Preparation method for combination electrode for lithium extraction from salt lakes
By using a nitrogen-doped carbon nanotube layer with a gradient structure to coat the electrode active material in a salt lake lithium extraction electrode, the problem of excessive lithium ion reaction rate and impurity embedding is solved, and the purity of lithium ions and the stability of the electrode material are improved. .
Patent Information
- Application Number
- PCT/CN2023/084458
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
During the lithium extraction process from salt lakes, the reaction rate of lithium ions inside the electrode is too fast, causing impurity cations to be embedded inside the electrode and reducing the purity of lithium ions.
The electrode active material is coated with nitrogen-doped carbon nanotube layers of different thicknesses, modified with dopamine and formulated with pore formers, enhancers, conductive agents, and binders to form a gradient electrode slurry, which is then coated on the current collector. A gradient structure is formed to control the diffusion rate of lithium ions and the stability of the electrode material.
It effectively reduces the reaction rate of lithium ions inside the electrode, avoids the insertion of impurity cations, improves the purity of lithium ions in the salt lake lithium recovery solution, and enhances the stability and recycling performance of the electrode material.
Smart Images

Figure CN2023084458_03102024_PF_FP_ABST
Abstract
Description
A method for preparing a composite electrode for lithium extraction from salt lakes Technical Field
[0001] The present application relates to the technical field of lithium extraction from salt lakes, and in particular to a method for preparing a composite electrode for lithium extraction from salt lakes. Background Art
[0002] In the process of extracting lithium from salt lakes using electrochemical methods, the solution diffuses slowly inside the electrode, and the electrode reaction reacts sequentially from the electrode surface to the inside of the electrode. During the production process, the cell voltage is usually increased to speed up the reaction rate. However, when a larger voltage is applied, the electrochemical reaction rate is much faster than the diffusion rate of the solution inside the electrode, and the reaction is easily controlled by external diffusion. When the electrode is controlled by external diffusion, the reaction rate of lithium ions inside the electrode is accelerated, and unreacted lithium ions are rapidly consumed. The lithium ions in the solution cannot be replenished to the inside of the electrode in time. At this time, the coexisting impurity cations in the solution are easily embedded in the internal electrode material and released into the solution, thereby reducing the purity of lithium ions in the recovered liquid.
[0003] Related technology discloses a method for preparing an electrode for electrochemical lithium extraction, which is characterized in that it includes the following steps: mixing a lithium extraction material with a conductive agent, a pore-forming agent, an inorganic hydrophilic nanomaterial, an adhesive, and N-methylpyrrolidone to prepare a slurry, and then evenly coating the slurry on a current collector, and drying and immersing the slurry in water to obtain the electrode for electrochemical lithium extraction. The electrode improves the selectivity of the electrode active material for lithium ions by coating the surface of the electrode active material with a graphene oxide / manganese ion sieve composite that has hydrophilicity and selective transmission of lithium ions; however, the lithium content of the brine after treatment is still relatively high.
[0004] Therefore, how to reduce the content of lithium in brine has become a technical problem that needs to be solved urgently by those skilled in the art.
[0005] Summary of the Invention
[0006] The purpose of this application is to overcome the shortcomings of the existing technology and provide a method for preparing a composite electrode for lithium extraction from salt lakes. The composite electrode reduces the reaction rate of lithium ions inside the electrode while increasing the diffusion rate of ions, so that the lithium extraction process is under electrochemical control, thereby avoiding the embedding of impurity ions into the electrode and improving the purity of lithium ions in the salt lake lithium extraction recovery liquid.
[0007] To achieve the above objectives, the technical solutions adopted in this application are:
[0008] A method for preparing a composite electrode for extracting lithium from a salt lake comprises the following steps:
[0009] dispersing nitrogen-containing organic matter and carbon nanotubes in a first solvent, heating under reflux, filtering, drying, washing with water, and drying to obtain nitrogen-doped carbon nanotubes;
[0010] Taking n portions of nitrogen-doped carbon nanotubes of different masses, dispersing the nitrogen-doped carbon nanotubes and the electrode active material in a second solvent, ball-milling, and drying, respectively, to obtain n electrode active materials coated with nitrogen-doped carbon nanotube layers of different thicknesses; dispersing the nitrogen-doped carbon nanotubes and the electrode active material in a second solvent, ball-milling, and drying, respectively, to obtain n electrode active materials coated with nitrogen-doped carbon nanotube layers of different thicknesses; wherein the mass of the electrode active material corresponding to each portion of nitrogen-doped carbon nanotube is the same;
[0011] The prepared nitrogen-doped carbon nanotube layer-coated electrode active materials are added to a dopamine solution for modification, filtering, washing, and drying to obtain n types of electrode active materials with modified nitrogen-doped carbon coating layers of different thicknesses;
[0012] The electrode active material of the modified nitrogen-doped carbon coating layer is respectively prepared with a pore former, a reinforcing agent, a conductive agent, a binder and a third solvent to form n portions of electrode slurry, and the electrode slurry is sequentially coated on a current collector, dried, rolled and soaked in water to form n layers of active coating, so that the mass of the pore former in each active coating layer decreases gradually in a direction away from the current collector, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases gradually;
[0013] Wherein, n is a positive integer ≥2.
[0014] The present application prepares nitrogen-doped carbon nanotubes first, and then mixes nitrogen-doped carbon nanotubes of different masses with electrode active materials of the same mass to obtain n types of electrode active materials coated with nitrogen-doped carbon nanotube layers of different thicknesses; then, each of the materials is modified with dopamine, and then, n portions of electrode slurry are prepared by mixing the mixture with a pore-forming agent, a reinforcing agent, a conductive agent, a binder, and a third solvent, and the mixture is applied to a current collector, respectively, so that the mass of the pore-forming agent in each active coating layer decreases gradually along the direction away from the current collector, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases gradually.
