Semiconductor structure and manufacturing method therefor
Through the combination of laser heating and underlying silicon technology, the problem of insufficient filling of holes in the semiconductor structure is solved, the density and conductivity of the silicon material layer are improved, the yield of the semiconductor structure is improved, and the negative impact on the performance of other structures is avoided. Influence.
Patent Information
- Application Number
- PCT/CN2023/097828
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-06-01
- Publication Date
- 2024-10-03
AI Technical Summary
During the high-integration-density manufacturing process of semiconductor structures, the shortening of the spacing between adjacent structures leads to an increase in the hole aspect ratio, which affects the filling effect of the filling material and reduces the yield of the semiconductor structure.
Laser heating treatment technology is used to locally heat the initial silicon material layer to melt and recrystallize it to form a silicon material layer with low defect density. Combined with the underlying silicon formed at the bottom of the blind hole, it provides better recrystallization conditions and avoids the formation of voids. Improve density and conductive properties.
The density and conductive properties of the silicon material layer of the semiconductor structure are improved, the yield of the semiconductor structure is enhanced, and the adverse effects of laser processing on the performance of other structures are avoided.
Smart Images

Figure CN2023097828_03102024_PF_FP_ABST
Abstract
Description
Semiconductor structure and method for manufacturing the same
[0001] Cross-references
[0002] This application claims priority to Chinese patent application entitled “Semiconductor Structure and Manufacturing Method Thereof” filed on March 27, 2023, application number 202310312374.6, which is incorporated herein by reference in its entirety. Technical Field
[0003] The embodiments of the present disclosure relate to the field of semiconductor technology, and in particular to a semiconductor structure and a method for manufacturing the same. Background Art
[0004] As semiconductor structures develop toward higher integration densities, the manufacturing methods of semiconductor structures face greater challenges. For example, due to the shortening of the spacing between adjacent structures, the aspect ratio of the holes formed between adjacent structures becomes larger, which is likely to have an adverse effect on the subsequent filling of the holes with filling materials, thereby being detrimental to improving the yield of the semiconductor structure.
[0005] Summary of the Invention
[0006] The embodiments of the present disclosure provide a semiconductor structure and a method for manufacturing the same, which are at least beneficial to improving the yield of the semiconductor structure.
[0007] According to some embodiments of the present disclosure, on the one hand, an embodiment of the present disclosure provides a method for manufacturing a semiconductor structure, comprising: providing a substrate having at least one blind hole therein; forming a bottom layer of silicon at least at the bottom of the blind hole using an epitaxial growth process; forming an initial silicon material layer filling the remaining blind holes, the melting point of the initial silicon material layer being lower than the melting point of the bottom layer of silicon; using a laser to process the initial silicon material layer so that the initial silicon material layer melts; and cooling the initial silicon material layer after the laser treatment so that the initial silicon material layer recrystallizes to form a silicon material layer.
[0008] In some embodiments, in the step of processing the initial silicon material layer with a laser, voids in the initial silicon material layer are eliminated.
[0009] In some embodiments, the silicon material layer includes at least one of single crystal silicon or polycrystalline silicon, and a defect density of the silicon material layer is lower than a defect density of the initial silicon material layer.
[0010] In some embodiments, the working mode of the laser includes a pulsed laser, and the use of the laser to process the initial silicon material layer includes: sequentially performing N pulsed laser processes on the initial silicon material layer located in the blind hole to achieve local heating of the initial silicon material layer located in the blind hole, wherein N is a positive integer, and as the number of times increases, the energy density of the pulsed laser remains unchanged or increases.
[0011] In some embodiments, the energy density of the pulsed laser is in the range of 0.3 mJ / cm2 to 0.7 mJ / cm2.
[0012] In some embodiments, the wavelength of the pulse laser is 532 nm, and the pulse width of the pulse laser is 10 ns.
[0013] In some embodiments, as the number of times increases, the energy density of the pulsed laser first remains unchanged and then gradually increases. When the energy density of the pulsed laser remains unchanged, the initial silicon material layer is preheated, and when the energy density of the pulsed laser increases, the melting of the initial silicon material layer is accelerated.
[0014] In some embodiments, in the step of processing the initial silicon material layer with a laser, a maximum temperature of the initial silicon material layer is between 1100° C. and 1400° C.
[0015] In some embodiments, in the step of processing the initial silicon material layer with a laser, a maximum depth of the melted initial silicon material layer along a depth direction of the blind hole is 400 nm to 500 nm.
[0016] In some embodiments, the working mode of the laser includes continuous laser, and the use of laser to process the initial silicon material layer includes: using the continuous laser to scan the substrate and the initial silicon material layer, and the energy density of the continuous laser when scanning the substrate is a first energy density, and the energy density of the continuous laser when scanning the initial silicon material layer is a second energy density, and the first energy density is lower than the second energy density.
[0017] In some embodiments, before forming the bottom silicon layer, the method further includes: cleaning the substrate.
[0018] In some embodiments, in the step of forming underlying silicon at least at the bottom of the blind hole using an epitaxial growth process, a silicon film layer is formed on the sidewall of the blind hole; the underlying silicon and the silicon film layer together form a contact hole, and the forming of an initial silicon material layer filling the blind hole includes: forming an initial silicon material layer filling the contact hole; in the step of processing the initial silicon material layer using a laser, the silicon film layer also melts; in the step of recrystallizing the initial silicon material layer, the silicon film layer in a molten state and the initial silicon material layer in a molten state recrystallize together.
[0019] In some embodiments, along the depth direction of the blind hole, the thickness of the underlying silicon ranges from 1 nm to 5 nm.
[0020] In some embodiments, the cooling process includes blowing an inert gas toward the initial silicon material layer after the laser treatment, and the pressure of the inert gas is in a range of 0.2 MPa to 1 MPa.
