to settle at room temperature for 30 min and was then placed in an oven at 80 ºC for 15 min. Next, an additional 1 mL of PDMS was added to the center of the master, and a clean 2 in x 2 in x 1 / 16 in glass plate (air plasma treated, 30 W, 2 min) was placed on top. The PDMS was allowed to spread completely under the glass plate, which was then secured in place using additional glass slides, and then placed in an oven at 80 ºC overnight. Excess-cured PDMS was removed from the edges of the pen array, which was then peeled off from the master. The pen array was then covered with a custom-made mask before using electron beam evaporation to apply 5 nm of Cr followed by 150 nm of Au.Docket No.30938 / 2023-039
[0066] Nanoreactor patterning and nanoparticle synthesis. A RuCoMnCr oxide OER catalyst megalibrary was synthesized using a PPL-enabled SPBCL method. All metal precursor inks were prepared in 1 M HCl at a concentration of 41.5 mM. Precursor inks were prepared as 5% poly(ethylene oxide)-b-poly(2-vinylpyridine) (PEO-b-P2VP) block copolymer w / v aqueous solutions with 1.0 mM metal salt. These values give a total metal-to-pyridine group molar ratio of 1:16. Specifically, 1.75 mL DI water, 200 µL polymer solution (50 mg / mL in DI water), and 50 µL metal precursor (in 1 M HCl) were mixed and shaken overnight in the dark before use. A polymer pen array containing 250,000 pen tips separated 30 microns apart was spray-coated with a quaternary ink gradient composed of Ru, Co, Mn, and Cr metal salt precursors and a poly(ethyleneoxide)-b-poly(2-vinylpyridine) (PEO-b-P2VP)) block copolymer to pattern nanoreactors onto a glassy carbon (GC) substrate (Fig.1). For the ink spraying, a pen array was first blown with N2 gas to remove any dust particles and then treated with air plasma at 30 W for 1 min. A custom-made mask was applied to the pen array to expose the central 1.5 cm x 1.5 cm area for patterning. The pen array was secured underneath a spray gun such that the nozzle was 11.5 cm above the pen array and centered over one corner of the exposed area of the pen array. An eco-SPRAY (ViscoTec) spray gun was used to iteratively spray 5 µL of ink at each corner of the array. The arrays were allowed to dry between each spray. The spray controller was programmed to deliver 5 µL of ink at a rate of 3 mL / min and a pressure of 0.5 bar. After spraying each corner, the entire pen array was placed in an environment of 100% relative humidity for 10 s before drying in air to improve the spray homogeneity. These spray gun conditions were fixed throughout all syntheses.
[0067] For nanoreactor patterning, the inked pen array and polystyrene-coated substrate were attached to a TERA-print M-series lithography instrument. Lithography was performed in an environment of 90% relative humidity at room temperature such that a 25 x 25 pattern of nanoreactors was deposited with 1 µm spacing. Each droplet was made by moving the substrate into contact with the pen array at an approaching velocity of 50 µm / s with a contact force of 2000-2100 mN, and this force was maintained for 1 s followed by a retraction at a velocity of 100 µm / s off the substrate before moving to the next patterning position. After characterization of the nanoreactor patterning, thermal annealing in a tube furnace was performed under a 150 sccm flow of H2with a 1 h ramp from room temperature to 150 ºC. Then, the following heating profiles were used: 6 h ramp from 150 ºC to 240 ºC, a hold at 240 ºC for 12 h, a ramp to 625 ºC in 2 h, a hold at 625 ºC for 6 h, and a cooling to room temperature naturally. The oxidation process was performed at 400 ºC for 15 minutes in air with a 40 min ramp. For the DPN-SPBCL nanoparticle synthesis, 41.5 µmol metal precursors were dissolvedDocket No.30938 / 2023-039 in 1 mL 1 M HCl and stirred overnight to form clear solutions. Ru, Co, Mn, and Cr solutions were mixed according to the ratio of 52:33:9:6 and stirred overnight to form precursor solution I.5 mg poly(2-vinylpyridine)-b-poly(ethylene oxide) was dissolved in 1 mL water and shake overnight to form a colorless solution II. 25 µL solution I was added into 1 mL solution II and stirred overnight to form a uniform polymer ink. Silicon nitride support film TEM grid sealed in the same box with a vial containing 1 mL hexane and 1 mL HDMS overnight to make the surface hydrophobic before use. The DPN pen array was treated with air plasma for 1 min to make the surface hydrophilic and then mounted onto an AFM (XE-150, Park Systems), coated with the polymer ink, and brought into contact with the hydrophobic silicon nitride TEM grid to write nanoreactor arrays under 80% relative humidity at 25 °C. The annealing program was the same as the megalibrary sample.