[0015] During the lithium extraction process of the composite electrode, the bottom of the electrode (close to the current collector side) consumes lithium ions too quickly due to cathode polarization. The lithium extraction process is controlled by diffusion, and cationic impurity metals such as sodium ions and magnesium ions enter the crystal lattice of the material through electrolysis. The present application uses active materials with different carbon coating thicknesses to layer and coat the lithium extraction electrode. The closer to the current collector, the thicker the bottom carbon coating layer is. While improving the conductivity, it reduces the contact area between the electrode material and the electrolyte, suppressing the electrochemical reaction rate of lithium ions to a certain extent, thereby reducing cathode polarization, avoiding the embedding of impurity cations into the crystal lattice, and improving the purity of lithium ions in the salt lake lithium extraction recovery liquid.
[0016] The high mineralization and viscosity of the brine hinder its mass transfer within the electrode, resulting in a lower lithium ion transfer rate at the bottom of the electrode. The addition of more pore-forming agent to the electrode slurry near the current collector layer than to the electrode surface layer away from the current collector increases the pores at the bottom of the electrode and enhances the mass transfer effect of the solution at the bottom of the electrode. Excessively large pores at the bottom of the electrode reduce the stability of the electrode material. Coating the surface of the bottom electrode material with a large amount of carbon as a skeleton can improve the stability of the electrode material. The synergistic effect of these two factors can increase the mass transfer rate of lithium ions at the bottom of the electrode while increasing the stability of the electrode material.
[0017] By coating the surface of the electrode material with carbon nanotubes, their stable structure forms stable ion channels, preventing lattice fractures caused by repeated lithium ion deintercalation and insertion, thereby improving the electrode's recyclability. The carbon coating forms a conductive network, reducing impedance, and the polydopamine loaded on the carbon nanotubes has a selective effect on lithium ions, improving the electrode's selectivity for lithium ions.
[0018] Nitrogen doping of carbon nanotubes can not only improve their hydrophilicity, but also the nitrogen-doped atoms can change the local charge density of carbon nanotubes, improve their electron transferability, and reduce the resistivity; at the same time, the nitrogen-containing functional groups introduced by nitrogen doping can significantly increase the specific capacity of carbon nanotube electrochemical capacitors.
[0019] As a preferred embodiment of the present application, the masses of the electrode active material of the modified nitrogen-doped carbon coating layer, the reinforcing agent, the conductive agent, the binder and the third solvent in each electrode slurry are the same.
[0020] As a preferred embodiment of the present application, the mass of the pore former in each electrode slurry is different.
[0021] By controlling the masses of the electrode active material, reinforcing agent, conductive agent, binder and third solvent of the modified nitrogen-doped carbon coating layer in each electrode slurry to be the same and the masses of the pore-forming agent to be different, the mass of the pore-forming agent in each active coating layer away from the current collector decreases gradually during coating, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases gradually.
[0022] As a preferred embodiment of the present application, the nitrogen-containing organic matter includes at least one of hydrazine hydrate, pyrimidine, ethylenediamine, and melamine.
[0023] As a preferred embodiment of the present application, the first solvent includes at least one of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, and acetone.
[0024] As a preferred embodiment of the present application, the mass ratio of the nitrogen-containing organic matter, the carbon nanotubes, and the first solvent is (2-10): (10-40): (100-1000).
[0025] As a preferred embodiment of the present application, the second solvent includes at least one of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, and acetone.
[0026] As a preferred embodiment of the present application, the electrode active material includes LiMn2O4, LiFePO4, LiNi x Co y Mn z At least one of O2, wherein x+y+z=1.
[0027] As a preferred embodiment of the present application, the mass ratio of the nitrogen-doped carbon nanotubes, the electrode active material, and the second solvent is (0.001-0.02):1:(1-10).
[0028] As a preferred embodiment of the present application, the mass concentration of the dopamine solution is 1 to 6 g / L.
[0029] As a preferred embodiment of the present application, the solid-to-liquid ratio of the carbon nanotube-coated electrode active material and the dopamine solution is 1 g: (4-20) mL.
[0030] As a preferred embodiment of the present application, the mass ratio of the electrode active material of the modified nitrogen-doped carbon coating layer to the pore former, reinforcing agent, conductive agent, binder and third solvent is 100: (5-35): (10-20): (5-20): (100-400).
[0031] As a preferred embodiment of the present application, the pore-forming agent is at least one of ammonium carbonate and ammonium bicarbonate.
[0032] As a preferred embodiment of the present application, the reinforcing agent includes chopped carbon fibers.
[0033] As a preferred embodiment of the present application, the conductive agent includes at least one of acetylene black and carbon black.
[0034] As a preferred embodiment of the present application, the binder includes polyvinylidene fluoride.
[0035] As a preferred embodiment of the present application, the third solvent includes N-methylpyrrolidone.
[0036] As a preferred embodiment of the present application, the coating amount of each electrode slurry is the same, which is 10-50 mg / cm 2 .
[0037] The beneficial effects of the present application are as follows: (1) During the lithium extraction process of the composite electrode, the bottom of the electrode (close to the current collector) consumes lithium ions too quickly due to cathode polarization. The lithium extraction process is controlled by diffusion, and cationic impurity metals such as sodium ions and magnesium ions enter the crystal lattice of the material through electrolysis. The present application uses active materials with different carbon coating thicknesses to layer and coat the lithium extraction electrode. The closer to the current collector, the thicker the bottom carbon coating is. While improving the conductivity, it also reduces the contact area between the electrode material and the electrolyte, inhibiting the electrochemical reaction rate of lithium ions to a certain extent, thereby reducing cathode polarization, avoiding the embedding of impurity cations into the crystal lattice, and improving the purity of lithium ions in the salt lake lithium extraction recovery solution; (2) by adding more pore-forming agent to the electrode slurry coated close to the current collector layer than to the electrode surface away from the current collector, the pores at the bottom of the electrode are increased, thereby enhancing the mass transfer effect of the solution at the bottom of the electrode. The pores at the bottom of the electrode are too large, which leads to reduced stability of the electrode material. Coating more carbon on the surface of the bottom electrode material as a skeleton can improve the stability of the electrode material. The synergistic effect of the two can increase the mass transfer rate of lithium ions at the bottom of the electrode while increasing the stability of the electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] FIG1 is a composite electrode prepared in Example 1.
