Porous electrode for extraction of lithium from salt lake by means of electrochemical de-intercalation method, and preparation method therefor and use thereof
By coating the electrode active material with sodium thiosulfate, a mass transfer channel is formed, which solves the problems of slow mass transfer of lithium ions and uneven distribution of pore-forming agents caused by high electrode coating density, and significantly improves the reaction rate and lithium extraction rate from salt lakes. efficiency.
Patent Information
- Application Number
- PCT/CN2023/084387
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
In the existing electrochemical deintercalation salt lake lithium extraction technology, the high coating density of the electrode results in slow mass transfer of lithium ions, which affects the lithium extraction rate, and the use of pore-forming agents causes uneven distribution.
Sodium thiosulfate is used to coat the electrode active material. By forming a mass transfer channel in the outer layer of the electrode active material, the contact area between the salt lake brine and the lithium extraction active site is increased, the lithium extraction reaction rate is improved, and by controlling the concentration of sodium thiosulfate The adding amount and drying conditions ensure that the pore size and porosity are within the appropriate range to avoid the problem of uneven distribution of pore-forming agents.
It significantly improves the lithium extraction reaction rate and efficiency, reduces the polarization in the electrochemical lithium extraction process, increases the solution transmission path, improves the lithium ion transmission efficiency, and avoids the problem of uneven distribution of pore formers.
Smart Images

Figure CN2023084387_03102024_PF_FP_ABST
Abstract
Description
A porous electrode for extracting lithium from salt lakes using electrochemical deintercalation, and its preparation method and application Technical Field
[0001] The present invention relates to a porous electrode for extracting lithium from salt lakes using an electrochemical deintercalation method, a preparation method thereof, and an application thereof, and belongs to the technical field of extracting lithium from salt lakes. Background Art
[0002] In recent years, the rapid development of new energy vehicles and chemical energy storage has driven a continuous increase in global demand for lithium resources, making lithium a key strategic resource. Natural lithium resources primarily exist in salt lake brine, seawater, and ores, with salt lake lithium accounting for approximately 70%. Consequently, extracting lithium from salt lake brine is gaining increasing attention.
[0003] Salt lake brine contains elements such as lithium, sodium, potassium, and magnesium. Methods for extracting lithium from salt lakes primarily include precipitation, solvent extraction, evaporative crystallization, electrodialysis, and ion exchange adsorption. However, these methods all have drawbacks, such as the high cost of electrodialysis and membrane separation, and the environmental pollution caused by solvent extraction agents. In recent years, researchers both domestically and internationally have conducted extensive research and exploration into new lithium extraction processes, with electrochemical lithium extraction technology showing promising potential.
[0004] The principle of electrochemical lithium extraction is to charge the working electrode in the electrolyte solution to release lithium ions to form a lithium-depleted electrode. The lithium-rich electrode and the lithium-depleted electrode are used as the anode and cathode respectively. Lithium salt solution is added to the anode and salt lake brine is added to the cathode. Driven by the external potential, Li in the brine is selectively embedded in the lithium-depleted electrode. At the same time, the lithium-rich electrode releases Li into the solution to form a lithium-depleted electrode. Through electrode exchange and cyclic operation, selective enrichment of lithium is achieved.
[0005] The low concentration of lithium in brine makes lithium extraction efficiency crucial for electrochemical deintercalation. However, the high coating density of the electrodes used slows lithium ion mass transfer within the electrodes, thus affecting the lithium extraction rate. Patents such as CN113293290A and CN113293290A disclose improving mass transfer within the electrode by adding soluble inorganic salts as pore-forming agents. However, the use of pore-forming agents can lead to uneven distribution, creating pores of varying sizes and hindering mass transfer.
[0006] Summary of the Invention
[0007] The purpose of the present invention is to overcome the shortcomings of the existing technology and provide a porous electrode for electrochemical deintercalation of lithium from salt lakes, as well as its preparation method and application; the porous electrode increases the contact area between salt lake brine and lithium extraction active sites, thereby improving the lithium extraction reaction rate.