[0068] The morphology and size of the resulting nanoparticles were characterized by scanning electron microscopy (SEM) and atomic force microscopy (AFM), which indicated that nanoparticles formed throughout the megalibrary were predominately single particle structures (>95% yield) (Fig.5). In the four quadrants of the megalibrary, the size of nanoparticles was, on average, 16.7 nm ± 2.5 nm for the Ru-rich region, 14.5 nm ± 2.5 nm for the Co-rich region, 14.5 nm ± 2.7 nm for the Mn-rich region, and 14.5 nm ± 3.1 nm for the Cr-rich region (Fig.5E to 5H). Finally, air oxidation at 400°C was used to transform the RuCoMnCr nanoparticle megalibrary into a RuCoMnCr oxide nanoparticle megalibrary (confirmed by scanning transmission electron microscopy (STEM), vide infra). Nanoparticles remained intact after the oxidation process (Fig. 2B to E), and the particle sizes slightly increased to 19.9 nm ± 2.7 nm, 15.9 nm ± 3.4 nm, 16.4 nm ± 3.3 nm, and 15.8 nm ± 2.8 nm for the Ru-, Co-, Mn-, and Cr-rich regions respectively (Fig. 2F to I), which was attributed to lattice expansion due to oxygen incorporation into the nanoparticles.
[0069] Electrocatalysis screening. Electrochemical screening was performed in accordance with the disclosure using a customized scanning droplet cell (SDC) (Fig.1) containing a reference electrode (saturated calomel electrode), a counter electrode (graphite), and a flowing electrolyte (0.5 M H2SO4, Ar-saturated) was moved laterally across the megalibrary (working electrode). During the scanning, a 500 µm diameter electrolyte droplet with a 1.27% atomic screening resolution was created at the SDC opening to perform serial measurements of electrochemical signals. The composition variance under one electrolyte droplet (diameter = 500 µm) was estimated to be 1.275%. The calculation follows these steps:Docket No.30938 / 2023-039 1) The composition range in x or y-direction for one element = 84% – 7.5% = 76.5% in the megalibrary according to the composition difference between two adjacent corners on the same edge. 2) Each pen tip had a separation of 30 microns and each polymer pen array had 500 x 500 pen tips for patterning. Therefore, each pen tip had a composition difference ^^^^^ ^ ^ ^^^^^^ ^^^ on average. ^^^^^^ ^ ^ ^^^^^^^ ^ ^ ^ ^^^^^^^ 3) Under one droplet, the composition variance ^^^^^
[0070] To evaluate OER activity, a set of cyclic(CV) experiments at four different scan rates over a non-faradaic region (0.9-1.0 V vs. RHE) was performed to determine the electrochemically active surface area (ECSA) across the whole chip (Fig.6 and 7B).
[0071] To measure the catalytic activity and produce catalytic current maps, the SDC head was scanned across the megalibrary at a slower velocity (300 µm / s) and at a constant applied potential of 1.7 V vs. RHE (Fig.7A). To analyze the data, the background current of bare GC was subtracted from the catalytic current, and the current was normalized with ECSA to generate a final specific activity (SA) map (Fig.2J). The M470 scanning electrochemical workstation, from BioLogic using scanning droplet cell (SDC) methodology was used to perform electrochemical screening. A custom 3-D printed SDC head from Mattiq. Inc. was used to mitigate fluctuations in droplet volume and ensure continuous contact with the substrate. A flowing 0.5 M H2SO4 electrolyte was circulating at a flow rate of 2 rpm in the SDC head through a pump (Masterflex Ismatec Reglo ICC Digital Pump), creating a droplet with a diameter of 500 µm. A three-electrode cell system was used to conduct all electrochemical tests. A saturated calomel electrode (SCE) reference electrode and a graphite counter electrode were embedded in the SDC head. The SCE was calibrated in a hydrogen-saturated 0.5 M H2SO4 electrolyte before use.