[0021] In some embodiments, the step of providing the base includes: providing a substrate; forming a plurality of parallel bit lines and a dielectric layer located between adjacent bit lines on the substrate, wherein the dielectric layer and the bit lines together enclose a plurality of blind holes, and the blind holes are capacitor contact holes; or forming a plurality of grooves for forming bit lines in the substrate, wherein the grooves have the blind holes, and the blind holes are used to form bit line contact layers.
[0022] According to some embodiments of the present disclosure, on the other hand, embodiments of the present disclosure further provide a semiconductor structure, comprising: a substrate having at least one blind hole therein; a silicon material layer located at least at the bottom and part of the sidewall of the blind hole, the defect density of the silicon material layer being lower than the defect density of amorphous silicon.
[0023] In some embodiments, the base includes: a substrate; a plurality of parallel bit lines located on the substrate and a dielectric layer located between adjacent bit lines, the dielectric layer and the bit lines together forming a plurality of blind holes; along the extension direction of the blind holes, the silicon material layer is located in the blind holes at a partial depth.
[0024] In some embodiments, the bit line includes multiple bit line contact layers and a bit line body that is in contact with the multiple bit line contact layers. The bit line contact layers are located in the blind holes and correspond one-to-one to the blind holes. The bit line body is located on the top surface of the bit line contact layers.
[0025] In some embodiments, the bit line includes a bit line contact layer, a diffusion barrier layer, a bit line conductive layer, a bit line first protective layer and a bit line second protective layer. A bit line may include multiple bit line contact layers. The multiple bit line contact layers in a bit line are all in contact with and connected to the same diffusion barrier layer. The bit line first protective layer and the bit line second protective layer jointly surround the side walls and top surface of the bit line.
[0026] In some embodiments, the substrate may include an active area, a shallow trench isolation structure and an isolation layer, the bit line contact layer is in contact with the active area, the diffusion barrier layer that is not in contact with the bit line contact layer is provided with the isolation layer and the shallow trench isolation structure, and the blind hole exposes part of the active area and the shallow trench isolation structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] One or more embodiments are exemplarily illustrated by the pictures in the corresponding drawings. These exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise stated, the pictures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the traditional technology, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0028] FIG1 is a schematic flow chart of a method for manufacturing a semiconductor structure according to an embodiment of the present disclosure;
[0029] 2 to 14 are schematic structural diagrams corresponding to the steps of a method for manufacturing a semiconductor structure provided in an embodiment of the present disclosure. DETAILED DESCRIPTION
[0030] As known from the background art, the yield of semiconductor structures needs to be improved.
[0031] The embodiment of the present disclosure provides a semiconductor structure and a manufacturing method thereof. In the manufacturing method, on the one hand, a laser is used to heat the initial silicon material layer, which is beneficial to avoid the presence of voids or gaps in the silicon material layer formed by the subsequent melting and recrystallization of the initial silicon material layer, thereby improving the density and conductivity of the silicon material layer; on the other hand, before forming the initial silicon material layer, a bottom silicon layer is formed at the bottom of the blind hole to provide the initial silicon material layer with better recrystallization conditions, thereby facilitating the formation of a silicon material layer with a lower defect density; on the other hand, since the laser can achieve the effect of local heating and the laser can achieve the effect of rapid temperature increase, when the laser is used to make the initial silicon material layer in a high-temperature molten state, the temperature effect of the laser on other structures adjacent to the initial silicon material layer can be ignored, and will not adversely affect other properties of the semiconductor structure. Therefore, the manufacturing method of the semiconductor structure provided by an embodiment of the present disclosure improves the density and conductivity of the formed silicon material layer while avoiding the adverse effects of the process of forming the silicon material layer on other parts of the semiconductor structure.
[0032] The following describes various embodiments of the present disclosure in detail with reference to the accompanying drawings. However, those skilled in the art will appreciate that many technical details are provided in the various embodiments of the present disclosure to help readers better understand the embodiments of the present disclosure. However, even without these technical details and the various variations and modifications based on the following embodiments, the technical solutions claimed in the embodiments of the present disclosure can be implemented.
[0033] An embodiment of the present disclosure provides a method for manufacturing a semiconductor structure. The method for manufacturing a semiconductor structure provided by an embodiment of the present disclosure will be described in detail below with reference to the accompanying drawings. Figure 1 is a flow chart of the method for manufacturing a semiconductor structure provided by an embodiment of the present disclosure; Figures 2 to 14 are structural schematic diagrams corresponding to the steps of the method for manufacturing a semiconductor structure provided by an embodiment of the present disclosure. It should be noted that, in order to facilitate description and clearly illustrate the steps of the method for manufacturing a semiconductor structure, Figures 2 to 14 in an embodiment of the present disclosure are all schematic diagrams of the partial structures of the semiconductor structure.
[0034] 1 to 14 , the method for manufacturing a semiconductor structure includes the following steps.
[0035] S101 : Referring to FIG. 2 to FIG. 6 , a substrate 100 is provided, wherein the substrate 100 has at least one blind hole 110 therein.
[0036] In some embodiments, referring to FIG. 3 and FIG. 4 , the step of providing a base 100 may include providing a substrate 101 , forming a plurality of grooves 112 in the substrate 101 for forming bit lines 102 , the grooves 112 having blind holes 110 therein, and the blind holes 110 for forming bit line contact layers 122 .
[0037] It should be noted that Figure 3 is a schematic diagram of a partial top view of the structure of the substrate 100 in the manufacturing method provided by an embodiment of the present disclosure, and Figure 4 schematically shows a groove 112 and a blind hole 110 in the substrate 101 for forming a bit line 102. The bit line 102 is drawn in perspective. The area enclosed by the dotted line in Figure 3 is the area where the groove 112 is located in the substrate 101; Figure 4 is a schematic diagram of the cross-sectional structure of the substrate 100 shown in Figure 2 along the first cross-sectional direction AA1.
[0038] In one example, referring to Figures 3 and 4, the bit line 102 includes multiple bit line contact layers 122 and a bit line body 132 that is in contact with the multiple bit line contact layers 122. The bit line contact layers 122 are located in the blind holes 110 and the bit line contact layers 122 correspond one-to-one to the blind holes 110. The bit line body 132 is located on the top surface of the bit line contact layer 122.