[0008] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a porous electrode, comprising the following steps:
[0009] S1: adding the electrode active material to molten sodium thiosulfate, mixing uniformly at 55-65°C, and cooling to obtain the sodium thiosulfate-coated electrode active material;
[0010] S2: adding a binder to an organic solvent and stirring to obtain a mixed solution A; adding the sodium thiosulfate-coated electrode active material and the conductive agent obtained in step S1 to the mixed solution A and stirring evenly to obtain an electrode slurry;
[0011] S3: coating the electrode slurry obtained in step S2 on the surface of the current collector and drying it to obtain a porous electrode; wherein the mass of sodium thiosulfate is 10-20% of the mass of the electrode active material.
[0012] Specifically, the melting temperature of the sodium thiosulfate is 55-65°C.
[0013] In the present invention, sodium thiosulfate can be transformed from a solid state to a liquid state at 55-65°C. The molten sodium thiosulfate has good fluidity and can be fully and evenly mixed with the electrode active material. After cooling, the molten sodium thiosulfate solidifies in the internal pores of the electrode active material and is wrapped around the outside of the electrode active material. After the sodium thiosulfate-coated electrode active material, conductive agent, binder and other components are evenly mixed, the binder is coated on the outer layer of the electrode active material particles. When the electrode is dried, the binder solidifies, and the sodium thiosulfate is heated and volatilized to produce gas, forming a mass transfer channel between the electrode active material and the binder, thereby increasing the contact area between the salt lake brine and the lithium extraction active site, improving the mass transfer efficiency of the salt lake brine, and increasing the reaction rate of lithium extraction.
[0014] The present invention uses sodium thiosulfate to coat the outside of the electrode active material and then heat it to volatilize to form pores. There is no need to add a pore-forming agent during the preparation of the electrode slurry, thus avoiding the problem of uneven distribution of the pore-forming agent to form pores of different sizes.
[0015] In step S2 , there is no specific requirement for the stirring time of the binder and the organic solvent, as long as the binder is stirred until it is completely dissolved.
[0016] In step S2, the stirring time of adding the sodium thiosulfate-coated electrode active material and the conductive agent to the mixed solution A is preferably 5-10 hours. Within the above time, the sodium thiosulfate-coated electrode active material and the conductive agent can be better dispersed in the mixed solution A.
[0017] As an improvement of the above technical solution, the mass of the sodium thiosulfate is 10-20% of the mass of the electrode active material.
[0018] In order to improve the overall permeability of the electrode plate, strengthen the mass transfer effect of the solution inside the electrode, and reduce the polarization of the electrochemical lithium extraction process, one of the effective methods is to increase the transmission path of the solution by pore formation. In the present invention, the amount of sodium thiosulfate added is related to the pore size and porosity of the porous electrode, and needs to be controlled within an appropriate range. If the amount of sodium thiosulfate added is too low, it is difficult to form a coating layer of a certain thickness on the surface of the electrode active material, resulting in the pore size and porosity of the porous electrode being too small, and unable to effectively serve as a solution mass transfer channel; if the amount of sodium thiosulfate added is too high, it is easy to cause the porosity of the porous electrode to be too high, and the strength of the electrode plate is reduced. The present invention selects the mass of sodium thiosulfate to be 10-20% of the mass of the electrode active material, which can control the coating content to 10-20%, so that sufficiently large pores can be formed in the pore formation process; the pore-forming agents in the prior art, whether using a solid phase method or a precipitation method, cannot form a coating layer with such a high content on the surface of the electrode active material. Preferably, the mass of sodium thiosulfate is 12-18% of the mass of the electrode active material, and the obtained porous electrode has a better lithium extraction effect.
[0019] As an improvement of the above technical solution, the mass of the binder is 8-12% of the mass of the electrode active material.
[0020] As an improvement of the above technical solution, the mass of the conductive agent is 5-15% of the mass of the electrode active material.