[0072] The working electrode was the RuCoMnCr oxide megalibrary. The electrochemically active surface area (ECSA) was determined by: ECSA = Cdl / Cs, where Cdlis the double-layer capacitance and Csis the specific capacitance of the sample. In this study, a general specific capacitance of Cs = 0.65 mF cm−2was used based on previous research of Ru / Ir oxides. Cdlwas determined by the equation Cdl= Ic / ^, where Icis the charging current and ^ is the scanDocket No.30938 / 2023-039 rate. A series of cyclic voltammetry (CV) tests in the non-faradaic potential region 0.9-1.0 V versus the reversible hydrogen electrode (RHE) under four different scan rates (400, 200, 150, and 100 mV s−1) were performed. The Cdlwas obtained by fitting the slope of the Icversus ^ curve. The ECSA measurement was programmed to allow the SDC head to scan and collect the CV signal every 1000 micron step in x and y-directions across the whole chip. Automated data processing methods were employed to analyze >1,000 CV datasets and generate the position-to-ECSA mapping, and outlier points > 3 standard deviations from the mean were removed from the dataset. After ECSA measurement, the SDC head was programmed to scan across the megalibrary at a slow velocity of 300 µm / s at a constant applied potential of 1.7 V vs. RHE, collecting a discrete datapoint every 100 µm x-step and every 500 µm y-step. Automated data processing was then applied to generate the position-to-current mapping, and outliers were handled similarly to the ECSA procedure. To interpolate between data points in each map, the Delaunay triangulation and barycentric interpolation was used to attain ECSA values for the more finely discretized current measurements. To obtain a position-to-specific activity (SA) mapping, the background current of the substrate was subtracted from the catalytic current and normalized the resulting current with ECSA. Finally, the SDC coordinate system was adjusted to the spray gun coordinate system by cross-comparing the optical image of the substrate before and after electrochemical measurements to get accurate position-to-composition mapping, finishing a set of mappings to get current, ECSA, SA, and composition from each position across the megalibrary. To find representative samples for performance studies, data points were first separated into four quantiles (each level is 25%) based on SAs. Then, within each quantile, the SA compositions were identified subject to the constraints that no two data points were within 2000 µm of each other and that the chosen data point was within 2 standard deviations of SAs compared against all points within a 2500 µm x 2500 µm square centered on the chosen point. These constraints were designed to ensure greater compositional sampling and avoid local outliers, respectively.
[0073] The regions having the highest activity on the SA map were identified by cross- comparing the optical image of the GC substrate after PPL and electrochemical measurements, respectively (Fig.7D and E). The elemental composition at a given position on the megalibrary were determined using energy-dispersive x-ray spectroscopy (EDX) and inductively coupled plasma mass spectrometry (ICP-MS). Through this process, two highly active regions with a diameter of 1000 µm were observed (circles, Fig.2J). On average, these regions corresponded to Ru52Co33Mn9Cr6oxide and Ru29Co35Mn16Cr20oxide compositions, with Ru52Co33Mn9Cr6oxide showing the highest OER activity, and were thus chosen for scaled-up synthesis and analysis.Docket No.30938 / 2023-039
[0074] Catalysts synthesis and characterization on a large scale. Ru52Co33Mn9Cr6oxide nanoparticles were resynthesized on a silicon nitride membrane via SPBCL and dip-pen nanolithography (DPN) for high-angle annular dark-field STEM (HAADF-STEM) and EDX characterization. After the membrane was annealed under H2, the size of the replicated Ru52Co33Mn9Cr6 was similar to the particles synthesized by PPL (Fig.8), and the HAADF-STEM image indicated a plane spacing of 0.21 nm, which corresponds to a (200) facet for Ru metallic nanoparticles. The STEM-EDX mapping revealed that Ru, Co, Mn, and Cr were distributed uniformly throughout the nanoparticle (Figs.9 and 10). A native metal oxide shell was observed on the nanoparticle surface, which is attributed to the highly reactive nature of Co, Mn, and Cr metals that oxidize upon exposure to the atmosphere (Fig.9F). After oxidation, changes in the structure and elemental distribution in the nanoparticle are observed. Specifically, oxygen diffuses into the core of the nanoparticle leading to a slight lattice expansion from 0.21 nm to 0.23 nm (Fig.3A), which indicates the transformation from metal to oxide (Fig.3B to G and fig. 11). After 4 CV cycles and subsequent OER measurements, there were no detectable changes in morphology (Figs.12-14).