[0039] In other embodiments, referring to FIG. 5 and FIG. 6 , the step of providing the base 100 may include: providing a substrate 101; forming a plurality of parallel bit lines 102 and a dielectric layer 103 located between adjacent bit lines 102 on the substrate 101, wherein the dielectric layer 103 and the bit lines 102 together enclose a plurality of blind holes 110, and the blind holes 110 are capacitor contact holes.
[0040] It should be noted that FIG5 is another partial cross-sectional structural schematic diagram of the substrate 100 in the manufacturing method provided in one embodiment of the present disclosure, and FIG6 is a top structural schematic diagram of the substrate 100 shown in FIG5 .
[0041] In some embodiments, referring to Figure 5, the bit line 102 includes a bit line contact layer 122, a diffusion barrier layer 142, a bit line conductive layer 152, a bit line first protection layer 162 and a bit line second protection layer 172, wherein a bit line 102 may include multiple bit line contact layers 122, and the multiple bit line contact layers 122 in a bit line 102 are all in contact with and connected to the same diffusion barrier layer 142, and the bit line first protection layer 162 and the bit line second protection layer 172 jointly surround the side walls and top surface of the bit line 102 to achieve insulation between the bit line 102 and other conductive structures.
[0042] In some embodiments, referring to FIG. 5 , the first bitline protection layer 162 is located within the second bitline protection layer 172. In some embodiments, the first bitline protection layer 162 may be made of silicon oxide, and the second bitline protection layer 172 may be made of silicon nitride. In some embodiments, the bitline contact layer 122 may be made of doped polysilicon, the diffusion barrier layer 142 may be made of titanium nitride, and the bitline conductive layer 152 may be made of tungsten.
[0043] Continuing with FIG. 5 , substrate 101 may include an active area 111, a shallow trench isolation structure 121, and an isolation layer 131. A bitline contact layer 122 is in contact with active area 111. Isolation layer 131 is provided between diffusion barrier layer 142, which is not in contact with bitline contact layer 122, and shallow trench isolation structure 121 to further ensure insulation between bitlines 102 excluding bitline contact layer 122 and substrate 101. In some embodiments, shallow trench isolation structure 121 may be made of silicon oxide or silicon nitride, and isolation layer 131 may be made of silicon oxide.
[0044] 5 , the blind via 110 exposes a portion of the active area 111 and the shallow trench isolation structure 121 .
[0045] It is understandable that the capacitor contact holes are subsequently used to form capacitor contact layers. Referring to FIG. 6 , there are multiple blind holes 110 between adjacent bit lines 102 , and one blind hole 110 corresponds to one capacitor contact layer formed subsequently.
[0046] It should be noted that the method for manufacturing a semiconductor structure provided in an embodiment of the present disclosure includes, but is not limited to, applications in the various embodiments described above. It is understood that the method for manufacturing a semiconductor structure provided in an embodiment of the present disclosure, in which the subsequent solution of forming a silicon material layer in the blind via 110 is ultimately applicable to any scenario requiring the formation of a silicon material layer in a groove or hole, can improve the density and conductivity of the silicon material layer while preventing the process of forming the silicon material layer from adversely affecting other parts of the semiconductor structure.
[0047] S102 : Referring to FIG. 7 to FIG. 9 , an epitaxial growth process is used to form an underlying silicon layer 104 at least at the bottom of the blind hole 110 .
[0048] It should be noted that Figures 7 to 9 illustrate three embodiments of forming the underlying silicon 104 at the bottom of the blind via 110 using an epitaxial growth process. Figures 8 and 9 both use an existing blind via 110 as a capacitor contact hole as an example. In actual applications, the embodiments of the existing underlying silicon 104 shown in Figures 8 and 9 are also applicable when the blind via 110 is used to form a bitline contact layer. Furthermore, depending on the application of the blind via 110, the underlying silicon 104 can be a relatively flat thin layer as shown in Figure 7, or a thin layer forming a groove as shown in Figures 8 and 9.
[0049] In some embodiments, after the blind hole 110 is formed, an epitaxial growth process may be directly used to form the underlying silicon 104 at least at the bottom of the blind hole 110 .
[0050] In other embodiments, before forming the underlying silicon layer 104, the method for manufacturing the semiconductor structure may further include: cleaning the substrate 100. It is understood that, before performing the epitaxial growth process, the substrate 100 including the blind vias 110 is first cleaned to remove impurities that may remain in the blind vias 110, such as interlayer oxides, hydrogen-containing impurities, or water vapor. This helps provide better growth conditions for the epitaxial growth process. For example, based on the clean bottom of the blind vias 110, it is beneficial to form the underlying silicon layer 104 with a lower defect density. Furthermore, it prevents impurities remaining in the blind vias 110 from reducing the conductivity of the silicon material layer subsequently formed in the blind vias 110, thereby helping to reduce the contact resistance between the active region 111 and the silicon material layer, thereby improving the device performance of the semiconductor structure.
[0051] It can be understood that the use of an epitaxial growth process to form the underlying silicon 104 is conducive to forming an underlying silicon 104 with high density and stable structure. Moreover, due to the characteristics of the epitaxial growth process, it is conducive to forming an underlying silicon 104 with a thinner thickness, thereby helping to improve the film uniformity of the underlying silicon 104. When the doped ions in the subsequent silicon material layer enter the underlying silicon 104, the thickness of the underlying silicon 104 is thinner, which is more conducive to the diffusion of doped ions into the underlying silicon 104, so as to ensure that the concentration of doped ions in the underlying silicon 104 is high, so as to ensure good conductivity of the underlying silicon 104.
[0052] In some embodiments, the cleaning process includes plasma cleaning, for example, using plasma containing argon or nitrogen to remove impurities remaining in the blind via 110 and provide a better growth environment for the subsequent epitaxial growth process.