[0021] As an improvement of the above technical solution, the mass of the organic solvent is 120-150% of the mass of the electrode active material.
[0022] Under the premise of ensuring that the final electrode material has good hydrophilicity, conductivity, and permeability, the content of each component in the slurry should be controlled within a certain proportion. On the one hand, if the amount of conductive agent, binder, etc. added is too little, the permeability, conductivity and structural strength of the electrode material cannot be guaranteed; on the other hand, if the amount of conductive agent, binder, etc. added is too little, it is easy to cause the proportion of electrode active material to be too low, resulting in a decrease in the amount of lithium extracted per unit area; if the amount of organic solvent added is too little, it is easy to cause insufficient dissolution of the binder, and the final slurry viscosity is too high, which is not conducive to the coating of the slurry; if the amount of organic solvent added is too much, the slurry fluidity is too high, which is difficult to coat, and the solid matter is easy to settle and stratify during the drying process, resulting in an imbalance in the proportion of the final electrode material and reduced electrochemical performance.
[0023] As an improvement of the above technical solution, the drying temperature is 100-120° C., and the drying time is 10-20 hours.
[0024] In the present invention, if the drying temperature is too low, sodium thiosulfate will not be able to volatilize to form pores, thereby reducing the mass transfer effect of the solution; if the drying temperature is too high, there will be too much binder on the electrode surface, and sodium thiosulfate will volatilize in large quantities, causing the pores inside the porous electrode to collapse, resulting in a decrease in the reaction rate of lithium extraction.
[0025] As an improvement of the above technical solution, the active material is at least one of lithium iron phosphate, lithium manganese iron phosphate, and lithium manganate; and the conductive agent is acetylene black and / or Ketjen black.
[0026] As an improvement of the above technical solution, the binder is PVDF; and the organic solvent is N-methylpyrrolidone.
[0027] In the present invention, the electrode active material has properties such as lithium ion transport and migration channels, redox reaction sites, and a chemically stable lattice structure, and should have a stable electrochemical operating window in aqueous solution. By controlling the redox potential of the electrode, lithium ions can be selectively embedded in and extracted from the electrode active material. PVDF has a minimal effect on the specific surface area of the porous electrode, while acetylene black and / or Ketjen black can accelerate the rate of electrochemical lithium removal and improve lithium extraction efficiency.
[0028] Specifically, the current collector in the present invention is titanium mesh or carbon fiber cloth.
[0029] As an improvement to the above technical solution, the electrode slurry can be coated on the surface of the current collector by using a process such as spin coating or scraping coating.
[0030] In a second aspect, the present invention provides a porous electrode prepared by the porous electrode preparation method.
[0031] In a third aspect, the present invention also provides the use of the porous electrode in extracting lithium from salt lakes using the electrochemical deintercalation method.
[0032] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention first uses sodium thiosulfate to coat the electrode active material. In the process of mixing the electrode active material, conductive agent, binder, etc. into a slurry, the binder is coated on the outer layer of the electrode active material particles. In the subsequent electrode drying process, the sodium thiosulfate is heated and volatilized to produce gas, and a mass transfer channel is formed outside the electrode active material particles, which increases the contact between the liquid and the active reaction sites and improves the lithium extraction reaction rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] FIG1 is a curve showing the change of lithium concentration in the anolyte over time. DETAILED DESCRIPTION
[0034] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and accompanying drawings, its purpose is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. Unless otherwise specified, the experimental reagents and instruments involved in the implementation of the present invention are all commonly used ordinary reagents and instruments.