[0075] Similar to the megalibrary screening, different atomic compositions of Ru, Co, Mn, and Cr precursor solutions were prepared. Next, the dispersion was sprayed coated on platinized Ti felt (Fuel cell store, product code: 592800) which was then annealed in air at 400oC for 1 h with a 5oC / min ramp rate. The loading of electrocatalyst on platinized Ti felt was determined to be 2 to 3 mg / cm2. Two methods were used to prepare the working electrode in electrochemical measurements. In the first method, the electrocatalysts were synthesized using a sol-gel method. For example, for Ru52Co33Mn9Cr6 oxide, 0.13 mmol Ru (RuCl33H2O, 33.99 mg), 0.0825 mmol Co (CoCl210.71 mg), 0.0225 mmol Mn (MnCl2, 2.83 mg), and 0.015 mmol Cr precursor (CrCl36H2O, 4 mg) were dissolved in 8 mL of ethanol in a 30 mL vial and shaken for 1 h. Then 60 mg of PVP (MW: 10,000) were added into the vial and shaken till all PVP was dissolved. After stirring the solution for 3 h, 12 mL of ethanol were added, and the vial was placed in a 65oC oil bath to evaporate the ethanol. The remaining powder was collected and uniformly spread in a quartz boat to heat treat in a muffle furnace at 400 °C with a 5 °C / min ramp rate and annealed for 3 hrs. For OER activity test, 3 mg of electrocatalyst and 1 mg carbon black were added to a 1 mL ethanol and 12 µL Nafion (Sigma Aldrich) to prepare the electrocatalyst ink.16.7 µL of ink were drop cast on a GC rotating disk electrode with a diameter of 5 mm for OER activity evaluation. In the second method, the platinized Ti-felt (active geometric area of 1 cm2) was used directly as the working electrode to study the activity correlation and catalyst stability. OER electrochemical performance of synthesized catalystsDocket No.30938 / 2023-039 was evaluated in a typical three-electrode setup in 0.5 M H2SO4. Ag / AgCl was used as the reference electrode, and a platinum coil was used as the counter electrode. The OER activity was measured using a linear sweep voltammetry at a scan rate of 5 mV / s within the range from 1.2 V to 2 V (vs. RHE). The evaluation of ECSA used a similar method as in the megalibrary characterization. Specifically, the scanning non-faradic region is 1.0 to 1.1 V vs. RHE and the scan rates are 50, 40, 30, 20, and 10 mV / s.