[0053] In some embodiments, referring to FIG8 or FIG9 , in the step of forming the underlying silicon 104 at least at the bottom of the blind hole 110 (refer to FIG5 ) using an epitaxial growth process, a silicon film layer 114 is formed on the sidewalls of the blind hole 110 ; the underlying silicon 104 and the silicon film layer 114 together form a contact hole 120 .
[0054] In one example, referring to FIG8 , in the step of forming the underlying silicon 104 at the bottom of the blind hole 110 (refer to FIG5 ), the silicon film layer 114 is formed only on the sidewalls of the blind hole 110. In another example, referring to FIG8 , in the step of forming the underlying silicon 104 at the bottom of the blind hole 110 (refer to FIG5 ), the silicon film layer 114 is formed on the sidewalls of the blind hole 110 and the top surface of the bit line 102.
[0055] In the above example, the material of the bottom silicon 104 may be single crystal silicon or densified undoped polysilicon, and the material of the silicon film layer 114 may be polysilicon.
[0056] It should be noted that in order to distinguish the underlying silicon 104 and the silicon film layer 114 in Figures 8 and 9, different filling methods are used for the underlying silicon 104 and the silicon film layer 114. It can be understood that the underlying silicon 104 and the silicon film layer 114 can be formed in the same step by an epitaxial growth process, that is, the underlying silicon 104 and the silicon film layer 114 are an integrated molding structure.
[0057] In the above example, it can be understood that before the initial silicon material layer is formed, a bottom silicon layer 104 is formed at the bottom of the blind hole 110. Subsequently, during the cooling and recrystallization process of the molten initial silicon material layer, the molten initial silicon material layer can use the bottom silicon layer 104 as a seed layer and recrystallize along the crystal orientation of the crystals in the bottom silicon layer 104, so that the silicon material layer finally formed includes at least one of single crystal silicon or polycrystalline silicon, thereby facilitating the improvement of the density of the silicon material layer. Moreover, the bottom silicon layer 104 provides better recrystallization conditions for the molten initial silicon material layer, which is conducive to further reducing the defect density of the silicon material layer itself, thereby facilitating the improvement of the yield of the silicon material layer and the semiconductor structure. In addition, the use of an epitaxial growth process to form the bottom silicon layer 104 at least at the bottom of the blind hole 110 is conducive to reducing the roughness of the bottom corner of the blind hole 110 through the bottom silicon layer 104, which is conducive to improving the film uniformity of the initial silicon material layer subsequently formed on the basis of the bottom silicon layer 104.
[0058] It is understandable that, during the subsequent melting process of the initial silicon material layer, the laser heating temperature can also be controlled so that the underlying silicon 104 is also melted; during the subsequent cooling and recrystallization process of the molten initial silicon material layer, the molten underlying silicon 104 crystallizes earlier than the molten initial silicon material layer. Therefore, the underlying silicon 104 that is crystallized first is beneficial to providing better recrystallization conditions for the initial silicon material layer that is still in a molten state, which is beneficial to further reduce the defect density of the silicon material layer itself, thereby helping to improve the yield of the silicon material layer and the semiconductor structure.
[0059] In some embodiments, referring to Figures 7 to 9, the thickness D of the bottom silicon 104 along the depth direction Z of the blind hole 110 ranges from 1 nm to 5 nm. It is understandable that the formation of the bottom silicon 104 serves as a seed layer for the subsequent recrystallization of the melted initial silicon material layer, so the thickness of the bottom silicon 104 does not need to be too thick. In addition, the time required for the epitaxial growth process to form the bottom silicon 104 is long. Therefore, the thickness D of the bottom silicon 104 ranges from 1 nm to 5 nm, which is beneficial for ensuring that the bottom silicon 104 is relatively thin while avoiding the excessive time spent on forming the bottom silicon 104. This is beneficial for improving the yield of the subsequently formed semiconductor structure and improving the preparation efficiency of the semiconductor structure. In addition, if the thickness D of the bottom silicon 104 is too large, for example, greater than 5 nm, it is not conducive to the dopant ions in the initial silicon material layer to enter the bottom silicon 104 when the initial silicon material layer is deposited in the next step, which is not conducive to improving the conductive properties of the capacitor contact layer finally formed.
[0060] It should be noted that, for the convenience of description, the subsequent steps are described using the example shown in FIG9 .
[0061] S103 : With reference to FIG. 7 and FIG. 10 , or with reference to FIG. 9 and FIG. 11 , an initial silicon material layer 105 is formed to fill the remaining blind holes 110 . The melting point of the initial silicon material layer 105 is lower than that of the underlying silicon 104 .
[0062] In some embodiments, referring to Figures 7 and 10, the bottom silicon 104 is formed only at the bottom of the blind hole 110, the sidewalls of the blind hole 110 and the top surface of the substrate 100 are exposed, and the initial silicon material layer 105 is located on the sidewalls of the blind hole 110 and the top surface of the substrate 100.
[0063] In other embodiments, referring to Figures 9 and 11, an underlying silicon layer 104 is formed at the bottom of the blind hole 110 (refer to Figure 5), and a silicon film layer 114 is formed on the sidewall of the blind hole 110. On the basis that the underlying silicon layer 104 and the silicon film layer 114 together surround the contact hole 120, the step of forming the initial silicon material layer 105 that fills the blind hole 110 may include: forming the initial silicon material layer 105 that fills the contact hole 120.
[0064] In the above embodiment, referring to FIG. 10 or FIG. 11 , when the initial silicon material layer 105 is formed to fill the remaining blind holes 110 (refer to FIG. 5 ), due to the formation process and the influence of the aspect ratio of the remaining blind holes 110 , the initial silicon material layer 105 is likely to have voids 115 inside. The voids 115 will reduce the film uniformity of the initial silicon material layer 105 and reduce the conductive properties of the initial silicon material layer 105 itself. It is understandable that the voids 115 can be macroscopic holes.
[0065] In some embodiments, the method of forming the initial silicon material layer 105 includes CVD (Chemical Vapor Deposition), and the raw material for forming the initial silicon material layer 105 includes silane.