[0039] FIG2 is a comparison chart of the rejection rates of the electrodes of Example 1 and Comparative Example 1 for impurity ions. DETAILED DESCRIPTION
[0040] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0041] There is no particular limitation on the specific dispersing and stirring treatment methods.
[0042] In this application, unless otherwise stated, all parts are by mass.
[0043] The reagents and instruments used in this application without indicating the manufacturer are all conventional products that can be purchased from the market.
[0044] Example 1
[0045] A method for preparing a composite electrode for extracting lithium from a salt lake comprises the following steps:
[0046] (1) 8 g of hydrazine hydrate and 5 g of carbon nanotubes were dispersed in 100 mL of deionized water, stirred evenly, heated under reflux for 6 h, and filtered to obtain a solid. The solid was then washed with water and freeze-dried to obtain nitrogen-doped carbon nanotubes;
[0047] (2) taking three nitrogen-doped carbon nanotubes of different masses, and recording them as the first nitrogen-doped carbon nanotube, the second nitrogen-doped carbon nanotube, and the third nitrogen-doped carbon nanotube;
[0048] The first nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with the first nitrogen-doped carbon nanotube layer, wherein the mass ratio of the first nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.015:1:1;
[0049] The second nitrogen-doped carbon nanotubes and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with a second nitrogen-doped carbon nanotube layer, wherein the mass ratio of the second nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol was 0.01:1:1;
[0050] The third nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with a third nitrogen-doped carbon nanotube layer, wherein the mass ratio of the third nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.05:1:1;
[0051] (3) The electrode active material coated with the first nitrogen-doped carbon nanotube layer, the electrode active material coated with the second nitrogen-doped carbon nanotube layer, and the electrode active material coated with the third nitrogen-doped carbon nanotube layer were added to a 5 g / L dopamine solution at the same solid-liquid ratio of 1 g:7.5 mL for coating modification, filtered, and dried to obtain the electrode active material coated with the modified first nitrogen-doped carbon nanotube layer, the electrode active material coated with the modified second nitrogen-doped carbon nanotube layer, and the electrode active material coated with the modified third nitrogen-doped carbon nanotube layer, respectively.
[0052] [Corrected 07.05.2023 according to Rule 91] (4) 200 g of the electrode active material coated with the modified first nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fibers, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 60 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-1 slurry;
[0053] [Corrected 07.05.2023 according to Rule 91] 200 g of the electrode active material coated with the modified second nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fibers, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 40 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was designated as 3-2 slurry;
[0054] [Corrected 07.05.2023 according to Rule 91] 200 g of the electrode active material coated with the modified third nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fibers, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 20 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was designated as 3-3 slurry;
[0055] The 3-1 slurry, 3-2 slurry, and 3-3 slurry were sprayed on the surface of the current collector titanium mesh in sequence, with a coating density of 25 mg / cm 2 After each layer of slurry is coated, the coating layer is dried at low temperature at 70°C for 10 minutes. After the last layer of electrode slurry is coated and dried at low temperature, the entire electrode is dried at 100°C for 5 hours. After the electrode is dried, it is rolled to a thickness of 500μm. It is then immersed in water, and the water is changed every 0.5 hours, for a total of 3 times, to obtain a composite electrode for lithium extraction from salt lakes.
[0056] The prepared composite electrode for lithium extraction from salt lakes is shown in FIG1 , comprising a current collector titanium mesh 1, active coatings 3-1, 3-2, and 3-3 located on the surface of the current collector titanium mesh; the mass of the pore-forming agent in each active coating decreases gradually in the direction away from the current collector, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases gradually;
[0057] Among them, the active coating 3-1, the active coating 3-2, and the active coating 3-3 respectively contain the electrode active material S1 coated with the modified first nitrogen-doped carbon nanotube layer, the electrode active material S2 coated with the modified second nitrogen-doped carbon nanotube layer, and the electrode active material S3 coated with the modified third nitrogen-doped carbon nanotube layer, and the active coating further contains ammonium bicarbonate 2;
[0058] The electrode active material S1 coated with the modified first nitrogen-doped carbon nanotube layer includes lithium iron phosphate S11 and the modified first nitrogen-doped carbon nanotube layer S12 coated on the surface of the lithium iron phosphate.
[0059] Lithium extraction experiment: The prepared composite electrode was used as the anode and nickel foam was used as the cathode. The electrodes were placed in a 20 g / L NaCl solution and a voltage of 1 V was applied across the electrodes until the current density was lower than 0.5 A / m 2, obtaining a lithium-deficient electrode. The electrolysis apparatus was separated into a cathode chamber and an anode chamber using an anion membrane. The prepared lithium-rich electrode and lithium-deficient electrode were placed in the anode chamber and cathode chamber, respectively. 4.5 L of brine with a lithium concentration of 0.68 g / L was injected into the cathode chamber, and 2 L of a 5 g / L NaCl solution was injected into the anode chamber as the supporting electrolyte. A voltage of 0.9 V was applied to the anode and cathode, and electrolysis was performed at 20°C for 4 hours. The lithium ion concentration and brine impurity concentration before and after electrolysis were measured using an inductively coupled plasma spectrometer (ICP), as shown in Table 1.
[0060] Table 1
[0061] Comparative Example 1
[0062] 200g of lithium iron phosphate and 10g of short carbon fiber, 30g of acetylene black, 25g of PVDF, and 40g of ammonium bicarbonate were mixed evenly, and then 300g of N-methyl pyrrolidone was added and stirred evenly to obtain an electrode slurry coated on the surface of the current collector titanium mesh. The coating thickness was the same as in Example 1. The coating layer was dried at 70°C for 10 minutes and then dried at 100°C for 5 hours. After the electrode was dried, it was immersed in water and the water was changed every 0.5 hours. The water was changed 3 times to obtain a lithium iron phosphate electrode for electrochemical lithium extraction. Lithium was extracted under the same technical parameters as in Example 1. The lithium concentration in the brine was reduced from 1.75g / L to 0.33g / L, the lithium concentration in the anode lithium-rich solution increased to 5.21g / L, and the lithium extraction rate was 81%.