[0076] To determine whether the catalyst activity observed in the megalibrary correlates with comparable materials synthesized on a large-scale form, catalysts were directly synthesized on a platinized Ti felt and performed electrochemical measurements. To check for correlation, a group of 10 catalysts was sampled across four SA quantiles (excellent, good, medium, and bad) identified during megalibrary screening (Table 1). Table 1 Excellent xySA in megalibrarySA in Validation (mA / cm2) (mA / cm2)Co Cr Mn Ru16157 2190 2.18 1.98 0.33 0.06 0.09 0.52 2 1490 4857 1.48 1.22 0.10 0.03 0.27 0.60 3 6757 5690 1.44 1.32 0.28 0.16 0.20 0.36 Good xySA in(mmAe / cgmal2ib)rarySA in Validation (A / cm2)Co Cr Mn Ru45757 5190 1.17 0.93 0.25 0.12 0.21 0.43 5 8957 690 1.15 1.23 0.55 0.06 0.04 0.35 6 4357 5190 1.07 1.17 0.18 0.09 0.24 0.50 Medium xySA in megalSA in Validation (mA / cm2ibrary)(A / cm2)Co Cr Mn Ru75757 8190 0.95 0.99 0.16 0.20 0.35 0.28 8 4657 10190 0.83 0.54 0.08 0.20 0.50 0.21 Badx ySA in megal(mA / cm2ibrarySA in Validation )(A / cm2)Co Cr Mn Ru911857 190 0.61 0.46 0.73 0.07 0.02 0.18 10 13857 116900.48 0.50 0.18 0.70 0.09 0.03
[0077] To avoid researcher bias, an algorithm was used to make the selections. The algorithm-chosen compositions were then synthesized via direct precursor spray coating on a TiDocket No.30938 / 2023-039 felt electrode followed by annealing in air at 400 ºC for 1 h. Ti felt was used as the electrode support because it is used as the anode gas diffusion layer in PEMWEs. The SAs of these samples at 1.7 V vs. RHE were measured in a typical three-electrode setup, using a platinum coil as the counter electrode and Ag / AgCl as the reference electrode (Figs.15). Remarkably, the SAs of these 10 synthesized catalysts showed a strong linear correlation with the SAs determined from the megalibrary (R2= 0.91) (Fig.4A) despite dramatically different synthesis methods, catalyst loading, choice of substrate electrode, and measurement methods. Taken together, the results provide confidence that activity profiles measured in the megalibrary reflect the scaled-up forms of the catalysts.
[0078] The most active Ru52Co33Mn9Cr6 oxide exhibited an overpotential of 219 mV at a geometric current density of 10 mA / cm2on the GC electrode during a rotating disk electrode measurement (Fig.4B), which is 86 mV lower than the overpotential of commercial RuO2.
[0079] Structural characterization was performed of the scaled-up Ru52Co33Mn9Cr6 oxide catalyst and compared with the nanoparticles synthesized using SPBCL and DPN methods. STEM images showed a uniform size distribution below 10 nm (Fig.4C and D), and HR- HAADF-STEM revealed a plane spacing of 0.32 nm, corresponding to the (110) facets of rutile phase RuO2 (Fig.4D). The fast Fourier transform (FFT) (inset of Fig.4D) indicated the existence of RuO2 (200) and (211) facets with a plane spacing of 0.23 nm and 0.17 nm, respectively. EDX results showed uniform distributions of Ru, Co, Mn, and Cr across the sample (Fig.4E to 4J and fig.16), in accordance with the megalibrary results (Fig.3C to G). The grazing incidence X-ray diffraction (GIXRD) results suggested that the diffraction peak at 2θ = 28.1° corresponded to the (110) facet of rutile phase RuO2, which was the dominant phase in the catalyst accompanied by a noticeable amount of spinel phase Co3O4 evidenced by the preferred (311) crystal facet. (Fig.17). The nanoparticle grain size was between 7-9 nm, which is smaller but close to the particle size in PPL (Fig.2F-I). X-ray photoelectron spectroscopy (XPS) was performed to study the near-surface oxidation states of the catalyst elements (Figs. 18 and 19 and Table 2).Docket No.30938 / 2023-039 Table 2 Assigned Assigned Ratio (%) oxidation Ratio (%) Region oxidation state 2 state 1 As-prepared As-prepared Ru3p 4+ 100 - - Co2p 3+ 79 2+ 21 Mn2p 4+ 100 - - Cr2p 3+ 65 6+ 35
[0080] Due to the overlap of Ru 3d and C 1s peaks (Fig.19A), Ru 3p peaks were used for analysis. The Ru peaks at 463.0 eV and 485.4 eV were assigned to Ru4+3p3 / 2and Ru4+3p1 / 2, respectively (Fig.19B), which match the STEM and EDX results (Fig.4C to J). The Co 2p peaks were deconvoluted into 3 sets of peaks (779.6 eV and 795.0 eV, 781.5 eV and 797.3 eV, and 785.3 eV and 803.0 eV) (Fig.19C), corresponding to Co3+, Co2+, and satellite peaks, respectively. Although the chemical states of Mn were difficult to determine due to the low concentration and the very similar binding energies of Mn2+2p3 / 2, Mn3+2p3 / 2, and Mn4+in the 2p3 / 2 region energy level splitting (4.7 eV) of Mn 3s peaks indicated the Mn are mostly Mn4+(Fig. 19D and E). The Cr 2p3 / 2 peak was deconvoluted into peaks from Cr6+(577.9 eV) and Cr3+(575.5 eV) (Fig.19F).