[0035] Example 1
[0036] This embodiment provides a method for preparing a porous electrode for extracting lithium from salt lakes using an electrochemical deintercalation method, comprising the following steps:
[0037] S1: Sodium thiosulfate is heated to 55°C and melted to a liquid state; lithium iron phosphate is then added to the molten sodium thiosulfate, stirred at 55°C for 4 hours, cooled to room temperature, and the resulting product is ground and crushed to obtain sodium thiosulfate-coated lithium iron phosphate; wherein the mass of the sodium thiosulfate is 10% of the mass of the lithium iron phosphate;
[0038] S2: Add PVDF to N-methylpyrrolidone and stir under vacuum until completely dissolved to obtain a mixed solution A; add the sodium thiosulfate-coated lithium iron phosphate and acetylene black obtained in step S1 to the mixed solution A and stir under vacuum for 5 hours to obtain an electrode slurry; wherein the mass of PVDF is 8% of the mass of lithium iron phosphate, the mass of acetylene black is 5% of the mass of lithium iron phosphate, and the mass of N-methylpyrrolidone is 120% of the mass of lithium iron phosphate;
[0039] S3: The electrode slurry obtained in step S2 is coated on the titanium mesh with a coating density of 150 mg lithium iron phosphate / cm 2 The product was dried at 120°C for 10 h to obtain a porous electrode.
[0040] Example 2
[0041] This embodiment provides a method for preparing a porous electrode for extracting lithium from salt lakes using an electrochemical deintercalation method, comprising the following steps:
[0042] S1: Sodium thiosulfate is heated to 60°C and melted into a liquid state; lithium iron phosphate is then added to the molten sodium thiosulfate, stirred at 60°C for 6 hours, cooled to room temperature, and the resulting product is ground and crushed to obtain sodium thiosulfate-coated lithium iron phosphate; wherein the mass of the sodium thiosulfate is 20% of the mass of the lithium iron phosphate;
[0043] S2: Add PVDF to N-methylpyrrolidone and stir under vacuum until completely dissolved to obtain a mixed solution A; add the sodium thiosulfate-coated lithium iron phosphate and acetylene black obtained in step S1 to the mixed solution A and stir under vacuum for 10 hours to obtain an electrode slurry; wherein the mass of PVDF is 12% of the mass of the lithium iron phosphate, the mass of acetylene black is 15% of the mass of the lithium iron phosphate, and the mass of N-methylpyrrolidone is 150% of the mass of the lithium iron phosphate;
[0044] S3: The electrode slurry obtained in step S2 is coated on the titanium mesh with a coating density of 200 mg lithium iron phosphate / cm 2 The product was dried at 120°C for 14 h to obtain a porous electrode.
[0045] Example 3
[0046] This embodiment provides a method for preparing a porous electrode for extracting lithium from salt lakes using an electrochemical deintercalation method, comprising the following steps:
[0047] S1: Sodium thiosulfate is heated to 65°C and melted to a liquid state; lithium iron phosphate is then added to the molten sodium thiosulfate, stirred at 65°C for 8 hours, cooled to room temperature, and the resulting product is ground and crushed to obtain sodium thiosulfate-coated lithium iron phosphate; wherein the mass of the sodium thiosulfate is 15% of the mass of the lithium iron phosphate;
[0048] S2: Add PVDF to N-methylpyrrolidone and stir under vacuum until completely dissolved to obtain a mixed solution A; add the sodium thiosulfate-coated lithium iron phosphate and acetylene black obtained in step S1 to the mixed solution A and stir under vacuum for 8 hours to obtain an electrode slurry; wherein the mass of PVDF is 10% of the mass of lithium iron phosphate, the mass of acetylene black is 12% of the mass of lithium iron phosphate, and the mass of N-methylpyrrolidone is 135% of the mass of lithium iron phosphate;
[0049] S3: The electrode slurry obtained in step S2 is coated on the titanium mesh with a coating density of 200 mg lithium iron phosphate / cm 2 The product was dried at 100°C for 20 h to obtain a porous electrode.
[0050] Example 4
[0051] This embodiment provides a method for preparing a porous electrode for extracting lithium from salt lakes using the electrochemical deintercalation method. The only difference between this embodiment and Example 1 is that in step S1, the mass of sodium thiosulfate is 12% of the mass of lithium iron phosphate.