[0066] In some embodiments, the initial silicon material layer 105 may be polysilicon.
[0067] S104: using laser to process the initial silicon material layer 105 so that the initial silicon material layer 105 melts.
[0068] In some embodiments, referring to FIG. 10 , the silicon film layer 114 is not formed simultaneously with the formation of the underlying silicon 104 , and thus, in the step of processing the initial silicon material layer 105 with a laser, only the initial silicon material layer 105 is melted.
[0069] In other embodiments, referring to FIG11 and FIG12 , after forming a bottom silicon layer 104 at the bottom of a blind hole 110 (see FIG5 ) and forming a silicon film layer 114 on the sidewalls of the blind hole 110, the silicon film layer 114 is also melted during the laser treatment of the initial silicon material layer 105. It should be noted that in FIG12 , the molten initial silicon material layer 105 and the molten silicon film layer 114 are collectively depicted as the to-be-crystallized layer 106.
[0070] It can be understood that not only the melting point of the initial silicon material layer 105 is lower than the melting point of the underlying silicon 104, but the melting point of the silicon film layer 114 is also lower than the melting point of the underlying silicon 104. Therefore, in the step of using laser to process the initial silicon material layer 105, the initial silicon material layer 105 and the silicon film layer 114 will both melt. Subsequently, the initial silicon material layer 105 in a molten state and the silicon film layer 114 in a molten state, that is, the layer to be crystallized 106, are cooled and recrystallized to form a silicon material layer.
[0071] In addition, in the step of using laser to process the initial silicon material layer 105, the laser heating temperature can be controlled. When the initial silicon material layer 105 and the silicon film layer 114 melt, the underlying silicon 104 also melts; in the subsequent cooling and recrystallization process of the melted initial silicon material layer 105 and the melted silicon film layer 114, the melted underlying silicon 104 is farthest from the heat source and crystallizes first. Therefore, the underlying silicon 104 that is crystallized first is beneficial to providing better recrystallization conditions for the initial silicon material layer 105 and the silicon film layer 114 that are still in a molten state.
[0072] In some embodiments, the initial silicon material layer 105 and the silicon film layer 114 may both be made of polysilicon.
[0073] In some embodiments, referring to FIG11 and FIG12 , during the step of laser processing the initial silicon material layer 105, voids 115 in the initial silicon material layer 105 are eliminated. This helps ensure that the silicon material layer subsequently formed based on the melted initial silicon material layer 105 does not have macroscopic void defects, thereby improving the film uniformity and conductive properties of the silicon material layer.
[0074] Furthermore, because the laser can achieve a localized heating effect, it can generate relatively high temperatures in both the initial silicon material layer 105 and the silicon film layer 114. At this time, the temperatures generated in other structures adjacent to the initial silicon material layer 105 and the silicon film layer 114 are relatively low, meaning that the laser has a relatively small impact on the temperatures generated in other structures adjacent to the initial silicon material layer 105 and the silicon film layer 114. Furthermore, because the laser can achieve a rapid temperature increase, the high temperature persists in the initial silicon material layer 105 and the silicon film layer 114 for a relatively short period of time, and the temperature impact on other structures adjacent to the initial silicon material layer 105 and the silicon film layer 114 also lasts for a relatively short period of time. Therefore, even if the laser is used to cause the initial silicon material layer 105 and the silicon film layer 114 to be in a high-temperature molten state, the temperature impact generated by the laser on other structures adjacent to the initial silicon material layer 105 and the silicon film layer 114 is negligible, and will not adversely affect other properties of the semiconductor structure.
[0075] The working mode of the laser is described in detail below through two embodiments.
[0076] In some embodiments, the laser operation mode may include a pulsed laser, and the step of using the laser to treat the initial silicon material layer 105 may include: referring to FIG11 , sequentially performing N pulsed laser treatments on the initial silicon material layer 105 located in the blind hole 110 (refer to FIG5 ) to achieve localized heating of the initial silicon material layer 105 located in the blind hole 110, where N is a positive integer, and the energy density of the pulsed laser remains constant or increases as the number of treatments increases. It will be understood that performing N pulsed laser treatments on the initial silicon material layer 105 is beneficial in heating the initial silicon material layer 105 to a molten state, reducing the duration of the high temperature generated by the laser, and further preventing the high temperature from adversely affecting the semiconductor structure.
[0077] It is understandable that in the step of performing N pulse laser treatments on the initial silicon material layer 105 in the blind hole 110 (see FIG. 5 ), the silicon film layer 114 and / or the underlying silicon 104 may also be melted.
[0078] In some embodiments, as the number of pulses increases, the energy density of the pulsed laser initially remains constant and then gradually increases. When the energy density of the pulsed laser remains constant, the initial silicon material layer 105 is preheated, and when the energy density of the pulsed laser increases, the melting of the initial silicon material layer 105 is accelerated. It is understood that heating the initial silicon material layer 105 by preheating followed by high-temperature heating is beneficial for rapidly heating the initial silicon material layer 105 to a molten state while reducing the initial temperature fluctuation of the initial silicon material layer 105. This further helps to avoid an increase in the defect density in the initial silicon material layer 105 caused by excessive temperature fluctuations.
[0079] In some embodiments, the energy density of the pulsed laser can be in the range of 0.3 mJ / cm 2 ~0.7mJ / cm 2 For example, the energy density of a pulse laser is 0.35mJ / cm 2 , 0.4mJ / cm 2 , 0.45mJ / cm 2 , 0.5mJ / cm 2 , 0.55mJ / cm 2 , 0.6mJ / cm 2 or 0.65 mJ / cm 2 .
[0080] In some embodiments, the wavelength of the pulsed laser can be 532 nm. It is understood that the wavelength of the pulsed laser is a key factor affecting the laser radiation depth. Along direction Z, the radiation depth of a laser with a wavelength of 532 nm ranges from 200 nm to 300 nm. It is understood that in practical applications, the laser radiation depth can also be controlled by adjusting the laser energy density and the time interval between different laser bursts.