[0063] FIG2 is a comparison chart of the rejection rates of the electrodes of Example 1 and Comparative Example 1 for impurity ions. It can be seen that the composite electrode of the present application can reduce the adsorption of impurity cations and significantly improve the purity of lithium in the recovered liquid.
[0064] Example 2
[0065] A method for preparing a composite electrode for extracting lithium from a salt lake comprises the following steps:
[0066] (1) 8 g of hydrazine hydrate and 5 g of carbon nanotubes were dispersed in 100 mL of deionized water, stirred evenly, heated under reflux for 6 h, and filtered to obtain a solid. The solid was then washed with water and freeze-dried to obtain nitrogen-doped carbon nanotubes;
[0067] (2) taking two nitrogen-doped carbon nanotubes of different masses, and recording them as the first nitrogen-doped carbon nanotube, the second nitrogen-doped carbon nanotube, and the third nitrogen-doped carbon nanotube;
[0068] The first nitrogen-doped carbon nanotubes, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3O2, adding it to anhydrous ethanol, uniformly dispersing it by ultrasonication at 500W, and then transferring it to a ball mill for ball milling. After ball milling, drying it, and cooling it to room temperature, to obtain an electrode active material coated with a first nitrogen-doped carbon nanotube layer, wherein the mass ratio of the first nitrogen-doped carbon nanotube, lithium iron phosphate, and anhydrous ethanol is 0.015:1:1;
[0069] The second nitrogen-doped carbon nanotubes, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, added to anhydrous ethanol, uniformly dispersed by 500W ultrasonic dispersion, and then transferred to a ball mill for ball milling. After ball milling, it was dried and cooled to room temperature to obtain an electrode active material coated with a second nitrogen-doped carbon nanotube layer, wherein the mass ratio of the second nitrogen-doped carbon nanotube, lithium iron phosphate, and anhydrous ethanol was 0.01:1:1;
[0070] (3) The electrode active material coated with the first nitrogen-doped carbon nanotube layer and the electrode active material coated with the second nitrogen-doped carbon nanotube layer were added to a 5 g / L dopamine solution at the same solid-liquid ratio of 1 g:7.5 mL for coating modification, filtered, and dried to obtain the modified electrode active material coated with the first nitrogen-doped carbon nanotube layer and the modified electrode active material coated with the second nitrogen-doped carbon nanotube layer, respectively.
[0071] (4) Add 200 g of the modified first nitrogen-doped carbon nanotube layer-coated electrode active material, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 65 g of ammonium bicarbonate to 300 g of N-methylpyrrolidone and stir evenly to obtain an electrode slurry, which is recorded as 3-1 slurry;
[0072] 200 g of the electrode active material coated with the modified second nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 25 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-2 slurry;
[0073] Spray 3-1 slurry and 3-2 slurry onto the surface of the current collector titanium mesh in sequence, with a coating density of 25 mg / cm 2 After each layer of slurry is coated, the coating layer is dried at low temperature at 70°C for 10 minutes. After the last layer of electrode slurry is coated and dried at low temperature, the entire electrode is dried at 100°C for 5 hours. After the electrode is dried, it is rolled to a thickness of 500μm. It is then immersed in water, and the water is changed every 0.5 hours, for a total of 3 times, to obtain a composite electrode for lithium extraction from salt lakes.
[0074] The prepared composite electrode for lithium extraction from salt lakes comprises a current collector titanium mesh and two active coating layers of equal thickness; the mass of the pore-forming agent in each active coating layer decreases gradually in a direction away from the current collector, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases gradually;
[0075] Wherein, each active coating layer contains an electrode active material S1 coated with a modified first nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified second nitrogen-doped carbon nanotube layer, and an electrode active material coated with a modified third nitrogen-doped carbon nanotube layer, and the active coating layer also contains ammonium bicarbonate;
[0076] The modified first nitrogen-doped carbon nanotube layer coated electrode active material includes LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and coated on LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 surface modification of the first nitrogen-doped carbon nanotube layer.
[0077] Lithium extraction experiment: The prepared composite electrode was used as the anode and nickel foam was used as the cathode. The electrodes were placed in a 20 g / L NaCl solution and a voltage of 1 V was applied across the electrodes until the current density was lower than 0.5 A / m 2 , obtaining a lithium-deficient electrode. The electrolysis apparatus was separated into a cathode chamber and an anode chamber using an anion membrane. The prepared lithium-rich and lithium-deficient electrodes were placed in the anode and cathode chambers, respectively. 4.5 L of brine with a lithium concentration of 0.68 g / L was injected into the cathode chamber, and 2 L of a 5 g / L NaCl solution was injected into the anode chamber as the supporting electrolyte. A voltage of 0.9 V was applied to the anode and cathode, and electrolysis was performed at 20°C for 4 hours. The lithium ion concentration and brine impurity concentration before and after electrolysis were measured using an inductively coupled plasma spectrometer (ICP), as shown in Table 2.
[0078] Table 2
[0079] Comparative Example 2
[0080] LiNi 1 / 3 Co 1 / 3 Mn 1 / 3After mixing 200g of O2 with 10g of short carbon fiber, 30g of acetylene black, 25g of PVDF, and 65g of ammonium bicarbonate, 300g of N-methyl pyrrolidone was added and stirred evenly to obtain an electrode slurry coated on the surface of the current collector titanium mesh. The coating thickness was the same as in Example 1. The coating layer was dried at 70°C for 10 minutes and then dried at 100°C for 5 hours. After the electrode was dried, it was immersed in water and the water was changed every 0.5 hours. The water was changed 3 times to obtain a lithium iron phosphate electrode for electrochemical lithium extraction. Lithium was extracted under the same technical parameters as in Example 2. The lithium concentration in the lithium-rich solution at the anode rose to 5.19g / L, and the lithium extraction rate was 80%.