[0052] Example 5
[0053] This embodiment provides a method for preparing a porous electrode for extracting lithium from salt lakes using the electrochemical deintercalation method. The only difference between this embodiment and Example 1 is that in step S1, the mass of sodium thiosulfate is 14% of the mass of lithium iron phosphate.
[0054] Example 6
[0055] This embodiment provides a method for preparing a porous electrode for extracting lithium from salt lakes using the electrochemical deintercalation method. The only difference between this embodiment and Example 1 is that in step S1, the mass of sodium thiosulfate is 18% of the mass of lithium iron phosphate.
[0056] Comparative Example 1
[0057] This comparative example provides a method for preparing a porous electrode for extracting lithium from salt lakes using an electrochemical deintercalation method, comprising the following steps:
[0058] S1: lithium iron phosphate, acetylene black, and PVDF were added to N-methyl pyrrolidone in a mass ratio of 8:1:1 and mixed to obtain an electrode slurry; wherein the mass ratio of lithium iron phosphate, acetylene black, and PVDF was lithium iron phosphate:acetylene black:PVDF=8:1:1, and the mass of N-methyl pyrrolidone was 120% of the mass of lithium iron phosphate;
[0059] S2: The electrode slurry obtained in step S1 is coated on the titanium mesh with a coating density of 150 mg lithium iron phosphate / cm 2 The product was dried at 120°C for 10 h to obtain a porous electrode.
[0060] Comparative Example 2
[0061] This comparative example provides a method for preparing a porous electrode for extracting lithium from salt lakes using an electrochemical deintercalation method, comprising the following steps:
[0062] S1: Add PVDF to N-methylpyrrolidone and stir under vacuum until completely dissolved to obtain mixed solution A; add lithium iron phosphate, acetylene black, and sodium bicarbonate to mixed solution A and stir under vacuum for 5 hours to obtain electrode slurry; wherein the mass of PVDF is 8% of the mass of lithium iron phosphate, the mass of acetylene black is 5% of the mass of lithium iron phosphate, the mass of sodium bicarbonate is 30% of the mass of lithium iron phosphate, and the mass of N-methylpyrrolidone is 120% of the mass of lithium iron phosphate;
[0063] S2: The electrode slurry obtained in step S1 is coated on the titanium mesh with a coating density of 150 mg lithium iron phosphate / cm 2 The product was dried at 120°C for 10 h to obtain a porous electrode.
[0064] Comparative Example 3
[0065] This comparative example provides a method for preparing a porous electrode for extracting lithium from salt lakes using the electrochemical deintercalation method. The only difference between this comparative example and Example 1 is that in step S1, the mass of sodium thiosulfate is 8% of the mass of lithium iron phosphate.
[0066] Comparative Example 4
[0067] This comparative example provides a method for preparing a porous electrode for extracting lithium from salt lakes using the electrochemical deintercalation method. The only difference between this comparative example and Example 1 is that in step S1, the mass of sodium thiosulfate is 30% of the mass of lithium iron phosphate.
[0068] Lithium extraction experiment: Use the prepared lithium iron phosphate electrode as the anode, nickel foam as the cathode, and 20g / L NaCl solution as the electrolyte. Apply a 1.0V voltage across the electrode until the current density is less than 0.5A / m2 to produce a delithiated electrode.
[0069] The electrolysis device was separated into an anode chamber and a cathode chamber by an anion exchange membrane. The prepared electrochemical lithium extraction electrode and lithium desorption electrode were placed in the anode chamber and cathode chamber respectively. Brine was injected into the cathode chamber and NaCl solution was injected into the anode chamber. A voltage of 0.3 V was applied to the anode and cathode for constant voltage electrolysis for 8 hours.
[0070] The changes in the anode lithium concentration during the lithium extraction process of the embodiment and the comparative example are shown in FIG1 , and the changes in the ion concentration of the brine before and after the reaction of the embodiment and the comparative example and the composition of the anode liquid after the lithium extraction are shown in Table 1 .