[0081] In some embodiments, the pulse width of the pulsed laser may be 10 ns. It is understood that the duration of a single pulse of laser light is 10 ns. In other embodiments, the pulse width of the pulsed laser light may also be less than 10 ns.
[0082] In some embodiments, N is 1 to 10, that is, the number of times the initial silicon material layer 105 is processed using the pulse laser can be 1 to 10 times in total.
[0083] In one example, N is 4. When the initial silicon material layer 105 is pulsed laser treated for the first time, the energy density of the pulsed laser is 0.35 mJ / cm 2 When the initial silicon material layer 105 is pulsed laser treated for the second time, the energy density of the pulsed laser is 0.35mJ / cm 2 When the initial silicon material layer 105 is pulsed laser treated for the third time, the energy density of the pulsed laser is 0.4mJ / cm 2 When the initial silicon material layer 105 is pulsed laser treated for the fourth time, the energy density of the pulsed laser is 0.45mJ / cm 2 In addition, the interval between the first pulse laser treatment and the second pulse laser treatment is 100 ns, the interval between the second pulse laser treatment and the third pulse laser treatment is 50 ns, and the interval between the third pulse laser treatment and the fourth pulse laser treatment is 150 ns.
[0084] In another example, N is 4. When the initial silicon material layer 105 is subjected to pulse laser treatment for the first time, the surface temperature of the initial silicon material layer 105 ranges from 690°C to 710°C; when the initial silicon material layer 105 is subjected to pulse laser treatment for the second time, the surface temperature of the initial silicon material layer 105 ranges from 950°C to 970°C; when the initial silicon material layer 105 is subjected to pulse laser treatment for the third time, the surface temperature of the initial silicon material layer 105 ranges from 990°C to 1010°C; and when the initial silicon material layer 105 is subjected to pulse laser treatment for the fourth time, the surface temperature of the initial silicon material layer 105 ranges from 1290°C to 1310°C. Furthermore, the interval between the first and second pulse laser treatments is 40 ns, the interval between the second and third pulse laser treatments is 240 ns, and the interval between the third and fourth pulse laser treatments is 40 ns.
[0085] In some embodiments, the total time duration for processing the initial silicon material layer with the pulsed laser may be 1000 ns.
[0086] In some embodiments, during the step of laser processing the initial silicon material layer 105, the maximum temperature of the initial silicon material layer 105 is between 1100° C. and 1400° C. This helps ensure that when the initial silicon material layer 105 is molten, the underlying silicon 104 does not melt, and subsequently serves as a seed layer for the recrystallization of the molten initial silicon material layer 105.
[0087] In some embodiments, during the step of laser processing the initial silicon material layer 105, the maximum depth of the melted initial silicon material layer 105 along the depth direction Z of the blind via 110 is 400 nm to 500 nm. This helps prevent other devices deeper in the semiconductor structure from being affected by temperature along the direction Z and away from the laser.
[0088] In other embodiments, the working mode of the laser may include continuous laser, and the step of using laser to process the initial silicon material layer 105 may include: using continuous laser to scan the substrate 100 and the initial silicon material layer 105, and the energy density of the continuous laser when scanning the substrate 100 is a first energy density, and the energy density of the continuous laser when scanning the initial silicon material layer 105 is a second energy density, and the first energy density is lower than the second energy density.
[0089] In the above embodiment, it is understood that when the laser irradiates the surface of the initial silicon material layer 105, the surface of the initial silicon material layer 105 absorbs the laser energy, causing the temperature of the initial silicon material layer 105 to rise above its melting point. As a result, the initial silicon material layer 105 begins to partially melt, and the heat gradually diffuses in the direction Z away from the laser, causing the liquid silicon / amorphous silicon interface to move downward, ultimately molten the entire initial silicon material layer 105. Furthermore, based on the formation of the silicon film layer 114, during the above laser processing step, the silicon film layer 114 will also gradually melt until the entire layer is molten.
[0090] S105 : with reference to FIG. 11 to FIG. 13 , the initial silicon material layer 105 after the laser treatment is cooled to recrystallize the initial silicon material layer 105 to form a silicon material layer 107 .
[0091] In some embodiments, after the silicon film layer 114 is formed, in the step of recrystallizing the initial silicon material layer 105 , the molten silicon film layer 114 and the molten initial silicon material layer 105 are recrystallized together.
[0092] It can be understood that, with reference to Figures 12 and 13, after the layer to be crystallized 106 is formed, the laser processing is stopped and the layer to be crystallized 106 is cooled. At this time, the underlying silicon 104 located at the bottom of the blind hole 110 (see Figure 5) serves as a seed layer, and the layer to be crystallized 106 is recrystallized with the underlying silicon 104 as the seed layer until the layer to be crystallized 106 is completely recrystallized to form the silicon material layer 107. It should be noted that in Figure 12, the initial silicon material layer 105 in a molten state and the silicon film layer 114 in a molten state are collectively depicted as the layer to be crystallized 106, and in Figure 13, the layer to be crystallized 106 after complete recrystallization is depicted as the silicon material layer 107.
[0093] In some embodiments, cooling the initial silicon material layer 105 after the laser treatment includes blowing an inert gas toward the initial silicon material layer 105 after the laser treatment. The inert gas may include at least one of nitrogen and argon.
[0094] In some embodiments, the pressure of the inert gas ranges from 0.2 MPa to 1 MPa.
[0095] In other embodiments, the cooling process of the initial silicon material layer 105 after the laser treatment may be: allowing the initial silicon material layer 105 after the laser treatment to cool naturally.
[0096] In some embodiments, the silicon material layer 107 includes at least one of single crystal silicon or polycrystalline silicon, and the defect density of the silicon material layer 107 is lower than the defect density of the initial silicon material layer 105. This facilitates improving the conductivity of capacitor contact layers, bit line contact layers, or other electrical contact layers subsequently fabricated using the silicon material layer 107 as a raw material, ensuring a lower defect density.