[0081] Example 3
[0082] A method for preparing a composite electrode for extracting lithium from a salt lake comprises the following steps:
[0083] (1) 8 g of hydrazine hydrate and 5 g of carbon nanotubes were dispersed in 100 mL of deionized water, stirred evenly, heated under reflux for 6 h, and filtered to obtain a solid. The solid was then washed with water and freeze-dried to obtain nitrogen-doped carbon nanotubes;
[0084] (2) taking four nitrogen-doped carbon nanotubes of different masses, and recording them as the first nitrogen-doped carbon nanotube, the second nitrogen-doped carbon nanotube, the third nitrogen-doped carbon nanotube, and the fourth nitrogen-doped carbon nanotube;
[0085] The first nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with the first nitrogen-doped carbon nanotube layer, wherein the mass ratio of the first nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.01:1:1;
[0086] The second nitrogen-doped carbon nanotubes and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with a second nitrogen-doped carbon nanotube layer, wherein the mass ratio of the second nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol was 0.007:1:1;
[0087] The third nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with a third nitrogen-doped carbon nanotube layer, wherein the mass ratio of the third nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.004:1:1;
[0088] The fourth nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with a fourth nitrogen-doped carbon nanotube layer, wherein the mass ratio of the fourth nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.001:1:1;
[0089] (3) The electrode active material coated with the first nitrogen-doped carbon nanotube layer, the electrode active material coated with the second nitrogen-doped carbon nanotube layer, the electrode active material coated with the third nitrogen-doped carbon nanotube layer, and the electrode active material coated with the fourth nitrogen-doped carbon nanotube layer are added to a 5 g / L dopamine solution at the same solid-liquid ratio of 1 g:7.5 mL for coating and modification, filtered, and dried to obtain the electrode active material coated with the modified first nitrogen-doped carbon nanotube layer, the electrode active material coated with the modified second nitrogen-doped carbon nanotube layer, the electrode active material coated with the third nitrogen-doped carbon nanotube layer, and the electrode active material coated with the modified fourth nitrogen-doped carbon nanotube layer, respectively.
[0090] (4) Add 200 g of the modified first nitrogen-doped carbon nanotube layer-coated electrode active material, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 64 g of ammonium bicarbonate to 300 g of N-methylpyrrolidone and stir evenly to obtain an electrode slurry, which is recorded as 3-1 slurry;
[0091] 200 g of the electrode active material coated with the modified second nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 48 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-2 slurry;
[0092] 200 g of the electrode active material coated with the modified third nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 32 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-3 slurry;
[0093] 200 g of the electrode active material coated with the modified fourth nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 32 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-4 slurry;
[0094] Spray 3-1 slurry, 3-2 slurry, 3-3 slurry, and 3-4 slurry onto the surface of the current collector titanium mesh in sequence, with a coating density of 25 mg / cm 2After each layer of slurry is coated, the coating layer is dried at low temperature at 70°C for 10 minutes. After the last layer of electrode slurry is coated and dried at low temperature, the entire electrode is dried at 100°C for 5 hours. After the electrode is dried, it is rolled to a thickness of 500μm. It is then immersed in water, and the water is changed every 0.5 hours, for a total of 3 times, to obtain a composite electrode for lithium extraction from salt lakes.
[0095] The prepared composite electrode for lithium extraction from salt lakes includes a current collector titanium mesh and four active coating layers of the same thickness; the mass of the pore-forming agent in each active coating layer decreases gradually in the direction away from the current collector, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases gradually;
[0096] Wherein, each active coating layer contains an electrode active material coated with a modified first nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified second nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified third nitrogen-doped carbon nanotube layer, and an electrode active material coated with a modified fourth nitrogen-doped carbon nanotube layer, and the active coating layer also contains ammonium bicarbonate;
[0097] Lithium extraction experiment: The prepared composite electrode was used as the anode and nickel foam was used as the cathode. The electrodes were placed in a 20 g / L NaCl solution and a voltage of 1 V was applied across the electrodes until the current density was lower than 0.5 A / m 2 , obtaining a lithium-deficient electrode. The electrolysis apparatus was separated into a cathode chamber and an anode chamber using an anion membrane. The prepared lithium-rich and lithium-deficient electrodes were placed in the anode and cathode chambers, respectively. 4.5 L of brine with a lithium concentration of 0.68 g / L was injected into the cathode chamber, and 2 L of a 5 g / L NaCl solution was injected into the anode chamber as the supporting electrolyte. A voltage of 0.9 V was applied to the anode and cathode, and electrolysis was performed at 20°C for 4 hours. The lithium ion concentration and brine impurity concentration before and after electrolysis were measured using an inductively coupled plasma spectrometer (ICP), as shown in Table 3.
[0098] Table 3
[0099] Comparative Example 3
[0100] 200g of lithium iron phosphate, 10g of short carbon fiber, 30g of acetylene black, 25g of PVDF, and 32g of ammonium bicarbonate were mixed evenly, and then 300g of N-methyl pyrrolidone was added and stirred evenly to obtain an electrode slurry coated on the surface of the current collector titanium mesh. The coating thickness was the same as in Example 3. The coating layer was dried at 70°C for 10 minutes and then dried at 100°C for 5 hours. After the electrode was dried, it was immersed in water and the water was changed every 0.5 hours. The water was changed 3 times to obtain a lithium iron phosphate electrode for electrochemical lithium extraction. Lithium was extracted under the same technical parameters as in Example 3. The lithium concentration in the lithium-rich anode solution rose to 5.25g / L, and the lithium extraction rate was 82%.