[0081] The foregoing description is given for clearness of understanding only, and no unnecessary limitations should be understood therefrom, as modifications within the scope of the disclosure may be apparent to those having ordinary skill in the art.
[0082] All patents, patent applications, government publications, government regulations, and literature references cited in this specification are hereby incorporated herein by reference in their entirety. In the case of conflict, the present description, including definitions, will control.
[0083] Throughout the specification, where the compounds, compositions, methods, and / or processes are described as including components, steps, or materials, it is contemplated that the compounds, compositions, methods, and / or processes can also comprise, consist essentially of, or consist of any combination of the recited components or materials, unless described otherwise. Component concentrations can be expressed in terms of weight concentrations, unless specifically indicated otherwise. Combinations of components are contemplated to include homogeneous and / or heterogeneous mixtures, as would be understood by a person of ordinary skill in the art in view of the foregoing disclosure.
Claims
Docket No.30938 / 2023-039 What is claimed is:
1. A method of screening a nanoparticle megalibrary for catalytic activity, comprising: disposing a substrate comprising the nanoparticle megalibrary in a scanning droplet cell comprising: a scanning droplet cell head comprising a reference electrode and a counter electrode arranged within the scanning droplet cell head, and an electrolyte in fluid communication with the scanning droplet cell head and adapted to be circulated into the scanning droplet cell head; forming a droplet of the electrolyte at the scanning droplet cell head, the droplet having a diameter of less than about 500 micrometers, and arranged such that a gap of about 50 micrometers to about 100 micrometers is disposed between the substrate and the droplet; obtaining an electrochemically active surface area (ECSA) of the sample via a set of cyclic voltammetry measurements taken a discrete regions across the substrate using at least four different scan rates comprising: disposing the scanning droplet cell head with the droplet of electrolyte in a first region of the substrate and measuring a cyclic voltammetry signal at each of the at least four different scan rates, moving the scanning droplet cell head with the droplet of electrolyte to a second region of the substrate and measuring a cyclic voltammetry signal at each of the at least four different scan rates at the second region, a distance between the first region and the second region of the substrate being no more than 2000 micrometers, and repeating moving the scanning droplet cell head and measuring a cyclic voltammetry signal at further regions of the substrate such that a cyclic voltammetry signal is measured at the at least four different scan rates at a plurality of regions across the substrate, with a distance between each adjacent region being no more than 2000 micrometers; moving the scanning droplet cell head with the droplet of the electrolyte across the substrate at a substantially constant rate with a substantially constant applied potential and collecting electrochemical signal data at discrete locations as the scanning droplet cell head is moved across the substrate; andDocket No.30938 / 2023-039 correlating the set of cyclic voltammetry measurements to an electrochemically active surface area and forming a position-to-specific activity mapping of the substrate by subtracting a background current of the substrate and normalizing the electrochemical signal data measured at the discrete locations across the substrate, wherein the megalibrary comprises at least 100,000 nanoparticles arranged on the substrate.
2. The method of claim 1, further comprising an alignment process performed before obtaining the set of cyclic voltammetry measurements, the alignment process comprising: positioning the scanning droplet cell head at each corner of the substrate and recording a height of the substrate at each corner; and adjusting the substrate to achieve a position of the substrate in which a height difference between each corner is less than 10 micrometers.
3. The method of claim 1, wherein the droplet has a diameter of about 300-500 micrometers.
4. The method of any one of the preceding claims, wherein the electrolyte is acidic, and the acidic electrolyte has a pH of about 0 to about 4.
5. The method of any one of the preceding claims, wherein the electrolyte comprises one or more of HClO4, H2SO4, HNO3, and HCl.