[0097] It can be understood that since the melting point of the initial silicon material layer 105 is lower than the melting point of the underlying silicon 104, the initial silicon material layer 105 is in a molten state when heated, which can make the underlying silicon 104 in a non-molten state. Then, during the cooling and recrystallization process of the molten initial silicon material layer 105, the molten initial silicon material layer 105 can use the underlying silicon 104 as a seed layer and recrystallize along the crystal orientation of the crystal in the underlying silicon 104, so that the finally formed silicon material layer 107 includes at least one of single crystal silicon or polycrystalline silicon, which is beneficial to improve the density of the silicon material layer 107.
[0098] In some embodiments, after forming the silicon material layer 107, the manufacturing method of the semiconductor structure may further include: referring to Figure 13, performing chemical mechanical polishing on the silicon material layer 107; referring to Figure 13, back-etching the silicon material layer 107, and the remaining silicon material layer 107 serves as an electrical contact layer, and the electrical contact layer is located in a partial depth blind hole 110 (refer to Figure 5).
[0099] It should be noted that FIG. 13 schematically shows the silicon material layer 107 after chemical mechanical polishing.
[0100] In summary, on the one hand, using a laser to heat the initial silicon material layer 105 is beneficial to avoid the presence of voids or gaps in the silicon material layer 107 formed by the subsequent melting and recrystallization of the initial silicon material layer 105, thereby improving the density and conductivity of the silicon material layer 107; on the other hand, before forming the initial silicon material layer 105, a bottom silicon 104 is formed at the bottom of the blind hole 110 to provide better recrystallization conditions for the initial silicon material layer 105, thereby facilitating the formation of a silicon material layer 107 with a lower defect density; on the other hand, since the laser can achieve the effect of local heating and the laser can achieve the effect of rapid temperature increase, when the initial silicon material layer 105 is in a high-temperature molten state by the laser, the temperature effect generated by the laser on other structures adjacent to the initial silicon material layer 105 can be ignored, and will not adversely affect other properties of the semiconductor structure. Therefore, the manufacturing method of the semiconductor structure provided by an embodiment of the present disclosure improves the density and conductivity of the formed silicon material layer 107 while avoiding the process of forming the silicon material layer 107 from adversely affecting other parts of the semiconductor structure.
[0101] Another embodiment of the present disclosure further provides a semiconductor structure formed by the manufacturing method provided in one embodiment of the present disclosure. The semiconductor structure provided in another embodiment of the present disclosure will be described in detail below with reference to the accompanying drawings. It should be noted that any parts that are identical or corresponding to the aforementioned embodiments will not be repeated here.
[0102] 14 , the semiconductor structure includes: a substrate 100 having at least one blind hole 110 (see FIG5 ); and a silicon material layer 107 located at least at the bottom and a portion of the sidewall of the blind hole 110 , wherein the defect density of the silicon material layer 107 is lower than that of amorphous silicon.
[0103] In some embodiments, the silicon material layer 107 includes at least one of single crystal silicon or polycrystalline silicon. When the silicon material layer 107 is subsequently used as a capacitor contact layer, a bit line contact layer or other electrical contact layer, it is beneficial to improve the conductive performance of the film layer and ensure that it has a lower defect density, thereby helping to improve the yield of the semiconductor structure and device performance.
[0104] In some embodiments, with reference to Figures 5 and 14, the base 100 may include: a substrate 101; a plurality of parallel bit lines 102 located on the substrate 101 and a dielectric layer 103 located between adjacent bit lines 102, the dielectric layer 103 and the bit lines 102 together enclosing a plurality of blind holes 110; and a silicon material layer 107 located in a partial depth of the blind holes 110 along an extension direction Z of the blind holes 110.
[0105] It should be noted that FIG14 is only a specific application scenario of the finally formed silicon material layer 107 . In actual applications, the silicon material layer 107 formed by the manufacturing method provided in an embodiment of the present disclosure includes but is not limited to being used as a capacitor contact layer.
[0106] In summary, in the semiconductor structure formed by the manufacturing method provided in one embodiment of the present disclosure, the defect density of the silicon material layer 107 is lower than the defect density of amorphous silicon, which is beneficial to improving the yield of the semiconductor structure and device performance.
[0107] Those skilled in the art will appreciate that the above-described embodiments are specific examples for implementing the present disclosure, and in actual applications, various changes may be made to them in form and detail without departing from the spirit and scope of the embodiments of the present disclosure. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the embodiments of the present disclosure. Therefore, the scope of protection of the embodiments of the present disclosure shall be based on the scope defined in the claims.
Claims
1. A method for manufacturing a semiconductor structure, comprising: Providing a substrate (100), wherein the substrate (100) has at least one blind hole (110); Using an epitaxial growth process to form a bottom layer of silicon (104) at least at the bottom of the blind hole (110); forming an initial silicon material layer (105) that fills the remaining blind holes (110), wherein the melting point of the initial silicon material layer (105) is lower than the melting point of the bottom silicon (104); Processing the initial silicon material layer (105) with a laser so that the initial silicon material layer (105) is melted; The initial silicon material layer (105) after the laser treatment is cooled to allow the initial silicon material layer (105) to recrystallize, thereby forming a silicon material layer (107).
2. The manufacturing method according to claim 1, wherein: In the step of processing the initial silicon material layer (105) with laser, voids (115) in the initial silicon material layer (105) are eliminated.
3. The manufacturing method according to claim 1 or 2, wherein: The silicon material layer (107) includes at least one of single crystal silicon or polycrystalline silicon, and the defect density of the silicon material layer (107) is lower than the defect density of the initial silicon material layer (105).
4. The manufacturing method according to any one of claims 1 to 3, wherein: The working mode of the laser includes pulsed laser, and the processing of the initial silicon material layer (105) with the laser includes: The initial silicon material layer (105) located in the blind hole (110) is sequentially subjected to N pulse laser treatments to achieve local heating of the initial silicon material layer (105) located in the blind hole (110), wherein N is a positive integer, and as the number of times increases, the energy density of the pulse laser remains unchanged or increases.