[0101] Example 4
[0102] A method for preparing a composite electrode for extracting lithium from a salt lake comprises the following steps:
[0103] (1) 8 g of hydrazine hydrate and 5 g of carbon nanotubes were dispersed in 100 mL of deionized water, stirred evenly, heated under reflux for 6 h, and filtered to obtain a solid. The solid was then washed with water and freeze-dried to obtain nitrogen-doped carbon nanotubes;
[0104] (2) taking five nitrogen-doped carbon nanotubes of different masses, and recording them as the first nitrogen-doped carbon nanotube, the second nitrogen-doped carbon nanotube, the third nitrogen-doped carbon nanotube, the fourth nitrogen-doped carbon nanotube, and the fifth nitrogen-doped carbon nanotube;
[0105] The first nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with the first nitrogen-doped carbon nanotube layer, wherein the mass ratio of the first nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.02:1:1;
[0106] The second nitrogen-doped carbon nanotubes and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with a second nitrogen-doped carbon nanotube layer, wherein the mass ratio of the second nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol was 0.017:1:1;
[0107] The third nitrogen-doped carbon nanotubes and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with a third nitrogen-doped carbon nanotube layer, wherein the mass ratio of the third nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol was 0.014:1:1;
[0108] The fourth nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with a fourth nitrogen-doped carbon nanotube layer, wherein the mass ratio of the fourth nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.011:1:1;
[0109] The fifth nitrogen-doped carbon nanotube and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with the fifth nitrogen-doped carbon nanotube layer, wherein the mass ratio of the fourth nitrogen-doped carbon nanotube, lithium iron phosphate, and anhydrous ethanol was 0.008:1:1;
[0110] (3) The electrode active material coated with the first nitrogen-doped carbon nanotube layer, the electrode active material coated with the second nitrogen-doped carbon nanotube layer, the electrode active material coated with the third nitrogen-doped carbon nanotube layer, the electrode active material coated with the fourth nitrogen-doped carbon nanotube layer, and the electrode active material coated with the fifth nitrogen-doped carbon nanotube layer are added to a 5 g / L dopamine solution at the same solid-liquid ratio of 1 g:7.5 mL for coating modification, filtered, and dried to obtain the modified electrode active material coated with the first nitrogen-doped carbon nanotube layer, the modified electrode active material coated with the second nitrogen-doped carbon nanotube layer, the modified electrode active material coated with the third nitrogen-doped carbon nanotube layer, the modified electrode active material coated with the fourth nitrogen-doped carbon nanotube layer, and the modified electrode active material coated with the fifth nitrogen-doped carbon nanotube layer, respectively.
[0111] (4) Add 200 g of the modified first nitrogen-doped carbon nanotube layer-coated electrode active material, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 56 g of ammonium bicarbonate to 300 g of N-methylpyrrolidone and stir evenly to obtain an electrode slurry, which is recorded as 3-1 slurry;
[0112] 200 g of the electrode active material coated with the modified second nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 48 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-2 slurry;
[0113] 200 g of the electrode active material coated with the modified third nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 40 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-3 slurry;
[0114] 200 g of the electrode active material coated with the modified fourth nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 32 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-4 slurry;
[0115] 200 g of the electrode active material coated with the modified fifth nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 24 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-5 slurry;
[0116] Spray 3-1 slurry, 3-2 slurry, 3-3 slurry, 3-4 slurry and 3-5 slurry onto the surface of the current collector titanium mesh in sequence, with a coating density of 25 mg / cm 2 After each layer of slurry is coated, the coating layer is dried at low temperature at 70°C for 10 minutes. After the last layer of electrode slurry is coated and dried at low temperature, the entire electrode is dried at 100°C for 5 hours. After the electrode is dried, it is rolled to a thickness of 500μm. It is then immersed in water, and the water is changed every 0.5 hours, for a total of 3 times, to obtain a composite electrode for lithium extraction from salt lakes.
[0117] The prepared composite electrode for lithium extraction from salt lakes includes a current collector titanium mesh and five active coating layers of the same thickness; the mass of the pore-forming agent in each active coating layer decreases gradually in the direction away from the current collector, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases gradually;
[0118] Wherein, each active coating layer contains an electrode active material coated with a modified first nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified second nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified third nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified fourth nitrogen-doped carbon nanotube layer, and an electrode active material coated with a modified fifth nitrogen-doped carbon nanotube layer, and the active coating layer also contains ammonium bicarbonate;
[0119] Lithium extraction experiment: The prepared composite electrode was used as the anode and nickel foam was used as the cathode. The electrodes were placed in a 20 g / L NaCl solution and a voltage of 1 V was applied across the electrodes until the current density was lower than 0.5 A / m 2, obtaining a lithium-deficient electrode. The electrolysis apparatus was separated into a cathode chamber and an anode chamber using an anion membrane. The prepared lithium-rich electrode and lithium-deficient electrode were placed in the anode chamber and cathode chamber, respectively. 4.5 L of brine with a lithium concentration of 0.68 g / L was injected into the cathode chamber, and 2 L of a 5 g / L NaCl solution was injected into the anode chamber as the supporting electrolyte. A voltage of 0.9 V was applied to the anode and cathode, and electrolysis was performed at 20°C for 4 hours. The lithium ion concentration and brine impurity concentration before and after electrolysis were measured using an inductively coupled plasma spectrometer (ICP), as shown in Table 43.
[0120] Table 4
[0121] Comparative Example 4
[0122] 200g of lithium iron phosphate, 10g of short carbon fiber, 30g of acetylene black, 25g of PVDF, and 40g of ammonium bicarbonate were mixed evenly, and then 300g of N-methyl pyrrolidone was added and stirred evenly to obtain an electrode slurry coated on the surface of the current collector titanium mesh. The coating thickness was the same as in Example 4. The coating layer was dried at 70°C for 10 minutes and then dried at 100°C for 5 hours. After the electrode was dried, it was immersed in water and the water was changed every 0.5 hours. The water was changed 3 times to obtain a lithium iron phosphate electrode for electrochemical lithium extraction. Lithium was extracted under the same technical parameters as in Example 4. The lithium concentration in the lithium-rich anode solution rose to 5.25g / L, and the lithium extraction rate was 82%.