[0071] Table 1
[0072] From the experimental data of Example 1, Examples 4-6 and Comparative Examples 3-4 in Table 1, it can be seen that the amount of sodium thiosulfate added has a significant effect on the lithium extraction effect of the porous electrode. When the mass of sodium thiosulfate accounts for <10% or greater than 20% of the mass of the electrode active material, the lithium concentration in the brine after lithium extraction is high, and the lithium concentration in the anolyte is low; when the mass of sodium thiosulfate is 12-18% of the mass of the electrode active material, the lithium extraction effect of the porous electrode is better, the lithium concentration in the brine after lithium extraction is lower, and the lithium concentration in the anolyte is higher.
[0073] From the experimental data of Example 1 and Comparative Examples 1-2 in Table 1, it can be seen that the pore-forming agent has a greater influence on the lithium extraction effect of the porous electrode. The porous electrode of Comparative Example 1 does not contain a pore-forming agent, and the lithium concentration in the brine after lithium extraction is 0.31 g / L; the lithium concentration in the anolyte is 2.29 g / L; compared with Example 1, the porous electrode of Comparative Example 2 uses sodium bicarbonate as a pore-forming agent, and the lithium concentration in the brine after lithium extraction is reduced by 16%; the lithium concentration in the anolyte increases by 7%; the porous electrode of Example 1 uses sodium thiosulfate as a pore-forming agent, and the lithium concentration in the brine after lithium extraction is reduced by 51.6%; the lithium concentration in the anolyte increases by 27.9%; This shows that the use of sodium thiosulfate as a pore-forming agent in the present invention has achieved significant results compared with the prior art.
[0074] Finally, it should be noted that the above embodiments are used to illustrate the technical solutions of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A method for preparing a porous electrode, characterized in that: The following steps are involved: S1: adding the electrode active material to the molten sodium thiosulfate, mixing evenly at 55-65° C., and cooling to obtain the electrode active material coated with sodium thiosulfate; S2: adding a binder to an organic solvent and stirring to obtain a mixed solution A; adding the sodium thiosulfate-coated electrode active material and the conductive agent obtained in step S1 to the mixed solution A and stirring to obtain an electrode slurry; S3: coating the electrode slurry obtained in step S2 on the surface of the current collector and drying it to obtain a porous electrode; The mass of sodium thiosulfate is 10-20% of the mass of the electrode active material.
2. The preparation method according to claim 1, characterized in that The mass of the sodium thiosulfate is 12-18% of the mass of the electrode active material.
3. The preparation method according to claim 1, characterized in that: The mass of the binder is 8-12% of the mass of the electrode active material.
4. The preparation method according to claim 1, characterized in that: The mass of the conductive agent is 5-15% of the mass of the electrode active material.
5. The preparation method according to claim 1, characterized in that: The mass of the organic solvent is 120-150% of the mass of the electrode active material.
6. The preparation method according to claim 1, characterized in that: In step S3, the drying temperature is 100-120° C., and the drying time is 10-20 hours.
7. The preparation method according to claim 1, characterized in that: The electrode active material is at least one of lithium iron phosphate, lithium iron manganese phosphate and lithium manganate; the conductive agent is acetylene black and / or Ketjen black.
8. The preparation method according to claim 1, characterized in that: The binder is PVDF; the organic solvent is N-methylpyrrolidone.
9. A porous electrode, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the porous electrode as claimed in claim 9 in extracting lithium from salt lakes using the electrochemical deintercalation method.
Citation Information
Patent Citations
Method for forming porous material
CN101609809A
Graphene-coated sulfur / porous carbon composite positive electrode material and preparation method thereof
CN103560235A
Spherical composite positive pole material for lithium sulfur battery and preparation method and application of spherical composite positive pole material
CN104466138A
Electrode material for salt lake lithium extraction and preparation method and application of electrode material
CN113293290A
Preparation method of composite porous electrode material for lithium extraction
CN113293312A