5. The manufacturing method according to claim 4, wherein: The energy density of the pulse laser is in the range of 0.3 mJ / cm2 to 0.7 mJ / cm2.
6. The manufacturing method according to claim 4 or 5, wherein: The wavelength of the pulse laser is 532 nm, and the pulse width of the pulse laser is 10 ns.
7. The manufacturing method according to any one of claims 4 to 6, wherein: As the number of times increases, the energy density of the pulsed laser remains unchanged at first and then gradually increases. When the energy density of the pulsed laser remains unchanged, the initial silicon material layer (105) is preheated, and when the energy density of the pulsed laser increases, the melting of the initial silicon material layer (105) is accelerated.
8. The manufacturing method according to any one of claims 1 to 7, wherein: In the step of processing the initial silicon material layer (105) with laser, the maximum value of the temperature of the initial silicon material layer (105) is 1100° C. to 1400° C.
9. The manufacturing method according to any one of claims 1 to 7, wherein: In the step of processing the initial silicon material layer (105) with laser, the maximum depth of the melted initial silicon material layer (105) along the depth direction (Z) of the blind hole (110) is 400nm to 500nm.
10. The manufacturing method according to claim 1, wherein: The working mode of the laser includes continuous laser, and the processing of the initial silicon material layer (105) with the laser includes: The continuous laser is used to scan the substrate (100) and the initial silicon material layer (105), and the energy density of the continuous laser when scanning the substrate (100) is a first energy density, and the energy density of the continuous laser when scanning the initial silicon material layer (105) is a second energy density, and the first energy density is lower than the second energy density.
11. The manufacturing method according to any one of claims 1 to 10, wherein: Before forming the bottom silicon (104), the method further includes: cleaning the substrate (100).
12. The manufacturing method according to any one of claims 1 to 11, wherein: In the step of forming a bottom silicon layer (104) at least at the bottom of the blind hole (110) by using an epitaxial growth process, a silicon film layer (114) is formed on the side wall of the blind hole (110); The bottom silicon (104) and the silicon film layer (114) together enclose a contact hole (120), and the forming of an initial silicon material layer (105) that fills the blind hole (110) comprises: forming an initial silicon material layer (105) that fills the contact hole (120); In the step of using laser to process the initial silicon material layer (105), the silicon film layer (114) is also melted; In the step of recrystallizing the initial silicon material layer (105), the silicon film layer (114) in a molten state and the initial silicon material layer (105) in a molten state are recrystallized together.
13. The manufacturing method according to any one of claims 1 to 12, wherein: Along the depth direction (Z) of the blind hole (110), the thickness of the bottom silicon (104) ranges from 1 nm to 5 nm.
14. The manufacturing method according to any one of claims 1 to 13, wherein: The cooling process comprises: blowing an inert gas toward the initial silicon material layer (105) after the laser treatment, wherein the pressure of the inert gas has a numerical range of 0.2 MPa to 1 MPa.
15. The manufacturing method according to any one of claims 1 to 14, wherein: The step of providing the substrate (100) comprises: Providing a substrate (101); A plurality of bit lines (102) arranged in parallel and a dielectric layer (103) located between adjacent bit lines (102) are formed on the substrate (101), wherein the dielectric layer (103) and the bit lines (102) together enclose a plurality of blind holes (110), and the blind holes (110) are capacitor contact holes; Alternatively, a plurality of grooves (112) for forming the bit lines (102) are formed in the substrate (101), the blind holes (110) are provided in the grooves (112), and the blind holes (110) are used to form the bit line contact layers (122).
16. A semiconductor structure comprising: A substrate (100), wherein the substrate (100) has at least one blind hole (110); The silicon material layer (107) is at least located at the bottom and part of the sidewall of the blind hole (110), and the defect density of the silicon material layer (107) is lower than the defect density of amorphous silicon.
17. The semiconductor structure of claim 16, wherein: The substrate (100) comprises: A substrate (101); A plurality of bit lines (102) arranged in parallel on the substrate (101) and a dielectric layer (103) located between adjacent bit lines (102), wherein the dielectric layer (103) and the bit lines (102) together enclose a plurality of blind holes (110); Along the depth direction (Z) of the blind hole (110), the silicon material layer (107) is located in a partial depth of the blind hole (110).
18. The semiconductor structure of claim 17, wherein: The bit line (102) comprises a plurality of bit line contact layers (122) and a bit line body (132) that is in contact with the plurality of bit line contact layers (122); the bit line contact layers (122) are located in the blind holes (110) and the bit line contact layers (122) correspond to the blind holes (110) one by one; and the bit line body (132) is located on the top surface of the bit line contact layers (122).
19. The semiconductor structure of claim 17, wherein: The bit line (102) comprises a bit line contact layer (122), a diffusion barrier layer (142), a bit line conductive layer (152), a first bit line protection layer (162) and a second bit line protection layer (172); one bit line (102) may comprise a plurality of bit line contact layers (122); the plurality of bit line contact layers (122) in one bit line (102) are all in contact with and connected to the same diffusion barrier layer (142); the first bit line protection layer (162) and the second bit line protection layer (172) jointly surround the side wall and top surface of the bit line (102).
20. The semiconductor structure of claim 19, wherein: The substrate (101) may include an active area (111), a shallow trench isolation structure (121) and an isolation layer (131); the bit line contact layer (122) is in contact with the active area (111); the isolation layer (131) is provided between the diffusion barrier layer (142) that is not in contact with the bit line contact layer (122) and the shallow trench isolation structure (121); and the blind hole (110) exposes a portion of the active area (111) and the shallow trench isolation structure (121).
Citation Information
Patent Citations
Method for forming long seamless filling amorphous silicon groove
CN103094075A
Super junction depth groove filling process
CN103855002A
Method for filling groove to form contact
CN108962894A
Indirect heating method employing laser
CN110476229A
Method of eliminating voids in W plugs