[0123] Example 5
[0124] A method for preparing a composite electrode for extracting lithium from a salt lake comprises the following steps:
[0125] (1) 8 g of hydrazine hydrate and 5 g of carbon nanotubes were dispersed in 100 mL of deionized water, stirred evenly, heated under reflux for 6 h, and filtered to obtain a solid. The solid was then washed with water and freeze-dried to obtain nitrogen-doped carbon nanotubes;
[0126] (2) taking 6 nitrogen-doped carbon nanotubes of different masses, and recording them as the first nitrogen-doped carbon nanotube, the second nitrogen-doped carbon nanotube, the third nitrogen-doped carbon nanotube, the fourth nitrogen-doped carbon nanotube, the fifth nitrogen-doped carbon nanotube, and the sixth nitrogen-doped carbon nanotube;
[0127] The first nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with the first nitrogen-doped carbon nanotube layer, wherein the mass ratio of the first nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.012:1:1;
[0128] The second nitrogen-doped carbon nanotubes and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with a second nitrogen-doped carbon nanotube layer, wherein the mass ratio of the second nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol was 0.011:1:1;
[0129] The third nitrogen-doped carbon nanotubes and lithium iron phosphate are added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture is dried and cooled to room temperature to obtain an electrode active material coated with a third nitrogen-doped carbon nanotube layer, wherein the mass ratio of the third nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol is 0.010:1:1;
[0130] The fourth nitrogen-doped carbon nanotubes and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with a fourth nitrogen-doped carbon nanotube layer, wherein the mass ratio of the fourth nitrogen-doped carbon nanotubes, lithium iron phosphate, and anhydrous ethanol was 0.009:1:1;
[0131] The fifth nitrogen-doped carbon nanotube and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with the fifth nitrogen-doped carbon nanotube layer, wherein the mass ratio of the fourth nitrogen-doped carbon nanotube, lithium iron phosphate, and anhydrous ethanol was 0.008:1:1;
[0132] The sixth nitrogen-doped carbon nanotube and lithium iron phosphate were added to anhydrous ethanol, uniformly dispersed by ultrasonication at 500W, and then transferred to a ball mill for ball milling. After ball milling, the mixture was dried and cooled to room temperature to obtain an electrode active material coated with a fifth nitrogen-doped carbon nanotube layer, wherein the mass ratio of the fourth nitrogen-doped carbon nanotube, lithium iron phosphate, and anhydrous ethanol was 0.007:1:1;
[0133] (3) The electrode active material coated with the first nitrogen-doped carbon nanotube layer, the electrode active material coated with the second nitrogen-doped carbon nanotube layer, the electrode active material coated with the third nitrogen-doped carbon nanotube layer, the electrode active material coated with the fourth nitrogen-doped carbon nanotube layer, the electrode active material coated with the fifth nitrogen-doped carbon nanotube layer, and the electrode active material coated with the sixth nitrogen-doped carbon nanotube layer are added to a 5 g / L dopamine solution at the same solid-liquid ratio of 1 g:7.5 mL for coating and modification, filtered, and dried to obtain the modified electrode active material coated with the first nitrogen-doped carbon nanotube layer, the modified electrode active material coated with the second nitrogen-doped carbon nanotube layer, the modified electrode active material coated with the third nitrogen-doped carbon nanotube layer, the modified electrode active material coated with the fourth nitrogen-doped carbon nanotube layer, the modified electrode active material coated with the fifth nitrogen-doped carbon nanotube layer, and the modified electrode active material coated with the sixth nitrogen-doped carbon nanotube layer, respectively.
[0134] (4) Add 200 g of the modified first nitrogen-doped carbon nanotube layer-coated electrode active material, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 70 g of ammonium bicarbonate to 300 g of N-methylpyrrolidone and stir evenly to obtain an electrode slurry, which is recorded as 3-1 slurry;
[0135] 200 g of the electrode active material coated with the modified second nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 58 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-2 slurry;
[0136] 200 g of the electrode active material coated with the modified third nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 46 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-3 slurry;
[0137] 200 g of the electrode active material coated with the modified fourth nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 34 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-4 slurry;
[0138] 200 g of the modified fifth nitrogen-doped carbon nanotube layer-coated electrode active material, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 22 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-5 slurry;
[0139] 200 g of the electrode active material coated with the modified sixth nitrogen-doped carbon nanotube layer, 10 g of chopped carbon fiber, 30 g of acetylene black, 25 g of polyvinylidene fluoride, and 10 g of ammonium bicarbonate were added to 300 g of N-methylpyrrolidone and stirred to obtain an electrode slurry, which was recorded as 3-5 slurry;
[0140] Spray 3-1 slurry, 3-2 slurry, 3-3 slurry, 3-4 slurry, 3-5 slurry, and 3-6 slurry onto the surface of the current collector titanium mesh in sequence, with a coating density of 25 mg / cm 2 After each layer of slurry is coated, the coating layer is dried at low temperature at 70°C for 10 minutes. After the last layer of electrode slurry is coated and dried at low temperature, the entire electrode is dried at 100°C for 5 hours. After the electrode is dried, it is rolled to a thickness of 500μm. It is then immersed in water, and the water is changed every 0.5 hours, for a total of 3 times, to obtain a composite electrode for lithium extraction from salt lakes.