6. The method of any one of the preceding claims, wherein measuring the electrochemical signal comprises measuring an electrochemical signal for catalysis of oxygen evolution reaction, hydrogen evolution reaction, hydrogen oxidation reaction, or oxygen reduction reaction.
7. The method of claim 6, wherein measuring the electrochemical signal comprises measuring an electrochemical signal for catalysis of oxygen evolution reaction activity.
8. The method of claim 7, wherein the droplet is scanned across the megalibrary with a constant applied potential of about 1.5 V to about 1.8 V.Docket No.30938 / 2023-039 9. The method of any one of the preceding claims, further comprising generating a visual display mapping of the measured electrochemical signal activity linked to the compositions of the nanoparticles under the droplet.
10. The method of any one of the preceding claims, wherein the scanning droplet cell head is moved at a substantially constant rate of 50 micrometers / s to 500 micrometers / s.
11. The method of any one of the preceding claims, wherein the megalibrary comprises nanoparticles having at least 250,000 different compositions.
12. The method of any one of the preceding claims, wherein the megalibrary comprises at least 1 million nanoparticles.
13. The method of any one of the preceding claims, wherein the nanoparticles are each oxides comprising Ru, Co, Mn, and Cr.
14. The method of any one of the preceding claims, wherein the electrolyte is pumped by a pump to the scanning droplet cell head at a rotating speed of the pump of about 1 rpm to about 4 rpm to form the electrolyte droplet.
15. The method of any one of the preceding claims, wherein correlating the set of the set of cyclic voltammetry measurements to an electrochemically active surface area and forming a position-to-specific activity mapping comprising using Delaunay triangulation and barycentric extrapolation methods to generate the position-to-specific activity map.
16. The method of any one of the preceding claims, wherein a variation of composition of the nanoparticles within an area of the droplet is less than 5%. 17 The method of any one of the preceding claims, wherein the variation of composition of the nanoparticles within the area of the droplet is less than 3%.
18. The method of any one of the preceding claims, wherein a variation of composition of the nanoparticles within an area of the droplet is less than 1.5%.Docket No.30938 / 2023-039 19. The method of any one of the preceding claims, wherein a variation of composition of the nanoparticles within an area of the droplet is about 1.27%.
20. A catalyst for oxygen evolution reaction, wherein the catalyst is an Ru51.2-52.8Co32.5-33.5Mn8.9-9.1Cr5.9-6.1or Ru28.5-29.5Co34.5-35.5Mn15.8-16.2Cr19.7-20.3oxide.
21. A catalyst for oxygen evolution reaction, wherein the catalyst is an Ru52Co33Mn9Cr6 oxide and Ru29Co35Mn16Cr20oxide.
22. A catalyst for oxygen evolution reaction, wherein the catalyst is: Ru22.7-23.3Co40.4-41.6Mn12.8-13.2Cr22.7-23.3oxide; Ru13.8-14.2Co34.5-35.5Mn15.8-16.2Cr24.6-25.4 oxide; Ru48.3-49.7Co32.5-33.5Mn10.8-11.2Cr6.9-7.1 oxide; Ru35.5-36.5Co37.4-38.6Mn12.8-13.2Cr12.8-13.2 oxide; Ru59.1-60.9Co9.9-10.2Mn26.6-27.4Cr2.96-3.05 oxide; Ru35.5-36.5Co27.6-28.4Mn19.7-20.3Cr15.8-16.2 oxide; Ru23.6-24.4Co59.1-60.9Mn3.9-4.1Cr11.8-12.2 oxide; or Ru25.6-26.4Co59.1-60.9Mn3.9-4.1Cr9-10.2 oxide.
23. A catalyst for oxygen evolution reaction, wherein the catalyst is: Ru23Co41Mn13Cr23 oxide; Ru14Co35Mn16Cr25oxide; Ru49Co33Mn11Cr7 oxide; Ru36Co38Mn13Cr13oxide; Ru60Co10Mn27Cr3 oxide; Ru36Co28Mn20Cr16oxide; Ru24Co60Mn4Cr12 oxide; or Ru26Co60Mn4Cr10oxide.
Citation Information
Patent Citations
Compositions for electrolyte fuel cells and other electrochemical conversion devices
US20210309845A1