[0141] The prepared composite electrode for lithium extraction from salt lakes includes a current collector titanium mesh and six active coating layers of the same thickness; the mass of the pore-forming agent in each active coating layer decreases gradually in the direction away from the current collector, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases gradually;
[0142] Wherein, each active coating layer contains an electrode active material coated with a modified first nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified second nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified third nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified fourth nitrogen-doped carbon nanotube layer, an electrode active material coated with a modified fifth nitrogen-doped carbon nanotube layer, and an electrode active material coated with a modified sixth nitrogen-doped carbon nanotube layer, and the active coating layer also contains ammonium bicarbonate;
[0143] Lithium extraction experiment: The prepared composite electrode was used as the anode and nickel foam was used as the cathode. The electrodes were placed in a 20 g / L NaCl solution and a voltage of 1 V was applied across the electrodes until the current density was lower than 0.5 A / m 2 , obtaining a lithium-deficient electrode. The electrolysis apparatus was separated into a cathode chamber and an anode chamber using an anion membrane. The prepared lithium-rich and lithium-deficient electrodes were placed in the anode and cathode chambers, respectively. 4.5 L of brine with a lithium concentration of 0.68 g / L was injected into the cathode chamber, and 2 L of a 5 g / L NaCl solution was injected into the anode chamber as the supporting electrolyte. A voltage of 0.9 V was applied to the anode and cathode, and electrolysis was performed at 20°C for 4 hours. The lithium ion concentration and brine impurity concentration before and after electrolysis were measured using an inductively coupled plasma spectrometer (ICP), as shown in Table 5.
[0144] Table 4
[0145] Comparative Example 5
[0146] 200g of lithium iron phosphate, 10g of short carbon fiber, 30g of acetylene black, 25g of PVDF, and 34g of ammonium bicarbonate were mixed evenly, and then 300g of N-methyl pyrrolidone was added and stirred evenly to obtain an electrode slurry coated on the surface of the current collector titanium mesh. The coating thickness was the same as in Example 4. The coating layer was dried at 70°C for 10 minutes and then dried at 100°C for 5 hours. After the electrode was dried, it was immersed in water and the water was changed every 0.5 hours. The water was changed 3 times to obtain a lithium iron phosphate electrode for electrochemical lithium extraction. Lithium was extracted under the same technical parameters as in Example 5. The lithium concentration in the lithium-rich anode solution rose to 4.95g / L, and the lithium extraction rate was 80%.
[0147] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application and are not intended to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present application.
Claims
1. A method for preparing a composite electrode for lithium extraction from salt lakes, It is characterized in that The following steps are involved: Dispersing nitrogen-containing organic matter and carbon nanotubes in a first solvent, heating to reflux, filtering, drying, washing with water, and drying to obtain nitrogen-doped carbon nanotubes; Taking n portions of nitrogen-doped carbon nanotubes of different masses, respectively dispersing the nitrogen-doped carbon nanotubes and the electrode active material in a second solvent, ball-milling, and drying, respectively obtaining n electrode active materials coated with nitrogen-doped carbon nanotube layers of different thicknesses; wherein the mass of the electrode active material corresponding to each portion of the nitrogen-doped carbon nanotube is the same; The prepared nitrogen-doped carbon nanotube layer-coated electrode active materials are added to a dopamine solution for modification, filtering, washing, and drying to obtain n types of electrode active materials with modified nitrogen-doped carbon coating layers of different thicknesses; The electrode active material of the modified nitrogen-doped carbon coating layer is respectively prepared with a pore former, a reinforcing agent, a conductive agent, a binder and a third solvent to prepare n portions of electrode slurry, and the electrode slurry is sequentially coated on a current collector, and then dried, rolled and immersed in water to form n layers of active coatings, so that the mass of the pore former in each active coating layer away from the current collector decreases in a gradient manner, and the thickness of the modified nitrogen-doped carbon coating layer in the electrode active material of the modified nitrogen-doped carbon coating layer decreases in a gradient manner; Wherein, n is a positive integer ≥2.
2. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The masses of the electrode active material of the modified nitrogen-doped carbon coating layer, the reinforcing agent, the conductive agent, the binder and the third solvent in each electrode slurry are the same.
3. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The mass of pore former in each electrode slurry is different.
4. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The nitrogen-containing organic matter includes at least one of hydrazine hydrate, pyrimidine, ethylenediamine and melamine.
5. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The first solvent includes at least one of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, and acetone.
6. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The mass ratio of the nitrogen-containing organic matter, the carbon nanotubes and the first solvent is (2-10): (10-40): (100-1000).
7. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The second solvent includes at least one of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, and acetone.
8. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The electrode active material includes LiMn 2 O 4 、LiFePO 4 、LiNi x Co y Mn z O 2 At least one of , where x+y+z=1.
9. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The mass ratio of the nitrogen-doped carbon nanotubes, the electrode active material and the second solvent is (0.001-0.02):1:(1-10).
10. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The mass concentration of the dopamine solution is 1-6 g / L.
11. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The solid-to-liquid ratio of the carbon nanotube-coated electrode active material and the dopamine solution is 1 g: (4-20) mL.
12. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The mass ratio of the electrode active material of the modified nitrogen-doped carbon coating layer to the pore former, the reinforcing agent, the conductive agent, the binder and the third solvent is 100:(5-35):(10-20):(5-20):(100-400).
13. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The pore-forming agent is at least one of ammonium carbonate and ammonium bicarbonate; and / or The reinforcement includes chopped carbon fibers.
14. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 13, It is characterized in that The conductive agent comprises at least one of acetylene black and carbon black; and / or The binder comprises polyvinylidene fluoride; and / or The third solvent includes N-methylpyrrolidone.
15. The method for preparing a composite electrode for extracting lithium from a salt lake according to claim 1, It is characterized in that The coating amount of each electrode slurry is the same, both 10-50 mg / cm 2 .
Citation Information
Patent Citations
High-selectivity lithium extraction electrode and preparation method thereof
CN113278819A
Electrode material for salt lake lithium extraction and preparation method and application of thereof
CN113278820A
Preparation method of crown ether modified electrode for salt lake lithium extraction
CN113293300A
Composite-coated lithium iron phosphate and preparation method therefor, and lithium ion battery
US20180097228A1
Positive electrode and method for making the same, and battery using the same
US20200067073A1
Cited By
Lithium iron phosphate carbon nanotube composite material and preparation method thereof
CN119240653A